An aramid composite insulating paper based on highly thermally conductive nanofibers, its preparation method and application
By constructing a three-dimensional multi-level micro-nano assembly structure of boron nitride nanotubes/meta-aramid fibers through electrospinning and hot pressing processes, the problems of low thermal conductivity and poor flexibility of aramid insulating paper are solved, and precise control of thermal conductivity and porosity is achieved, providing a key insulating material for high power density power electronic equipment.
Patent Information
- Application Number
- CN202611206067.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-10
- Publication Date
- 2026-11-17
AI Technical Summary
Existing aramid insulating paper has low thermal conductivity, and it is difficult to maintain flexibility and insulation properties while improving thermal conductivity. Traditional processes make it difficult to achieve precise control of porosity and orderly arrangement of thermally conductive fillers.
Boron nitride nanotube/meta-aramid fiber composite nanofibers were pre-prepared using electrospinning technology. A three-dimensional multi-level micro-nano assembly structure was constructed through wet papermaking and hot pressing. The interfacial affinity was enhanced by combining polyvinylpyrrolidone modifier, thereby achieving the directional arrangement of thermally conductive fillers and precise control of porosity.
It significantly improves the thermal conductivity of aramid insulating paper while maintaining excellent tensile strength and electrical insulation properties, meeting the thermal management requirements of high power density power electronic equipment.
Smart Images

Figure CN123108993A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of insulating materials technology, specifically to an aramid composite insulating paper based on highly thermally conductive nanofibers, its preparation method, and its application. Background Technology
[0002] With the continuous evolution of new energy equipment, ultra-high voltage power transmission, and high-frequency power electronic systems towards higher power density and lighter weight, the heat dissipation requirements of key equipment such as motor drive systems, converter transformers, and high-power radio frequency devices are increasing exponentially. The thermal management reliability of their internal insulation components has become a core factor restricting the overall system lifespan and safety margin. Meta-aramid PMIA insulating paper, with its excellent heat resistance, electrical insulation strength, chemical stability, and good flexibility, occupies an important position in power equipment insulation systems, especially suitable for harsh service conditions involving high voltage, high temperature, and complex mechanical stress coupling. However, aramid molecular chains have a rigid aromatic ring backbone, resulting in a lack of interchain phonon transport channels, and their intrinsic thermal conductivity is generally below 0.3 W·m. - ¹·K - ¹ This leads to the easy local accumulation of heat inside the insulating paper, thereby accelerating the thermal aging of the material and inducing insulation failure.
[0003] Introducing highly thermally conductive inorganic fillers into aramid insulating paper to construct a composite thermally conductive system is currently the mainstream technical approach to improve its heat dissipation performance. Boron nitride nanotubes (BNNTs), as one-dimensional hollow tubular thermally conductive materials, possess extremely high axial thermal conductivity and excellent electrical insulation properties, making them a highly promising component for enhancing thermal conductivity. However, using boron nitride nanotubes as thermally conductive fillers faces the following problems: 1) BNNTs have a smooth surface and strong chemical inertness, resulting in extremely weak interfacial bonding with the aramid matrix. Direct blending makes it difficult to achieve uniform dispersion, easily leading to severe agglomeration. This not only fails to form an effective thermal conductive pathway but also introduces additional thermal resistance due to strong phonon scattering at the interface, making it difficult to effectively release the performance advantages of high thermal conductivity fillers on a macroscopic scale. 2) Aramid insulating paper produced by traditional papermaking processes has a natural micron-scale pore structure. These pores are not only key structural units for achieving electrical isolation and structural flexibility but also "break-circuit" nodes for heat conduction. How to transform "pore barriers" into "heat conduction channels" through orderly structural design while maintaining reasonable porosity to preserve the flexibility, deformation adaptability, and dielectric properties of insulating paper has long been an unresolved structural design contradiction. 3) The improvement of thermal conductivity and the control of pore structure are fundamentally contradictory under the traditional process framework. Increasing the filler content helps to improve thermal conductivity, but it inevitably exacerbates the rigidity and density of the fiber network, leading to a sharp decrease in the flexibility of the insulating paper and an increase in brittleness, making it difficult to meet the engineering processing requirements of actual wrapping, bending, etc. Conversely, if more pores are retained to maintain flexibility, the heat conduction channels cannot be effectively connected. This trade-off between multiple properties of "thermal conductivity-insulation-mechanical properties" constitutes a performance barrier that is difficult for existing technologies to overcome.
