A high-weather-resistant, low-load-bearing modified bitumen waterproof membrane for roofing
By using silica aerogel-modified lightweight filler and chemical cross-linking technology, combined with multiple weather-resistant synergistic measures, the problems of insufficient weather resistance and excessive load of traditional modified bitumen waterproof membranes have been solved, resulting in a modified bitumen waterproof membrane with high weather resistance and low load, suitable for lightweight steel structures and existing building roofs.
Patent Information
- Application Number
- CN202611465332.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-20
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional modified bitumen waterproof membranes have insufficient weather resistance under long-term exposed use conditions, rapid degradation of thermal aging performance, and large unit area mass, making them unsuitable for scenarios such as lightweight steel structure roofs and renovation of existing building roofs.
The system employs silica aerogel-modified lightweight filler, chemical cross-linking anchoring, and multiple weather-resistant synergistic technologies. Through the combination of lightweight mineral particle layers, upper and lower modified asphalt coating layers, base reinforcement layers, and isolation layers, a multi-level porous structure and chemical cross-linking network are formed, which enhances interfacial adhesion. Combined with the synergistic effect of rutile nano-titanium dioxide and composite weather-resistant additives, the system improves weather resistance and reduces load.
It achieves improved heat resistance, low-temperature flexibility, and tackiness of the roll material while reducing the mass per unit area, enhancing interfacial bonding strength, and extending service life, making it suitable for load-sensitive roofing projects.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of building waterproofing materials technology, specifically a high weather-resistant, low-load modified bitumen waterproofing membrane for roofing. Background Technology
[0002] With the increasing demands for durability and safety in building roof waterproofing projects, traditional modified bitumen waterproof membranes generally suffer from insufficient weather resistance and rapid degradation of thermal aging performance under long-term exposed use, leading to premature failure of the waterproof layer and frequent leaks. At the same time, conventional products have a large unit area mass, placing high demands on the roof structure load, which significantly restricts their application in scenarios such as lightweight steel structure roofs, large-span spatial structures, and renovation of existing building roofs. In recent years, energy conservation, emission reduction, and lightweight design of building roofs have become important directions for industry development. Developing new modified bitumen waterproof membranes that combine excellent weather resistance and low surface density is of great significance for extending the service life of roof waterproof layers, reducing structural loads, improving construction efficiency, and promoting the green and low-carbon development of buildings.
[0003] Chinese invention patent application CN109968782A discloses a modified bitumen coating material and its preparation method, and a mineral granule modified bitumen waterproof membrane and its preparation method. By mass parts, the modified bitumen coating material includes: 45-50 parts of petroleum bitumen, 5-10 parts of hot-mix bitumen, 12-15 parts of SBS, 2-4 parts of polyethylene wax, 2-5 parts of tackifying resin, and 20-35 parts of filler. The mineral granule modified bitumen waterproof membrane overcomes the defects of existing waterproof membranes, such as insufficient base strength, poor adhesion of mineral granules, and the inability to balance the fluidity and heat resistance of the coating material.
[0004] Chinese invention patent application CN109161354A discloses a thermal insulation, sound insulation, and UV-resistant polymer self-adhesive waterproof membrane and its preparation method. The membrane includes an anti-aging layer, an AL reflective layer, a thermal insulation and sound insulation layer, a waterproof adhesive layer, and an isolation layer. The anti-aging layer is prepared by mixing PE, PET, polysulfide rubber, triethyl acetylglucosamine, and isophthalic acid ester in a mass ratio of 80:65:11:7:5. The waterproof membrane has good thermal insulation, sound insulation, and UV resistance.
[0005] The waterproof membrane in the above technical solution still uses heavy filler and high-density mineral particles as the covering material, which has a large unit area mass and a high roof static load, making it difficult to be used in load-limited scenarios such as existing building roof renovation and light steel structure roof. Summary of the Invention
[0006] The purpose of this invention is to provide a high-weather-resistant, low-load modified bitumen waterproof membrane for roofing. By using silica aerogel-modified lightweight filler, chemical cross-linking anchoring, and multiple weather-resistant synergistic technologies, it solves the problems of excessive load, insufficient weather resistance, and poor interlayer bonding of traditional modified bitumen waterproof membranes.
[0007] The objective of this invention can be achieved through the following technical solutions:
[0008] A high-weather-resistant, low-load-bearing modified bitumen waterproof membrane for roofing comprises, from top to bottom, a lightweight mineral particle layer, an upper modified bitumen coating layer, a reinforcing base layer, a lower modified bitumen coating layer, and a release layer.
