A high-adhesion, mildew-resistant decorative paper and its preparation method

By using isosorbide-modified waterborne polyurethane on the front side of the decorative paper and setting a bonding-promoting layer composed of polyvinyl alcohol on the back side, the coating stability and bonding problems of decorative paper under high temperature and high humidity conditions are solved, achieving durable anti-mildew performance and strong bonding effect.

CN123109003APending Publication Date: 2026-11-17HANGZHOU ABLE DECORATIVE MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611376225.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-07
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Under high temperature and high humidity conditions, the cohesive strength and adhesion stability of the coating of existing decorative paper decrease, and the water resistance and interfacial bonding ability of the back adhesive promoting layer are insufficient, which makes the decorative paper prone to curling, bubbling or local peeling when used for a long time.

Method used

Isosorbide-modified waterborne polyurethane is used as the film-forming material for the functional printing layer, and an adhesive promoting layer is set on the back of the decorative paper. The adhesive promoting layer is composed of polyvinyl alcohol, oxidized starch, cellulose ether and nanocellulose, forming a stable composite structure, which improves the cohesive bonding and adhesive performance of the coating.

Benefits of technology

It enhances the coating adhesion stability and bonding strength of decorative paper in humid and hot environments, reduces the migration of anti-mildew components, and improves the anti-mildew performance and wall bonding ability of decorative paper.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123109003A_ABST
    Figure CN123109003A_ABST
Patent Text Reader

Abstract

This application discloses a high-adhesion-performance anti-mildew decorative paper and its preparation method. The decorative paper includes a base paper, a functional printing layer on the front side, and an adhesive-promoting layer on the back side. The functional printing layer includes isosorbide-modified waterborne polyurethane, ε-polylysine-modified nanocellulose, pigments, dispersants, wetting agents, defoamers, and water. The nanocellulose, after oxidation, condenses and reduces with ε-polylysine to form an immobilized anti-mildew component. The adhesive-promoting layer includes polyvinyl alcohol, oxidized starch, cellulose ether, nanocellulose, citric acid, and water. In preparation, the waterborne polyurethane and modified nanocellulose are formulated into a functional printing composition and applied to the front side of the base paper. The adhesive-promoting composition is then coated onto the back side of the base paper, and the finished product is obtained after drying. This application can improve the adhesion stability of the functional printing layer and the dry and wet adhesive bonding ability of the back side of the decorative paper, reduce the migration of anti-mildew components, and maintain a long-lasting anti-mildew effect in humid and hot environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the technical field of waterborne polyurethane coatings and decorative paper functional coatings, specifically relating to a high-adhesion, mildew-resistant decorative paper with isosorbide-modified waterborne polyurethane as the film-forming material and its preparation method. Background Technology

[0002] Decorative paper is an important component of wallpaper, furniture finishes, and interior decoration materials. During production, it is typically applied to the base paper through printing or coating to form a decorative layer with colors, textures, or patterns. When used on walls, in addition to a stable bond between the decorative layer on the front and the base paper, the back of the decorative paper must also be wetted and bonded to the wallpaper adhesive to prevent peeling, bubbling, or localized detachment over extended use. Most existing decorative papers use water-based acrylic resin, water-based polyurethane, or their blends as film-forming materials, and then add anti-mold agents to impart anti-mold properties. However, the printed layer formed by ordinary water-based resins will absorb water and soften under high temperature and humidity conditions, causing a decrease in the coating's cohesive strength and the adhesion stability between the coating and the base paper. Adding small-molecule or water-soluble anti-mold components through physical blending can also cause them to migrate into the environment when exposed to humidity, washing, or damp walls, gradually weakening the anti-mold effect over time and potentially increasing the risk of mold release into the indoor environment.

[0003] Generally, decorative paper does not have a special structure for promoting adhesion on the back, or it is only coated with a hydrophilic material such as polyvinyl alcohol or starch. Although this type of back coating can improve the wetting effect of wallpaper glue on the paper surface to a certain extent, its water resistance, interfacial bonding ability and wet heat stability are poor. When exposed to high humidity environment for a long time, it is prone to water absorption and swelling, reduced cohesive strength and even separation from the decorative base paper. It cannot simultaneously take into account the initial adhesion strength and wet adhesion retention ability.

[0004] Therefore, there is a need to provide a high-adhesion-performance anti-mildew decorative paper and a method for preparing the decorative paper. While improving the film-forming system and fixing of the anti-mildew components in the functional printing layer on the front side, a composite adhesive-promoting layer is set on the back side of the decorative base paper, so that the decorative paper has stable and firm front coating adhesion performance; long-lasting anti-mildew performance; low migration of anti-mildew components and good dry and wet wall adhesion ability. Summary of the Invention

[0005] To address the aforementioned deficiencies, this application provides a high-adhesion-performance mildew-resistant decorative paper, comprising a decorative base paper, a functional printing layer disposed on the front side of the decorative base paper, and an adhesive-promoting layer disposed on the back side of the decorative base paper; The functional printed layer comprises, by weight, 100 parts of isosorbide-modified waterborne polyurethane, 1-8 parts of ε-polylysine-modified nanocellulose, 15-50 parts of pigment, 0.3-2 parts of dispersant, 0.1-1 parts of wetting agent, 0.1-0.8 parts of defoamer, and 20-80 parts of water; The isosorbide-modified waterborne polyurethane is prepared from polymeric diols, aliphatic diisocyanates and / or alicyclic diisocyanates, carboxyl-type hydrophilic chain extenders, isosorbide, small molecule diol chain extenders, non-organotin catalysts, neutralizers and water. The ε-polylysine-modified nanocellulose is prepared by oxidizing nanocellulose with periodate to form oxidized nanocellulose, followed by condensation reaction with ε-polylysine and reduction with borohydride. The bonding promoting layer comprises, by weight, 100 parts polyvinyl alcohol, 20-60 parts oxidized starch, 2-10 parts cellulose ether, 1-5 parts nanocellulose, 0.5-3 parts citric acid, and 400-900 parts water.

[0006] Furthermore, the raw materials for preparing the isosorbide-modified waterborne polyurethane include, by weight, 100 parts of polymeric diol, 25-55 parts of aliphatic diisocyanate and / or alicyclic diisocyanate, 3-8 parts of carboxyl-type hydrophilic chain extender, 2-10 parts of isosorbide, 1-6 parts of small molecule diol chain extender, 0.02-0.15 parts of non-organotin catalyst, 1-6 parts of neutralizing agent, and 150-350 parts of water.

[0007] Further, the polymeric diol is one or more of polycarbonate diol, polyester diol, or polyether diol; the aliphatic diisocyanate is one or two of hexamethylene diisocyanate or trimethylhexamethylene diisocyanate; the alicyclic diisocyanate is one or two of isophorone diisocyanate or dicyclohexylmethane diisocyanate; the carboxyl-type hydrophilic chain extender is one or two of 2,2-dimethylolpropionic acid or 2,2-dimethylolbutyric acid; the small molecule diol chain extender is one or more of 1,4-butanediol, ethylene glycol, or neopentyl glycol; the non-organotin catalyst is one or more of bismuth carboxylate catalyst, zinc carboxylate catalyst, or zirconium chelate catalyst; and the neutralizing agent is one or more of triethylamine, N,N-dimethylethanolamine, potassium hydroxide, or sodium hydroxide.

[0008] Furthermore, the bismuth carboxylate catalyst is one or both of bismuth isooctanoate or bismuth neodecanoate; the zinc carboxylate catalyst is one or both of zinc isooctanoate or zinc neodecanoate; and the zirconium chelate catalyst is one or more of tetrazirconium tetraacetylacetonate, di-n-propoxybis(ethyl acetoacetate)zirconium or diisopropoxybis(ethyl acetoacetate)zirconium.

[0009] Furthermore, the raw materials for preparing the ε-polylysine modified nanocellulose, by weight, include 100 parts of nanocellulose, 10-40 parts of periodate, 5-25 parts of ε-polylysine, and 1-8 parts of borohydride on a dry basis.

[0010] Furthermore, the nanocellulose is one or more of cellulose nanofibers, cellulose nanocrystals, or bacterial cellulose; the periodate is one or two of sodium periodate or potassium periodate; the ε-polylysine is one or two of ε-polylysine free base or ε-polylysine hydrochloride; and the borohydride is one or two of sodium borohydride or potassium borohydride.

[0011] Furthermore, the polyvinyl alcohol is partially hydrolyzed polyvinyl alcohol, fully hydrolyzed polyvinyl alcohol, or a combination thereof; the oxidized starch is one or more of oxidized corn starch, oxidized cassava starch, or oxidized potato starch; the cellulose ether is one or more of sodium carboxymethyl cellulose, hydroxyethyl cellulose, or hydroxypropyl methyl cellulose; and the nanocellulose in the bonding promoting layer is one or more of cellulose nanofibers or cellulose nanocrystals.

[0012] Further, the pigment is one or more of titanium dioxide, iron oxide pigment, phthalocyanine pigment, or quinacridone pigment; the dispersant is one or more of polyacrylate dispersant, maleic acid-containing copolymer salt dispersant, or phosphate ester dispersant; the wetting agent is one or two of polyether-modified silicone wetting agent or nonionic polyether wetting agent; and the defoamer is one or more of polyether-modified silicone defoamer, mineral oil defoamer, or polyether defoamer.

[0013] Furthermore, the titanium dioxide is pigment-grade titanium dioxide, which is one or both of rutile titanium dioxide and anatase titanium dioxide; the iron oxide pigment is one or more of iron oxide red, iron oxide yellow, or iron oxide black; the phthalocyanine pigment is one or both of phthalocyanine blue or phthalocyanine green; and the quinacridone pigment is one or more of quinacridone red, quinacridone violet, or quinacridone fuchsin.

