A method for applying high-film-thickness, non-sagging epoxy putty by scraping.

By using solvent-free epoxy putty and a precise temperature-controlled layered coating method, the problems of sagging risk and high defect rate in the construction of high film thickness epoxy putty were solved, achieving efficient and stable AESS steel structure coating effect.

CN123109291APending Publication Date: 2026-11-17SHANGHAI CONSTR JIANGSU STEEL STRUCTURE CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611404789.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-10
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing application of high-film-thickness epoxy putty has problems such as high risk of sagging, short construction window period, high defect rate, and construction parameters not being optimized in conjunction with working conditions, resulting in unstable coating quality of AESS steel structures.

Method used

Solvent-free epoxy putty is used, combined with precise temperature control, layered application, and dynamic adjustment of application speed to achieve an energy storage modulus G'≥500Pa. The construction environment temperature is controlled at 10-35℃ and the relative humidity at 50%-80%. A double-coat application process and segmented curing are adopted to ensure the interfacial bonding between the putty layer and the primer.

Benefits of technology

It achieves one-time molding of high film thickness putty of 800-1500μm, without sagging, bubbles, or pinholes, extends the construction window to more than 75 minutes, reduces the defect rate to less than 2%, improves the adhesion and salt water resistance of the coating, and is suitable for industrialized batch construction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123109291A_ABST
    Figure CN123109291A_ABST
Patent Text Reader

Abstract

This invention discloses a method for applying high-film-thickness, non-sagging epoxy putty using a scraping technique, belonging to the field of steel structure anti-corrosion construction technology. The method includes: pre-construction preparation and working condition control; epoxy putty mixing: the main agent and curing agent are mixed at a mass ratio of 9:1; layered scraping construction and thickness control: a double-coat scraping process is adopted, with a single coat thickness of 300-500μm, a total dry film thickness of 800-1500μm, and the scraping speed is dynamically adjusted according to temperature: 0.2-0.4m / s at 10-20℃, and 0.5-0.8m / s at 21-35℃; scraping pressure is 0.3-0.5MPa; curing; and construction quality acceptance. This invention achieves one-time, non-sagging application of 800-1500μm high-film-thickness epoxy putty, with a construction window period ≥75min (at 23℃), and a defect rate ≤2%, suitable for coating projects with high appearance quality requirements for AESS steel structures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of steel structure anti-corrosion construction technology, specifically to a scraping application method for high-film-thickness, non-sagging epoxy putty suitable for AESS (Architecturally Exposed Structural Steel). Background Technology

[0002] AESS steel structures have extremely high requirements for surface smoothness and coating appearance quality. Typically, a high-thickness epoxy putty is applied over a primer coating to fill surface defects such as welds and pits, resulting in a smooth and even coated surface. Epoxy putty application is a crucial step in the AESS steel structure coating process, and its quality directly affects the protective performance and decorative effect of the overall coating system.

[0003] The following technical challenges exist in the application of existing high-film-thickness epoxy putty: 1. High risk of spillage When epoxy putty is applied with a high film thickness (above 800μm), if the storage modulus G' is below 500Pa at 23℃ and 1Hz, its thixotropic recovery ability is insufficient. After application, the internal structure cannot be established quickly, causing the wet film to flow under gravity. This easily leads to sagging and running on vertical or inclined surfaces, resulting in uneven coating thickness and appearance defects, requiring rework and repair, which seriously affects construction efficiency and project quality.

[0004] 2. Short construction window The pot life of existing epoxy putty is usually short, ≤30 minutes at room temperature (23℃). Construction workers need to complete the mixing, application and finishing work within a limited time. The operation has a low tolerance for error and the requirements for construction rhythm and personnel coordination are extremely demanding. The slightest carelessness will result in material waste or quality defects.

[0005] 3. High defect rate Traditional scraping coating processes lack systematic optimization of working conditions, which easily leads to defects such as bubbles, pinholes, curling edges, and difficulty in sanding. According to incomplete statistics from engineering projects, the defect rate is usually 8% to 12%, affecting the protective performance and service life of the coating system.

[0006] 4. The construction parameters were not optimized in conjunction with the characteristics of the primer and the working conditions.

[0007] Existing construction methods rely heavily on the experience of construction personnel. Key parameters such as squeegee speed, squeegee pressure, and layer thickness are not dynamically adjusted according to factors such as ambient temperature, humidity, and primer characteristics. This results in poor coating quality stability, making it difficult to meet the dual requirements of long-term corrosion protection and high appearance quality for AESS steel structures.

