A large-size flat fragile lid and its preparation method

The large-size flat, fragile cover, integrally foamed with rigid polyurethane foam and epoxy-reinforced mesh fabric, solves the problems of forward breakage and reverse negative pressure, achieving lightweighting and improved safety, and is suitable for the safety requirements of multi-unit launch boxes.

CN123111004APending Publication Date: 2026-11-17GUIZHOU AEROSPACE TIANMA ELECTRICAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611306868.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-26
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing large-size flat fragile covers have insufficient reliability in breaking under positive pressure and insufficient bearing capacity under negative pressure. Furthermore, the foam sandwich structure shrinks greatly during molding and has poor material interface bonding, making it difficult to meet the safety requirements of multi-unit launch boxes.

Method used

The rigid polyurethane foam core layer and epoxy reinforced mesh layer are integrally foamed and molded. The directional asymmetric weak groove is designed with the groove openings intersecting along the diagonal and circumferential directions. Through chemical bonding and mechanical interlocking, the breaking path is controlled and the interfacial bonding strength is enhanced.

Benefits of technology

It achieves precise control of positive crushing pressure, enhances reverse negative pressure bearing capacity, avoids large-scale splashing, and has a lightweight overall material with good weather resistance and sealing properties, making it suitable for long-term storage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123111004A_ABST
    Figure CN123111004A_ABST
Patent Text Reader

Abstract

This application relates to the field of missile launch box cover technology, specifically a large-size flat fragile cover and its manufacturing method. The fragile cover is greater than 1m in length and width and greater than 40mm in thickness. It is integrally molded from polyurethane foam and epoxy-reinforced mesh fabric, with weak grooves formed along the diagonal and circumferential directions on the cover surface. The cross-sectional shape of the weak grooves ensures that the bottom of the groove breaks under tensile stress under positive pressure, while the groove walls are compressed under negative pressure, resulting in strong resistance to negative pressure. During manufacturing, the problem of large-size shrinkage is solved by mold shrinkage compensation, the addition of hollow microspheres, and controlled post-curing. The mesh fabric uses semi-cured epoxy prepreg to form a strong interface bond with the foam. The fragile cover of this invention is lightweight, has controllable positive breakage pressure, and high resistance to negative pressure, meeting the requirement that adjacent box covers are not damaged during the launch of multi-launch boxes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of missile launch box cover technology, specifically a large-size flat fragile cover and its preparation method. Background Technology

[0002] The launch canister cover is a crucial component of a box-type missile launch system. It must be reliably sealed during storage and transportation, and open rapidly at launch without causing excessive interference to the missile. For multi-launch canisters, when one canister is launched, the covers of adjacent canisters will be subjected to negative pressure caused by the strong flow of exhaust gases, thus requiring that the adjacent canister covers not be damaged. Simultaneously, the launch canister cover itself must break along a pre-designed weak point under relatively low positive pressure (from inside the canister to the outside), clearing a path for the missile.

[0003] Currently, commonly used launch box covers include metal blasting covers and fragile composite material covers. Metal blasting covers require the use of pyrotechnics, posing safety hazards and adding weight. Existing fragile composite material covers are mostly made of glass fiber reinforced resin, achieving controlled breakage through pre-designed weak points. However, for large-sized flat covers with dimensions exceeding 1 meter in length and width and a thickness exceeding 40 mm, using pure fiberglass presents problems such as high weight, high cost, and difficulty in controlling molding shrinkage. While foam sandwich structures can reduce weight, bonding the foam core to the reinforced panel is difficult for large sizes, and the high shrinkage rate of polyurethane foam during foaming can easily cause the cover to warp and detach, resulting in uneven pressure resistance. Furthermore, the weak point design of existing fragile covers generally only focuses on forward breakage, insufficiently guaranteeing the reverse negative pressure bearing capacity, making it difficult to meet the negative pressure protection requirements of adjacent boxes.

[0004] Therefore, there is an urgent need to develop a large-size flat fragile cover that can reliably break along the weak area under positive pressure and resist large reverse negative pressure, while solving the problems of large shrinkage and poor material interface bonding during the molding of large-size foam sandwich structures. Summary of the Invention

[0005] To address the aforementioned technical problems in the prior art, this application provides a large-size, fragile flat cap and its manufacturing method. Specifically, this is achieved through the following technical solution: A large-size flat fragile cover includes a rectangular flat body composed of a polyurethane foam core layer (1), an epoxy reinforced mesh fabric layer on the upper surface (2), and an epoxy reinforced mesh fabric layer on the lower surface (3); the length and width of the rectangular flat body are both greater than 1m, and the thickness is greater than 40mm; a weak groove is provided on the upper surface and / or lower surface of the rectangular flat body, the weak groove including a diagonal groove (4) extending along two diagonals and a circumferential groove (5) extending along the periphery of the cover, the diagonal groove and the circumferential groove intersecting or connecting; the cross-sectional shape of the weak groove is set so that when the cover is subjected to positive pressure from inside the box to outside the box, the bottom of the groove is stretched and breaks, and when subjected to negative pressure from outside the box to inside the box, the groove wall is pressed against the bottom of the groove and is compressed, the reverse bearing capacity is greater than the positive breaking pressure.