[0004] Although existing studies have shown that the densification of aramid insulating paper can be controlled through hot pressing, there is still no effective process solution for achieving precise and stable control of porosity over a wide range while simplifying process variables, and simultaneously inducing thermally conductive fillers to form an orderly orientation arrangement in key spatial positions. Summary of the Invention
[0005] This invention addresses the problems existing in the prior art by providing an aramid composite insulating paper based on highly thermally conductive nanofibers, its preparation method, and its application.
[0006] The technical solution adopted in this invention is: a method for preparing aramid composite insulating paper based on highly thermally conductive nanofibers, comprising the following steps: Step 1: Add boron nitride nanotube dispersion to meta-aramid fiber dispersion, stir and react thoroughly to obtain spinning solution, and use electrospinning to obtain composite nanofiber membrane; Step 2: The composite nanofiber membrane is sheared to obtain composite nanofiber fragments; Step 3: The composite nanofiber fragments, aramid precipitated fibers, and aramid chopped fibers obtained in Step 2 are mixed and dispersed in a solvent, and then wet-processed, dehydrated, and dried to obtain aramid thermally conductive base paper substrate; the composite nanofiber fragments, aramid precipitated fibers, and aramid chopped fibers are 15-40 parts, 20-45 parts, and 30-50 parts by weight, respectively; Step 4: The aramid thermally conductive base paper substrate obtained in Step 3 is subjected to hot pressing to obtain the desired aramid composite insulating paper; wherein the hot pressing temperature is the glass transition temperature of meta-aramid.
[0007] Furthermore, the preparation process of the intermediate aramid fiber dispersion in step 1 is as follows: Meta-aramid fibers and lithium chloride were added to a solvent and stirred thoroughly under heating conditions to obtain a meta-aramid fiber dispersion. The mass ratio of meta-aramid fiber to lithium chloride is 2–4:1, the heating temperature is 140 °C, and the stirring speed is 800 r / min.
[0008] Furthermore, the preparation process of the boron nitride nanotube dispersion is as follows: Boron nitride nanotubes and polyvinylpyrrolidone are added to a solvent, and a boron nitride nanotube dispersion is obtained by stirring and ultrasonic dispersion. The mass of polyvinylpyrrolidone accounts for 5% of the mass of boron nitride nanotubes, the stirring time is 2 h, and the ultrasonic treatment is 30 min; The diameter of boron nitride nanotubes ranges from 30 to 50 nm, and the average length is 10 μm.
[0009] Furthermore, the mass ratio of the boron nitride nanotubes to the meta-aramid fibers is 5–25:100.
[0010] Furthermore, in step 1, the heating temperature is 60 ℃ and the stirring reaction time is 12 h.
[0011] Furthermore, the voltage in the electrospinning is 15–25 kV, the collector rotation speed is 800 rpm, the collector is a rotating drum structure, the distance between the needle and the collector is 10–15 cm, and the spinning solution flow rate is 0.3–0.8 mL / h.
[0012] Furthermore, in step 4, the hot pressing temperature is 260–290°C, the hot pressing pressure is 5–10 MPa, and the hot pressing time is 30–60 s.
[0013] A composite insulating paper based on highly thermally conductive nanofibers is disclosed. The composite insulating paper uses chopped aramid fibers as a skeleton network and precipitated aramid fibers as a bonding component to wrap the fiber intersection nodes of the skeleton network. Composite nanofiber fragments are dispersed and interwoven in the macroscopic pores formed by the interlacing of chopped aramid fibers to form a three-dimensional multi-level micro-nano assembly structure. The composite nanofiber fragments are boron nitride nanotubes / meta-aramid fibers.
[0014] Furthermore, in the aramid composite insulating paper, the composite nanofiber fragments, aramid precipitated fibers, and aramid chopped fibers are present in weight proportions of 15-40 parts, 20-45 parts, and 30-50 parts, respectively; the mass ratio of boron nitride nanotubes to meta-aramid fibers in the composite nanofiber fragments is 5-25:100.
[0015] An application of aramid composite insulating paper based on highly thermally conductive nanofibers, wherein the aramid composite insulating paper is used as an insulating component of electronic devices.