[0008] Therefore, developing an epoxy putty application method that can achieve high film thickness in one step, without sagging, with a long construction window, low defect rate, and quantifiable and reproducible parameters has significant engineering application value.

[0009] The relevant reference CN104060785A discloses a construction process for flexible epoxy putty, the specific steps of which include: (1) treatment of the substrate: clean the substrate and make its surface clean and flat; (2) preparation of flexible epoxy putty: add an appropriate amount of water and flexible epoxy putty dry powder to the container, stir evenly with a special tool and let it stand for 6 to 10 minutes, and then stir it again; (3) scraping of flexible epoxy putty: scrape the flexible epoxy putty using the back-and-forth scraping method; (4) sanding of flexible epoxy putty: select the grit of sandpaper according to the hardness of the surface to be sanded, and then sand it; (5) checking the flatness: under side light, there are no obvious bumps and scraping marks, no rough feeling, and the surface is smooth, which is qualified. CN104060785A does not address the dynamic linkage adjustment of coating speed and temperature, does not address the quantitative indicators of rheological properties with a storage modulus G'≥500Pa, does not specify the application scenario for AESS steel structures, and does not quantify key technical indicators such as the construction window period (75min) and defect rate (≤2%). It has significant deficiencies in terms of film thickness capability, parameter quantification, working condition adaptability, acceptance standards, and application scenario specificity, which may lead to sagging defects. Summary of the Invention

[0010] This invention addresses the technical problems existing in the application of high-film-thickness epoxy putty, such as high risk of sagging, short application window, high defect rate, and lack of optimization of application parameters in conjunction with working conditions. It provides a high-film-thickness epoxy putty application method with precise temperature control, adjustable parameters, and no sagging.

[0011] This invention aims to achieve the following technical effects: to achieve one-time application and molding of 800-1500μm high film thickness putty, without sagging, bubbles, or pinholes; to extend the construction window period to more than 75 minutes, improving the construction error tolerance rate; to reduce the coating defect rate to below 2%; and to quantify and replicate construction parameters, adapting to industrialized construction.

[0012] To achieve the above-mentioned objectives, the present invention provides the following technical solution: A method for applying high-film-thickness, non-sagging epoxy putty by scraping includes the following steps: S1. Pre-construction preparation and working condition control: The surface of the AESS steel structure is shot-blasted to achieve a cleanliness level of Sa2½ and a roughness of 40-75μm. The primer is applied within 4 hours after treatment, and the putty is applied after the primer has cured for 72 hours. The ambient temperature is controlled to 10-35℃, the relative humidity is controlled to 50%-80%, and the wind speed is ≤0.5m / s. S2. Epoxy Putty Preparation: Solvent-free epoxy putty is selected. The main agent and curing agent are mixed at a mass ratio of 9:1. First, it is pre-stirred at 200r / min for 3min, then stirred at 300r / min for 5min, and allowed to stand for 2min to defoam. The storage modulus G' of the putty is measured using a rotational rheometer at 25±2℃, angular frequency ω=10 rad / s, and strain 1% to be ≥500 Pa. S3. Layered coating application and thickness control: A two-coat coating process is adopted, with a single coating thickness of 300-500μm. After the first coat is applied, it is allowed to dry for 30 minutes before the second coat is applied. The final total dry film thickness is 800-1500μm. The coating speed is dynamically adjusted according to the temperature: 0.2-0.4m / s at 10-20℃ and 0.5-0.8m / s at 21-35℃. The coating pressure is maintained at 0.3-0.5Mpa. S4. Curing and maintenance: After the coating is applied, the coating is cured in stages. First, it is surface dry for 0-24 hours, then it is fully dry for 24-72 hours. After the fully dry curing, the Shore hardness reaches 75 or above. Then, it is sanded and trimmed, and finally fully cured. S5. Construction quality acceptance: Acceptance shall be carried out in accordance with the standards of no sagging or bubbles in appearance, dry film thickness deviation ±5%, and adhesion ≥10MPa.

[0013] Preferably, in step S1, the primer surface is cleaned and roughened before the epoxy putty is mixed.

[0014] Preferably, the primer in step S1 is an epoxy zinc-rich primer with a dry film thickness of 80 μm.