[0014] Further, the polyacrylate dispersant is one or more of sodium polyacrylate, ammonium polyacrylate, or potassium polyacrylate; the copolymer salt dispersant containing maleic acid units is one or more of acrylic acid-maleic acid copolymer sodium salt, acrylic acid-maleic acid copolymer ammonium salt, styrene-maleic anhydride copolymer sodium salt, or styrene-maleic anhydride copolymer ammonium salt; and the phosphate ester type dispersant is one or more of lauryl alcohol polyoxyethylene ether phosphate, isotretinoin polyoxyethylene ether phosphate, or stearyl alcohol polyoxyethylene ether phosphate.

[0015] Furthermore, the polyether-modified silicone wetting agent is one or more of polyoxyethylene ether-modified polydimethylsiloxane, polyoxypropylene ether-modified polydimethylsiloxane, or polyoxyethylene-polyoxypropylene ether-modified polydimethylsiloxane; the nonionic polyether wetting agent is one or more of lauryl alcohol polyoxyethylene ether, isotretinoin polyoxyethylene ether, secondary alcohol polyoxyethylene ether, or acetylene glycol polyoxyethylene ether.

[0016] Further, the polyether-modified silicone defoamer is one or more of the following: polyoxypropylene ether-modified polydimethylsiloxane defoamer, polyoxyethylene-polyoxypropylene ether-modified polydimethylsiloxane defoamer, or polyether-grafted polysiloxane defoamer; the mineral oil defoamer is one or more of the following: white oil-type defoamer, hydrogenated paraffin-based mineral oil defoamer, or hydrogenated naphthenic mineral oil defoamer; the polyether defoamer is one or more of the following: polyoxypropylene glycol defoamer, polyoxyethylene-polyoxypropylene block copolymer defoamer, or polyoxypropylene glycerol ether defoamer.

[0017] This application also provides a method for preparing the high-adhesion, mildew-resistant decorative paper as described above, comprising the following steps: S1: After dehydrating the polymeric diol and isosorbide, it is mixed with aliphatic diisocyanate and / or alicyclic diisocyanate and non-organotin catalyst for prepolymerization reaction. Carboxyl hydrophilic chain extender and small molecule diol chain extender are added to continue the reaction. Then, a neutralizing agent is added for neutralization, and water is added under shear conditions for dispersion to obtain isosorbide modified waterborne polyurethane. S2: Disperse nanocellulose in water, add periodate for oxidation reaction, wash, add ε-polylysine for condensation reaction, add borohydride for reduction, centrifuge and wash the obtained product and redisperse to obtain ε-polylysine modified nanocellulose dispersion. S3: Mix isosorbide-modified waterborne polyurethane, ε-polylysine-modified nanocellulose dispersion, pigment, dispersant, wetting agent, defoamer and water to obtain an anti-mildew waterborne printing composition; S4: Print or coat the anti-mildew water-based printing composition onto the front side of the decorative base paper, and dry it to form the functional printing layer; S5: Polyvinyl alcohol, oxidized starch, cellulose ether, nanocellulose, citric acid and water are mixed to prepare a bonding accelerator composition. The bonding accelerator composition is coated on the back of the decorative base paper and dried to form the bonding accelerator layer, thereby obtaining a mildew-resistant decorative paper with high bonding performance.

[0018] Further, in step S1, the temperature of the prepolymerization reaction is 75℃~90℃ and the time is 2h~4h. After adding the carboxyl-type hydrophilic chain extender and the small molecule diol chain extender, the reaction temperature is 60℃~80℃ and the time is 1h~3h. The neutralization temperature is 30℃~50℃ and the neutralization time is 20min~60min. In step S2, the oxidation reaction is carried out under light-protected conditions, with a reaction temperature of 25℃~45℃ and a reaction time of 2h~8h; the condensation reaction has a pH of 7.0~9.0, a reaction temperature of 25℃~50℃, and a reaction time of 2h~8h; the reduction reaction has a pH of 8.0~10.0 and a reaction time of 1h~4h; after the reduction reaction is completed, the obtained product is centrifuged and washed 3~6 times with deionized water, and the washed product is redispersed in deionized water.

[0019] Further, in step S4, the printing or coating is performed using one of gravure printing, flexographic printing, screen printing, roller coating, or blade coating, and the dry coating weight of the functional printed layer is 3 g / m². 2 ~12g / m 2 The drying temperature is 70℃~110℃, and the drying time is 1min~5min; in step S5, the dry coating amount of the bonding accelerator layer is 2g / m 2 ~8g / m 2 The drying temperature is 80℃~120℃ and the drying time is 1min~6min.

[0020] Compared with the prior art, this application has the following beneficial effects: 1. This application uses isosorbide-modified waterborne polyurethane as the main film-forming material for the functional printing layer. The rigid bicyclic structure of isosorbide can participate in the construction of polyurethane segments and, together with polymeric diols, hydrophilic chain extenders, and small molecule diols, regulate the soft and hard segment composition of polyurethane, enhance the cohesive bonding of the functional printing layer and the interfacial interaction with the decorative base paper fibers, thereby improving the adhesion stability of the functional printing layer and slowing down the water absorption softening and interfacial peeling of the coating under humid and hot conditions.

[0021] 2. This application uses periodate to oxidize nanocellulose, forming active groups on the surface of the nanocellulose that can react with the amino groups of ε-polylysine. Subsequently, a stable immobilized structure is formed through condensation and borohydride reduction. This structure can load ε-polylysine onto the surface of nanocellulose, retaining its anti-mildew effect while reducing its migration and loss in washing, humid, and high-temperature and high-humidity environments, thus giving the decorative paper a more durable anti-mildew ability.

[0022] 3. This application provides a bonding-promoting layer on the back of the decorative base paper, composed of polyvinyl alcohol, oxidized starch, cellulose ether, nanocellulose, and citric acid. Polyvinyl alcohol provides continuous film formation, oxidized starch improves the affinity between wallpaper adhesive and paper fibers, cellulose ether regulates coating uniformity and water retention, nanocellulose strengthens the internal structure of the back coating layer, and citric acid promotes stable bonding between the polyhydroxy components. The synergistic effect of these components enhances the wetting, penetration, and bonding of the wallpaper adhesive to the back of the decorative paper, and strengthens the adhesion retention under humid and hot conditions.

[0023] 4. This application places the functional printing layer on the front and the adhesive-promoting layer on the back on opposite sides of the same decorative base paper, allowing the front decorative, mildew-proof, and coating adhesion functions to work independently yet collaboratively with the back wall adhesive function. The waterborne polyurethane system, non-organotin catalytic system, and waterborne printing and coating processes used reduce the use of organic solvents and organotin compounds, and can be implemented using existing gravure printing, flexographic printing, or roll coating equipment. It features readily available raw materials, controllable processes, and suitability for continuous production. Attached Figure Description

[0024] The present application will be described in more detail below based on embodiments and with reference to the accompanying drawings. Wherein: Figure 1 This is a schematic diagram of the side cross-sectional structure of the high-adhesion mildew-resistant decorative paper of this application.

[0025] Figure 2 The graph shows the test results of the dry and wet 180° peel strength distribution and wet strength retention rate of Examples 1-3 and Comparative Examples 1-5 in Test Example 1.

[0026] Figure 3 The graph shows the high performance liquid chromatograms of formaldehyde derivatives, total volatile organic compound release, phthalate content, short-chain chlorinated paraffin content, residual vinyl chloride monomer content, and the proportion of migration limit occupancy for the formaldehyde derivatives in Examples 1-3 of Test Example 4.

[0027] Figure 4 The figures show the high-performance liquid chromatograms of residual diisocyanate derivatization in Examples 1-3 of Test Example 5 and the distribution of results from six independent determinations. Detailed Implementation

[0028] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0029] In some implementations, such as Figure 1 As shown, the high-adhesion-performance mildew-resistant decorative paper of this application includes a decorative base paper 1, a functional printing layer 2, and an adhesive-promoting layer 3. The functional printing layer 2, the decorative base paper 1, and the adhesive-promoting layer 3 are sequentially arranged from the front to the back along the thickness direction of the decorative paper. The functional printing layer 2 is disposed on the front side of the decorative base paper 1 and is formed by printing or coating and drying a mildew-resistant waterborne printing composition containing isosorbide-modified waterborne polyurethane, ε-polylysine-modified nanocellulose, and pigments. It is used to create a decorative effect and impart mildew-resistant properties to the decorative paper. The adhesive-promoting layer 3 is disposed on the back side of the decorative base paper 1 and is formed by coating and drying an adhesive-promoting composition containing polyvinyl alcohol, oxidized starch, cellulose ether, nanocellulose, and citric acid. It is used to improve the wetting and bonding effect of wallpaper adhesive on the back side of the decorative paper and enhance the adhesive stability between the decorative paper and the wall substrate. The decorative base paper 1 serves to support the functional printing layer 2 and the adhesive-promoting layer 3 and maintain the overall continuity of the decorative paper. Figure 1 This is only used to show the relative positional relationship between layers. The thickness of each layer in the diagram does not represent its actual thickness ratio.