[0016] The beneficial effects of this invention are: The composite nanofibers (BNNT@PMIA) obtained in this invention are obtained by electrospinning, with boron nitride nanotubes pre-oriented and arranged inside the nanofibers. The composite nanofibers are then introduced into the aramid insulating paper system as building blocks. This "pre-orientation-reassembly" strategy avoids the inherent defects of high aspect ratio fillers in traditional blending processes, which are difficult to disperse uniformly and have random orientation in the papermaking system. It ensures that BNNTs are highly axially oriented inside the nanofibers, providing a structural basis for long-range low-scattering transmission of phonons. The resulting composite insulating paper has a "three-level multi-scale micro-nano assembly structure" with micron-sized aramid chopped fibers as the spatial load-bearing skeleton, aramid precipitated fibers as the adhesive, and composite nanofibers as interwoven and nested functional units. By fully leveraging the synergistic functions of each component, the chopped fiber skeleton ensures the overall mechanical support and dimensional stability of the insulating paper, while the precipitated fibers act as a "structural adhesive" to achieve firm bonding at the fiber intersections. The composite nanofibers interspersed between the skeleton pores not only endow the material with thermal conductivity but also fill the structural gaps between the skeletons at the nanoscale, forming a continuous physical and functional network with multiple scales.
[0017] This invention utilizes a composite insulating paper that undergoes precise hot pressing at the glass transition temperature of meta-aramid fibers, achieving a wide range of adjustable porosity from 5% to 45%. At the glass transition temperature, aramid precipitated fibers and composite nanofibers undergo localized micro-melting and softening at the contact interface. The flowing nano-units selectively fill micron-sized pores under pressure, enabling precise control of the pore structure to meet the differentiated requirements of flexibility, impregnation, and dielectric properties for various applications. Furthermore, this process drives BNNTs to undergo orientation rearrangement at fiber crosslinking nodes, constructing a continuous thermally conductive "highway" across the fiber interface. This fundamentally solves the inherent contradiction in traditional technologies where thermal conductivity, porosity, and mechanical properties are compromised.
[0018] This invention uses polyvinylpyrrolidone (PVP) as a surface coating modifier for BNNT. The PVP molecular chains are wrapped around the BNNT surface through non-covalent bonding, which enhances the interfacial affinity between BNNT and the PMIA matrix, effectively suppresses the aggregation tendency of BNNT, and forms a flexible phonon coupling transition layer at the filler-matrix interface, reducing phonon mismatch scattering at the interface and lowering the interfacial thermal resistance.
[0019] The composite insulating paper obtained by this invention significantly improves thermal conductivity while maintaining excellent tensile strength, flexibility, and electrical insulation properties, providing a key material solution with significant engineering application value for the integrated thermal management and insulation requirements of high power density power electronic equipment. Attached Figure Description
[0020] Figure 1 This is a schematic diagram of the process for preparing aramid composite insulating paper based on highly thermally conductive nanofibers according to the present invention.
[0021] Figure 2 This is a transmission electron microscope (TEM) image of BNNT used in an embodiment of the present invention.
[0022] Figure 3 This is a surface SEM image of the aramid composite insulating paper obtained in Example 3 of the present invention.
[0023] Figure 4 This is a schematic diagram of the thermal conductivity of the aramid composite insulating paper obtained in Examples 1, 2, and 3 and Comparative Examples 1 and 2 of the present invention.
[0024] Figure 5 This is a schematic diagram showing the porosity of the aramid composite insulating paper obtained in Examples 1, 2, and 3 and Comparative Examples 1 and 2 of the present invention.
[0025] Figure 6 This is a schematic diagram showing the mechanical properties of the aramid composite insulating paper obtained in Examples 1, 2, and 3 and Comparative Examples 1 and 2 of the present invention. Detailed Implementation
[0026] The present invention will be further described below with reference to the accompanying drawings and specific embodiments.
[0027] like Figure 1 As shown, a method for preparing aramid composite insulating paper based on highly thermally conductive nanofibers includes the following steps: Step 1: Add the boron nitride nanotube dispersion to the meta-aramid fiber dispersion, stir thoroughly to obtain a spinning solution, and then use electrospinning to obtain a composite nanofiber membrane; the mass ratio of boron nitride nanotubes to meta-aramid fibers is 5–25:100. The heating temperature is 60 ℃, and the stirring reaction time is 12 h.
[0028] The preparation process of meta-aramid fiber dispersion is as follows: Meta-aramid fibers and lithium chloride were added to a solvent and stirred thoroughly under heating conditions to obtain a meta-aramid fiber dispersion. The mass ratio of meta-aramid fiber to lithium chloride is 2–4:1, the heating temperature is 140 °C, and the stirring speed is 800 r / min.
