Photomask preform substrates, photomask preform substrate assemblies, and methods for manufacturing them

By setting rectangular and strip-shaped regions in the splicing target area of ​​the photomask blank substrate and using local processing and fine polishing techniques, the problems of transfer position displacement and splicing error in EUVL were solved, and good splicing and transfer performance in high NA EUVL was achieved.

CN123113230APending Publication Date: 2026-11-17SHIN ETSU CHEMICAL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202610660056.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-16
Filing Date
2026-05-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies cannot effectively solve the problems of photomask transfer position displacement and splicing error in EUVL, especially under high NA conditions, the flatness of the photomask blank substrate is insufficient, which affects the exposure quality.

Method used

By setting rectangular and strip-shaped areas in the splicing target area of ​​the photomask blank substrate, and using local processing and fine polishing techniques, the high flatness of the splicing target area is ensured, and the displacement of the transfer position is reduced.

Benefits of technology

It achieves excellent splicing and transfer performance in high NA EUVL exposure, reduces transfer position displacement during exposure, and improves exposure quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123113230A_ABST
    Figure CN123113230A_ABST
Patent Text Reader

Abstract

A photomask blank substrate has two main surfaces, each consisting of a first main surface and a second main surface. Each of the first and second main surfaces is square, with one side measuring 152 mm and the other side measuring 152 mm. When a rectangular strip region is formed within a rectangular region on the first main surface, the flatness of the strip region is 10 nm or less. The rectangular region has a center at the intersection of the diagonals of the first main surface, a short side measuring 104 mm, and a long side measuring 132 mm. The short side is parallel to the edge of the first main surface. The rectangular shape has the short side of the rectangular region as one side, and its long side is 104 mm, with the short side being 1 mm–2 mm. This provides a photomask that reduces the displacement of the transfer position during exposure and achieves good transfer performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to photomask blank substrates as raw materials for photomasks used in photolithography, and in particular, to photomask blank substrates suitable for use in photolithography using far-ultraviolet (EUV) light as exposure light, and to photomask blank substrate groups consisting of two photomask blank substrates, and methods for manufacturing them. Background Technology

[0002] In recent years, with the growing attention garnered by AI and IoT, the need for massive data processing has arisen, necessitating acceleration and power efficiency. To meet this demand, improved IC chip performance is required, often achieved through circuit miniaturization. Miniaturization primarily employs techniques such as higher numerical aperture (NA) and shorter wavelength exposure light. However, in recent years, EUV lithography (EUVL), utilizing EUV light, has been put into practical use.

[0003] In EUVL, the photomask (exposure mask) is a crucial element. To achieve correct exposure, improving the flatness of the photomask blank substrate is essential. While dual-sided simultaneous polishing is commonly used in substrate manufacturing, it's insufficient for achieving the desired flatness for EUVL. To achieve high flatness, it's necessary to correct the flatness corresponding to the surface shape by polishing one surface at a time. This is done using local processing techniques such as local etching or local polishing. Local processing involves removing protruding portions of the substrate's main surface to bring the entire substrate closer to a flat surface. Furthermore, by using the wavefront correction function of the exposure apparatus, the surface shape of the photomask can be optically corrected, allowing the photomask to function as an optically highly flattened mask.

[0004] In a conventional optical system, the pattern formed in a rectangular area of ​​104 mm × 132 mm on the photomask is equally scaled down in the orthogonal directions of the surface (scaled down by an equal factor in the x and y directions) and transferred to a 26 mm × 33 mm area on the silicon wafer.

[0005] On the other hand, in recent years, there has also been a need for high field-attribute (NA) for EUVL, and deformable lenses have been used as the optical system. In this case, a pattern formed in a rectangular area of ​​104 mm × 132 mm on a photomask is asymmetrically transferred to a 26 mm × 16.5 mm area on a silicon wafer. Since only half the field can be transferred using a single photomask, a full-field pattern is formed by transferring a pattern connected to the previously transferred pattern using another photomask.

[0006] In this context, precise joining of half-field patterns is required without transfer position displacement, and a technique known as stitching has been extensively studied as a means to achieve this. Stitching makes it possible to join patterns without error, even in fine designs. However, stitching presents several technical challenges, and minimizing transfer position displacement caused by the photomask is also necessary.

[0007] JP-A 2011-141536 (Patent Document 1) discloses a mask glass substrate in which the portion corresponding to the holding surface of the exposure machine is not distorted. In this case, the flatness of two strip-shaped regions in the periphery of the square substrate surface where the photomask holding portion is located, from the edge of each of the two opposing edges inward from each edge to between 2 mm and 10 mm, and after removing 2 mm portions from both ends of the length direction of each edge, is controlled to be below a specified value.

[0008] JP-A 2017-44758 (Patent Document 2) describes a mask preform glass substrate for EUVL, suitable for EUVL projection systems using EUV exposure apparatus employing anamorphic lenses. In this EUVL mask preform glass substrate, by specifying the angle and ratio of local tilt in the shrinkage direction, the effect of edge roughness (LER) of the pattern formed on the wafer, which is caused by exposure using different shrinkage ratios in the x and y directions, can be suppressed.