[0030] Unless otherwise stated, all raw materials used in the embodiments of this application are commercially available industrial products or analytical reagents. Polycarbonate diols, polybutylene adipate diols, and polytetrahydrofuran ether diols with a number average molecular weight of 3000 can be purchased from Yuanli Chemical Group Co., Ltd., Shandong Yinuowei Polyurethane Co., Ltd., and Xinjiang Lanshan Tunhe Technology Co., Ltd., respectively, according to their corresponding molecular weight grades; hexamethylene diisocyanate (CAS No. 822-06-0), isophorone diisocyanate (CAS No. 4098-71-9), and dicyclohexylmethane diisocyanate (CAS No. 5124-30-1) can all be purchased from Wanhua Chemical Group Co., Ltd.; isosorbide (CAS No. 652-67-5) can be purchased from Jinan Hongbaifeng Industry and Trade Co., Ltd.; 2,2- Dimethylolpropionic acid (CAS No. 4767-03-7) and 2,2-dimethylolbutyric acid (CAS No. 10097-02-6) are available from Jiangxi Jiyu New Materials Co., Ltd.; 1,4-butanediol (CAS No. 110-63-4), ethylene glycol (CAS No. 107-21-1), neopentyl glycol (CAS No. 126-30-7), triethylamine (CAS No. 121-44-8), and N,N-dimethylethanolamine (CAS No. 108-01-0) are available from Shanghai Aladdin Biochemical Technology Co., Ltd. or Shanghai Maclean Biochemical Technology Co., Ltd.; bismuth neodecanoate (CAS No. 34364-26-6) is available from Xindian Chemical Materials (Shanghai) Co., Ltd. Zinc neodecanoate (CAS No. 27253-29-8) and tetrazirconium tetra(acetylacetone) (CAS No. 17501-44-9) are available from Shanghai Aladdin Biochemical Technology Co., Ltd.; ε-polylysine and ε-polylysine hydrochloride (CAS No. 28211-04-3) are available from Zhejiang Xinyinxiang Bioengineering Co., Ltd.; cellulose nanofibers, cellulose nanocrystals, and bacterial cellulose are available from Guilin Qihong Technology Co., Ltd.; sodium periodate (CAS No. 7790-28-5), potassium periodate (CAS No. 7790-21-8), and sodium borohydride (CAS No. 16940-66-2) are available from [unclear - likely a company name]. Potassium borohydride (CAS No. 13762-51-1) can be purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; polyvinyl alcohol (CAS No. 9002-89-5) can be purchased from Anhui Wanwei High-Tech Materials Co., Ltd.; oxidized corn starch, oxidized cassava starch, and oxidized potato starch can be purchased from domestic modified starch suppliers such as Shandong Fuyang Biotechnology Co., Ltd.; sodium carboxymethyl cellulose (CAS No. 9004-32-4), hydroxyethyl cellulose (CAS No. 9004-62-0), and hydroxypropyl methyl cellulose (CAS No. 9004-65-3) can be purchased from domestic cellulose ether suppliers such as Shandong Heda Group Co., Ltd.The titanium dioxide contained in the rutile titanium dioxide has the CAS number 13463-67-7 and can be purchased from Longbai Group Co., Ltd.; the CAS number of iron oxide yellow is 51274-00-1 and can be purchased from Zhejiang Huayuan Applied New Materials Co., Ltd.; the CAS number of phthalocyanine blue is 147-14-8 and can be purchased from Shuangle Pigment Co., Ltd.; the quinacridone red used in Example 3 can be CI Pigment Red 122, CAS number 980-26-7, and can be purchased from Baihehua Group Co., Ltd.; the dispersant, wetting agent and defoamer used can be purchased from Chongqing Kangpu Chemical Industry Co., Ltd., Baoerde New Materials Technology Co., Ltd. and Jiangsu Sixin Technology Application Research Institute Co., Ltd., respectively. The CAS number of 2,4-dinitrophenylhydrazine used in the test is 119-26-6, which was available from Shanghai Maclean Biochemical Technology Co., Ltd.; the CAS number of 1-(9-anthramethyl)piperazine is 126257-22-5, which was available from Shanghai Bid Pharmaceutical Technology Co., Ltd.; all other acid-base adjusters, chromatographic solvents, buffer salts, and standards, unless otherwise specified, were commercially available analytical grade or chromatographic grade products. The above suppliers are only used to demonstrate that the raw materials and reagents used in this application can be obtained through domestic commercial channels and do not constitute a limitation on the source of the raw materials.

[0031] Example 1

[0032] This embodiment provides a high-adhesion, mildew-resistant decorative paper, the preparation method of which includes the following steps S1-S5.

[0033] S1: Preparation of isosorbide-modified waterborne polyurethane.

[0034] 100 kg of polycarbonate diol with a number average molecular weight of 3000 and 10 kg of isosorbide were weighed and added to a reactor equipped with a stirring device, a temperature detection device, a nitrogen inlet, and a condenser. The mixture was dehydrated for 2 hours at 110°C and a vacuum of -0.09 MPa. After dehydration, nitrogen was introduced to lower the temperature of the material in the reactor to 75°C. Then, 40 kg of hexamethylene diisocyanate and 0.02 kg of bismuth neodecanoate were added, and a prepolymerization reaction was carried out at 75°C for 4 hours.

[0035] After the prepolymerization reaction was completed, 5.5 kg of 2,2-dimethylolbutyric acid and 3.5 kg of 1,4-butanediol were added to the reactor, and the reaction was continued at 70 °C for 1 h. Subsequently, the temperature of the reactants was lowered to 50 °C, and 3.5 kg of N,N-dimethylethanolamine was added, followed by a neutralization reaction at 50 °C for 40 min. After neutralization, under shear conditions with a stirring speed of 1200 r / min, 350 kg of deionized water was added over 30 min. After the water addition was completed, the mixture was further dispersed at 40 °C and 1200 r / min for 60 min to obtain an isosorbide-modified waterborne polyurethane dispersion.

[0036] S2: Preparation of ε-polylysine-modified nanocellulose dispersion.

[0037] Weigh 100 kg of cellulose nanofibers according to dry weight, add deionized water and disperse to form a cellulose nanofiber dispersion with a solid content of 2.0 wt%. Adjust the pH of the dispersion to 4.0 using a 10 wt% citric acid aqueous solution, add 25 kg of sodium periodate, and carry out an oxidation reaction for 5 h in the dark at 25°C.

[0038] After the oxidation reaction was completed, the resulting dispersion was centrifuged at 3000 r / min for 10 min, the supernatant was removed, and deionized water was added for redispersing. The oxidation product was washed three times in the same manner. The washed oxidized cellulose nanofibers were redispersed in deionized water, 15 kg of ε-polylysine free base was added, and the pH was adjusted to 8.0 using a 10 wt% sodium hydroxide aqueous solution. The condensation reaction was carried out at 50 °C for 2 h.

[0039] After the condensation reaction, the system temperature was lowered to 30℃, the pH was adjusted to 9.0 using a 10wt% sodium hydroxide aqueous solution, and 4.5 kg of sodium borohydride was added. The reduction reaction was carried out at 30℃ for 2.5 h. After the reduction reaction, the obtained product was centrifuged at 3000 r / min for 10 min, the supernatant was removed, and deionized water was added for redispersing. This process was repeated four times by centrifugation. The product obtained from the last centrifugation was redispersed in deionized water, and the solid content of the dispersion was adjusted to 10.0 wt% to obtain an ε-polylysine modified nanocellulose dispersion.

[0040] S3: Prepare an anti-mildew water-based printing composition.

[0041] Weigh 100 kg of isosorbide-modified aqueous polyurethane dispersion, 0.1 kg of polyoxyethylene ether-modified polydimethylsiloxane wetting agent, 1.1 kg of sodium polyacrylate dispersant, and 0.8 kg of white oil-type defoamer obtained in step S1. Weigh 1 kg of ε-polylysine-modified nanocellulose obtained in step S2 on a dry basis, and correspondingly weigh 10 kg of ε-polylysine-modified nanocellulose dispersion with a solid content of 10.0 wt%, wherein the dispersion carries 9 kg of water; additionally weigh 11 kg of deionized water, so that the total water mass in the functional printing layer formulation is 20 kg.

[0042] Isosorbide-modified aqueous polyurethane dispersion and deionized water were added to a dispersion container and stirred at 600 rpm for 10 min. Sodium polyacrylate dispersant and polyoxyethylene ether-modified polydimethylsiloxane wetting agent were added sequentially, and stirring was continued for another 10 min. Then, 50 kg of rutile titanium dioxide was added, and dispersion was carried out at 1200 rpm for 30 min. ε-polylysine-modified nanocellulose dispersion was added over 10 min, and stirring was continued at 500 rpm for 20 min. Finally, a white oil-based defoamer was added, and stirring was carried out at 300 rpm for 10 min to obtain an anti-mildew aqueous printing composition.

[0043] S4: Forms the functional printed layer on the front side.

[0044] The quantitative value was selected as 100g / m 2 The anti-mildew water-based printing composition obtained in step S3 is printed onto the front side of the decorative base paper using a gravure printing machine, and the dry coating amount of the functional printing layer is controlled to be 7.5 g / m². 2 The printed decorative base paper is dried at 70°C for 5 minutes to form a functional printing layer that continuously covers the front side of the decorative base paper.

[0045] S5: Forms a bonding-promoting layer on the back side.

[0046] Weigh out 100 kg of partially hydrolyzed polyvinyl alcohol, 20 kg of oxidized corn starch, 10 kg of sodium carboxymethyl cellulose, 0.5 kg of citric acid, and 3 kg of cellulose nanofibers on a dry basis. The cellulose nanofibers are prepared as an aqueous dispersion with a solid content of 10.0 wt%, with an actual feed mass of 30 kg including 27 kg of water; additionally weigh out 873 kg of deionized water, bringing the total water mass in the adhesive accelerator formulation to 900 kg.

[0047] First, add 600 kg of deionized water to the mixing tank. Then, while stirring, add 100 kg of partially hydrolyzed polyvinyl alcohol (PVA). Heat the system to 90°C and stir for 60 min to ensure complete dissolution of the PVA. Reduce the system temperature to 75°C, add 20 kg of oxidized corn starch, and continue stirring for 40 min. Pre-disperse 10 kg of sodium carboxymethyl cellulose (CCC) in 100 kg of deionized water. Add the resulting CCC dispersion to the mixing tank and stir at 600 rpm for 20 min. Dissolve 0.5 kg of citric acid in 10 kg of deionized water. Add the resulting citric acid aqueous solution and cellulose nanofiber dispersion to the mixing tank, then add the remaining 163 kg of deionized water. Stir at 500 rpm for 30 min to obtain the bonding-promoting composition.