[0009] The raw materials for the upper and lower modified asphalt coating layers, by weight, include 50-65 parts of 70# Grade A road asphalt, 5-10 parts of rubber softener, 3-8 parts of star-shaped SBS modifier, 2-4 parts of maleic anhydride-grafted SBS, 5-10 parts of rubber powder, 2-6 parts of styrene-butadiene rubber, 5-10 parts of lightweight filler modified silica powder, 2-4 parts of hollow glass microspheres, 0.8-1.0 parts of rutile nano titanium dioxide, 2-4 parts of C5 petroleum resin, and 0.8-3.8 parts of composite weather-resistant additives;
[0010] The lightweight mineral particle layer raw material, by mass parts, includes 42-47 parts silica aerogel composite modified suspension and 20-24 parts hydrophobic expanded perlite;
[0011] The base reinforcement layer uses 240g / m 2 Fiberglass reinforced polyester tire.
[0012] Furthermore, the specific preparation process of the silica aerogel composite modified suspension is as follows:
[0013] Anhydrous ethanol and Tween 80 were added to a reaction vessel, and silica aerogel powder was added under stirring conditions. The mixture was stirred for 20-30 minutes, and then silane coupling agent was added. The mixture was stirred for 15-20 minutes to obtain a silica aerogel composite modified suspension.
[0014] Furthermore, the mass ratio of anhydrous ethanol, Tween 80, silica aerogel powder, and silane coupling agent is 62-68:10-12:6-8:5-6.
[0015] Furthermore, the silane coupling agent is either KH-550 or KH-540.
[0016] Furthermore, the specific preparation process of the modified silica powder is as follows:
[0017] The silica aerogel composite modified suspension and silica micro powder with a particle size of 200 mesh were added to a reaction vessel, soaked at room temperature and pressure for 30-40 minutes, filtered, and dried to obtain modified silica micro powder.
[0018] Furthermore, the mass ratio of the silica aerogel composite modified suspension to silica micropowder is 42-47:20-24.
[0019] Furthermore, the specific preparation process of the lightweight mineral particle layer raw material is as follows:
[0020] A silica aerogel composite modified suspension and hydrophobic expanded perlite with a particle size of 16-40 mesh were added to a reactor, soaked at room temperature and pressure for 30-40 minutes, volatilized at room temperature, and dried to obtain a lightweight mineral particle layer raw material.
[0021] Furthermore, the specific preparation process of the modified asphalt coating material is as follows:
[0022] Add 70# Grade A road asphalt and rubber softener to a reactor and heat to 140-145℃. Then add star-shaped SBS modifier, maleic anhydride-grafted SBS, rubber powder and styrene-butadiene rubber. Raise the temperature to 160-165℃ and shear development for 1-2 hours. Then add lightweight filler modified silica powder, hollow glass microspheres, rutile nano titanium dioxide, C5 petroleum resin and composite weather-resistant additives. Stir for 30-40 minutes to obtain the modified asphalt coating material.
[0023] Furthermore, the composite weather-resistant additive is composed of antioxidant 1010, ultraviolet absorber UV-327 and carbon black in a mass ratio of 0.2-0.8:0.1-0.8:0.5-2.2.
[0024] Furthermore, the antioxidant is either antioxidant 1010 or antioxidant 1076.
[0025] Furthermore, the ultraviolet absorber is any one of the ultraviolet absorbers UV-327, UV-326, and UV-328.
[0026] Furthermore, the specific preparation process of the high weather-resistant, low-load modified bitumen waterproof membrane for roofing is as follows:
[0027] The modified bitumen coating material is evenly impregnated onto the upper and lower sides of the base reinforcement layer to form an upper modified bitumen coating layer and a lower modified bitumen coating layer. When the surface temperature of the upper modified bitumen coating layer is in a hot melt uncured state of 120-150℃, lightweight mineral particle layer material is evenly spread on its upper surface, and a pressure roller is used to press the lightweight mineral particles into the upper modified bitumen coating layer. The lower surface is covered with a PE release film and cooled and shaped to obtain a high weather-resistant and low-load modified bitumen waterproof membrane for roofing.
[0028] Furthermore, the thickness of the upper modified asphalt coating layer and the lower modified asphalt coating layer is ≥1mm.