[0029] The preparation process of boron nitride nanotube dispersion is as follows: Boron nitride nanotubes and polyvinylpyrrolidone are added to a solvent, and a boron nitride nanotube dispersion is obtained by stirring and ultrasonic dispersion. The mass of polyvinylpyrrolidone accounts for 5% of the mass of boron nitride nanotubes, the stirring time is 2 h, and the ultrasonic treatment is 30 min; The diameter of boron nitride nanotubes ranges from 30 to 50 nm, and the average length is 10 μm.
[0030] In electrospinning, the voltage is 15–25 kV, the collector speed is 800 rpm, the collector is a rotating drum structure, the distance between the needle and the collector is 10–15 cm, and the spinning solution flow rate is 0.3–0.8 mL / h.
[0031] Step 2: The composite nanofiber membrane is sheared to obtain composite nanofiber fragments; Step 3: The composite nanofiber fragments, aramid precipitated fibers and aramid chopped fibers obtained in Step 2 are mixed and dispersed in a solvent, and then wet-processed, dehydrated and dried to obtain aramid thermally conductive base paper substrate; the composite nanofiber fragments, aramid precipitated fibers and aramid chopped fibers are 15-40 parts, 20-45 parts and 30-50 parts by weight, respectively.
[0032] The wet papermaking process is as follows: Composite nanofiber fragments and chopped aramid fibers were mixed with water and placed in a standard fiber dissociator for dissociation at 10,000 rpm. Then, pulped and dissociated aramid precipitated fibers were added, and dissociation was continued for another 1,000 rpm. The mixed pulp was then poured into a paper forming machine for wet forming and dried for 10 minutes to obtain the prepared paper.
[0033] Step 4: The aramid thermally conductive base paper obtained in Step 3 is subjected to hot pressing to obtain the desired aramid composite insulating paper; wherein the hot pressing temperature is the glass transition temperature of meta-aramid. The hot pressing temperature is 260-290℃, the hot pressing pressure is 5-10 MPa, and the hot pressing time is 30-60 s.
[0034] The aramid composite insulating paper uses chopped aramid fibers as a backbone network, with precipitated aramid fibers as a binder component wrapped around the fiber intersections of the backbone network. Composite nanofiber fragments are dispersed and interwoven within the macroscopic pores formed by the interlacing of chopped aramid fibers, forming a three-dimensional, multi-level micro-nano assembly structure. The composite nanofiber fragments are boron nitride nanotubes / meta-aramid fibers. After thermo-pressing to control the glass transition temperature, the aramid precipitated fibers and BNNT@PMIA nanofibers undergo localized micro-melting and softening at the contact interface. The flowing nano-units selectively fill the micropores, making the internal porosity of the aramid composite insulating paper adjustable within the range of 5–45%, constructing a continuous thermally conductive pathway and a micro-nano composite dielectric barrier.
[0035] Example 1 A method for preparing aramid composite insulating paper based on highly thermally conductive nanofibers includes the following steps: Step 1: Add 6 g of meta-aramid fiber PMIA (using commercially available products) and 2 g of lithium chloride to 50 mL of DMAc, and then stir the mixture at 140 °C and 800 r / min for 12 h to obtain a PMIA dispersion.
[0036] 0.9 g of boron nitride nanotubes (BNNT) and 0.045 g of polyvinylpyrrolidone (PVP) powder were added to a mixture of 3.2 mL of DMAc and 1.6 mL of acetone. After stirring for 2 h, the mixture was sonicated for 30 min to obtain a BNNT dispersion. The BNNT tubes had a diameter of 30–50 nm and a length >10 μm.
[0037] The BNNT dispersion was added to the PMIA dispersion and stirred continuously at 60 °C for 12 h to obtain the BNNT@PMIA composite spinning solution.
[0038] The BNNT@PMIA composite spinning solution was placed in an electrospinning machine with an applied voltage of 20 kV, an ambient temperature of 35 ℃, a distance of 12 cm between the needle and the collector, a spinning solution flow rate of 0.5 mL / h, and a collector consisting of a rotating drum structure with a rotation speed of 800 rpm. Electrospinning was then performed to obtain the BNNT@PMIA composite nanofiber membrane.