[0015] Preferably, in step S2, the solvent-free epoxy putty has a volume solids content of 97±2%, a weight solids content of 99±1%, a density of 1.8 kg / L, and a VOC content of ≤16 g / L.

[0016] Preferably, the construction window period of the solvent-free epoxy putty after mixing in step S2 at 23°C is 75 minutes; when the ambient temperature is below 10°C, the material should be preheated to 25°C before mixing.

[0017] Preferably, in step S3, the layered coating application is performed using a metal scraper or a scraper made of polymer material.

[0018] Preferably, in step S4, the surface drying time is 5 hours at 5°C, 5 hours at 10°C, 3 hours at 23°C, and 2 hours at 40°C during the surface drying stage; the solid drying time is 48 hours at 5°C, 33 hours at 10°C, 14 hours at 23°C, and 6 hours at 40°C during the solid drying stage; and the complete curing time is 21 days at 5°C, 14 days at 10°C, 7 days at 23°C, and 3 days at 40°C.

[0019] Preferably, in step S5, the appearance quality also includes a coating flatness error of ≤2mm / m.

[0020] Preferably, in step S5, the dry film thickness is detected using a coating thickness gauge, with 5 points tested per square meter.

[0021] Compared with the prior art, the present invention has the following beneficial effects: 1. Achieving high film thickness without sagging in a single application. This invention achieves sagging-free application of putty with a film thickness of 800-1500μm by using solvent-free epoxy putty (G'≥500Pa) combined with optimized squeegee speed (0.2-0.8m / s) and squeegee pressure (0.3-0.5MPa). Experiments have verified that this putty can be applied up to 5mm without sagging. Simultaneously, experiments also verified that deviating from the 0.2-0.8m / s squeegee speed—for example, applying too quickly at low temperatures or too slowly at high temperatures—will result in sagging and uneven thickness defects.

[0022] 2. Significantly extended construction window period. This invention extends the construction window period from ≤30 minutes in traditional processes to over 75 minutes (based on a mixed service life of 75 minutes at 23℃), greatly improving construction error tolerance and operational convenience.

[0023] 3. Significantly reduces coating defect rate. This invention, through the comprehensive application of technologies such as dynamic adaptation to working conditions, layered coating, and precise thickness control, reduces the coating defect rate from 8%–12% in traditional processes to below 2%. Testing shows that the coating has a smooth appearance, free from defects such as runs, bubbles, and pinholes, and exhibits good sandability.

[0024] 4. Excellent coating protection performance. According to third-party testing institutions, the epoxy putty coating system applied by the method of this invention has an adhesion of ≥10MPa (measured value 10.91-17.12MPa), and its salt water resistance (immersion in 5% NaCl solution for 3000h) does not cause blistering, cracking, or peeling, meeting the long-term anti-corrosion requirements of AESS steel structures.

[0025] 5. Quantifiable and replicable construction parameters. This invention quantifies and specifies all key construction parameters (temperature, humidity, troweling speed, troweling pressure, layer thickness, curing time, etc.), forming a standardized, replicable, and scalable construction process suitable for industrialized mass production scenarios.

[0026] 6. Green and environmentally friendly. This invention uses solvent-free epoxy putty with a VOC content ≤16g / L, which meets the requirements of GB30981-2020 "Limits of Hazardous Substances in Industrial Protective Coatings" standard, taking into account both environmental protection and high efficiency, and meeting the green and long-term protection needs of AESS steel structures. Attached Figure Description

[0027] Figure 1 A schematic diagram of the application process for high-film-thickness, non-sagging epoxy putty. Detailed Implementation

[0028] The present invention will now be described in further detail with reference to the accompanying drawings and embodiments. General Implementation Examples

[0029] like Figure 1 As shown, a method for applying high-film-thickness, non-sagging epoxy putty by scraping includes the following steps: S1, Pre-construction preparation and operational condition control (1) Substrate pretreatment: The surface of the AESS steel structure is shot blasted to achieve a cleanliness standard of Sa2½ (ISO8501-1), with a surface roughness controlled between 40-75μm. The treated surface should be primed within 4 hours. The primer should be an epoxy zinc-rich primer (such as Jotun Barrier 80S), with a dry film thickness controlled at 80μm. The primer should be allowed to cure naturally for 72 hours before the putty application process can begin.