[0006] Furthermore, the cross-section of the weak groove is V-shaped, rectangular, or trapezoidal, the groove width is 4-10mm, the groove depth is 10%-60% of the cover thickness, and the V-shaped angle is 45°-90°.

[0007] Furthermore, the weak groove is formed on the upper surface of the cover, which faces the inside of the box. Under positive pressure, the cover bulges outward, causing the groove to open.

[0008] Furthermore, the polyurethane foam core layer (1) is a rigid closed-cell polyurethane foam with a density of 200-400 kg / m³. 3 The compressive strength is ≥1.5MPa; the upper surface epoxy-reinforced mesh layer (2) and the lower surface epoxy-reinforced mesh layer (3) each contain at least two layers of glass fiber mesh pre-impregnated with epoxy resin, and the mesh surface density is 200~500g / m². 2 Mesh size 4×4mm~10×7mm, etc. (material selection depends on requirements), epoxy resin content 30~50wt%.

[0009] Furthermore, 5-15 wt% of hollow glass microspheres are added to the polyurethane foam core layer (1).

[0010] Furthermore, the polyurethane foam core layer and the epoxy reinforced mesh layer are bonded together by chemical bonding and mechanical interlocking, and the interfacial tensile shear strength is greater than 0.6 MPa.

[0011] Furthermore, a silane coupling agent can be pre-coated onto the surface of the mesh fabric or a compatibilizer containing epoxy groups can be added to the foaming formulation.

[0012] Furthermore, the polyurethane foam formulation comprises: 100 parts polyol blend, 143 parts isocyanate (crude MDI), 4 parts hollow glass microspheres, 2.0 parts foam stabilizer, 1.7 parts catalyst, 5 parts foaming agent, and 10 parts flame retardant. The raw materials are mixed uniformly at high speed and then poured into the mold cavity. The pouring weight is based on a foam density of 380 kg / m³ after molding. 3calculate.

[0013] Furthermore, the hollow glass microspheres have a particle size of 50 μm.

[0014] The method for preparing the large-size, fragile flat cap specifically includes the following steps: S1. Mold preparation: Provide a mold with a rectangular cavity. The length and width of the cavity are enlarged by 0.5% to 1.5% of the target size of the cover as shrinkage compensation. The mold temperature is preheated to 40 to 60°C. S2. Lay-up: Epoxy-reinforced mesh fabric layers are sequentially laid in the upper and lower molds. The mesh fabric layers are pre-cut to fit the mold cavity and are pre-impregnated with epoxy resin and are in a semi-cured state. If the width of the mesh fabric is insufficient for the mold cavity size, it can be achieved by overlapping. S3. Fixing the upper mold mesh: The upper mold mesh is fixed by connecting and fixing metal wires such as iron wire and aluminum wire with a diameter of 2-4mm through the mold vent holes; S4. Casting and foaming: The polyurethane foam material, which is a uniform mixture of polyol component and isocyanate component, is poured into the mold cavity. The pouring amount is calculated based on the target foam density and the mold cavity volume. S5. Mold closing and foaming: After pouring the polyurethane foam material, immediately close and lock the mold to complete the foaming process within the mold. The foaming time is 5 to 10 minutes. S6. Post-curing: Post-curing at 90–110℃ for 1.5–3 hours to eliminate internal stress; S7. Weak groove machining: Using CNC milling and drilling, weak grooves are machined along the diagonal and circumferential areas on the designated surface of the formed blank. The groove shape, groove depth and groove width are precisely controlled according to the design parameters. Corresponding assembly holes are machined on the outside of the blank to obtain a large-size flat fragile cover.

[0015] Compared with the prior art, the technical effects created by this application are reflected in: 1. This application designs the weak groove as a directional asymmetric load-bearing structure, which can precisely control the positive crushing pressure within a low range of 0.03 to 0.08 MPa, and the reverse negative pressure bearing capacity can reach more than 0.1 MPa, thus meeting the negative pressure resistance requirements of the adjacent box cover during launch, i.e., "it is fragile, but the adjacent cover is not damaged".