[0048] The obtained adhesive accelerator composition was coated onto the back of the decorative base paper using a roller coater, and the dry coating weight of the adhesive accelerator layer was controlled to be 5 g / m². 2The paper was dried at 80℃ for 6 minutes. The dried decorative paper was then conditioned at 23℃ and 50% relative humidity for 24 hours to obtain a high-adhesion, mildew-resistant decorative paper.

[0049] Example 2

[0050] This embodiment provides a high-adhesion, mildew-resistant decorative paper, the preparation method of which includes the following steps.

[0051] S1: Preparation of isosorbide-modified waterborne polyurethane.

[0052] 100 kg of polybutylene adipate diol with a number average molecular weight of 3000 and 6 kg of isosorbide were weighed and added to a reactor equipped with a stirring device, a temperature detection device, a nitrogen inlet, and a condenser. The mixture was dehydrated for 2 hours at 110°C and a vacuum of -0.09 MPa. After dehydration, nitrogen was introduced to lower the temperature of the material in the reactor to 82°C. Then, 55 kg of isophorone diisocyanate and 0.085 kg of zinc neodecanoate were added, and a prepolymerization reaction was carried out at 82°C for 2 hours.

[0053] After the prepolymerization reaction was completed, 8 kg of 2,2-dimethylolpropionic acid and 6 kg of ethylene glycol were added to the reactor, and the reaction was continued at 80°C for 2 hours. Subsequently, the temperature of the reactants was lowered to 30°C, and 6 kg of triethylamine was added, followed by a neutralization reaction at 30°C for 60 minutes. After neutralization, 150 kg of deionized water was added over 30 minutes under shear conditions at a stirring speed of 1200 r / min. After the water addition was completed, the mixture was further dispersed at 40°C and 1200 r / min for 60 minutes to obtain an isosorbide-modified waterborne polyurethane dispersion.

[0054] S2: Preparation of ε-polylysine-modified nanocellulose dispersion.

[0055] Weigh 100 kg of cellulose nanocrystals on a dry basis, add deionized water, and disperse to form a cellulose nanocrystal dispersion with a solid content of 2.0 wt%. Adjust the pH of the dispersion to 4.0 using a 10 wt% citric acid aqueous solution, add 40 kg of potassium periodate, and carry out an oxidation reaction at 35°C in the dark for 8 hours.

[0056] After the oxidation reaction was completed, the resulting dispersion was centrifuged at 3000 r / min for 10 min, the supernatant was removed, and deionized water was added for redispersibility. The oxidation product was washed three times in the same manner. The washed oxidized cellulose nanocrystals were redispersed in deionized water, 25 kg of ε-polylysine hydrochloride was added, and the pH was adjusted to 7.0 with a 10 wt% sodium hydroxide aqueous solution. The condensation reaction was carried out at 25 °C for 5 h.

[0057] After the condensation reaction, the system temperature was adjusted to 35℃, the pH was adjusted to 10.0 using a 10wt% sodium hydroxide aqueous solution, and 8 kg of potassium borohydride was added. The reduction reaction was carried out at 35℃ for 4 h. After the reduction reaction, the obtained product was centrifuged at 3000 r / min for 10 min, the supernatant was removed, and deionized water was added for redispersing. The product was then centrifuged and washed 6 times in the same manner. The product obtained from the last centrifugation was redispersed in deionized water, and the solid content of the dispersion was adjusted to 10.0 wt% to obtain an ε-polylysine modified nanocellulose dispersion.

[0058] S3: Prepare an anti-mildew water-based printing composition.

[0059] Weigh 100 kg of the isosorbide-modified waterborne polyurethane dispersion, 2 kg of acrylic acid-maleic acid copolymer sodium salt dispersant, 0.55 kg of ethynylene glycol polyoxyethylene ether wetting agent, and 0.1 kg of polyoxyethylene-polyoxypropylene block copolymer defoamer obtained in step S1. Weigh 4.5 kg of the ε-polylysine-modified nanocellulose obtained in step S2 on a dry basis, and correspondingly weigh 45 kg of the ε-polylysine-modified nanocellulose dispersion with a solid content of 10.0 wt%, wherein the dispersion carries 40.5 kg of water; additionally weigh 9.5 kg of deionized water, so that the total water mass in the functional printing layer formulation is 50 kg.

[0060] Isosorbide-modified aqueous polyurethane dispersion and deionized water were added to a dispersion container and stirred at 600 rpm for 10 min. Then, acrylic acid-maleic acid copolymer sodium salt dispersant and ethynylene glycol polyoxyethylene ether wetting agent were added sequentially, and stirring was continued for another 10 min. Subsequently, 10 kg of iron oxide yellow and 5 kg of phthalocyanine blue were added, and dispersion was carried out at 1200 rpm for 30 min. ε-polylysine-modified nanocellulose dispersion was added over 10 min, and stirring was continued at 500 rpm for 20 min. Finally, polyoxyethylene-polyoxypropylene block copolymer defoamer was added, and stirring was carried out at 300 rpm for 10 min to obtain an anti-mildew aqueous printing composition.

[0061] S4: Forms the functional printed layer on the front side.

[0062] The quantitative value was selected as 100g / m 2 The anti-mildew water-based printing composition obtained in step S3 is printed twice onto the front side of the decorative base paper using a flexographic printing press. The total dry coating weight of the functional printing layer formed by the two printings is controlled to be 12 g / m². 2 The printed decorative base paper is dried at 90°C for 1 minute to form a functional printing layer that continuously covers the front side of the decorative base paper.

[0063] S5: Forms a bonding-promoting layer on the back side.

[0064] Weigh out 100 kg of fully hydrolyzed polyvinyl alcohol, 40 kg of oxidized cassava starch, 2 kg of hydroxyethyl cellulose, 1.75 kg of citric acid, and 5 kg of cellulose nanocrystals on a dry basis. The cellulose nanocrystals are prepared as an aqueous dispersion with a solid content of 10.0 wt%, with an actual feed mass of 50 kg including 45 kg of water; additionally weigh out 355 kg of deionized water, bringing the total water mass in the adhesive accelerator formulation to 400 kg.

[0065] First, add 230 kg of deionized water to the mixing tank, then add 100 kg of fully hydrolyzed polyvinyl alcohol while stirring. Heat the system to 95°C and stir for 60 min to ensure the polyvinyl alcohol is fully dissolved. Reduce the system temperature to 75°C, add 40 kg of oxidized cassava starch, and continue stirring for 40 min. Pre-disperse 2 kg of hydroxyethyl cellulose in 30 kg of deionized water, add the resulting hydroxyethyl cellulose dispersion to the mixing tank, and stir at 600 r / min for 20 min. Dissolve 1.75 kg of citric acid in 5 kg of deionized water, add the resulting citric acid aqueous solution and cellulose nanocrystal dispersion to the mixing tank, then add the remaining 90 kg of deionized water and stir at 500 r / min for 30 min to obtain the bonding-promoting composition.

[0066] The obtained adhesive accelerator composition was coated onto the back of the decorative base paper using a roller coater, and the dry coating weight of the adhesive accelerator layer was controlled to be 8 g / m². 2 Dry at 100℃ for 1 minute. After drying, conditioned the decorative paper at 23℃ and 50% relative humidity for 24 hours to obtain a mildew-resistant decorative paper with high bonding performance.

[0067] Example 3

[0068] This embodiment provides a high-adhesion, mildew-resistant decorative paper, the preparation method of which includes the following steps.

[0069] S1: Preparation of isosorbide-modified waterborne polyurethane.

[0070] 100 kg of polytetrahydrofuran ether diol with a number average molecular weight of 3000 and 2 kg of isosorbide were weighed and added to a reactor equipped with a stirring device, a temperature detection device, a nitrogen inlet, and a condenser. The mixture was dehydrated for 2 hours at 110°C and a vacuum of -0.09 MPa. After dehydration, nitrogen was introduced to raise the temperature of the material in the reactor to 90°C. Then, 25 kg of dicyclohexylmethane diisocyanate and 0.15 kg of tetra(acetylacetone)zirconium were added, and a prepolymerization reaction was carried out at 90°C for 3 hours.

[0071] After the prepolymerization reaction was completed, 3 kg of 2,2-dimethylolpropionic acid and 1 kg of neopentyl glycol were added to the reactor, and the reaction was continued at 60°C for 3 hours. The temperature of the reactants was then lowered to 40°C. 1 kg of potassium hydroxide was dissolved in 10 kg of deionized water to obtain a potassium hydroxide aqueous solution, which was added to the reactor and neutralized at 40°C for 20 minutes. After neutralization, under shear conditions with a stirring speed of 1200 r / min, the remaining 240 kg of deionized water was added over 30 minutes. After the water addition, dispersion was continued at 40°C and 1200 r / min for 60 minutes to obtain an isosorbide-modified waterborne polyurethane dispersion. The total amount of water in the potassium hydroxide aqueous solution and the water added in the dispersion step was 250 kg.

[0072] S2: Preparation of ε-polylysine-modified nanocellulose dispersion.

[0073] Weigh 100 kg of bacterial cellulose on a dry basis, add deionized water, and disperse it into a bacterial cellulose dispersion with a solid content of 2.0 wt%. Adjust the pH of the dispersion to 4.0 using a 10 wt% citric acid aqueous solution, add 10 kg of sodium periodate, and carry out an oxidation reaction at 45°C in the dark for 2 hours.

[0074] After the oxidation reaction was completed, the resulting dispersion was centrifuged at 3000 r / min for 10 min, the supernatant was removed, and deionized water was added for redispersibility. The oxidation products were washed three times in the same manner. The washed oxidized bacterial cellulose was redispersed in deionized water, 5 kg of ε-polylysine free base was added, and the pH was adjusted to 9.0 using a 10 wt% sodium hydroxide aqueous solution. The condensation reaction was carried out at 37.5℃ for 8 h.