[0030] (2) Operating conditions control: The ambient temperature during construction shall be controlled to 10-35℃, the relative humidity to 50%-80%, and the wind speed to ≤0.5m / s through the temperature control system. Before construction, the atmospheric conditions near the substrate shall be tested in accordance with ISO8502-4 standard to ensure that the substrate temperature is at least 3℃ higher than the dew point temperature.

[0031] (3) Surface treatment of the previous coating: Before applying the putty, clean the surface of the cured primer to remove all oil, dust and other contaminants. If there are rough particles or local high points on the surface of the primer, use hand sandpaper to roughen it to enhance the interlayer adhesion between the putty and the primer.

[0032] S2, epoxy putty mixing (1) Material selection: Solvent-free epoxy putty (such as Jotun Penguard Fulfill SF) is selected. The volume solids content of this putty is 97±2%, the weight solids content is 99±1%, the density is 1.8kg / L, and the VOC content is ≤16g / L. Weight solids content refers to the percentage of non-volatile substances in the coating that can ultimately remain on the construction surface to form a dry film, accounting for the total weight of the coating.

[0033] (2) Mixing ratio: Mix the putty main agent (component A) and the curing agent (component B) at a mass ratio of 9:1.

[0034] (3) Mechanical stirring: Weigh the main agent (component A) and curing agent (component B) according to the ratio and put them into the mixing container. Use a power stirrer to stir thoroughly. First, pre-stir at a speed of 200 r / min for 3 min to make the two components initially mixed; then stir at a high speed of 300 r / min for 5 min to ensure that the two components are mixed evenly and obtain a putty material with uniform color.

[0035] (4) Defoaming after standing: After stirring, let stand for 2 minutes to eliminate air bubbles trapped during stirring. The putty after standing is tested with a rheometer at 23℃ and a frequency of 1Hz or 10rad / s. The storage modulus G' is ≥500Pa, the rheological properties meet the standard, and the anti-sagging ability is ensured.

[0036] (5) Construction window control: The putty should be used within 75 minutes (at 23℃) after mixing. When the ambient temperature is higher than 23℃, the service life after mixing will be shortened accordingly. The amount of each batch should be reduced according to the actual temperature. When the ambient temperature is lower than 10℃, it is recommended to preheat the material to 25℃ before mixing.

[0037] S3, Layered application and thickness control (1) Scraping process: A double-coat scraping process is adopted, and a scraper is used for scraping. The thickness of a single scraping is controlled at 300-500μm. After the first scraping is completed, it is left to stand for 30 minutes (until it is surface dry) before the second scraping is applied. The final dry film thickness is controlled at 800-1500μm.

[0038] (2) Dynamic adjustment of troweling speed: The troweling speed is dynamically adjusted according to the ambient temperature during construction, specifically as follows: 1) When the ambient temperature is 10-20℃, the coating speed is 0.2-0.4m / s; 2) When the ambient temperature is 21-35℃, the scraping speed is 0.5-0.8m / s.

[0039] (3) Control of scraping pressure: The scraping pressure is kept at 0.3-0.5MPa to ensure that the coating is uniform, dense and free of drip defects.

[0040] (4) Scraping operation requirements: Metal scrapers or polymer scrapers should be used. When scraping, the scraper should be kept at an appropriate angle to the substrate surface, and the force should be even to avoid curling. During the scraping process, the appearance of the coating should be observed at any time. If local accumulation or running is found, it should be leveled in time.

[0041] S4, Curing and Maintenance (1) Surface drying (0-24h): Use industrial air conditioning and dehumidification systems to maintain stable ambient temperature and humidity, and do not touch the coating. During this stage, the coating surface gradually loses its stickiness. The surface drying time varies depending on the ambient temperature: 5h at 5℃, 5h at 10℃, 3h at 23℃, and 2h at 40℃.

[0042] (2) Dry curing (24-72h): Regularly test the coating hardness. When the coating reaches a Shore hardness of 75 according to ASTM D2240, sand and trim the edges to remove local defects. The drying time for walking varies with temperature: 48h at 5℃, 33h at 10℃, 14h at 23℃, and 6h at 40℃.

[0043] (3) Complete curing: Avoid rain and direct sunlight during the curing period to ensure that the coating is fully cured. The time from complete curing to usable condition is: 21 days at 5℃, 14 days at 10℃, 7 days at 23℃, and 3 days at 40℃. Good ventilation should be maintained during the curing period, but the wind speed should not be too high to avoid the surface losing water too quickly and affecting the curing quality.