[0029] Furthermore, the total thickness of the high weather-resistant, low-load modified bitumen waterproof membrane for roofing is 3-4 mm.
[0030] Furthermore, the pressing depth of the pressure roller is one-third to one-half the particle size of the light mineral particles.
[0031] The beneficial effects of this invention are:
[0032] 1. This invention utilizes the synergistic effect of silica aerogel-modified silica micropowder, hollow glass microspheres, and hydrophobic expanded perlite to construct a multi-level porous structure in the modified asphalt coating layer and lightweight mineral particle layer. This reduces the unit area mass of the roll material while lowering the thermal conductivity of the coating layer, which helps to reduce the load on the roof structure and reduce internal heat accumulation. It is suitable for roof projects that are sensitive to loads.
[0033] 2. This invention utilizes a silane coupling agent to introduce amino active groups on the surface of silica powder and hydrophobic expanded perlite. During hot melting and hot pressing, the amino groups undergo ring-opening amidation with the maleic anhydride-grafted SBS anhydride groups in the modified asphalt coating layer, forming a chemical cross-linking anchoring network at the interface between the coating layer and the lightweight mineral particle layer. This chemical bonding, combined with the physical interlocking of the pressure roller, helps to improve the interfacial adhesion between the lightweight coating particles and the asphalt layer, reducing the risk of particle detachment.
[0034] 3. This invention uses the multi-level porous structure inside the modified asphalt coating layer to block heat conduction, combined with the reflection and scattering of external radiation by the rutile nano-titanium dioxide and lightweight mineral particle layer, and the capture of free radicals and absorption of ultraviolet rays by the composite weather-resistant additives, to form a synergistic mechanism of internal heat insulation and surface protection, which helps to delay the thermo-oxidative aging and photodegradation of modified asphalt under long-term exposure conditions.
[0035] 4. Under the premise of low light filler content, this invention achieves good tensile properties, low temperature flexibility and tack by synergistic toughening and adhesion enhancement of star-shaped SBS, styrene-butadiene rubber, rubber powder and C5 petroleum resin, combined with chemical cross-linking interface enhancement, so that the roll material maintains good tensile properties, low temperature flexibility and tack. Moreover, the preparation process is compatible with conventional hot melt construction method and does not require additional adjustments to the existing construction method. Detailed Implementation
[0036] To further illustrate the technical means and effects of the present invention in achieving the intended purpose, the following detailed description of the specific implementation methods, features and effects of the present invention, in conjunction with preferred embodiments, is provided below.
[0037] Example 1: This example provides a high weather-resistant, low-load modified bitumen waterproof membrane for roofing, which, from top to bottom, comprises a lightweight mineral particle layer, an upper modified bitumen coating layer, a base reinforcement layer, a lower modified bitumen coating layer, and an isolation layer, and is prepared through the following steps:
[0038] S1: According to the mass fraction, 65 parts of anhydrous ethanol and 11 parts of Tween 80 were added to the reactor, 7 parts of silica aerogel powder were added at 600 r / min, and the mixture was stirred at 900 r / min for 25 min. Then, 5 parts of silane coupling agent KH-550 were added and stirred for 17 min to obtain silica aerogel composite modified suspension.
[0039] S2: According to the mass fraction, 44 parts of silica aerogel composite modified suspension and 9 parts of silica micro powder with a particle size of 200 mesh were added to the reactor, soaked at room temperature and pressure for 35 min, filtered, and the filter cake was dried at 55℃ to constant weight to obtain modified silica micro powder.
[0040] S3: According to the mass fraction, 44 parts of silica aerogel composite modified suspension and 22 parts of hydrophobic expanded perlite with a particle size of 28 mesh were added to the reactor, soaked at room temperature and pressure for 35 minutes, removed and volatilized at room temperature in a fume hood for 25 hours, and dried at 55℃ for 25 hours to obtain the light mineral particle layer raw material.
[0041] S4: According to the mass fraction, 57 parts of 70# Grade A road asphalt and 7 parts of rubber softener were added to the reactor and heated to 142℃. Then, 5 parts of star-shaped SBS modifier, 3 parts of maleic anhydride-grafted SBS, 7.5 parts of rubber powder and 4 parts of styrene-butadiene rubber were added. The temperature was raised to 162℃ at a shear rate of 4100 r / min and sheared for 1.5 h. Then, 7 parts of lightweight filler modified silica powder, 3 parts of hollow glass microspheres, 0.9 parts of rutile nano titanium dioxide, 0.5 parts of antioxidant 1010, 0.4 parts of ultraviolet absorber UV-327, 3 parts of C5 petroleum resin and 1.3 parts of carbon black were added and stirred for 35 min to obtain the modified asphalt coating material.