[0039] Step 2: The BNNT@PMIA composite nanofiber membrane was subjected to cyclic shearing in a high-shear homogenizer to obtain composite nanofiber fragments (shearing at 10000 r / min for 60s each time, with a 30s interval, for 3 cycles).
[0040] Step 3: Mix the composite nanofiber fragments and aramid chopped fibers (using aramid 1313) with water, and place the mixture in a standard fiber dissociator to loosen it at 10,000 rpm. Add the pulped and loosened aramid precipitated fibers (using commercially available products), and continue loosening for 1,000 rpm. Then pour the mixed slurry into a paper forming machine for wet forming, and dry for 10 minutes to obtain the aramid thermally conductive base paper substrate. The mass ratio of composite nanofiber fragments, aramid chopped fibers, and aramid precipitated fibers is 15:50:35.
[0041] Step 4: The aramid thermally conductive base paper substrate obtained in Step 3 is hot-pressed at a temperature of 280 ℃, a pressure of 10 MPa, and a time of 60 s. After cooling, aramid composite insulating paper is obtained.
[0042] Example 2 A method for preparing aramid composite insulating paper based on highly thermally conductive nanofibers includes the following steps: Step 1: Add 6 g of meta-aramid fiber PMIA and 3 g of lithium chloride to 50 mL of DMAc, and then stir the mixture at 140 °C and 800 r / min for 12 h to obtain PMIA dispersion.
[0043] 1.5 g of boron nitride nanotubes (BNNTs) and 0.075 g of polyvinylpyrrolidone (PVP) powder were added to a mixture of 3.2 mL of DMAc and 1.6 mL of acetone. The mixture was stirred for 2 h and then sonicated for 30 min to obtain a BNNT dispersion. The BNNTs had a diameter of 30–50 nm and a length >10 μm.
[0044] The BNNT dispersion was added to the PMIA dispersion and stirred continuously at 60 °C for 12 h to obtain the BNNT@PMIA composite spinning solution.
[0045] The BNNT@PMIA composite spinning solution was placed in an electrospinning machine with an applied voltage of 25 kV, an ambient temperature of 35 ℃, a distance of 10 cm between the needle and the collector, a spinning solution flow rate of 0.3 mL / h, and a collector consisting of a rotating drum structure with a rotation speed of 800 rpm. Electrospinning was then performed to obtain the BNNT@PMIA composite nanofiber membrane.
[0046] Step 2: The BNNT@PMIA composite nanofiber membrane was subjected to cyclic shearing in a high-shear homogenizer to obtain composite nanofiber fragments (shearing at 10000 r / min for 60s each time, with a 30s interval, for 3 cycles).
[0047] Step 3: Mix the composite nanofiber fragments and aramid chopped fibers with water, and decompose them in a standard fiber disintegrator at 10,000 rpm. Add the pulped and decomposed aramid precipitated fibers, and continue decomposition for 1,000 rpm. Then, pour the mixed slurry into a paper forming machine for wet forming, and dry for 10 minutes to obtain the aramid thermally conductive base paper substrate. The mass ratio of composite nanofiber fragments, aramid chopped fibers, and aramid precipitated fibers is 28:37:35.
[0048] Step 4: The aramid thermally conductive base paper substrate obtained in Step 3 is hot-pressed at a temperature of 260 ℃, a pressure of 5 MPa, and a time of 40 s. After cooling, aramid composite insulating paper is obtained.
[0049] Example 3 A method for preparing aramid composite insulating paper based on highly thermally conductive nanofibers includes the following steps: Step 1: Add 6 g of meta-aramid fiber PMIA and 1.5 g of lithium chloride to 50 mL of DMAc, and then stir the mixture at 140 °C and 800 r / min for 12 h to obtain a PMIA dispersion.
[0050] 0.3 g of boron nitride nanotubes (BNNT) and 0.015 g of polyvinylpyrrolidone (PVP) powder were added to a mixture of 3.2 mL of DMAc and 1.6 mL of acetone. After stirring for 2 h, the mixture was sonicated for 30 min to obtain a BNNT dispersion. The BNNT tubes had a diameter of 30–50 nm and a length >10 μm.
[0051] The BNNT dispersion was added to the PMIA dispersion and stirred continuously at 60 °C for 12 h to obtain the BNNT@PMIA composite spinning solution.
