Aero-engine tooth seal structure and preparation method

By employing a gradient multilayer structure and surface microtexture in the aero-engine comb seal structure, the problem of interfacial thermal stress concentration caused by the difference in thermal expansion coefficients between the copper-silver-zinc alloy ring and the nickel-based high-temperature alloy bushing was solved, thereby improving the bonding strength and service life.

CN123109792APending Publication Date: 2026-11-17HANGFA GENERAL AVIATION POWER TECHNOLOGY (SHANGHAI) CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611611782.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing aero-engine comb seal structures, the difference in thermal expansion coefficients between the copper-silver-zinc alloy ring and the nickel-based high-temperature alloy bushing leads to concentrated thermal stress at the interface, making them prone to cracking. Furthermore, the existing diffusion welding schemes, with their single copper intermediate layer, are insufficient in relieving thermal stress and have a single interface bonding mechanism, resulting in problems such as interface cracking and insufficient bonding strength.

Method used

A gradient multilayer structure is adopted, including a Ni layer, a NiCu layer, a CuAg layer, and an Ag layer. The layers are metallurgically bonded by high-temperature diffusion welding, forming a gradient transition in the coefficient of thermal expansion from the alloy bushing side to the copper-silver-zinc alloy ring side. Combined with surface microtexture, micro-mechanical interlocking is achieved, enhancing the interfacial bonding strength.

Benefits of technology

It effectively alleviates the concentration of thermal stress at the interface, improves the service life of the structure under thermal cycling conditions, enhances the interface bonding strength, reduces the risk of interface cracking, and improves the joint toughness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123109792A_ABST
    Figure CN123109792A_ABST
Patent Text Reader

Abstract

This invention discloses a serrated sealing structure for an aero-engine and its fabrication method, comprising: an alloy bushing and a copper-silver-zinc alloy ring coaxially disposed within the inner hole of the alloy bushing, and a gradient multilayer structure metallurgically bonded and fixed between the alloy bushing and the copper-silver-zinc alloy ring by high-temperature diffusion welding; the inner ring surface of the alloy bushing is also machined with a serrated structure, and the gradient multilayer structure is metallurgically bonded and fixed to the outer surface of the serrated structure along the tooth profile. The gradient multilayer structure is formed by sequentially stacking multiple different materials to ensure that the coefficient of thermal expansion of the serrated sealing structure gradually increases from the alloy bushing side to the copper-silver-zinc alloy ring side, thereby alleviating thermal stress concentration. This invention, through the gradient multilayer structure, achieves a gradual transition in the coefficient of thermal expansion at the interface, avoiding abrupt changes in thermal strain at a single interface, thus effectively reducing thermal stress concentration at the interface and is expected to significantly improve the service life of the structure under thermal cycling conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of aero-engine technology, and in particular, to an aero-engine tooth sealing structure. Furthermore, this invention also relates to a method for fabricating an aero-engine tooth sealing structure. Background Technology

[0002] Grate seals are a type of non-contact dynamic sealing structure widely used in aero-engines, primarily for oil-gas isolation in compressor stage, turbine stage, blade tip, and bearing cavity lubrication sealing systems. Grate seals utilize the sudden expansion and contraction of channels to increase flow resistance and limit fluid leakage. When fluid passes through the throttling gap, the pressure energy of the upstream fluid is converted into velocity energy through the throttling effect, and then dissipated as heat energy through turbulent vortices within the tooth cavity.

[0003] In the compressor and turbine components of aero-engines, the teeth and sealing rings experience rubbing contact during high-speed rotation. Therefore, a copper-silver-zinc alloy, possessing good thermal conductivity, low hardness, and excellent lubrication and plasticity, is typically used as the wear layer for the sealing rings. A common approach is to apply a copper-silver-zinc alloy wear sealing layer to the inner surface of the alloy bushing (such as nickel-based high-temperature alloy bushings like GH600 and GH4169). During rotation, the sealing teeth scrape against this layer, thus achieving both lubrication and sealing.

[0004] (1) Limitations of thermal spraying process Existing copper-silver-zinc wear seals typically employ thermal spraying, directly applying copper-silver-zinc alloy powder to the inner surface of the alloy bushing. However, coatings produced using this spraying process should not be too thick, and the adhesion between the coating and the substrate is not high. This process suffers from the following problems: ① Insufficient coating bonding strength: The sprayed coating mainly relies on mechanical interlocking with the substrate and lacks metallurgical bonding, resulting in limited bonding strength. During use, the coating is prone to blistering and peeling due to insufficient bonding force. ② Bubbling defects during processing: Bubbling defects may occur during the spraying process, affecting product quality and first-pass yield; ③ Failure during service: The coating is prone to oxidation, blistering and peeling during use, which reduces the sealing and lubrication effect of the coating on engine parts and thus affects the performance of the engine.

[0005] (2) Deficiencies of the existing diffusion welding solution (CN105665912A) Patent CN105665912A discloses a diffusion welding method for an engine sealing structure, which uses a prefabricated copper-silver-zinc alloy ring to replace the thermal spray coating and achieves the connection through diffusion welding. The main technical features of this solution include: plating a single copper layer (thickness 0.005-0.008 mm) on the alloy bushing or the copper-silver-zinc alloy ring; an interference fit between the copper-silver-zinc alloy ring and the alloy bushing (interference amount 0.03-0.05 mm); and performing diffusion welding at 715-725℃ for 180-240 minutes.