[0042] S5: The modified asphalt coating material is evenly impregnated onto the base reinforcement layer (using 240g / m²). 2On both sides of the fiberglass reinforced polyester membrane, an upper modified bitumen coating layer and a lower modified bitumen coating layer are formed. The thickness of the coating layer on each side is controlled to be ≥1mm, and the total thickness is 3mm. At the end of the roll production line, when the surface temperature of the upper modified bitumen coating layer is in a hot-melt uncured state of 135℃, lightweight mineral granule raw materials are evenly spread on its surface, and a pressure roller is used to press the lightweight mineral granules into the upper modified bitumen coating layer. The pressing depth is one-third to one-half of the particle size of the lightweight mineral granules. The lower surface is covered with a PE release film and cooled and shaped to obtain a high weather-resistant and low-load modified bitumen waterproof roll for roofing.
[0043] By treating silica micropowder and hydrophobic expanded perlite with silica aerogel and KH-550 modification system respectively, amino silane segments are loaded on the surface of both. During hot melting and hot pressing, the anhydride groups of maleic anhydride grafted with SBS undergo ring-opening amidation reaction with the amino groups of modified silica micropowder and light mineral particles, forming a chemical cross-linking anchoring network between the modified asphalt coating layer and the light mineral particle layer, significantly improving the interlayer bonding strength. At the same time, modified silica micropowder and hollow glass microspheres construct a multi-level porous structure in the modified asphalt coating layer, synergistically reducing thermal conductivity and density. Combined with the hydrophobic expanded perlite in the light mineral particle layer and the nano titanium dioxide in the modified asphalt coating layer, a dual weather-resistant barrier of internal heat insulation and surface reflection is formed.
[0044] Example 2: This example provides a high weather-resistant, low-load modified bitumen waterproof membrane for roofing, which, from top to bottom, comprises a lightweight mineral particle layer, an upper modified bitumen coating layer, a base reinforcement layer, a lower modified bitumen coating layer, and an isolation layer, and is prepared through the following steps:
[0045] S1: According to the mass fraction, 62 parts of anhydrous ethanol and 10 parts of Tween 80 were added to the reactor, 6 parts of silica aerogel powder were added at 550 r / min, and the mixture was stirred at 850 r / min for 20 min. Then, 5 parts of silane coupling agent KH-550 were added and stirred for 15 min to obtain silica aerogel composite modified suspension.
[0046] S2: According to the mass fraction, 42 parts of silica aerogel composite modified suspension and 8 parts of silica micro powder with a particle size of 200 mesh were added to the reactor, soaked at room temperature and pressure for 30 min, filtered, and the filter cake was dried at 50℃ to constant weight to obtain modified silica micro powder.
[0047] S3: According to the mass fraction, 42 parts of silica aerogel composite modified suspension and 20 parts of hydrophobic expanded perlite with a particle size of 16 mesh were added to the reactor, soaked at room temperature and pressure for 30 min, removed and volatilized at room temperature in a fume hood for 24 h, and dried at 50℃ for 24 h to obtain the light mineral particle layer raw material.
[0048] S4: According to the mass fraction, add 50 parts of 70# Grade A road asphalt and 5 parts of rubber softener to the reactor, heat to 140℃, then add 3 parts of star-shaped SBS modifier, 2 parts of maleic anhydride grafted SBS, 5 parts of rubber powder and 2 parts of styrene-butadiene rubber, and heat to 160℃ under a shear rate of 4000 r / min, shear development for 1 h, then add 5 parts of lightweight filler modified silica powder, 2 parts of hollow glass microspheres, 0.8 parts of rutile nano titanium dioxide, 0.2 parts of antioxidant 1010, 0.1 parts of ultraviolet absorber UV-327, 2 parts of C5 petroleum resin and 0.5 parts of carbon black, stir for 30 min to obtain the modified asphalt coating material.