[0075] After the condensation reaction, the system temperature was adjusted to 40℃, the pH was adjusted to 8.0 using a 10wt% citric acid aqueous solution, and 1kg of sodium borohydride was added. The reduction reaction was carried out at 40℃ for 1 hour. After the reduction reaction, the obtained product was centrifuged at 3000r / min for 10min, the supernatant was removed, and deionized water was added for redispersing. The product was then centrifuged and washed three times in the same manner. The product obtained from the last centrifugation was redispersed in deionized water, and the solid content of the dispersion was adjusted to 10.0wt% to obtain an ε-polylysine modified nanocellulose dispersion.

[0076] S3: Prepare an anti-mildew water-based printing composition.

[0077] Weigh 100 kg of isosorbide-modified aqueous polyurethane dispersion, 0.3 kg of isotridecyl polyoxyethylene ether phosphate dispersant, 1 kg of polyoxyethylene-polyoxypropylene ether modified polydimethylsiloxane wetting agent, and 0.45 kg of polyoxypropylene ether modified polydimethylsiloxane defoamer obtained in step S1. Weigh 8 kg of ε-polylysine-modified nanocellulose obtained in step S2 on a dry basis, and correspondingly weigh 80 kg of ε-polylysine-modified nanocellulose dispersion with a solid content of 10.0 wt%, wherein the dispersion carries 72 kg of water; separately weigh 8 kg of deionized water, so that the total water mass in the functional printing layer formulation is 80 kg.

[0078] Isosorbide-modified aqueous polyurethane dispersion and deionized water were added to a dispersion container and stirred at 600 rpm for 10 min. Then, isotridecyl alcohol polyoxyethylene ether phosphate dispersant and polyoxyethylene-polyoxypropylene ether modified polydimethylsiloxane wetting agent were added sequentially, and stirring was continued for another 10 min. Subsequently, 30 kg of quinacridone red was added, and dispersion was carried out at 1200 rpm for 30 min. ε-polylysine-modified nanocellulose dispersion was added over 10 min, and stirring was continued at 500 rpm for 20 min. Finally, polyoxypropylene ether modified polydimethylsiloxane defoamer was added, and stirring was carried out at 300 rpm for 10 min to obtain an anti-mildew aqueous printing composition.

[0079] S4: Forms the functional printed layer on the front side.

[0080] The quantitative value was selected as 100g / m 2 The anti-mildew water-based printing composition obtained in step S3 is coated onto the front side of the decorative base paper using a roller coater, and the dry coating amount of the functional printing layer is controlled to be 3 g / m². 2 The coated decorative base paper is dried at 110°C for 3 minutes to form a functional printing layer that continuously covers the front side of the decorative base paper.

[0081] S5: Forms a bonding-promoting layer on the back side.

[0082] Weigh out 60 kg of partially hydrolyzed polyvinyl alcohol, 40 kg of fully hydrolyzed polyvinyl alcohol, 60 kg of oxidized potato starch, 6 kg of hydroxypropyl methylcellulose, 3 kg of citric acid, 0.5 kg of cellulose nanofibers and 0.5 kg of cellulose nanocrystals (on a dry basis). Prepare a composite aqueous dispersion with a total solids content of 10.0 wt% using the cellulose nanofibers and cellulose nanocrystals. The actual feed mass of the composite aqueous dispersion is 10 kg, including 9 kg of water. Additionally, weigh out 641 kg of deionized water, bringing the total water mass in the adhesive accelerator formulation to 650 kg.

[0083] First, add 450 kg of deionized water to the mixing tank. While stirring, add 60 kg of partially hydrolyzed polyvinyl alcohol and 40 kg of fully hydrolyzed polyvinyl alcohol sequentially. Heat the system to 92°C and stir for 60 min to fully dissolve the two types of polyvinyl alcohol. Reduce the system temperature to 75°C, add 60 kg of oxidized potato starch, and continue stirring for 40 min. Pre-disperse 6 kg of hydroxypropyl methylcellulose in 80 kg of deionized water. Add the resulting hydroxypropyl methylcellulose dispersion to the mixing tank and stir at 600 r / min for 20 min. Dissolve 3 kg of citric acid in 10 kg of deionized water. Add the resulting citric acid aqueous solution and cellulose nanofiber-cellulose nanocrystal composite aqueous dispersion to the mixing tank, then add the remaining 101 kg of deionized water and stir at 500 r / min for 30 min to obtain the bonding-promoting composition.

[0084] The obtained adhesive accelerator composition was coated onto the back of the decorative base paper using a roller coater, and the dry coating weight of the adhesive accelerator layer was controlled to be 2 g / m². 2 The paper was dried at 120℃ for 3.5 minutes. The dried decorative paper was then conditioned at 23℃ and 50% relative humidity for 24 hours to obtain a high-adhesion, mildew-resistant decorative paper.

[0085] Comparative Example 1 This comparative example is based on Example 1, and the only difference from Example 1 is that 10 kg of isosorbide is not added in step S1, and the amount of 1,4-butanediol added is adjusted from 3.5 kg to 13.5 kg, replacing isosorbide with an equal mass of 1,4-butanediol; other raw materials, raw material amounts, operating steps and process parameters are the same as in Example 1.

[0086] The difference between this comparative example and the other comparative examples is that this comparative example only changes the chain extension composition of the waterborne polyurethane, without changing the fixation method of ε-polylysine on the nanocellulose, nor the bonding promoting layer. Among them, Comparative Example 2 does not use ε-polylysine at all, Comparative Example 3 uses a physical blending method of ε-polylysine and bacterial cellulose, Comparative Example 4 does not have a bonding promoting layer, and Comparative Example 5 uses a single polyvinyl alcohol back coating. This comparative example still uses ε-polylysine-modified nanocellulose formed by condensation and reduction and a complete composite bonding promoting layer to separately verify the role of isosorbide in the chain extension of waterborne polyurethane.

[0087] Comparative Example 2 This comparative example is based on Example 2, and the only difference from Example 2 is that the potassium periodate oxidation, ε-polylysine condensation and potassium borohydride reduction treatments described in step S2 are not performed, and the ε-polylysine modified nanocellulose is replaced by 4.5 kg of unmodified cellulose nanocrystals on a dry basis in step S3; other raw materials, raw material dosages, operating steps and process parameters are the same as in Example 2.

[0088] The difference between this comparative example and the others is that this comparative example retains isosorbide-modified waterborne polyurethane and a complete composite bonding accelerator layer, but the functional printed layer contains no ε-polylysine. Comparative example 1 retains immobilized ε-polylysine while omitting isosorbide; comparative example 3 still adds ε-polylysine but only physically blends it with bacterial cellulose; comparative example 4 completely omits the bonding accelerator layer; and comparative example 5 simplifies the composite bonding accelerator layer to a single polyvinyl alcohol back coating. This comparative example is used to individually verify the contribution of the introduction of ε-polylysine to the anti-mildew performance.

[0089] Comparative Example 3 This comparative example is based on Example 3, and the only difference from Example 3 is that: in step S2, sodium periodate and sodium borohydride are not added, and oxidation, condensation and reduction reactions are not carried out. Instead, bacterial cellulose and ε-polylysine free base are directly mixed according to a dry basis mass ratio of 100:5 to prepare a physical blend dispersion; in step S3, the ε-polylysine modified nanocellulose dispersion is replaced with the same dry basis mass of the physical blend dispersion; other raw materials, raw material amounts, operating steps and process parameters are the same as in Example 3.

[0090] The difference between this comparative example and other comparative examples is that this comparative example retains isosorbide, ε-polylysine, nanocellulose, and a complete composite bonding accelerator layer. However, the ε-polylysine and bacterial cellulose are only physically mixed and do not form reduced and stable carbon-nitrogen bonds. Comparative example 1 omits isosorbide but retains immobilized ε-polylysine; comparative example 2 does not add ε-polylysine at all; comparative example 4 completely omits the bonding accelerator layer; and comparative example 5 uses a single polyvinyl alcohol back coating. This comparative example is used to compare the differences between the physically blended and immobilized ε-polylysine structures in terms of antifungal durability and anti-migration performance under humid and hot conditions.

[0091] Comparative Example 4 This comparative example is based on Example 1, and the only difference from Example 1 is that after completing step S4 and forming the functional printing layer on the front side, step S5 is not performed, and the adhesive promoting layer is not prepared on the back side of the decorative base paper; other raw materials, raw material dosage, operating steps and process parameters are the same as in Example 1.

[0092] The difference between this comparative example and the others is that this comparative example retains isosorbide-modified waterborne polyurethane and ε-polylysine-modified nanocellulose formed by condensation and reduction, but completely omits the adhesive accelerator layer on the back of the decorative base paper. Comparative example 1 has a complete adhesive accelerator layer but omits isosorbide; comparative example 2 has a complete adhesive accelerator layer but does not add ε-polylysine; comparative example 3 has a complete adhesive accelerator layer but uses a physical blending method of ε-polylysine and bacterial cellulose; comparative example 5 still has a back coating layer but uses only polyvinyl alcohol and water. Therefore, this comparative example is used to verify the necessity of the overall adhesive accelerator layer and, by comparing with comparative example 5, can further examine the different effects of not having a back coating layer at all versus having only a single polyvinyl alcohol back coating layer on the adhesive performance of decorative paper.

[0093] Comparative Example 5 This comparative example is based on Example 2, and the only difference from Example 2 is that in step S5, when preparing the adhesive promoting composition, only 100 kg of fully hydrolyzed polyvinyl alcohol and 400 kg of water are used, and 40 kg of oxidized cassava starch, 2 kg of hydroxyethyl cellulose, 5 kg of cellulose nanocrystals and 1.75 kg of citric acid are not added; the dry coating weight of the resulting adhesive promoting layer is still 8 g / m². 2 The coating method, drying temperature, and drying time were the same as in Example 2; other raw materials, raw material dosage, operating steps, and process parameters were the same as in Example 2.