[0006] The following problems exist with this scheme (2): 1. Limitations of a single copper interlayer: Using only a single copper layer as an interlayer is insufficient to fully alleviate the thermal stress caused by the difference in thermal expansion coefficients between the copper-silver-zinc alloy (thermal expansion coefficient of approximately 19×10-6 / ℃) and the nickel-based high-temperature alloy (thermal expansion coefficient of approximately 13×10-6 / ℃). Under the high-temperature alternating load conditions of actual engine operation, the concentration of interfacial thermal stress is still prominent, and there is a risk of interfacial cracking. 2. Problems caused by interference fit: Interference fit (0.03~0.05mm) will generate large assembly stress during the assembly process, which may cause uneven deformation of copper-silver-zinc alloy ring and affect the uniformity of sealing gap; at the same time, interference fit has extremely high requirements for the machining accuracy of parts, which increases manufacturing cost and machining difficulty. 3. Simple interface bonding mechanism: It relies solely on the metallurgical bonding of diffusion welding, lacks additional mechanical reinforcement mechanisms, and has limited room for improvement in interface bonding strength. 4. Cr precipitation problem: During the diffusion bonding process between nickel-based superalloys (such as GH600) and copper-silver-zinc alloys, Cr elements are prone to precipitate and accumulate at the interface, producing CrP brittle phase, which leads to joint embrittlement and reduces welding quality. Summary of the Invention

[0007] This invention provides a sealing structure and preparation method for aero-engine gratings to solve the problem of interface thermal stress concentration and easy cracking caused by the large difference in thermal expansion coefficients between the copper-silver-zinc alloy ring and the nickel-based high-temperature alloy bushing in the prior art. At the same time, it solves the technical problems of insufficient thermal stress relief and single interface bonding mechanism in the existing diffusion welding scheme.

[0008] The technical solution adopted in this invention is as follows: A comb-shaped sealing structure for an aero-engine includes: an alloy bushing and a copper-silver-zinc alloy ring coaxially disposed in the inner hole of the alloy bushing, and a gradient multilayer structure metallurgically bonded and fixed between the alloy bushing and the copper-silver-zinc alloy ring by high-temperature diffusion welding; the inner ring surface of the alloy bushing is also machined with a comb-shaped structure, and the gradient multilayer structure is also metallurgically bonded and fixed to the outer surface of the comb-shaped structure along the tooth shape direction. The gradient multilayer structure is formed by stacking multiple different materials in sequence to make the coefficient of thermal expansion of the comb-shaped sealing structure gradually increase from the alloy bushing side to the copper-silver-zinc alloy ring side to alleviate thermal stress concentration.

[0009] Furthermore, the gradient multilayer structure includes a Ni layer, a NiCu layer, a CuAg layer, and an Ag layer stacked sequentially. The Ni layer is metallurgically bonded to the inner ring wall of the alloy bushing and the outer surface of the comb structure, and the Ag layer is metallurgically bonded to the outer ring wall of the copper-silver-zinc alloy ring.

[0010] Furthermore, the thickness of the Ni layer is 0.008–0.015 mm, the thickness of the NiCu layer is 0.010–0.020 mm, the thickness of the CuAg layer is 0.010–0.020 mm, the thickness of the Ag layer is 0.003–0.008 mm, and the total thickness of the gradient multilayer structure is 0.031–0.063 mm.

[0011] Furthermore, the tooth surfaces and cavity surfaces of the comb structure, as well as the inner ring wall of the alloy bushing, are all machined with several micron-sized pits to form a surface microtexture; the gradient multilayer structure is also used to melt and fill the micropits during the diffusion welding process to form a micro-mechanical interlock after solidification.

[0012] Furthermore, each micropit has a diameter of 80–150 μm and a depth of 20–40 μm, and the center distance between two adjacent micropits is 150–300 μm. The area occupied by several micropits on the inner ring wall of the alloy bushing and the outer surface of the comb structure is 30%–60%.

[0013] According to another aspect of the present invention, a method for preparing a serrated sealing structure is also provided, for preparing an aero-engine serrated sealing structure as described above. The preparation method includes the following steps: preliminary preparation: preparing an alloy bushing with a serrated structure on the inner ring wall and a copper-silver-zinc alloy ring; preparing a gradient multilayer structure: preparing a gradient multilayer structure on the inner ring wall of the alloy bushing and the outer surface of the serrated structure using plasma spraying or multilayer annular foil stacking method; dissimilar alloy assembly: positioning and installing the copper-silver-zinc alloy ring into the gradient multilayer structure to form an assembly; diffusion welding: placing the assembly into a vacuum diffusion welding device for vacuum high-temperature diffusion welding.

[0014] Furthermore, the inner ring wall and outer surface of the comb structure of the alloy bushing prepared in step "Preliminary Preparation" also have a surface microtexture formed by micro-pits with several micrometer-sized pores; the preparation of the alloy bushing in step "Preliminary Preparation" specifically includes the following steps: precision machining of the inner hole of the alloy bushing; machining of the comb structure of the inner ring wall of the alloy bushing; pre-cleaning; preparation of the surface microtexture of the inner ring wall and outer surface of the comb structure of the alloy bushing; post-cleaning and finishing of the surface microtexture.

[0015] Furthermore, the step "Preparation of Gradient Multilayer Structure" employs plasma spraying, specifically including the following steps: Plasma spraying gradient layer: Pure Ni powder, NiCu alloy powder, CuAg alloy powder, and pure Ag powder are sequentially sprayed onto the inner ring surface of the alloy bushing using plasma gradient spraying equipment to form a gradient multilayer structure; Hot isostatic pressing densification treatment: The entire alloy bushing after spraying is subjected to hot isostatic pressing densification treatment; Precise inner hole calibration: The inner ring of the alloy bushing is micro-finished according to assembly requirements.