[0049] S5: The modified asphalt coating material is evenly impregnated onto the base reinforcement layer (using 240g / m²). 2 On both sides of the fiberglass reinforced polyester membrane, an upper modified bitumen coating layer and a lower modified bitumen coating layer are formed. The thickness of the coating layer on each side is controlled to be ≥1mm, and the total thickness is 3mm. At the end of the roll production line, when the surface temperature of the upper modified bitumen coating layer is in a hot-melt uncured state of 120℃, lightweight mineral granule raw materials are evenly spread on its surface, and a pressure roller is used to press the lightweight mineral granules into the upper modified bitumen coating layer. The pressing depth is one-third to one-half of the particle size of the lightweight mineral granules. The lower surface is covered with a PE release film and cooled and shaped to obtain a high weather-resistant and low-load modified bitumen waterproof roll for roofing.
[0050] Example 3: This example provides a high weather-resistant, low-load modified bitumen waterproof membrane for roofing, which, from top to bottom, comprises a lightweight mineral particle layer, an upper modified bitumen coating layer, a base reinforcement layer, a lower modified bitumen coating layer, and an isolation layer, and is prepared through the following steps:
[0051] S1: According to the mass fraction, 68 parts of anhydrous ethanol and 12 parts of Tween 80 were added to the reactor, 8 parts of silica aerogel powder were added at 650 r / min, and the mixture was stirred at 950 r / min for 30 min. Then, 6 parts of silane coupling agent KH-550 were added and stirred for 20 min to obtain silica aerogel composite modified suspension.
[0052] S2: According to the mass fraction, 47 parts of silica aerogel composite modified suspension and 10 parts of silica micro powder with a particle size of 200 mesh were added to the reactor, soaked at room temperature and pressure for 40 min, filtered, and the filter cake was dried at 60℃ to constant weight to obtain modified silica micro powder.
[0053] S3: According to the mass fraction, 47 parts of silica aerogel composite modified suspension and 24 parts of hydrophobic expanded perlite with a particle size of 40 mesh were added to the reactor and soaked at room temperature and pressure for 40 min. After being taken out, the mixture was volatilized at room temperature in a fume hood for 26 h and dried at 60℃ for 26 h to obtain the light mineral particle layer raw material.
[0054] S4: According to the mass fraction, 65 parts of 70# Grade A road asphalt and 10 parts of rubber softener were added to the reactor and heated to 145℃. Then, 8 parts of star-shaped SBS modifier, 4 parts of maleic anhydride-grafted SBS, 10 parts of rubber powder and 6 parts of styrene-butadiene rubber were added. The temperature was raised to 165℃ under a shear rate of 4200 r / min and sheared for 2 hours. Then, 10 parts of lightweight filler modified silica powder, 4 parts of hollow glass microspheres, 1.0 part of rutile nano titanium dioxide, 0.8 parts of antioxidant 1010, 0.8 parts of ultraviolet absorber UV-327, 4 parts of C5 petroleum resin and 2.2 parts of carbon black were added and stirred for 40 minutes to obtain the modified asphalt coating material.
[0055] S5: The modified asphalt coating material is evenly impregnated onto the base reinforcement layer (using 240g / m²). 2 On both sides of the fiberglass reinforced polyester membrane, an upper modified bitumen coating layer and a lower modified bitumen coating layer are formed. The thickness of the coating layer on each side is controlled to be ≥1mm, and the total thickness is 4mm. At the end of the roll production line, when the surface temperature of the upper modified bitumen coating layer is in a hot-melt uncured state of 150℃, lightweight mineral granule raw materials are evenly spread on its upper surface, and a pressure roller is used to press the lightweight mineral granules into the upper modified bitumen coating layer. The pressing depth is one-third to one-half of the particle size of the lightweight mineral granules. The lower surface is covered with a PE release film and cooled and shaped to obtain a high weather-resistant and low-load modified bitumen waterproof roll for roofing.
[0056] Example 4: This example provides a high weather-resistant and low-load modified bitumen waterproof membrane for roofing. The difference from Example 1 is that KH-540 is used instead of KH-550 in step S1.
[0057] Example 5: This example provides a high weather-resistant and low-load modified bitumen waterproof membrane for roofing. The difference from Example 1 is that antioxidant 1076 is used instead of antioxidant 1010 in step S4.
[0058] Example 6: This example provides a high weather-resistant and low-load modified bitumen waterproof membrane for roofing. The difference from Example 1 is that UV absorber UV-326 is used instead of UV absorber UV-327 in step S4.
[0059] The sources of some of the raw materials involved in the examples are as follows:
[0060] Silica aerogel powder: porosity ≥90%, purchased from Langfang Langkes New Material Technology Co., Ltd.