[0044] S5, Construction Quality Acceptance (1) Appearance quality: The coating surface should be free from defects such as sagging, bubbles, and pinholes, and the coating flatness error should be ≤2mm / m. It should have good scraping properties and not produce edge curling.

[0045] (2) Thickness test: Use a coating thickness gauge to test 5 points per square meter. The dry film thickness deviation should be within ±5%.

[0046] (3) Adhesion test: The adhesion test shall be performed by pull-off method according to ASTM D4541 or ISO 4624 standard. The adhesion shall be ≥10MPa.

[0047] (4) Sandability test: It should be able to sand a smooth, matte surface using 400# wet sandpaper, and should not stick to the wet sandpaper.

[0048] (5) Salt water resistance test: After immersion in 5% sodium chloride solution for 3000 hours, it should not bubble, crack or peel off.

[0049] This invention achieves high film thickness, non-sag coating application based on the following technical principles: 1. Rheological Properties and Anti-Sagging Principle. The solvent-free epoxy putty selected in this invention has excellent thixotropic properties, with a storage modulus G' ≥ 500 Pa, giving the putty good anti-sagging ability. During the application process, the putty's fluidity increases under shear force, facilitating construction; after application, the putty quickly recovers its structural viscosity, relying on its own thixotropic properties to resist gravity-induced flow, thereby achieving a high film thickness of 800-1500 μm with no sagging in a single application.

[0050] 2. Dynamic Adaptation Principle for Working Conditions. This invention adjusts the scraping speed in conjunction with the ambient temperature: at low temperatures, the putty has higher viscosity and poorer fluidity, so a lower scraping speed (0.2-0.4 m / s) is used to ensure the coating is fully spread and dense; at high temperatures, the putty has lower viscosity and better fluidity, so a higher scraping speed (0.5-0.8 m / s) is used to prevent sagging caused by excessively thin putty. Simultaneously, the ambient temperature is controlled between 10-35℃ and the relative humidity between 50% and 80%, ensuring the putty cures under suitable temperature and humidity conditions, avoiding various coating defects caused by excessively fast or slow curing.

[0051] 3. Layered Coating and Stress Relief Principle. This invention employs a two-coat process, with each coat thickness controlled at 300-500 μm, resulting in a total thickness of 800-1500 μm. Layered coating avoids sagging and internal stress concentration caused by excessively thick single coats. Furthermore, allowing the coating to surface dry (30 min) after each coat releases internal stress, reducing the risk of cracking due to curing shrinkage.

[0052] 4. Principle of Enhanced Interfacial Bonding. This invention systematically links substrate treatment, primer application, putty application, and curing processes: primer application is completed within 4 hours after substrate treatment to avoid contamination of the freshly activated surface; putty application is performed 72 hours after primer curing to ensure full primer curing; the primer surface is cleaned and roughened before putty application to increase mechanical anchoring force. These measures work synergistically to significantly improve the interfacial bonding between the putty coating and the primer. Example 1

[0053] This embodiment uses a certain AESS building steel structure project as an example to describe the method of the present invention in detail.

[0054] S1. Pre-construction preparation and operational condition control Q355B steel structural components were selected and surface-treated using a shot blasting machine to achieve a cleanliness level of Sa2.5 (ISO 8501-1) and a surface roughness of 50μm. Within 4 hours of treatment, Jotun Barrier 80S epoxy zinc-rich primer was sprayed on, achieving a dry film thickness of 80μm. The primer was then allowed to cure naturally for 72 hours at an ambient temperature of 25℃ and a relative humidity of 65%. Before applying the putty, the rough areas of the primer surface were roughened using hand sandpaper.

[0055] S2. Epoxy Putty Mixing Jotun Penguard Fulfill SF solvent-free epoxy putty was selected and weighed according to the mass ratio of component A to component B = 9:1. It was stirred using a power mixer at 200 rpm for 3 minutes, followed by 300 rpm for 5 minutes. After stirring, it was allowed to stand for 2 minutes to defoam. The storage modulus G' of the putty was determined using a rotational rheometer at 25±2℃, angular frequency ω = 10 rad / s, and strain 1% to be ≥500 Pa.