[0016] Furthermore, in the step "Preparation of gradient multilayer structure", a multilayer annular foil stacking method is used. The specific operation is as follows: pure Ni annular foil, NiCu alloy annular foil, CuAg alloy annular foil, and pure Ag annular foil are stacked sequentially on the inner ring surface of the alloy bushing.

[0017] Furthermore, in the step "dissimilar alloy assembly", the copper-silver-zinc alloy ring gap is inserted into the inner hole of the gradient multilayer structure to achieve a gap of 0.01–0.03 mm between them; in the step "diffusion welding forming", the welding temperature is 700–730℃; the welding pressure is 5–15 MPa; the holding time is 120–180 minutes; and the vacuum degree is ≤5×10⁻⁶. -3 Pa; After completing the "diffusion welding forming" step, the following steps are also included: Finished product inspection: The finished product of the comb sealing structure is inspected for dimensional accuracy, interface bonding quality, and sealing gap uniformity.

[0018] The present invention has the following beneficial effects: In existing technologies, the coefficient of thermal expansion of copper-silver-zinc alloys is approximately 19 × 10⁻⁶. -6 At / ℃, the coefficient of thermal expansion of nickel-based superalloys (such as GH600) is approximately 13×10⁻⁶. -6 The difference between the two is significant, and this thermal expansion mismatch will generate large thermal stress at the interface during the diffusion welding cooling process and the actual service thermal cycle of the engine. In the aero-engine comb seal structure of this invention, a gradient multilayer structure is metallurgically bonded and fixed between the alloy bushing and the copper-silver-zinc alloy ring by high-temperature diffusion welding. This gradient multilayer structure is formed by sequentially stacking various different materials to reduce the thermal expansion coefficient of the comb seal structure from Ni (approximately 13 × 10⁻⁶) to Ni (approximately 13 × 10⁻⁶). -6 / ℃) towards copper-silver-zinc alloy (approximately 19×10) -6 The coefficient of thermal expansion (C / ℃) increases gradually. This gradient in the coefficient of thermal expansion allows for a gradual transition in interfacial thermal strain, avoiding abrupt changes in thermal strain at a single interface. This effectively reduces thermal stress concentration at the interface and is expected to significantly improve the service life of the structure under thermal cycling conditions. Compared to a single copper interlayer (C / ℃), which has a coefficient of thermal expansion of approximately 17 × 10⁻⁶, this gradient is more efficient. -6 / ℃, which is significantly different from the base materials on both sides), the gradient design of the present invention has a significant advantage in relieving thermal stress, and it solves the problem of thermal expansion mismatch between dissimilar metals from the material source; In the method for preparing the comb-like sealing structure of this invention, a gradient multilayer structure is prepared on the inner ring wall of the alloy bushing and the outer surface of the comb-like structure 11 using plasma spraying or multilayer annular foil stacking, so that the coefficient of thermal expansion is lower than that of the alloy bushing side (approximately 13 × 10⁻⁶). -6 / ℃) toward the copper-silver-zinc alloy ring side (approximately 19×10) -6 The gradient multilayer structure features a smooth transition (at / ℃), avoiding the concentration of interfacial thermal stress caused by abrupt changes in the coefficient of thermal expansion in a single copper intermediate layer. This gradient multilayer transition design solves the problem of thermal expansion mismatch between dissimilar metals from the material's fundamental perspective. The Ni layer in the gradient multilayer structure has good solid solubility with Cr at high temperatures, and Cr tends to dissolve in the Ni layer rather than agglomerate at the interface, thus effectively reducing the formation of brittle CrP phases and improving joint toughness. This invention provides two parallel gradient multilayer preparation methods: plasma spraying and foil stacking. Enterprises can flexibly choose according to the inner hole size and existing equipment conditions, exhibiting strong industrial adaptability.

[0019] In addition to the objectives, features, and advantages described above, the present invention has other objectives, features, and advantages. The invention will now be described in further detail with reference to the figures. Attached Figure Description

[0020] The accompanying drawings, which form part of this application, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings: Figure 1 This is a schematic diagram of the aero-engine comb seal structure according to a preferred embodiment of the present invention; Figure 2 This is a schematic diagram of the surface microtexture of the alloy bushing grate structure (before the gradient multilayer structure is set); Figure 3 This is a schematic diagram of the distribution of multilayer structures in a gradient multilayer structure; Figure 4 The process flow diagram of the method for preparing the toothed sealing structure of the present invention.

[0021] Legend: 1. Alloy bushing; 11. Fence structure; 12. Surface microtexture; 2. Copper-silver-zinc alloy ring; 3. Gradient multilayer structure; 31. Ni layer; 32. NiCu layer; 33. CuAg layer; 34. Ag layer. Detailed Implementation

[0022] The embodiments of the present invention will be described in detail below with reference to the accompanying drawings. However, the present invention can be implemented in many different ways as defined and covered below. Examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.

[0023] Those skilled in the art will understand that, unless specifically stated otherwise, the term "comprising" as used in this specification means the presence of the stated features, integers, steps, operations, components, and / or components, but does not exclude the presence or addition of one or more other features, integers, steps, operations, components, and / or combinations thereof. It should be understood that when we say a component is "connected" to another component, it can be directly connected to the other component or connected via an intermediate component. The term "and / or" as used herein includes all or any unit and all combinations of one or more associated listed items. The terms "first" and "second," etc., in this specification and claims are used to distinguish different objects, not to describe a particular order.