[0061] Silica powder: particle size 200 mesh, density 2.8 g / cm³ 3 The materials were purchased from Hebei Guanchuan New Materials Technology Co., Ltd.
[0062] Hydrophobic expanded perlite: particle size 16-40 mesh, purchased from Lingshou County Chengyang Mining Co., Ltd.;
[0063] 70# Grade A road asphalt: purchased from Hebei Xinhai Chemical Group Co., Ltd.;
[0064] Rubber softener: also known as asphalt modifier, purchased from Panjin Hansen Petrochemical Co., Ltd.;
[0065] Star-shaped SBS modifier: Model LG411S, purchased from Tianjin LG Botian Chemical Co., Ltd.;
[0066] Maleic anhydride-grafted SBS: injection molding grade, model SH014-ZH, purchased from Dongguan Shenghao Plastic Raw Materials Co., Ltd.
[0067] Rubber powder: 60 mesh particle size, purchased from Liaoning Fengyue Renewable Resources Co., Ltd.
[0068] Styrene-butadiene rubber: 92% content, purchased from Shandong Haifang Rubber Technology Co., Ltd.
[0069] Hollow glass microspheres: Model TTC40, purchased from Xinyang City Bolite Perlite Technology Co., Ltd.;
[0070] Rutile nano titanium dioxide: premium grade, brand Lanke Titanium, purchased from Langfang Lanke Chemical Group Co., Ltd.
[0071] Antioxidants 1010 and 1067: Compound B225, purchased from Beijing Tiangang Additives Co., Ltd.
[0072] UV absorbers UV-327 and UV-326: purchased from Shandong Tunan New Materials Co., Ltd.
[0073] C5 petroleum resin: CAS No. 156-66-52, purity 99%, purchased from Puyang Ruicheng Chemical Co., Ltd.;
[0074] Carbon black: Model HC3505, purchased from Zibo Heli Pigment Co., Ltd.
[0075] Comparative Example 1: This comparative example provides a high weather-resistant and low-load modified bitumen waterproof membrane for roofing. The difference from Example 1 is that silica powder is used instead of modified silica powder in step S4.
[0076] Comparative Example 2: This comparative example provides a high weather-resistant, low-load modified bitumen waterproof membrane for roofing. The difference from Example 1 is that hydrophobic expanded perlite is used instead of lightweight mineral particle layer raw material in step S5.
[0077] Comparative Example 3: This comparative example provides a high weather-resistant, low-load modified bitumen waterproof membrane for roofing. The difference from Example 1 is that maleic anhydride-grafted SBS, rutile nano-titanium dioxide, C5 petroleum resin, and hollow glass microspheres are removed in step S4.
[0078] The performance of the high weather-resistant, low-load modified bitumen waterproof membranes for roofing prepared in Examples 1-6 and Comparative Examples 1-3 was tested.
[0079] Referring to GB 23441-2009 "Self-adhesive polymer-modified bitumen waterproof membrane", the heat resistance, low temperature performance, elongation at break, tack, peel strength and impermeability of the waterproof membrane were tested.
[0080] Weather resistance: Refer to GB 18242-2008 "Elastomer Modified Bituminous Waterproof Membrane" standard.
[0081] The test results are as follows:
[0082] Table 1 Performance Test Overview
[0083] project Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Comparative Example 1 Comparative Example 2 Comparative Example 3 <![CDATA[Mass per unit area (kg / m 2 )]]> 3.15 3.30 4.05 3.12 3.16 3.15 3.45 3.55 3.55 Heat resistance (°C) 105 100 110 105 105 102 98 100 95 Low-temperature flexibility (°C) -30 -25 -35 -30 -30 -30 -20 -22 -15 Tensile force (N / 50mm) 1180 1080 1280 1190 1170 1180 980 1020 860 Elongation at break (%) 50 45 55 51 49 50 40 42 32 Holding power (min) 35 28 42 36 34 35 22 24 18 Peel strength (N / mm) 1.8 1.5 2.0 1.8 1.8 1.8 1.2 1.3 1.0 Impermeability (0.2MPa, 120min) impermeable impermeable impermeable impermeable impermeable impermeable impermeable impermeable impermeable Tensile strength retention rate (%) after 1500 hours of artificial climate aging 92 85 94 93 88 89 76 78 62 Elongation retention rate (%) after 1500 hours of artificial climate aging 88 82 91 89 85 86 74 75 58
[0084] As shown in Table 1, the unit area mass of Examples 1-6 is relatively light, which may be due to the synergistic density reduction effect of lightweight fillers and hollow glass microspheres. The hydrophobic expanded perlite in the lightweight mineral particle layer is also a porous lightweight material, which reduces the weight of the roll material.