[0052] The BNNT@PMIA composite spinning solution was placed in an electrospinning machine with an applied voltage of 15 kV, an ambient temperature of 25 ℃, a distance of 15 cm between the needle and the collector, a spinning solution flow rate of 0.8 mL / h, and a collector consisting of a rotating drum structure with a rotation speed of 800 rpm. Electrospinning was then performed to obtain the BNNT@PMIA composite nanofiber membrane.
[0053] Step 2: The BNNT@PMIA composite nanofiber membrane was subjected to cyclic shearing in a high-shear homogenizer to obtain composite nanofiber fragments (shearing at 10000 r / min for 60s each time, with a 30s interval, for 3 cycles).
[0054] Step 3: Mix the composite nanofiber fragments and aramid chopped fibers with water, and decompose them in a standard fiber disintegrator at 10,000 rpm. Add the pulped and decomposed aramid precipitated fibers, and continue decomposition for 1,000 rpm. Then, pour the mixed slurry into a paper forming machine for wet forming, and dry for 10 minutes to obtain the aramid thermally conductive base paper substrate. The mass ratio of composite nanofiber fragments, aramid chopped fibers, and aramid precipitated fibers is 40:30:30.
[0055] Step 4: The aramid thermally conductive base paper substrate obtained in Step 3 is hot-pressed at a temperature of 290 ℃, a pressure of 8 MPa, and a time of 30 s. After cooling, aramid composite insulating paper is obtained.
[0056] Comparative Example 1 Comparative Example 1 is pure aramid insulating paper, prepared by the following method: Aramid chopped fibers were mixed with water and subjected to a standard fiber dissociation apparatus for 10,000 revolutions per minute. Then, beaten and dissociated aramid precipitated fibers were added, and the dissociation was continued for another 1,000 revolutions per minute. The mixed slurry was then poured into a paper forming apparatus for wet forming, and dried for 10 minutes to obtain aramid base paper. The mass ratio of aramid chopped fibers to aramid precipitated fibers was 55:45.
[0057] Aramid base paper substrate is heated at 280 ℃, with a hot pressing pressure of 10 MPa and a hot pressing time of 60 s, and then cooled to obtain aramid composite insulating paper.
[0058] Comparative Example 2 The other steps in this comparative example are the same as in Example 3, except that the hot pressing temperature is 100 ℃, the hot pressing pressure is 10 MPa, the hot pressing time is 60 s, and after cooling, aramid composite insulating paper is obtained.
[0059] The thermal conductivity of the aramid composite insulating papers obtained in Examples 1, 2, and 3, and Comparative Examples 1 and 2 was tested. The thermal diffusivity in the planar direction of each sample was measured using the laser flare method (LFA) and converted into thermal conductivity. The results are as follows: Figure 4 As shown in the figure, the thermal conductivity of the composite insulating paper obtained in the embodiment is significantly better than that of Comparative Example 1 and Comparative Example 2.
[0060] The increased content of composite nanofiber fragments leads to a significant increase in the thermal conductivity of the composite insulating paper. This is because the electrospinning process pre-orients BNNTs along the axial direction within the nanofibers. After wet papermaking, these pre-oriented thermally conductive units are interspersed among the macroscopic pores of the aramid chopped fiber skeleton, initially forming thermally conductive pathways spanning multiple scales. Subsequent hot-pressing control near the glass transition temperature (280℃) further drives the BNNT@PMIA nanofibers to undergo local micro-melting flow at the contact nodes, causing the BNNTs to rearrange with the matrix orientation and achieve a "seamless" thermal connection between the fiber interfaces, constructing a continuous phonon transport "highway".
[0061] As can be seen from Example 3 and Comparative Example 2, without sufficient hot pressing, the thermal conductivity was significantly lower than that of Example 3, despite having the same filler content. This indicates that thermally induced structural reconstruction near the glass transition temperature is a key process step in activating the connectivity of the thermally conductive network. Furthermore, the non-covalent coating of BNNT with PVP effectively improved its interfacial compatibility with the PMIA matrix, reduced interfacial phonon mismatch scattering, and further lowered the interfacial thermal resistance, collectively contributing to a significant improvement in thermal conductivity.