[0016] 2. This application uses rigid polyurethane foam and epoxy reinforced mesh fabric for integral molding. An interpenetrating network is formed between the foam and the mesh fabric, resulting in high bonding strength. This avoids the delamination defects of traditional bonding processes, and the mesh fabric improves the overall rigidity and local damage toughness of the cover.

[0017] 3. This application effectively solves the problem of large shrinkage during the molding of large-size, thick-section polyurethane foam by compensating for mold shrinkage, adding hollow glass microspheres, and controlling the post-curing process.

[0018] 4. The weak grooves opened along the diagonal and circumferential directions in this application form a clear priority fracture path. Under positive pressure, the cover can be regularly split into four or more fragments without producing large pieces of debris, thus improving missile launch safety.

[0019] 5. The large-size flat fragile lid obtained in this application is lightweight, reducing weight by 20% to 50% compared to pure fiberglass lids of the same size, and has good weather resistance and sealing performance, making it suitable for long-term storage. Attached Figure Description

[0020] Figure 1 a) is a top view of the fragile cover in an embodiment of the present invention; b) is a cross-sectional view of the fragile cover in an embodiment of the present invention. Detailed Implementation

[0021] The technical solution of this application will be further defined below with reference to specific implementation methods, but the scope of protection is not limited to the description.

[0022] Example 1: like Figure 1 As shown, a large-sized, fragile flat cover is used in a twin-launcher missile launcher. The cover is a rectangular flat plate with a length L=1300mm, a width W=1200mm, and a thickness T=43mm. The cover consists of a rigid polyurethane foam core layer 1, an epoxy-reinforced mesh fabric layer 2 on the upper surface, and an epoxy-reinforced mesh fabric layer 3 on the lower surface. The upper surface faces the inside of the launcher, and the lower surface faces the outside (the position of the weak groove can be adjusted as needed; in this example, the weak groove is located on the upper surface, meaning the groove opens when subjected to positive pressure).

[0023] The density of the rigid polyurethane foam core layer 1 is 380 kg / m³. 3 The compressive strength is 8.2 MPa, and the closed-cell rate is ≥95%. The upper epoxy-reinforced mesh layer 2 and the lower epoxy-reinforced mesh layer 3 are each composed of three layers of woven glass fiber mesh, with a single layer surface density of 450 g / m². 2 The resin content is 40wt%. The total thickness of the single-sided mesh fabric layer is approximately 3mm.

[0024] A weak groove is formed on the upper surface, including a diagonal groove 4 extending along two diagonals and a rectangular circumferential groove 5 40mm from the edge. The diagonal groove 4 extends outward from the center of the cover to the circumferential groove 5 and intersects with the circumferential groove. The groove cross-section is rectangular (e.g., ...). Figure 1 b) The groove width is 10mm and the groove depth is 10mm (approximately 23% of the thickness).

[0025] The method for preparing the fragile flat cap: S1. Mold preparation: The aluminum mold cavity size is 1310mm×1210mm. It is preheated to 53℃ and the mold cavity is coated with release agent.

[0026] S2. Laying layers: Lay mesh fabric layers in the lower mold and upper mold of the mold cavity respectively, and fix the mesh fabric of the upper mold with iron wire.

[0027] S3. Polyurethane foam formulation: 100 parts polyol blend, 143 parts isocyanate (crude MDI), 4 parts hollow glass microspheres (50μm particle size), 2.0 parts foam stabilizer, 1.7 parts catalyst, 5 parts blowing agent, and 10 parts flame retardant. After high-speed and uniform mixing of the raw materials, pour the mixture into the mold cavity. The pouring weight should be based on a foam density of 380 kg / m³ after molding. 3 calculate.

[0028] S4. After the foaming material is poured, quickly close the mold and let it stand. When the liquid overflows from the vent hole, immediately pull out the wire on the mesh cloth.

[0029] S5. After injection, the mold is cured in a 100℃ oven for 2 hours, and then demolded after natural cooling.

[0030] S6. Using a CNC milling machine, a weak groove is milled on the upper surface to machine diagonal grooves, circumferential grooves, and assembly holes. The finished product is obtained after machining.

[0031] The above embodiments are only for illustrating the technical concept and features of this application, and are intended to enable those skilled in the art to understand the content of this application and implement it accordingly. They should not be used to limit the scope of protection of this application. All equivalent changes or modifications made in accordance with the spirit and essence of this application should be included within the scope of protection of this application.