[0024] Reference Figure 1 A preferred embodiment of the present invention provides a grating sealing structure for an aero-engine, comprising: an alloy bushing 1 and a copper-silver-zinc alloy ring 2 coaxially disposed in the inner hole of the alloy bushing 1, and a gradient multilayer structure 3 metallurgically bonded and fixed between the alloy bushing 1 and the copper-silver-zinc alloy ring 2 by high-temperature diffusion welding; a grating structure 11 is also machined on the inner ring surface of the alloy bushing 1, and the gradient multilayer structure 3 is metallurgically bonded and fixed to the outer surface of the grating structure 11 along the tooth shape direction. The gradient multilayer structure 3 is formed by sequentially stacking multiple different materials to make the thermal expansion coefficient of the grating sealing structure gradually increase from the alloy bushing 1 side to the copper-silver-zinc alloy ring 2 side to alleviate thermal stress concentration.

[0025] In existing technologies, the coefficient of thermal expansion of copper-silver-zinc alloys is approximately 19 × 10⁻⁶. -6 At / ℃, the coefficient of thermal expansion of nickel-based superalloys (such as GH600) is approximately 13×10⁻⁶. -6The difference between the two is significant, and this thermal expansion mismatch will generate large thermal stress at the interface during the diffusion welding cooling process and the actual service thermal cycle of the engine. In the aero-engine comb seal structure of this invention, a gradient multilayer structure 3 is metallurgically bonded and fixed between the alloy bushing 1 and the copper-silver-zinc alloy ring 2 by high-temperature diffusion welding. This gradient multilayer structure 3 is formed by sequentially stacking multiple different materials to reduce the thermal expansion coefficient of the comb seal structure from Ni (approximately 13 × 10⁻⁶) to Ni (approximately 13 × 10⁻⁶). -6 / ℃) towards copper-silver-zinc alloy (approximately 19×10) -6 The coefficient of thermal expansion (C / ℃) increases gradually. This gradient in the coefficient of thermal expansion allows for a gradual transition in interfacial thermal strain, avoiding abrupt changes in thermal strain at a single interface. This effectively reduces thermal stress concentration at the interface and is expected to significantly improve the service life of the structure under thermal cycling conditions. Compared to a single copper interlayer (C / ℃), which has a coefficient of thermal expansion of approximately 17 × 10⁻⁶, this gradient is more efficient. -6 / ℃, which differs significantly from the base materials on both sides), the gradient design of this invention has a significant advantage in relieving thermal stress, and it solves the problem of thermal expansion mismatch between dissimilar metals from the material source.

[0026] Optionally, such as Figure 1 and Figure 3 As shown, the gradient multilayer structure 3 includes a Ni layer 31, a NiCu layer 32, a CuAg layer 33, and an Ag layer 34 stacked sequentially. The Ni layer 31 is metallurgically bonded to the inner ring wall of the alloy bushing 1 and the outer surface of the comb-like structure 11, while the Ag layer 34 is metallurgically bonded to the outer ring wall of the copper-silver-zinc alloy ring 2. In this invention, a gradient multilayer structure 3 with a compositional gradient transition is provided between the copper-silver-zinc alloy ring 2 and the alloy bushing 1. From the side closest to the alloy bushing 1, the layers are: Ni layer → Ni-30Cu layer → Cu-10Ag layer → Ag layer. The composition of the gradient multilayer structure 3 changes continuously, causing the coefficient of thermal expansion to decrease from approximately 13 × 10⁻⁶ on the alloy bushing 1 side (approximately 13 × 10⁻⁶). -6 / ℃) Towards the copper-silver-zinc alloy ring 2 (approximately 19×10) -6 The gradual transition (at / ℃) fundamentally alleviates the thermal stress concentration caused by the mismatch in thermal expansion between dissimilar metals. In this invention, the Ni layer 31 in the gradient multilayer structure 3 is in direct contact with the alloy bushing 1. Ni and Cr have good miscibility at high temperatures, and Cr tends to dissolve in the Ni layer rather than agglomerate at the interface to form a brittle CrP phase. This reduces the driving force for the precipitation of brittle phases from the perspective of material design and improves the joint toughness.

[0027] In this optional scheme, the alloy bushing 1 is made of GH4169, GH600, or GH536 nickel-based high-temperature alloy. A grating structure 11 is designed on the inner ring wall of the alloy bushing 1. The grating structure 11 includes multiple grates distributed circumferentially or axially, with cavities formed between adjacent grates. The copper-silver-zinc alloy ring 2 is a prefabricated ring nested on the outside of the gradient multilayer structure 3.

[0028] In this optional scheme, the thickness of Ni layer 31 is 0.008–0.015 mm, the thickness of NiCu layer 32 is 0.010–0.020 mm, the thickness of CuAg layer 33 is 0.010–0.020 mm, the thickness of Ag layer 34 is 0.003–0.008 mm, and the total thickness of the gradient multilayer structure 3 is 0.031–0.063 mm.