[0085] As shown in Table 1, the heat resistance of Examples 1-6 is higher than that of Comparative Examples 1 and 3. This may be because the star-shaped SBS modifier, maleic anhydride-grafted SBS and C5 petroleum resin in Examples 1-6 work together to form a stable three-dimensional cross-linked network in the asphalt matrix, which significantly improves the high-temperature deformation resistance of the modified asphalt.
[0086] As shown in Table 1, the low-temperature flexibility of Examples 1-6 is better than that of Comparative Examples 1-3. This may be because after the modified silica micropowder and lightweight mineral particles are modified by silica aerogel and silane coupling agent, the aminosilane segments loaded on the surface undergo ring-opening amidation reaction with the anhydride groups of maleic anhydride-grafted SBS, forming chemical crosslinks at the interface between the filler and the asphalt, reducing stress concentration defects. At the same time, styrene-butadiene rubber, rubber powder and star-shaped SBS synergistically toughen the material.
[0087] As shown in Table 1, the tensile strength and elongation at break of Examples 1-6 are higher than those of Comparative Examples 1-3. This may be because the amino groups on the surface of the modified silica powder and modified hydrophobic expanded perlite react chemically with the anhydride groups of maleic anhydride grafted onto SBS to form a chemically cross-linked anchoring network, which significantly enhances the interfacial bonding strength and stress transfer efficiency between the filler and the asphalt matrix.
[0088] As shown in Table 1, the tackiness of Examples 1-6 is higher than that of Comparative Examples 1-3. This may be because the tackifying effect of C5 petroleum resin and the interfacial compatibilizing effect of maleic anhydride-grafted SBS synergistically improve the cohesive strength and adhesion performance of the modified asphalt.
[0089] As shown in Table 1, the interlayer peel strength of Examples 1-6 is significantly higher than that of Comparative Examples 1-3. This may be because the light mineral particle layer raw material and the modified silica powder are loaded with amino groups on their surface after being modified by KH-550 or KH-540. During the hot melting and hot pressing process, they undergo ring-opening amidation reaction with the anhydride groups of maleic anhydride grafted with SBS, forming a chemical cross-linked anchoring network between the modified asphalt coating layer and the light mineral particle layer.
[0090] As shown in Table 1, the tensile strength retention rate and elongation retention rate of Examples 1-6 after 1500 hours of artificial climate aging are higher than those of Comparative Examples 1-3. This may be because the composite weathering additive (antioxidant + ultraviolet absorber + carbon black) in the examples, together with the rutile nano-titanium dioxide, hollow glass microspheres and aerogel modification system, form multiple weathering barriers with internal antioxidant and heat insulation and surface ultraviolet shielding and reflection. At the same time, the chemical cross-linking network reduces the aging cracks at the interface between the filler and the asphalt.
[0091] It should be noted that, in this document, terms such as “comprising,” “including,” or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus.
[0092] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention.
Claims
1. A high-weather-resistant, low-load-bearing modified bitumen waterproof membrane for roofing, comprising, from top to bottom, a lightweight mineral particle layer, an upper modified bitumen coating layer, a reinforcing base layer, a lower modified bitumen coating layer, and a release layer, characterized in that, The raw materials for the upper and lower modified asphalt coating layers, by weight, include 50-65 parts of 70# Grade A road asphalt, 5-10 parts of rubber softener, 3-8 parts of star-shaped SBS modifier, 2-4 parts of maleic anhydride-grafted SBS, 5-10 parts of rubber powder, 2-6 parts of styrene-butadiene rubber, 5-10 parts of lightweight filler modified silica powder, 2-4 parts of hollow glass microspheres, 0.8-1.0 parts of rutile nano-titanium dioxide, 2-4 parts of C5 petroleum resin, and 0.8-3.8 parts of composite weather-resistant additives. The lightweight mineral particle layer raw material, by mass, includes 42-47 parts silica aerogel composite modified suspension and 20-24 parts hydrophobic expanded perlite. The tire base reinforcement layer uses 240g / m 2 Fiberglass reinforced polyester tire.