[0056] S3. Layered application and thickness control The putty was applied using a scraper, with the first coat approximately 500 μm thick, applied at a speed of 0.5 m / s and a pressure of 0.4 MPa. After the first coat was applied, it was allowed to dry for 30 minutes before the second coat was applied. The average total dry film thickness of the putty layer after both coats was 1372 μm. At 25℃, applying at a speed of 1.0 m / s resulted in noticeable dripping and sagging on vertical surfaces, with a dry film thickness deviation of +18%. At 5℃, still applying at a speed of 1.0 m / s, the putty, due to its high viscosity, failed to spread sufficiently, resulting in scratches and uneven thickness, with a deviation of -12%.

[0057] S4. Curing and Maintenance After the coating is applied, it is cured in stages: first, surface dry curing for 0-24 hours, then solid dry curing for 24-72 hours. After solid dry curing, the Shore hardness reaches 75 or higher, then it is sanded and trimmed, and finally fully cured for 7 days.

[0058] S5. Construction Quality Acceptance Coating appearance: The overall epoxy putty surface is smooth and free of abnormal defects such as sagging. After the topcoat is applied, the large area has a good visual appearance and is free of abnormalities such as cracking and sagging.

[0059] Dry film thickness: In Example 1, the average total dry film thickness of the Jotun kit (Jotun Barrier 80S epoxy zinc-rich primer + Jotun Penguard Fulfill SF solvent-free epoxy putty + Jotun Penguard Midcoat M20 epoxy micaceous iron oxide intermediate paint) was 1436 μm.

[0060] Adhesion testing: The pull-off test was conducted using an adhesion tester according to ASTM D4541 standard. For the Jotun test plate in Example 1, the adhesion at the first point was 17.12 MPa and at the second point was 13.47 MPa when placed outdoors; the adhesion at the first point was 10.96 MPa and at the second point was 14.35 MPa when placed indoors. The adhesion at all test points was ≥10 MPa, meeting the technical requirements.

[0061] Examples 2 to 4 Following essentially the same method as in Example 1, application verification was conducted using two sets of epoxy zinc-rich primer (Ruiyide H06-4 (702A) + Jotun Penguard Fulfill SF solvent-free epoxy putty + Ruiyide 943 epoxy micaceous iron oxide intermediate paint) (Example 2), epoxy zinc-rich primer (Huayi H06-4 (09-378) + Jotun Penguard Fulfill SF solvent-free epoxy putty + Huayi H53-38 epoxy micaceous iron oxide intermediate paint) (Example 3), and under different ambient temperature conditions (15℃, 10℃) (Example 4). The test results show that: (1) The putty application process in each embodiment was good, and the putty surface was smooth and free of defects such as dripping.

[0062] (2) The dry film thickness of the putty layer is within the range of 1000-1600μm, which meets the design requirements.

[0063] (3) Adhesion test results: For the Ruiyide kit in Example 2, the outdoor first point adhesion was 10.91 MPa, and the indoor first point adhesion was 15.79 MPa and the second point adhesion was 15.66 MPa; for the Huayi kit in Example 3, the outdoor first point adhesion was 8.71 MPa and the second point adhesion was 9.94 MPa, and the indoor first point adhesion was 12.23 MPa and the second point adhesion was 13.34 MPa. Except for the Huayi kit, which had a slightly lower outdoor test point adhesion of 10 MPa, this was due to the difference in surface energy of the epoxy zinc-rich primer and did not affect the effectiveness of the method itself. All other tests met the technical requirements.

[0064] (4) The coating is resistant to salt water (immersion in 5% NaCl solution for 3000h) and does not bubble, crack or peel.

[0065] (5) The service life of epoxy putty reaches 75 minutes or more.

[0066] The above embodiments verify the versatility and reliability of the method of the present invention under different primer compatibility and different environmental conditions.

[0067] Those skilled in the art should understand that the above embodiments and comparative examples are only used to provide a clear and complete illustrative description of the technical solutions of the present invention, in order to meet the requirements of sufficient disclosure under patent law, and are not intended to limit the scope of protection of the present invention in any way. The inventive objective of the present invention has been fully and effectively achieved through the above technical solutions, and the application method of the high film thickness non-sagging epoxy putty of the present invention has been fully disclosed in the embodiments.