[0029] Specifically, the Ni layer 31 has a thickness of 0.008–0.015 mm; its function and positioning: it is close to the alloy bushing side, serving as a bonding layer and a diffusion barrier layer; its lower limit of 0.008 mm ensures that the Ni layer is continuous and dense, forming sufficient bonding strength with the alloy bushing 1, and effectively preventing excessive diffusion of subsequent Cu and Ag elements to the alloy bushing side; its upper limit of 0.015 mm avoids an excessively large proportion of low thermal expansion coefficient layers, preventing the gradient from changing too slowly on the alloy bushing side and too quickly at the subsequent interface, while controlling internal stress and cost; its relationship with thermal stress relief: the thermal expansion coefficient of Ni is close to that of the high-temperature alloy bushing, so using the Ni layer as a transition layer can avoid the direct contact between the alloy bushing 1 and the high thermal expansion coefficient copper alloy, which would cause a sudden change in thermal strain. The NiCu layer 32 has a thickness of 0.010–0.020 mm; its function is as an intermediate transition layer with a thermal expansion coefficient between Ni and CuAg; its beneficial effects are that this thickness range provides sufficient gradient transition space, allowing the thermal expansion coefficient to rise smoothly from the Ni layer to the CuAg layer, avoiding abrupt changes in thermal strain at a single interface; its lower limit of 0.010 mm can prevent the gradient from being too steep due to an excessively thin transition layer; its upper limit of 0.020 mm can avoid the accumulation of residual stress caused by excessive thermal resistance and an excessively thick transition layer; its relationship with thermal stress relief is that the NiCu layer is a key "buffer section" in the thermal expansion coefficient gradient, and its reasonable thickness can significantly reduce the shear stress and peel stress at the Ni / CuAg interface. CuAg layer 33, thickness 0.010~0.020mm; Function and positioning: Main thermal / electrical conductive layer, and also a high thermal expansion coefficient layer transitioning to the Ag layer and the copper-silver-zinc alloy ring; Beneficial effects: The thickness range ensures sufficient electrical and thermal conductive cross-section, which is conducive to the rapid diffusion of heat in the sealing structure, reducing the local thermal gradient. As a transition layer with a further increased thermal expansion coefficient, it can form a good thermal match with the Ag layer and the copper-silver-zinc alloy ring, avoiding stress concentration at the interface with a high thermal expansion coefficient. Relationship with thermal stress relief: The thicker CuAg layer can bear more thermal strain, allowing the thermal strain to be distributed layer by layer rather than concentrated at a certain interface. Ag layer 34 thickness 0.003~0.008mm; Functional positioning: the functional surface layer closest to the copper-silver-zinc alloy ring, with the highest coefficient of thermal expansion and good plasticity; Beneficial effects: the lower limit of 0.003mm can ensure the continuity and density of the Ag layer, and form good wetting or bonding with the copper-silver-zinc alloy ring; the upper limit of 0.008mm can control the amount of precious metals used, while avoiding the Ag layer from being too thick and having low strength, thus becoming a weak layer; Relationship with thermal stress relief: the Ag layer can relax some thermal stress through plastic deformation and creep, thereby reducing the peak thermal stress at the interface of the copper-silver-zinc alloy ring.

[0030] Specifically, the total thickness of the gradient multilayer structure 3 is 0.031–0.063 mm, which is the result of stacking four layers with varying thicknesses. Its beneficial effects are as follows: To ensure a complete gradient sequence: the lower limit ensures that the four layers of Ni, NiCu, CuAg, and Ag all reach the minimum effective thickness, forming a continuous gradient of thermal expansion coefficients; the upper limit avoids excessively thick transition layers.

[0031] Thermal strain transitions layer by layer: The four-layer structure causes the coefficient of thermal expansion to gradually increase from the alloy bushing side to the copper-silver-zinc alloy ring side, and the thermal strain is released step by step at multiple interfaces, avoiding abrupt changes in thermal strain at a single interface.

[0032] Reduced interfacial thermal stress concentration: After gradientization, the peak values ​​of interfacial shear stress and peel stress decrease, which is beneficial to improving service life under thermal cycling conditions.

[0033] Balancing lightweight and cost: The overall thickness is relatively thin, making it suitable as an interface transition layer, brazing layer, or plating layer in sealing structures without significantly increasing structural size and weight, while controlling the amount of precious metal Ag and strategic metal Ni used.

[0034] Process feasibility: This thickness range is compatible with multilayer electroplating, brazing, diffusion welding and other processes, which facilitates interlayer bonding.

[0035] Preferably, such as Figure 1 and Figure 2 As shown, the tooth surfaces and cavity surfaces of the comb structure 11, as well as the inner ring wall of the alloy bushing 1, are all machined with several micron-sized micropits to form a surface microtexture 12; the gradient multilayer structure 3 is also used to melt and fill the micropits during diffusion welding to form a micro-mechanical interlock after solidification. In this preferred embodiment, after several micron-sized micropits are machined on the outer surface of the comb structure 11 and the inner ring wall of the alloy bushing 1, the material of the gradient multilayer structure 3 conformally covers the inner wall of the micropits. Thus, during the diffusion welding process, under the action of temperature and pressure, the interface material undergoes plastic flow and atomic interdiffusion. The micropit structure plays two roles: ① Increase diffusion area: The surface microtexture 12 increases the actual contact area of ​​the interface by 30-60% compared with the geometric area, providing more channels for atomic diffusion; ② Microscopic mechanical interlocking: After the material of the gradient multilayer structure 3 flows into the micropit and solidifies, it forms an "anchoring" effect with the inner wall of the micropit. When the interface is subjected to shear or peel stress, the mechanical interlocking force provided by the micropit structure and the metallurgical bonding force of the interface work together to resist the external force, realizing a dual strengthening mechanism of metallurgical bonding + mechanical interlocking. It is expected that the interface bonding strength will be increased by more than 30% compared with the single metallurgical bonding scheme, thereby significantly improving the interface bonding strength.

[0036] Furthermore, several micro-pits are regularly arranged; each micro-pit has a diameter of 80-150 μm and a depth of 20-40 μm, and the center distance between two adjacent micro-pits is 150-300 μm. The area occupied by several micro-pits on the inner ring wall of the alloy bushing 1 and the outer surface of the comb structure 11 is 30%-60%, and they form micro-anchor points to achieve mechanical interlocking, forming a dual strengthening mechanism with metallurgical bonding.