[0094] The difference between this comparative example and other comparative examples is that this comparative example retains isosorbide-modified waterborne polyurethane and ε-polylysine-modified nanocellulose formed by condensation and reduction, while also retaining the back coating on the back of the decorative base paper. However, it simplifies the composite bonding accelerator system composed of polyvinyl alcohol, oxidized starch, cellulose ether, nanocellulose, and citric acid into a single back coating system containing only polyvinyl alcohol and water. Comparative example 1 omits isosorbide but retains the complete composite bonding accelerator layer; comparative example 2 completely omits ε-polylysine; comparative example 3 uses a physical blending method of ε-polylysine and bacterial cellulose; and comparative example 4 completely omits the bonding accelerator layer. Therefore, this comparative example is used to verify the effect of the composite bonding accelerator system composed of oxidized starch, cellulose ether, nanocellulose, and citric acid relative to the single polyvinyl alcohol back coating system. Furthermore, by comparing it with comparative example 4, it can be used to further examine the different effects of having only a single polyvinyl alcohol back coating versus having no back coating on the bonding performance of decorative paper. It should be noted that in the attached figures of the test results related to the following test examples, Examples 1-3 are denoted as E1, E2, and E3, respectively, and Comparative Examples 1-5 are denoted as C1, C2, C3, C4, and C5, respectively. Unless otherwise stated, the measurement results are expressed as arithmetic mean ± sample standard deviation; the mold resistance grade is an ordinal classification data and is expressed as the final consensus grade among parallel samples; results not detected are expressed as less than the method report limit and are not included in the mean calculation as zero values.

[0095] Test Example 1: Adhesive performance of decorative paper and adhesion performance of functional printed layers The finished products from Examples 1-3 and Comparative Examples 1-5 were cut into 25 mm × 150 mm test strips. Formaldehyde-free starch-based wallpaper adhesive from the same batch was used at a concentration of 150 g / m². 2 The wet adhesive application rate was determined by attaching the back of each test strip to a dust-free, flat fiber cement board and curing it for 7 days at 23 ℃ and 50% relative humidity. Eight parallel samples were prepared for each group. Dry samples were equilibrated for 48 hours at 23 ℃ and 50% relative humidity before testing; wet samples were treated for 24 hours at 40 ℃ and 90% relative humidity, and tested within 10 minutes after removal. The peel strength was determined according to the 180° peel test method in GB / T 2790-1995 "Adhesives - 180° Peel Strength Test Method - Flexible Materials vs. Rigid Materials", at a test speed of 100 mm / min, and the main failure locations were recorded. Separately, the front functional printed layer of the same batch of finished products was tested according to GB / T 9286-2021 "Cross-cut Test for Paints and Varnishes", with a cut interval of 1 mm. Three samples were tested in each group, and the worst grade was taken as the result for that group. The wet strength retention rate was calculated by multiplying the ratio of wet peel strength to dry peel strength by 100%. Test results are shown in Table 1 and... Figure 2 , Figure 2 (a) Violin plots of the 180° peel strength of Examples 1-3 and Comparative Examples 1-5 in dry and wet states. The scatter points in the plot represent 8 parallel samples, and the horizontal line in the middle represents the median. Figure 2 (b) represents the corresponding wet strength retention rate, with the dashed line representing the statistical reference line of 80%.

[0096] Table 1. Test results of adhesive properties and adhesion properties of functional printed layers.

[0097] The test results show that the dry peel strength of Examples 1-3 is 17.9 N / 25 mm to 20.2 N / 25 mm, and the wet peel strength is 14.9 N / 25 mm to 17.1 N / 25 mm. The wet strength retention rate of all three groups exceeds 80%. In terms of repeatability, the coefficient of variation for the dry data of Examples 1-3 is 2.7% to 3.0%, and the coefficient of variation for the wet data is 2.7% to 3.3%, showing relatively low dispersion. This indicates that the front and back layered structures can be stably formed in different embodiments.

[0098] Comparative Example 4, without any back adhesive promoting layer, showed a 56.5% and 70.2% decrease in dry and wet peel strength compared to Example 1, respectively. The damage was concentrated at the interface between the wallpaper adhesive and the back of the decorative base paper, indicating that the back adhesive promoting layer is a major structural factor improving the reliability of wall adhesion. Comparative Example 5, with only a single polyvinyl alcohol back coating, showed results higher than Comparative Example 4 but still significantly lower than Example 2. This indicates that the composite adhesive promoting composition formed by polyvinyl alcohol, oxidized starch, cellulose ether, nanocellulose, and citric acid not only increases initial bonding but also improves interface retention under humid and hot conditions. On the other hand, the cross-cutting grade of Comparative Example 1 changed from grade 0 in Example 1 to grade 2, indicating that the adhesion stability between the functional printing layer and the paper base decreased after the removal of isosorbide during the preparation process. Therefore, Table 1 and Appendix... Figure 2 The beneficial effect of supporting high bonding performance is achieved from two directions: adhesive bonding to the back wall and adhesion of the functional layer to the front.

[0099] Test Example 2: Initial anti-mildew performance and anti-mildew durability after washing Samples of 50 mm × 50 mm were cut from Examples 1-3 and Comparative Examples 1-5. For each sample, an unwashed group and a washed group were set up, with three parallel samples in each group. The washed group was placed in a stoppered container at a sample mass to deionized water volume ratio of 1 g: 50 mL, and shaken at 25 ℃ and 150 r / min for 24 h. After replacing with an equal volume of deionized water, shaking was continued for another 24 h. The samples were then dried at 40 ℃ to constant weight. The unwashed group was not treated with water. Both groups of samples were tested according to the mixed mold spore solution, culture conditions, and grading method specified in GB / T 1741-2020 "Determination of Antifungal Resistance of Paint Films". The samples were cultured at 28 ℃ and a relative humidity of not less than 85% for 28 days; the test was valid when the control culture medium showed normal growth. First, visual observation was performed. Then, samples with mold growth of less than 10% were observed under 50x magnification. The surface mold coverage was rated from 0 to 4. Simultaneously, the percentage of mold coverage in the effective observation area was calculated through image analysis. Image acquisition was conducted in a closed imaging chamber using a diffused light source with a color temperature of 5500K. The relative positions of the camera, sample platform, and light source were fixed, with the camera lens perpendicular to the sample surface and a shooting distance of 300mm. The output image was a lossless image with a resolution of at least 2048 pixels × 2048 pixels. A standard gray card was placed next to the sample for each shot, and exposure time, aperture, ISO, and white balance parameters were kept consistent. The same sample was photographed before inoculation and after 28 days of cultivation, with the area within 2mm of the sample edge considered the effective observation area. ImageJ version 1.54 image analysis software was used to process the images. After median filtering of the color difference images, the Otsu's maximum inter-class variance method was used to automatically determine the segmentation threshold. Morphological opening and closing operations were used to remove isolated noise and fill in colony areas. The threshold was not manually adjusted throughout the entire analysis process. The percentage of area covered by mold is calculated using the following formula: P=N m / Nt×100%, where P is the percentage of mold coverage area, N m N represents the number of pixels identified as mold-covered areas after image segmentation. t The total number of pixels in the effective observation area; the mold resistance level is still determined according to the method specified in GB / T 1741-2020, and the image analysis results serve as supplementary quantitative results. The test results are shown in Table 2.

[0100]

[0101] Table 2 shows that Examples 1-3 maintained a grade of 0 after two consecutive water washes, with no mold coverage observed, indicating that the anti-mold effect does not solely come from free active substances that can be rapidly carried away by water. Comparative Example 2, which replaced ε-polylysine-modified nanocellulose with unmodified nanocellulose, was grade 3 before washing and further increased to grade 4 after washing, demonstrating that unmodified nanocellulose itself cannot provide the required anti-mold effect. Comparative Example 3 used a physical blend of ε-polylysine and nanocellulose, initially also at grade 0, but after washing, it jumped three grades to grade 3; in contrast, Example 3 showed no change in grade after the same water wash procedure. This direction of grade migration indicates that similar initial anti-mold activity does not equate to similar durability; the immobilized structure formed through oxidation, condensation, and reduction significantly inhibits the migration of ε-polylysine in the aqueous phase. Comparative Examples 1, 4, and 5 still contained immobilized anti-mold components, thus maintaining a grade of 0, indicating that the change in the back adhesive layer was not the dominant factor in the change of anti-mold grade in this test.

[0102] Test Example 3: Overall durability after high temperature and high humidity accelerated treatment Examples 1-3 and Comparative Examples 1-5 were prepared as adhesive samples identical to those in Test Example 1 and continuously treated in a constant temperature and humidity chamber at 40 ℃ and 90% relative humidity for 28 days. Five independent samples were taken at 0 days, 7 days, 14 days, and 28 days respectively, and placed in an environment at 23 ℃ and 50% relative humidity for 2 hours. The 180° peel strength was then measured according to the method in Test Example 1. The 28-day retention rate was calculated as the ratio of the 28-day peel strength to the 0-day peel strength. After 28 days of treatment, additional samples were subjected to a functional printed layer cross-cut test and a GB / T 1741-2020 mildew resistance test.

[0103] Volatile substances were detected using two analytical pathways. The TVOC release from the finished product was determined according to the climate chamber method in Appendix B of GB 18585-2023; triethylamine, N,N-dimethylethanolamine, and any residual organic solvents that may be present in the formulation were screened using headspace GC-MS; diamine hydrolysis products corresponding to the diisocyanates used were supplemented with derivatization LC-MS / MS screening. The reporting limit for each target analyte was 0.001 mg / m³. 3 If the result is below the reporting limit, it is recorded as "not detected". Test results are shown in Tables 3 and 4.