[0062] The porosity of the composite insulating paper in Examples 1, 2, and 3, and Comparative Examples 1 and 2 was determined using mercury intrusion porosimetry. The results are as follows: Figure 5 As shown in the figure, the porosity of the composite insulating paper prepared in the embodiments of the present invention can be precisely controlled within a wide range (approximately 5% to 45%). Furthermore, as the BNNT@PMIA nanofiber content increases and the hot-pressing parameters remain constant, the porosity exhibits a monotonically decreasing trend. This is consistent with the nanofiber filling of the micron-scale framework pores and the localized micro-melting filling effect induced by hot pressing. Comparative Example 1 (pure aramid insulating paper) has a porosity of approximately 42%. Comparative Example 2 (not fully remodeled) has a porosity of approximately 38% because the hot-pressing temperature is much lower than the glass transition temperature, preventing effective flow filling between fibers. In contrast, Example 3, with the same filler content, has a porosity reduced to approximately 12% after hot pressing at 290°C. This indicates that hot pressing near the glass transition temperature can drive selective micro-melting between the aramid precipitated fibers and the BNNT@PMIA nanofibers at the contact interface. The flowing nano-units preferentially fill the micron-scale voids, thereby significantly reducing the porosity while maintaining the integrity of the framework.
[0063] Hot pressing technology allows for continuous adjustment of porosity within the range of 5% to 45% by regulating parameters such as temperature (260–290℃), pressure (5–15MPa), and time (30–90s). This provides a flexible structural design space to meet different application scenarios (such as requiring high porosity to ensure impregnation or low porosity to improve thermal conductivity and breakdown strength), fundamentally solving the problem of mutual constraint between porosity and thermal conductivity in traditional processes.
[0064] Tensile tests were performed on the composite insulating papers prepared in Examples 1, 2, and 3, and Comparative Examples 1 and 2, using a universal testing machine. Stress-strain curves were recorded, and tensile strength and elongation at break were extracted. The results are as follows: Figure 6 As shown in the figure, the tensile strength of Examples 1, 2, and 3 of the present invention is significantly better than that of Comparative Example 2 (without sufficient thermal reconstruction), and compared with Comparative Example 1 (pure aramid paper), it can still maintain a high mechanical level after introducing a high content of inorganic filler. The BNNT@PMIA nanofiber content of Example 3 is as high as 40%, but its tensile strength is only slightly lower than that of pure aramid paper, and the elongation at break is maintained within an acceptable range. This is attributed to the following structural synergistic effects: the spatial load-bearing skeleton composed of micron-sized aramid chopped fibers provides overall structural rigidity; the aramid precipitated fibers act as an adhesive to firmly wrap the fiber cross nodes and enhance the interfacial bonding; and the BNNT@PMIA nanofibers interspersed between the skeleton not only undertake the function of thermal conduction, but also transform the contact points between fibers into "welding" nodes through nanoscale physical entanglement and local micro-melting fusion induced by hot pressure, effectively transferring and dispersing the load, and avoiding stress concentration and brittle fracture caused by filler agglomeration in traditional blending. Comparing Example 3 with Comparative Example 2, it can be seen that Comparative Example 2, which was not sufficiently hot-pressed, lacked interfacial fusion and relied solely on physical overlap between fibers, resulting in significantly insufficient tensile strength and low elongation at break. This indicates that hot-pressing near the glass transition temperature can not only optimize the pore structure but also significantly improve the overall mechanical stability and flexibility of the material through node reinforcement, enabling it to meet the reliable service requirements of power equipment under complex working conditions such as wrapping, bending, and vibration.
[0065] This invention utilizes electrospinning technology to pre-prepare BNNT@PMIA composite nanofibers to achieve the pre-oriented arrangement of BNNTs. These composite nanofibers are then used as functional building blocks, assembled with aramid chopped fibers and aramid precipitated fibers via wet papermaking to form a "three-level multi-scale micro-nano assembly structure." Combined with a hot-pressing control process near the glass transition temperature, the porosity is precisely adjustable within the range of 5% to 45%, simultaneously driving the orientation rearrangement of BNNTs at fiber crosslinking nodes to construct a continuous thermally conductive network. Polyvinylpyrrolidone (PVP) is used as a surface modifier for BNNTs, significantly enhancing the interfacial affinity between BNNTs and the PMIA matrix. Combined with the localized micro-melting fusion structure between fibers, the composite material maintains excellent electrical insulation properties while also possessing superior thermal conductivity and good tensile strength. This invention, through precise multi-scale structural design and interfacial control, successfully solves the long-standing technical bottleneck of sacrificing balance in multiple performance aspects (thermal conductivity, porosity, and mechanical properties), providing a highly promising key insulating material for the thermal management system of next-generation high-power-density equipment, and possessing significant engineering application value.