[0037] Reference Figure 4 The preferred embodiment of the present invention also provides a method for preparing a toothed sealing structure, used to prepare an aero-engine toothed sealing structure as described above, the preparation method comprising the following steps: S10: Preliminary preparation: Prepare an alloy bushing 1 with a comb-like structure 11 on the inner ring wall and a copper-silver-zinc alloy ring 2; S20: Preparation of gradient multilayer structure 3: Gradient multilayer structure 3 is prepared on the inner ring wall of alloy bushing 1 and the outer surface of comb structure 11 by plasma spraying or multilayer annular foil stacking method. S30: Dissimilar alloy assembly: The copper-silver-zinc alloy ring 2 is positioned and installed into the gradient multilayer structure 3 to form an assembly; S40: Diffusion welding forming: The assembly is placed into a vacuum diffusion welding equipment for vacuum high-temperature diffusion welding.

[0038] In the method for preparing the comb-like sealing structure of this invention, a gradient multilayer structure 3 is prepared on the inner ring wall of the alloy bushing 1 and the outer surface of the comb-like structure 11 using plasma spraying or multilayer annular foil stacking, so that the coefficient of thermal expansion is reduced from the alloy bushing side (approximately 13 × 10⁻⁶). -6 / ℃) toward the copper-silver-zinc alloy ring side (approximately 19×10) -6 The gradient multilayer structure 3 features a smooth transition (at / ℃), avoiding the concentration of interfacial thermal stress caused by abrupt changes in the coefficient of thermal expansion of a single copper intermediate layer. This gradient multilayer transition design fundamentally solves the problem of thermal expansion mismatch between dissimilar metals. The Ni layer in the gradient multilayer structure 3 exhibits good solid solubility with Cr at high temperatures, with Cr tending to dissolve in the Ni layer rather than agglomerate at the interface. This effectively reduces the formation of brittle CrP phases and improves joint toughness. This invention provides two parallel gradient multilayer fabrication methods: plasma spraying and foil stacking. Enterprises can flexibly choose based on the inner hole size and existing equipment conditions, demonstrating strong industrial adaptability.

[0039] Optionally, the inner ring wall and outer surface of the comb structure 11 of the alloy bushing 1 prepared in step "S10: Preliminary Preparation" also have a surface microtexture 12 formed by micropits with several micrometer-sized pores. The preparation of the alloy bushing 1 in step "Preliminary Preparation" specifically includes the following steps: S11: Precision machining of the inner hole of alloy bushing 1; S12: Machining of the inner ring wall of the alloy bushing 1 with a tooth structure 11; Specifically, a special carbide turning tool for forming the inner hole is selected to machine the continuous annular tooth structure 11 in the circumferential direction of the inner hole in one go, and the tooth top surface, the double side walls of the tooth and the bottom surface of the tooth cavity are completely machined. S13: Pre-cleaning; S14: Preparation of surface microtexture 12 on the inner ring wall and outer surface of the comb structure 11 of the alloy bushing 1. Specifically, a long rod-type internal hole laser processing device equipped with an end micro galvanometer is used to extend into the inner cavity of the alloy bushing 1 to carry out full-area texture processing; the workpiece is clamped with its outer circle centered and rotated at a uniform speed. The laser beam deflection angle is precisely controlled by the galvanometer to achieve full-coverage scanning etching of the comb tooth top surface, double-sided tooth sidewalls, tooth cavity bottom surface, and the remaining inner ring wall surfaces of the alloy bushing 1, forming a regular matrix-like micron-level micro-pit array. The preferred range of microtexture parameters is: micro-pit diameter 80-150 μm, micro-pit depth 20-40 μm, micro-pit center distance 150-300 μm, and area occupancy 30%-60%. S15: Cleaning and finishing after surface microtexturing 12. Specifically, the alloy bushing 1 with microtextured surface is subjected to full-area degreasing and impurity removal treatment to remove molten spatter and debris generated during laser processing.

[0040] In this optional scheme, when preparing the copper-silver-zinc alloy ring 2, the copper-silver-zinc alloy ring 2 is prefabricated according to the size of the alloy bushing 1. The copper-silver-zinc alloy ring 2 is obtained by machining after homogenization heat treatment of the cast blank.

[0041] Optionally, step "S20: Preparation of gradient multilayer structure 3" is prepared using plasma spraying, which specifically includes the following steps: S21: Plasma spraying gradient layer: Pure Ni powder, NiCu alloy powder, CuAg alloy powder and pure Ag powder are sequentially sprayed on the inner ring surface of the alloy bushing 1 using plasma gradient spraying equipment to form a gradient multilayer structure 3. S22: Hot isostatic pressing densification treatment: The entire alloy bushing 1 after spraying is subjected to hot isostatic pressing densification treatment; S23: Precise inner hole calibration: Perform micro-finishing on the inner ring of alloy bushing 1 according to assembly requirements.

[0042] In this optional scheme, step S21 specifically involves: using a dedicated plasma gradient spraying equipment for internal holes, configured with four independent precision powder feeding systems, corresponding to pure Ni powder, Ni-30Cu alloy powder, Cu-10Ag alloy powder, and pure Ag powder, respectively. Based on the inner hole forming base surface and microtexture structure of the alloy bushing 1, the powder feeding rate of the four channels is dynamically and linearly adjusted to form a continuous composition gradient transition layer on the inner annular cylindrical surface of the alloy bushing 1, consisting of a Ni layer → Ni-30Cu layer → Cu-10Ag layer → Ag layer. The thicknesses of each layer are as follows: Ni layer 0.008~0.015mm, Ni-30Cu layer 0.010~0.020mm, Cu-10Ag layer 0.010~0.020mm, pure Ag layer 0.003~0.008mm, and total thickness 0.031~0.063mm.