[0104] Table 3. Detection results of bonding, mildew prevention and TVOC during high temperature and high humidity treatment.

[0105] Table 4. Screening results of target volatiles before and after high temperature and high humidity treatment

[0106] The tests were conducted after continuous treatment in a constant temperature and humidity chamber for 28 days. The peel strength of Examples 1-3 decreased slowly with increasing treatment time (0 days, 7 days, 14 days, and 28 days), without any sudden drop at any particular point in time; the average retention rate after 28 days was 84.9%. The average retention rate of Comparative Examples 1-5 was 58.7%, and the decrease was more pronounced in Comparative Examples 1, 3, 4, and 5 during the 14-28 day period, indicating that damp heat aging amplifies the differences between different interfacial structures. Example 2 maintained 17.6 N / 25 mm at 28 days and maintained a cross-cut adhesion rating of 0, showing the most stable overall durability; Comparative Example 4 had the lowest retention rate, corresponding to its lack of a back adhesive accelerator layer.

[0107] The anti-mold results exhibited a different distinguishing dimension from the adhesive bonding results: Comparative Examples 2 and 3 achieved anti-mold resistance levels of 4 and 3, respectively, while Comparative Examples 1, 4, and 5, despite insufficient adhesive bonding performance, maintained an anti-mold resistance level of 0 after 28 days. This result eliminates the possibility of explaining the differences in anti-mold resistance solely by the overall coating integrity and further supports that immobilized ε-polylysine is the main source of durable anti-mold properties. Regarding volatility, the TVOC detection results at 28 days were not higher than those at 0 days; the release of detectable neutralizing agents decreased with treatment time, and the corresponding diamines and residual solvents were all below the reporting limits; no trend of increased secondary release induced by damp heat treatment was observed.

[0108] Test Example 4: Verification of Hazardous Substance Limits in Finished Products Take the finished products from Examples 1-3 and prepare parallel specimens according to the specifications of each testing method. According to the current GB 18585-2023 "Limits of Hazardous Substances in Wallpaper for Interior Decoration and Renovation Materials", the following tests were conducted: Formaldehyde and TVOC emissions were determined according to the climate chamber conditions, loading rate, ventilation rate, and sampling procedures specified in Appendix B of this standard; Phthalate emissions were determined according to the methods specified in GB / T37860-2019 "Determination of Phthalate Esters in Paper, Paperboard and Paper Products", and the sums of dibutyl phthalate (DBP), butyl benzyl phthalate (BBP), and di(2-ethylhexyl) phthalate (DEHP), as well as the sums of diisononyl phthalate (DINP), diisodecyl phthalate (DIDP), and di-n-octyl phthalate (DNOP) were calculated separately; Short-chain chlorinated paraffins were determined according to the methods specified in GB / T 40263-2021 "Determination of Short-chain Chlorinated Paraffins in Textiles"; Migratory barium, cadmium, chromium, lead, arsenic, mercury, selenium, and antimony were determined according to GB... The polyvinyl chloride monomer was processed according to Appendix A of 18585-2023 and determined by ICP-MS; residual vinyl chloride monomer was determined by gas chromatography as specified in GB / T 4615-2013 "Determination of Residual Vinyl Chloride Monomer in Polyvinyl Chloride by Gas Chromatography". The report limits for short-chain chlorinated paraffins and vinyl chloride monomer were 10 mg / kg and 0.02 mg / kg, respectively. The test results are shown in Tables 5 and 6. Figure 3 , Figure 3 (a) is a high-performance liquid chromatogram of the formaldehyde released from the finished products of Examples 1-3 after derivatization with 2,4-dinitrophenylhydrazine. Figure 3 (b) represents the total release of volatile organic compounds. Figure 3 (c) represents the phthalate content in the two groups. Figure 3 (d) represents the content of short-chain chlorinated paraffins. Figure 3 (e) represents the residual vinyl chloride monomer content. Figure 3 (f) represents the proportion of the measured values ​​of the eight migratable elements relative to their corresponding limits. Figure 3 (d) and Figure 3 (e) Plot the results for undetected results conservatively at the reporting limits of 10 mg / kg and 0.02 mg / kg, respectively. The column height does not represent the actual detected concentration. The red dashed line represents the limit value of GB 18585-2023.

[0109] Table 5. Test results of volatile matter, plasticizer, short-chain chlorinated paraffin and vinyl chloride monomer in the finished product.

[0110] Table 6. Detection results of migratable elements in the finished product

[0111] From Table 5 and Figure 3(a) It can be seen that the formaldehyde release amounts in Examples 1, 2, and 3 are 0.005 mg / m³, respectively. 3 0.006 mg / m 3 and 0.004 mg / m 3 They accounted for 0.020 mg / m³ respectively. 3 The limits are 25%, 30%, and 20%. Figure 3 (a) The response order of the formaldehyde derivative chromatographic peaks in Example 2 was higher than that in Example 1, and in Example 1 it was higher than that in Example 3, which is consistent with the quantitative results in Table 5. The total volatile organic compound release amounts in Examples 1-3 were 0.16 mg / m³, respectively. 3 0.18 mg / m 3 and 0.12 mg / m 3 The values ​​were 0.60 mg / m³. 3 The limits were 26.7%, 30.0%, and 20.0%. Among them, the formaldehyde release and total volatile organic compound release of Example 3 were the lowest; although the corresponding results of Example 2 were relatively higher among the three groups, they were only 30% of the corresponding limits.

[0112] In Examples 1-3, the total phthalates (DBP+BBP+DEHP) in the first group were 18 mg / kg, 22 mg / kg, and 15 mg / kg, respectively, representing only 1.8%, 2.2%, and 1.5% of the 1000 mg / kg limit. The total phthalates (DINP+DIDP+DNOP) in the second group were 24 mg / kg, 31 mg / kg, and 20 mg / kg, respectively, representing 2.4%, 3.1%, and 2.0% of the corresponding limits. The short-chain chlorinated paraffins in all three groups were below the method reporting limit of 10 mg / kg; even conservatively calculated according to the reporting limit, their proportion of the 1500 mg / kg limit was still less than 0.67%. The residual vinyl chloride monomers were all below the method reporting limit of 0.02 mg / kg; even conservatively calculated according to the reporting limit, they were still less than 10% of the 0.20 mg / kg limit.

[0113] From Table 6 and Figure 3 (f) It can be seen that the occupancy rate of the limit values ​​for the eight migratable elements in Examples 1-3 does not exceed 4.0%. Among them, the occupancy rate of the limit value for barium is 2.0%–3.6%, for chromium it is 2.5%–3.7%, for lead it is 2.2%–3.4%, for arsenic it is 2.6%–4.0%, and for antimony it is 1.6%–2.1%; the occupancy rates of the limit values ​​for cadmium, mercury, and selenium do not exceed 0.8%. Among all migratable elements, the arsenic content in Example 2 is 0.32 mg / kg, which has the highest occupancy rate, but it is still only 4.0% of the 8 mg / kg limit. (See Tables 5 and 6 for details.) Figure 3As a result, the test results of all hazardous substances in Examples 1-3 were lower than the corresponding limits specified in GB 18585-2023 "Limits of Hazardous Substances in Wallpaper for Interior Decoration and Renovation Materials", and no test item was close to the limit.

[0114] Test Example 5: Migration of intermediate product residues, residual diisocyanates, and antifungal components 5.1 Detection of Residual Diisocyanate Content in Waterborne Polyurethane Aqueous polyurethane dispersions prepared in step S1 of Examples 1-3 were used for analysis. Example 1 was used to detect hexamethylene diisocyanate, Example 2 for isophorone diisocyanate, and Example 3 for dicyclohexylmethane diisocyanate. The analytical methods followed the principles of 1-(9-anthramethyl)piperazine (MAP) derivatization and HPLC-UV / fluorescence detection in the NIOSH NMAM 5525 MAP derivatization HPLC-UV / fluorescence detection. Recovery, linearity, and precision were validated for the aqueous polyurethane dispersion matrix. 1.000 g of dispersion was weighed, and excess MAP acetonitrile solution was added. The mixture was reacted for 30 min under light-protected conditions, filtered through a 0.45 μm polytetrafluoroethylene membrane, and then injected. A C8 column (150 mm × 4.6 mm, 5 μm particle size) was used at a column temperature of 30 °C and an injection volume of 30 μL. Gradient elution was performed using acetonitrile and phosphate / formate buffer. UV detection was performed at 253 nm, and fluorescence detection was performed using excitation at 368 nm and emission at 409 nm. Quantification was achieved using external standard curves of three diisocyanate MAP derivatives, with each sample measured independently six times.

[0115] 5.2 HPLC Detection of Eluent and Migration Solution of Modified Nanocellulose Collect the supernatant obtained from the final centrifugation and washing in steps S2 of Examples 1-3. Periodate was detected by ion chromatography-conductivity, water-soluble boron was determined by ICP-OES and expressed as elemental boron, and free ε-polylysine was determined by matrix-spike validated cation exchange HPLC.

[0116] In addition, a total area of ​​100 cm² was cut from the finished products of Examples 1-3, Comparative Example 2, and Comparative Example 3. 2 The test pieces were mixed with 200 mL of deionized water and shaken at 40 ℃ and 100 r / min for 24 h. The migration solution was filtered through a 0.22 μm filter membrane, and the free ε-polylysine was measured and converted to the migration amount per unit area. Three independent samples were set up for each group. Comparative Example 2, ε-polylysine-free modified nanocellulose, was used to evaluate the method blank; Comparative Example 3 used a physical blend structure to evaluate the inhibitory effect of the immobilized structure on migration. The test results are shown in Tables 7 and 8. Figure 4 , Figure 4 (a) is a three-column chromatogram obtained by MAP derivatization HPLC analysis. The three columns correspond to hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI) and dicyclohexylmethane diisocyanate (H12MDI) respectively. Each column, from top to bottom, represents the standard, blank matrix and corresponding example sample. Figure 4 (b) The residual monomer scatter plots, mean and standard deviation of each of the six independent measurements in Examples 1-3; RT represents the retention time.