Claims

1. A large-sized, fragile flat lid, characterized in that, The rectangular flat plate body consists of a polyurethane foam core layer (1), an epoxy reinforced mesh fabric layer on the upper surface (2), and an epoxy reinforced mesh fabric layer on the lower surface (3). The length and width of the rectangular flat plate body are both greater than 1m, and the thickness is greater than 40mm. Weak grooves are provided on the upper surface and / or lower surface of the rectangular flat plate body. The weak grooves include diagonal grooves (4) extending along two diagonals and circumferential grooves (5) extending along the periphery of the cover. The diagonal grooves and circumferential grooves intersect or connect. The cross-sectional shape of the weak grooves is set so that when the cover is subjected to positive pressure from inside the box to outside the box, the bottom of the groove is stretched and breaks. When subjected to negative pressure from outside the box to inside the box, the groove wall is pressed against the bottom of the groove and the reverse bearing capacity is greater than the positive breaking pressure.

2. The large-size flat fragile cover according to claim 1, characterized in that, The cross-section of the weak groove is V-shaped, rectangular or trapezoidal, with a groove width of 4 to 10 mm, a groove depth of 10% to 60% of the cover thickness, and a V-shaped angle of 45° to 90°.

3. The large-size flat fragile cover according to claim 1, characterized in that, The weak groove is formed on the upper surface of the cover, which faces the inside of the box. Under positive pressure, the cover bulges outward, causing the groove to open.

4. The large-size flat fragile cover according to claim 1, characterized in that, The polyurethane foam core layer (1) is a rigid closed-cell polyurethane foam, with a density of 200-400 kg / m 3 , and a compressive strength of ≥1.5 MPa; the upper surface epoxy reinforced mesh cloth layer (2) and the lower surface epoxy reinforced mesh cloth layer (3) each comprise at least 2 layers of glass fiber mesh cloth pre-impregnated with epoxy resin, with a mesh cloth surface density of 200-500 g / m 2 , a mesh size of 4×4 mm-10×7 mm, etc., and an epoxy resin content of 30-50 wt%.

5. The large-size flat fragile cover according to claim 4, characterized in that, The polyurethane foam core layer (1) contains 5-15 wt% hollow glass microspheres.

6. The large-size flat fragile cover according to claim 4, characterized in that, The polyurethane foam core layer and the epoxy reinforced mesh layer are bonded together by chemical bonding and mechanical interlocking, and the interfacial tensile shear strength is greater than 0.6 MPa.

7. The large-size flat fragile cover according to claim 4, characterized in that, Pre-coat the surface of the mesh fabric with a silane coupling agent or add a compatibilizer containing epoxy groups to the foaming formulation.

8. The large-size flat fragile cover according to claim 1, characterized in that, The polyurethane foam formulation comprises: 100 parts polyol blend, 143 parts isocyanate, 4 parts hollow glass microspheres, 2.0 parts foam leveler, 1.7 parts catalyst, 5 parts foaming agent, and 10 parts flame retardant. The raw materials are mixed evenly at high speed and then poured into the mold cavity. The pouring weight is based on a foam density of 380 kg / m³ after molding. 3 calculate.

9. The large-size flat fragile cover according to claim 1, characterized in that, The hollow glass microspheres have a particle size of 50 μm.

10. The method for preparing the large-size flat fragile cap according to claim 1, characterized in that, Specifically, the steps include the following: S1. Mold preparation: Provide a mold with a rectangular cavity. The length and width of the cavity are enlarged by 0.5% to 1.5% of the target size of the cover as shrinkage compensation. The mold temperature is preheated to 40 to 60°C. S2. Lay-up: Epoxy-reinforced mesh fabric layers are sequentially laid in the upper and lower molds. The mesh fabric layers are pre-cut to the mold cavity size and are pre-impregnated with epoxy resin and are in a semi-cured state. If the width of the mesh fabric is insufficient for the mold cavity size, it can be achieved by overlapping. S3. Fixing the upper mold mesh: The upper mold mesh is fixed by connecting and fixing metal wires such as iron wire and aluminum wire with a diameter of 2-4mm through the mold vent holes; S4. Casting and foaming: The polyurethane foam material, which is a uniform mixture of polyol component and isocyanate component, is poured into the mold cavity. The pouring amount is calculated based on the target foam density and the mold cavity volume. S5. Mold closing and foaming: After pouring the polyurethane foam material, immediately close and lock the mold to complete the foaming process within the mold. The foaming time is 5 to 10 minutes. S6. Post-curing: Post-curing at 90–110℃ for 1.5–3 hours to eliminate internal stress; S7. Weak groove machining: Using CNC milling and drilling, weak grooves are machined along the diagonal and circumferential areas on the designated surface of the formed blank. The groove shape, groove depth and groove width are precisely controlled according to the design parameters. Corresponding assembly holes are machined on the outside of the blank to obtain a large-size flat fragile cover.