[0043] In this optional scheme, steps S22 and S23 are performed as follows: After spraying, the alloy bushing 1 is subjected to hot isostatic pressing (HIP) densification treatment (temperature 950–1050℃, pressure 100–150MPa, holding time 1–2h) to eliminate micropores generated by the plasma spraying process, significantly improving the density of the gradient transition layer, the interlayer bonding strength, and the adhesion performance with the substrate. After treatment, micro-internal hole finishing is performed according to assembly requirements to calibrate the dimensional accuracy of the workpiece.

[0044] Optionally, in step "S20: Preparation of Gradient Multilayer Structure 3", a multilayer annular foil stacking method is used. Specifically, pure Ni annular foil, NiCu alloy annular foil, CuAg alloy annular foil, and pure Ag annular foil are sequentially stacked on the inner ring surface of the alloy bushing 1. Specifically, the four annular foil layers are stacked sequentially from the substrate side to the outside on the inner wall of the alloy bushing: pure Ni annular foil (thickness 0.008–0.015 mm) → Ni-30Cu alloy annular foil (thickness 0.010–0.020 mm) → Cu-10Ag alloy annular foil (thickness 0.010–0.020 mm) → pure Ag annular foil (thickness 0.003–0.008 mm), ensuring that each foil layer is completely bonded, circumferentially gapless, and coaxially consistent, without misalignment, arching, or wrinkles.

[0045] Optionally, in step "S30: Dissimilar Alloy Assembly", the copper-silver-zinc alloy ring 2 is inserted into the inner hole of the gradient multilayer structure 3 with a gap of 0.01 to 0.03 mm between them. Specifically, Option A: The copper-silver-zinc alloy ring 2 is nested into the outer side of the prepared gradient multilayer structure 3 of the alloy bushing 1 to form an assembly. The copper-silver-zinc alloy ring 2 and the outer side of the gradient multilayer structure 3 are in a clearance fit with a gap of 0.01 to 0.03 mm. Option B: The copper-silver-zinc alloy ring 2 is nested into the outer side of the outermost pure Ag foil to form an assembly. The copper-silver-zinc alloy ring 2 and the outer side of the pure Ag foil are in a clearance fit with a gap of 0.01 to 0.03 mm. Specifically, a special coaxial mandrel tooling is used to assist in the assembly to ensure that the coaxiality of each layer of foil, the alloy bushing 1, and the copper-silver-zinc alloy ring 2 is consistent. In this optional scheme, a clearance fit replaces an interference fit: the copper-silver-zinc alloy ring 2 and the outer side of the gradient multilayer structure 3 (or the outer side of the outermost Ag foil / Ag layer) adopt a clearance fit (gap 0.01~0.03mm). No assembly stress is generated during the assembly process, which avoids the deformation of the copper-silver-zinc alloy ring 2, ensures the dimensional accuracy of the copper-silver-zinc alloy ring 2 and the uniformity of the sealing gap. At the same time, under the high temperature conditions of diffusion welding, thermal expansion will close the gap and achieve tight contact at the interface, thus not affecting the diffusion welding quality.

[0046] Optionally, in step "S40: Diffusion Welding Formation", the welding temperature is 700–730℃; the welding pressure is 5–15 MPa; the holding time is 120–180 minutes; and the vacuum degree is ≤5×10⁻⁶. -3 Pa. Specifically, the assembly from step S30 is placed into a vacuum diffusion welding device, and diffusion welding is carried out by setting the process parameters; welding temperature: 700~730℃; welding pressure: 5~15MPa; holding time: 120~180 minutes; vacuum degree: ≤5×10 -3 Pa; This temperature range, combined with the Ni layer design in the gradient multilayer structure 3, can reduce the volatilization of low-melting-point elements such as Cu and Zn and the excessive precipitation of Cr elements at the interface while ensuring sufficient atomic diffusion.

[0047] For the gradient multilayer structure 3 formed by plasma spraying, during the heating and holding pressure process, the intermediate layer material at the interface undergoes high-temperature softening and slight plastic flow, fully filling the micron-level micro-pit structure on the surface of the comb teeth. After cooling and solidification, a uniformly distributed micro-tenon and mortise mechanical interlocking structure is formed. At the same time, the micro-texture significantly increases the effective contact area of ​​the interface. Combined with the compositional compatibility characteristics of the gradient multilayer structure 3, it promotes full interdiffusion of interfacial atoms, forming a stable and dense metallurgical bond. For the gradient multilayer structure 3 formed by multilayer annular foil stacking, during the diffusion welding process, full atomic interdiffusion occurs simultaneously at the interfaces of the four foil layers. The original interlayer interfaces gradually diffuse and blur, eliminating delamination gaps and forming a quasi-gradient structure with continuous performance transition. The coefficient of thermal expansion gradually changes from the nickel-based substrate side to the copper-silver-zinc alloy side, achieving the same thermal stress relief effect as the sprayed gradient multilayer structure 3.

[0048] Preferably, after completing step "S40: diffusion bonding and forming", the method further includes the following step: S50: Finished Product Inspection: The finished product of the toothed sealing structure is inspected for dimensional accuracy, interface bonding quality, and sealing gap uniformity. Specifically, workpiece size constraints: The inner diameter of the bushing inner ring is ≥80mm (plasma spraying method) or ≥60mm (multi-layer annular foil stacking method) for standard mass production processes, which can simultaneously meet the internal working space requirements of laser textured, gradient spraying equipment, or foil stacking processes.