2. The high weather-resistant, low-load modified bitumen waterproof membrane for roofing according to claim 1, characterized in that, The specific preparation process of the silica aerogel composite modified suspension is as follows: Anhydrous ethanol and Tween 80 were added to a reaction vessel, and silica aerogel powder was added under stirring conditions. The mixture was stirred for 20-30 minutes, and then silane coupling agent was added. The mixture was stirred for 15-20 minutes to obtain a silica aerogel composite modified suspension.
3. The high weather-resistant, low-load modified bitumen waterproof membrane for roofing according to claim 2, characterized in that, The mass ratio of anhydrous ethanol, Tween 80, silica aerogel powder and silane coupling agent is 62-68:10-12:6-8:5-6; The silane coupling agent is either KH-550 or KH-540.
4. The high weather-resistant, low-load modified bitumen waterproof membrane for roofing according to claim 1, characterized in that, The specific preparation process of the modified silica powder is as follows: The silica aerogel composite modified suspension and silica micro powder with a particle size of 200 mesh were added to a reaction vessel, soaked at room temperature and pressure for 30-40 minutes, filtered, and dried to obtain modified silica micro powder.
5. The high weather-resistant, low-load modified bitumen waterproof membrane for roofing according to claim 4, characterized in that, The mass ratio of the silica aerogel composite modified suspension to silica micropowder is 42-47:20-24.
6. The high weather-resistant, low-load modified bitumen waterproof membrane for roofing according to claim 1, characterized in that, The specific preparation process of the lightweight mineral particle layer raw material is as follows: A silica aerogel composite modified suspension and hydrophobic expanded perlite with a particle size of 16-40 mesh were added to a reactor, soaked at room temperature and pressure for 30-40 minutes, volatilized at room temperature, and dried to obtain a lightweight mineral particle layer raw material.
7. The high weather-resistant, low-load modified bitumen waterproof membrane for roofing according to claim 1, characterized in that, The specific preparation process of the modified asphalt coating material is as follows: Add 70# Grade A road asphalt and rubber softener to a reactor and heat to 140-145℃. Then add star-shaped SBS modifier, maleic anhydride-grafted SBS, rubber powder and styrene-butadiene rubber. Raise the temperature to 160-165℃ and shear development for 1-2 hours. Then add lightweight filler modified silica powder, hollow glass microspheres, rutile nano titanium dioxide, C5 petroleum resin and composite weather-resistant additives. Stir for 30-40 minutes to obtain the modified asphalt coating material.
8. A high-weather-resistant, low-load-bearing modified bitumen waterproof membrane for roofing according to claim 7, characterized in that, The composite weather-resistant additive is composed of antioxidants, ultraviolet absorbers, and carbon black in a mass ratio of 0.2-0.8:0.1-0.8:0.5-2.
2. The antioxidant is either antioxidant 1010 or antioxidant 1076; The ultraviolet absorber is any one of ultraviolet absorbers UV-327, UV-326, and UV-328.
9. The high weather-resistant, low-load modified bitumen waterproof membrane for roofing according to claim 1, characterized in that, The specific preparation process of the high weather-resistant, low-load modified bitumen waterproof membrane for roofing is as follows: The modified bitumen coating material is evenly impregnated onto the upper and lower sides of the base reinforcement layer to form an upper modified bitumen coating layer and a lower modified bitumen coating layer. When the surface temperature of the upper modified bitumen coating layer is in a hot melt uncured state of 120-150℃, lightweight mineral particle layer material is evenly spread on its upper surface, and a pressure roller is used to press the lightweight mineral particles into the upper modified bitumen coating layer. The lower surface is covered with a PE release film and cooled and shaped to obtain a high weather-resistant and low-load modified bitumen waterproof membrane for roofing.
10. A high-weather-resistant, low-load-bearing modified bitumen waterproof membrane for roofing according to claim 9, characterized in that, The thickness of the upper modified asphalt coating layer and the lower modified asphalt coating layer is ≥1mm; The total thickness of the high weather-resistant, low-load modified bitumen waterproof membrane used for roofing is 3-4 mm; The pressing depth of the pressure roller is one-third to one-half of the particle size of the light mineral particles.
Citation Information
Patent Citations
Self adhered polymer waterproofing membrane with functions in heat insulation, sound insulation and ultraviolet resistance and preparation method thereof
CN109161354A
Modified asphalt coating material and preparation method thereof and mineral pellet-modified asphalt waterproof coil material and preparation method of mineral pellet-modified asphalt waterproof coil material
CN109968782A