[0117] From Table 7, Table 8 and Figure 4 It can be seen that the calibration curves R of the three target monomers 2 The concentrations were all no less than 0.9993, the spiked recoveries were 95.6%–97.4%, and the relative standard deviations (RSDs) for six determinations were 4.1%–5.6%, indicating that after MAP derivatization, the three structurally different diisocyanates could be stably and quantitatively determined in an aqueous polyurethane matrix. The residual monomer concentrations in Examples 1–3 were 0.82 mg / kg, 1.12 mg / kg, and 0.64 mg / kg, respectively. Combined with the method validation results, it can be seen that the derivatization high-performance liquid chromatography method used can stably detect different types of residual diisocyanate monomers. The above results indicate that after prepolymerization, chain extension, neutralization, and water dispersion treatment, the residual amount of unreacted diisocyanate monomers in the obtained aqueous polyurethane dispersion is at a low level, which is beneficial to reducing the potential release risk during subsequent printing, drying, and indoor application processes.

[0118] In Examples 1-3, the levels of periodate, water-soluble boron, and free ε-polylysine in the final wash supernatant were all in low quantities, indicating that 3-6 centrifugal washes effectively removed water-soluble reaction residues. In the product migration test, the migration amount of free ε-polylysine in Examples 1-3 was 0.35 mg / m³. 2 ~0.44 mg / m 2 The comparative example 3, which was physically blended, had a concentration of 8.72 mg / m³. 2 The average value of the three examples was 0.39 mg / m³. 2 Calculations showed that the immobilized structure reduced migration by 95.5% compared to Comparative Example 3. Comparative Example 2 was below the reporting limit, verifying that the method blank did not produce a false positive signal for ε-polylysine. This result corroborates the phenomenon in Test Example 2 where the antifungal grade of Comparative Example 3 decreased from level 0 to level 3 after washing with water: covalent immobilization simultaneously retains the surface antifungal effect and reduces the migration of active components into the aqueous phase.

[0119] Where there is no conflict, the same embodiment and different embodiments of this application can be combined with each other; the above description is only a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. A high-adhesion, mildew-resistant decorative paper, characterized in that, It includes decorative base paper, a functional printing layer disposed on the front side of the decorative base paper, and an adhesive promoting layer disposed on the back side of the decorative base paper; The functional printed layer comprises, by weight, 100 parts of isosorbide-modified waterborne polyurethane, 1-8 parts of ε-polylysine-modified nanocellulose, 15-50 parts of pigment, 0.3-2 parts of dispersant, 0.1-1 parts of wetting agent, 0.1-0.8 parts of defoamer, and 20-80 parts of water; The isosorbide-modified waterborne polyurethane is prepared from polymeric diols, aliphatic diisocyanates and / or alicyclic diisocyanates, carboxyl-type hydrophilic chain extenders, isosorbide, small molecule diol chain extenders, non-organotin catalysts, neutralizers and water. The ε-polylysine-modified nanocellulose is prepared by oxidizing nanocellulose with periodate to form oxidized nanocellulose, followed by condensation reaction with ε-polylysine and reduction with borohydride. The bonding promoting layer comprises, by weight, 100 parts polyvinyl alcohol, 20-60 parts oxidized starch, 2-10 parts cellulose ether, 1-5 parts nanocellulose, 0.5-3 parts citric acid, and 400-900 parts water.

2. The high-adhesion, mildew-resistant decorative paper according to claim 1, characterized in that, The raw materials for preparing the isosorbide-modified waterborne polyurethane include, by weight, 100 parts of polymeric diol, 25-55 parts of aliphatic diisocyanate and / or alicyclic diisocyanate, 3-8 parts of carboxyl-type hydrophilic chain extender, 2-10 parts of isosorbide, 1-6 parts of small molecule diol chain extender, 0.02-0.15 parts of non-organotin catalyst, 1-6 parts of neutralizing agent, and 150-350 parts of water.

3. The high-adhesion, mildew-resistant decorative paper according to claim 1, characterized in that, The polymeric diol is one or more of polycarbonate diol, polyester diol, or polyether diol; the aliphatic diisocyanate is one or two of hexamethylene diisocyanate or trimethylhexamethylene diisocyanate; the alicyclic diisocyanate is one or two of isophorone diisocyanate or dicyclohexylmethane diisocyanate; the carboxyl-type hydrophilic chain extender is one or two of 2,2-dimethylolpropionic acid or 2,2-dimethylolbutyric acid; the small molecule diol chain extender is one or more of 1,4-butanediol, ethylene glycol, or neopentyl glycol; the non-organotin catalyst is one or more of bismuth carboxylate catalyst, zinc carboxylate catalyst, or zirconium chelate catalyst; and the neutralizing agent is one or more of triethylamine, N,N-dimethylethanolamine, potassium hydroxide, or sodium hydroxide.

4. The high-adhesion, mildew-resistant decorative paper according to claim 1, characterized in that, The raw materials for preparing the ε-polylysine-modified nanocellulose, by weight, include 100 parts of nanocellulose, 10-40 parts of periodate, 5-25 parts of ε-polylysine, and 1-8 parts of borohydride on a dry basis.

5. The high-adhesion, mildew-resistant decorative paper according to claim 4, characterized in that, The nanocellulose is one or more of cellulose nanofibers, cellulose nanocrystals, or bacterial cellulose; the periodate is one or two of sodium periodate or potassium periodate; the ε-polylysine is one or two of ε-polylysine free base or ε-polylysine hydrochloride; and the borohydride is one or two of sodium borohydride or potassium borohydride.

6. The high-adhesion, mildew-resistant decorative paper according to claim 1, characterized in that, The polyvinyl alcohol is partially hydrolyzed polyvinyl alcohol, fully hydrolyzed polyvinyl alcohol, or a combination thereof; the oxidized starch is one or more of oxidized corn starch, oxidized cassava starch, or oxidized potato starch; the cellulose ether is one or more of sodium carboxymethyl cellulose, hydroxyethyl cellulose, or hydroxypropyl methyl cellulose; and the nanocellulose in the bonding promoting layer is one or more of cellulose nanofibers or cellulose nanocrystals.

7. The high-adhesion, mildew-resistant decorative paper according to claim 1, characterized in that, The pigment is one or more of titanium dioxide, iron oxide pigment, phthalocyanine pigment, or quinacridone pigment; the dispersant is one or more of polyacrylate dispersant, copolymer salt dispersant containing maleic acid unit, or phosphate ester type dispersant; the wetting agent is one or two of polyether modified silicone wetting agent or nonionic polyether wetting agent; the defoamer is one or more of polyether modified silicone defoamer, mineral oil defoamer, or polyether defoamer.

8. A method for preparing a high-adhesion, mildew-resistant decorative paper as described in any one of claims 1 to 7, characterized in that, Includes the following steps: S1: After dehydrating the polymeric diol and isosorbide, it is mixed with aliphatic diisocyanate and / or alicyclic diisocyanate and non-organotin catalyst for prepolymerization reaction. Carboxyl hydrophilic chain extender and small molecule diol chain extender are added to continue the reaction. Then, a neutralizing agent is added for neutralization, and water is added under shear conditions for dispersion to obtain isosorbide modified waterborne polyurethane. S2: Disperse nanocellulose in water, add periodate for oxidation reaction, wash, add ε-polylysine for condensation reaction, add borohydride for reduction, centrifuge and wash the obtained product and redisperse to obtain ε-polylysine modified nanocellulose dispersion. S3: Mix isosorbide-modified waterborne polyurethane, ε-polylysine-modified nanocellulose dispersion, pigment, dispersant, wetting agent, defoamer and water to obtain an anti-mildew waterborne printing composition; S4: Print or coat the anti-mildew water-based printing composition onto the front side of the decorative base paper, and dry it to form the functional printing layer; S5: Polyvinyl alcohol, oxidized starch, cellulose ether, nanocellulose, citric acid and water are mixed to prepare a bonding accelerator composition. The bonding accelerator composition is coated on the back of the decorative base paper and dried to form the bonding accelerator layer, thereby obtaining a mildew-resistant decorative paper with high bonding performance.

9. The preparation method according to claim 8, characterized in that, In step S1, the temperature of the prepolymerization reaction is 75℃~90℃ and the time is 2h~4h. After adding the carboxyl-type hydrophilic chain extender and the small molecule diol chain extender, the reaction temperature is 60℃~80℃ and the time is 1h~3h. The neutralization temperature is 30℃~50℃ and the neutralization time is 20min~60min. In step S2, the oxidation reaction is carried out under light-protected conditions, with a reaction temperature of 25℃~45℃ and a reaction time of 2h~8h; the condensation reaction has a pH of 7.0~9.0, a reaction temperature of 25℃~50℃, and a reaction time of 2h~8h; the reduction reaction has a pH of 8.0~10.0 and a reaction time of 1h~4h; after the reduction reaction is completed, the obtained product is centrifuged and washed 3~6 times with deionized water, and the washed product is redispersed in deionized water.

10. The preparation method according to claim 8, characterized in that, In step S4, the printing or coating is performed using one of gravure printing, flexographic printing, screen printing, roller coating, or blade coating, and the dry coating weight of the functional printed layer is 3 g / m². 2 ~12g / m 2 The drying temperature is 70℃~110℃, and the drying time is 1min~5min; in step S5, the dry coating amount of the bonding accelerator layer is 2g / m 2 ~8g / m 2 The drying temperature is 80℃~120℃ and the drying time is 1min~6min.