[0049] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. An aeroengine labyrinth seal arrangement, characterised in that, include: Alloy bushing (1) and copper-silver-zinc alloy ring (2) coaxially disposed in the inner hole of alloy bushing (1), and gradient multilayer structure (3) fixed between alloy bushing (1) and copper-silver-zinc alloy ring (2) by high-temperature diffusion welding metallurgical bonding. The inner ring surface of the alloy bushing (1) is also machined with a tooth structure (11). The gradient multilayer structure (3) is also metallurgically fixed to the outer surface of the tooth structure (11) along the tooth shape direction. The gradient multilayer structure (3) is formed by stacking multiple different materials in sequence to make the thermal expansion coefficient of the tooth sealing structure gradually increase from the alloy bushing (1) side to the copper-silver-zinc alloy ring (2) side to alleviate thermal stress concentration.

2. The aero-engine toothed sealing structure according to claim 1, characterized in that, The gradient multilayer structure (3) includes a Ni layer (31), a NiCu layer (32), a CuAg layer (33) and an Ag layer (34) stacked sequentially. The Ni layer (31) is metallurgically bonded to the inner ring wall of the alloy bushing (1) and the outer surface of the comb structure (11), and the Ag layer (34) is metallurgically bonded to the outer ring wall of the copper-silver-zinc alloy ring (2).

3. The aero-engine toothed sealing structure according to claim 2, characterized in that, The thickness of the Ni layer (31) is 0.008–0.015 mm, the thickness of the NiCu layer (32) is 0.010–0.020 mm, the thickness of the CuAg layer (33) is 0.010–0.020 mm, the thickness of the Ag layer (34) is 0.003–0.008 mm, and the total thickness of the gradient multilayer structure (3) is 0.031–0.063 mm.

4. The aero-engine toothed sealing structure according to claim 1, characterized in that, The tooth surface and cavity surface of the tooth structure (11) and the inner ring wall of the alloy bushing (1) are all machined with several micro-sized pits to form a surface microtexture (12). The gradient multilayer structure (3) is also used to melt-fill micro-pits during diffusion welding to form micro-mechanical interlocks after solidification.

5. The aero-engine toothed sealing structure according to claim 4, characterized in that, Several micro-pits are arranged in a regular pattern; Each micro-pit has a diameter of 80-150 μm and a depth of 20-40 μm. The center distance between two adjacent micro-pits is 150-300 μm. The area occupied by several micro-pits on the inner ring wall of the alloy bushing (1) and the outer surface of the comb structure (11) is 30%-60%.

6. A method of making a labyrinth seal structure, comprising: The method for preparing the aero-engine tooth sealing structure as described in any one of claims 1-5 includes the following steps: Preliminary preparations: an alloy bushing (1) with a comb-like structure (11) on the inner ring wall and a copper-silver-zinc alloy ring (2) were prepared. Preparation of gradient multilayer structure (3): Gradient multilayer structure (3) is prepared on the inner ring wall of alloy bushing (1) and the outer surface of comb structure (11) by plasma spraying or multilayer ring foil stacking. Dissimilar alloy assembly: The copper-silver-zinc alloy ring (2) is positioned and installed into the gradient multilayer structure (3) to form an assembly; Diffusion welding: The assembly is placed into a vacuum diffusion welding machine for vacuum high-temperature diffusion welding.

7. The method for preparing the toothed sealing structure according to claim 6, characterized in that, The inner ring wall of the alloy bushing (1) prepared by step "preliminary preparation" and the outer surface of the comb structure (11) also have a surface microtexture (12) formed by micropits with several micron-sized pores. The preparation of the alloy bushing (1) in the "Preliminary Preparation" step specifically includes the following steps: Precision machining of the inner hole of the alloy bushing (1); Machining of the comb tooth structure on the inner ring wall of the alloy bushing (1); Pre-cleaning; The surface microtexture (12) of the inner ring wall and the outer surface of the comb structure (11) of the alloy bushing (1) is prepared; Surface microtexture (12) followed by cleaning and finishing.

8. The method for preparing the toothed sealing structure according to claim 6, characterized in that, The step "Preparation of gradient multilayer structure (3)" uses plasma spraying, which specifically includes the following steps: Plasma spraying gradient layer: Pure Ni powder, NiCu alloy powder, CuAg alloy powder and pure Ag powder are sequentially sprayed on the inner ring surface of the alloy bushing (1) using a plasma gradient spraying equipment to form a gradient multilayer structure (3). Hot isostatic pressing densification treatment: The alloy bushing (1) after spraying is subjected to hot isostatic pressing densification treatment as a whole; Precise calibration of the inner hole: The inner ring of the alloy bushing (1) is subjected to micro-finishing according to the assembly requirements.

9. The method for preparing the toothed sealing structure according to claim 6, characterized in that, In step "Preparation of gradient multilayer structure (3)", a multilayer ring foil stacking method is used. The specific operation is as follows: pure Ni ring foil, NiCu alloy ring foil, CuAg alloy ring foil and pure Ag ring foil are stacked on the inner ring surface of the alloy bushing (1) in sequence.

10. The method for preparing the toothed sealing structure according to claim 6, characterized in that, In the step "dissimilar alloy assembly", the copper-silver-zinc alloy ring (2) is inserted into the inner hole of the gradient multilayer structure (3) with a gap of 0.01 to 0.03 mm between the two. In the step "diffusion welding forming", the welding temperature is 700-730 °C, the welding pressure is 5-15 MPa, the holding time is 120-180 minutes, and the vacuum degree is ≤5x10 -3 Pa. After completing the "diffusion bonding" step, the following steps are also included: Finished product inspection: The finished products of the toothed sealing structure are inspected for dimensional accuracy, interface bonding quality, and sealing gap uniformity.

Citation Information

Patent Citations

  • Diffusion welding method for sealing structure of engine

    CN105665912A