Claims
1. A method for preparing aramid composite insulating paper based on highly thermally conductive nanofibers, characterized in that, Includes the following steps: Step 1: Add boron nitride nanotube dispersion to meta-aramid fiber dispersion, stir and react thoroughly to obtain spinning solution, and use electrospinning to obtain composite nanofiber membrane; Step 2: The composite nanofiber membrane is sheared to obtain composite nanofiber fragments; Step 3: The composite nanofiber fragments, aramid precipitated fibers and aramid chopped fibers obtained in Step 2 are mixed and dispersed in a solvent, and then wet-processed, dehydrated and dried to obtain aramid thermally conductive base paper substrate; The composite nanofiber fragments, aramid precipitated fibers, and aramid chopped fibers are present in parts by weight of 15–40, 20–45, and 30–50, respectively. Step 4: The aramid thermally conductive base paper substrate obtained in Step 3 is subjected to hot pressing to obtain the desired aramid composite insulating paper; wherein the hot pressing temperature is the glass transition temperature of meta-aramid.
2. The method for preparing aramid composite insulating paper based on highly thermally conductive nanofibers according to claim 1, characterized in that, The preparation process of the intermediate aramid fiber dispersion in step 1 is as follows: Meta-aramid fibers and lithium chloride were added to a solvent and stirred thoroughly under heating conditions to obtain a meta-aramid fiber dispersion. The mass ratio of meta-aramid fiber to lithium chloride is 2–4:1, the heating temperature is 140 °C, and the stirring speed is 800 r / min.
3. The method for preparing aramid composite insulating paper based on highly thermally conductive nanofibers according to claim 2, characterized in that, The preparation process of the boron nitride nanotube dispersion is as follows: Boron nitride nanotubes and polyvinylpyrrolidone are added to a solvent, and a boron nitride nanotube dispersion is obtained by stirring and ultrasonic dispersion. The mass of polyvinylpyrrolidone accounts for 5% of the mass of boron nitride nanotubes, the stirring time is 2 h, and the ultrasonic treatment is 30 min; The diameter of boron nitride nanotubes ranges from 30 to 50 nm, and the average length is 10 μm.
4. The method for preparing aramid composite insulating paper based on highly thermally conductive nanofibers according to claim 3, characterized in that, The mass ratio of boron nitride nanotubes to meta-aramid fibers is 5–25:
100.
5. The method for preparing aramid composite insulating paper based on highly thermally conductive nanofibers according to claim 1, characterized in that, In step 1, the heating temperature is 60 °C and the stirring reaction time is 12 h.
6. The method for preparing aramid composite insulating paper based on highly thermally conductive nanofibers according to claim 1, characterized in that, The electrospinning process involves a voltage of 15–25 kV, a collector rotation speed of 800 rpm, a rotating drum structure for the collector, a distance of 10–15 cm between the needle and the collector, and a spinning solution flow rate of 0.3–0.8 mL / h.
7. The method for preparing aramid composite insulating paper based on highly thermally conductive nanofibers according to claim 1, characterized in that, In step 4, the hot pressing temperature is 260–290°C, the hot pressing pressure is 5–10 MPa, and the hot pressing time is 30–60 s.
8. The aramid composite insulating paper based on highly thermally conductive nanofibers obtained by any one of the preparation methods described in claims 1 to 7, characterized in that, The aramid composite insulating paper uses aramid short-cut fibers as a skeleton network and aramid precipitated fibers as an adhesive component wrapped around the fiber intersection nodes of the skeleton network; composite nanofiber fragments are dispersed and interwoven and nested in the macroscopic pores formed by the interlacing of aramid short-cut fibers, forming a three-dimensional multi-level micro-nano assembly structure; the composite nanofiber fragments are boron nitride nanotubes / meta-aramid fibers.
9. The aramid composite insulating paper based on highly thermally conductive nanofibers according to claim 8, characterized in that, The aramid composite insulating paper contains 15-40 parts by weight of composite nanofiber fragments, 20-45 parts by weight of aramid precipitated fibers, and 30-50 parts by weight of aramid chopped fibers; the mass ratio of boron nitride nanotubes to meta-aramid fibers in the composite nanofiber fragments is 5-25:
100.
10. The application of the aramid composite insulating paper based on highly thermally conductive nanofibers as described in any one of claims 8 to 9, characterized in that, The aramid composite insulating paper is used as an insulating component for electronic devices.