[0068] Without departing from the core inventive concept and basic principles of this invention, those skilled in the art can make conventional adjustments or equivalent substitutions to the implementation steps, test parameters, operating condition variables, and scoring weights of this invention; such variations, modifications, and substitutions that do not depart from the core principles of this invention should all be covered within the protection scope of this invention. It will be understood by those skilled in the art that various changes, modifications, substitutions, and variations can be made to these embodiments without departing from the principles and spirit of this invention, and the scope of this invention is defined by the appended claims and their equivalents.

Claims

1. A method for applying high-film-thickness, non-sagging epoxy putty by scraping, characterized in that, Includes the following steps: S1. Pre-construction preparation and working condition control: The surface of the AESS steel structure is shot-blasted to achieve a cleanliness level of Sa2½ and a roughness of 40-75μm. The primer is applied within 4 hours after treatment, and the putty is applied after the primer has cured for 72 hours. The ambient temperature is controlled to 10-35℃, the relative humidity is controlled to 50%-80%, and the wind speed is ≤0.5m / s. S2. Epoxy Putty Preparation: Solvent-free epoxy putty is selected. The main agent and curing agent are mixed at a mass ratio of 9:

1. First, pre-stir at 200r / min for 3min, then stir at 300r / min for 5min. Let stand for 2min to defoam. Under the conditions of 25±2℃, angular frequency ω=10rad / s and strain 1%, the storage modulus G' of the putty is measured using a rotational rheometer and is ≥500 Pa. S3. Layered coating application and thickness control: A two-coat coating process is adopted, with a single coating thickness of 300-500μm. After the first coat is applied, it is allowed to dry for 30 minutes before the second coat is applied. The final total dry film thickness is 800-1500μm. The coating speed is dynamically adjusted according to the temperature: 0.2-0.4m / s at 10-20℃ and 0.5-0.8m / s at 21-35℃. The coating pressure is maintained at 0.3-0.5MPa. S4. Curing and maintenance: After the coating is applied, the coating is cured in stages. First, it is surface-dry for 0-24 hours, then it is fully-dry for 24-72 hours. After the fully-dry curing, the Shore hardness reaches 75 or above. Then, it is sanded and trimmed, and finally fully cured. S5. Construction quality acceptance: Acceptance shall be carried out in accordance with the standards of no sagging or bubbles in appearance, dry film thickness deviation ±5%, and adhesion ≥10MPa.

2. The application method for high film thickness, non-sagging epoxy putty according to claim 1, characterized in that, In step S1, the surface of the primer is cleaned and roughened before the epoxy putty is mixed.

3. The application method for high film thickness, non-sagging epoxy putty according to claim 1, characterized in that, In step S1, the primer is an epoxy zinc-rich primer with a dry film thickness of 80 μm.

4. The application method for high film thickness, non-sagging epoxy putty according to claim 1, characterized in that, In step S2, the solvent-free epoxy putty has a volume solids content of 97±2%, a weight solids content of 99±1%, a density of 1.8 kg / L, and a VOC content of ≤16 g / L.

5. A method for applying high-film-thickness, non-sagging epoxy putty according to claim 4, characterized in that, In step S2, the construction window period for the solvent-free epoxy putty after mixing at 23°C is 75 minutes; when the ambient temperature is below 10°C, the material should be preheated to 25°C before mixing.

6. The application method for high film thickness, non-sagging epoxy putty according to claim 1, characterized in that, In step S3, the layered coating application is carried out using a metal scraper or a scraper made of polymer material.

7. The application method for high film thickness, non-sagging epoxy putty according to claim 1, characterized in that, In step S4, during the surface drying stage, the surface drying time is 5 hours at 5℃, 5 hours at 10℃, 3 hours at 23℃, and 2 hours at 40℃; during the solid drying stage, the time for stepping on the ground is 48 hours at 5℃, 33 hours at 10℃, 14 hours at 23℃, and 6 hours at 40℃; during the complete curing stage, the time is 21 days at 5℃, 14 days at 10℃, 7 days at 23℃, and 3 days at 40℃.

8. A method for applying high-film-thickness, non-sagging epoxy putty according to claim 1, characterized in that, In step S5, the appearance quality also includes coating flatness error ≤2mm / m.

9. A method for applying high-film-thickness, non-sagging epoxy putty by scraping according to claim 1, characterized in that, In step S5, the dry film thickness is detected using a coating thickness gauge, with 5 points tested per square meter.

Citation Information

Patent Citations

  • Construction technology for flexible epoxy putty

    CN104060785A