[0009] Citation List

[0010] Patent Document 1: JP-A 2011-141536

[0011] Patent Document 2: JP-A 2017-44758

[0012] Patent Document 3: JP-A 2010-194705 Summary of the Invention

[0013] However, the flatness of the photomask glass substrate described in JP-A 2011-141536 (Patent Document 1) is insufficient for EUVL. Furthermore, even in the EUVL mask blank glass substrate described in JP-A 2017-44758 (Patent Document 2), displacement of the transfer position cannot be adequately suppressed by considering only the local surface shape. Moreover, in JP-A 2011-141536 (Patent Document 1) and JP-A 2017-44758 (Patent Document 2), the surface shape in the region affecting the splicing of the main surface is not considered.

[0014] In view of the above, the present invention was completed, and the object of the present invention is to provide photomask blank substrates and photomask blank substrate sets, as well as methods for manufacturing them with high productivity, wherein the photomask blank substrates and photomask blank substrate sets provide photomasks that sufficiently suppress displacement of the transfer position and enable good stitching in exposures using the photomasks, especially in exposures using high NA / EUVL.

[0015] In order to apply stitching in exposures using high NA EUVL, it is necessary to consider the surface shape of the areas that affect the stitching. To achieve good bonding, the inventors have focused on the surface shape of the target stitching areas of the photomask, particularly the surface shape of the target stitching areas of the substrate used for the photomask blank (which is the raw material for the photomask).

[0016] To address the aforementioned issues, the inventors conducted in-depth research on photomask blank substrates used for applying spliced ​​photomasks, and thus discovered that the flatness of the splicing target area (a parameter affecting the transfer position displacement) is important. Specifically, the inventors have found that in a photomask blank substrate having two main surfaces, each of which is square with one side of 152 mm and the other side of 152 mm, on the first main surface, in a rectangular region centered at the intersection of the diagonals of the first main surface, with a short side of 104 mm and a long side of 132 mm (the short side is parallel to the edge of the first main surface), the flatness of a strip region with the short side of the rectangular region as one side is important in photomask blank substrates used for applying spliced ​​photomasks.

[0017] Furthermore, the inventors have discovered that the above-mentioned problems can be solved by the following solutions.

[0018] (1) In the case of a photomask blank substrate, which is a photomask blank substrate with good flatness in a strip-shaped region, the strip-shaped region is rectangular, with one or two short sides of the rectangular region as one side, the long side being 104 mm and the short side being 1 to 2 mm, or

[0019] (2) In the case of a photomask preform substrate group consisting of two photomask preform substrates, it is a photomask preform substrate group in which the flatness of the composite surface is good. The composite surface is rectangular, with one side measuring 104 mm and the other side measuring 2 to 4 mm. The composite surface is formed by connecting the surface of a strip-shaped region of one photomask preform substrate with the surface of a strip-shaped region of another photomask preform substrate in such a way that their reference planes overlap. In addition, the inventors have discovered that when manufacturing photomask preform substrates or photomask preform substrate groups, considering the flatness of the strip-shaped region or the flatness of the composite surface, high-productivity manufacturing can be achieved by performing local processing, thus completing the present invention.

[0020] Therefore, the present invention provides the following photomask preform substrate, photomask preform substrate group, method for manufacturing photomask preform substrate, and method for manufacturing photomask preform substrate group.

[0021] 1. A photomask blank substrate having two main surfaces, each consisting of a first main surface and a second main surface, wherein the first main surface and the second main surface are each square with one side of 152 mm and the other side of 152 mm.

[0022] When a strip region with a rectangular shape is provided in a rectangular region on the first main surface, the flatness of the strip region is 10 nm or less, wherein the rectangular region has a center at the intersection of the diagonals of the first main surface, a short side of 104 mm and a long side of 132 mm, the short side being parallel to the edge of the first main surface, and the rectangular shape having one short side as one side, the long side being 104 mm, and the short side being 1 mm-2 mm.

[0023] 2. The photomask blank substrate according to Project 1, wherein the ratio of the flatness of the strip region to the flatness of the rectangular region is 0.3 or less.

[0024] 3. The photomask blank substrate according to Project 1, wherein...

[0025] When two strip regions are set in the rectangular region, the flatness of each of the two strip regions is 10 nm or less, wherein each strip region has a rectangular shape, and the rectangular shape has each of the two short sides of the rectangular region as one side, the long side being 104 mm and the short side being 1 mm - 2 mm.

[0026] 4. The photomask blank substrate according to Project 3, wherein the flatness ratio of each of the two strip regions to the flatness of the rectangular region is 0.3 or less.

[0027] 5. The photomask blank substrate according to item 1 or 3, wherein the flatness of the rectangular region is 30 nm or less.

[0028] 6. The photomask blank substrate according to item 1 or 3, having a thickness of 6.35 mm.

[0029] 7. A photomask preform substrate assembly, comprising two photomask preform substrates, each photomask preform substrate having two main surfaces consisting of a first main surface and a second main surface, wherein the first main surface and the second main surface are each square in shape with one side of 152 mm and the other side of 152 mm.

[0030] In each of the two photomask blank substrates,

[0031] When a strip region with a rectangular shape is formed in a rectangular region on the first main surface, the flatness of the composite surface with the rectangular shape is 10 nm or less.

[0032] The rectangular region has a center at the intersection of the diagonals of the first main surface, a short side of 104 mm, and a long side of 132 mm. The short side is parallel to the edge of the first main surface. The rectangular shape of the strip region is defined by one of its short sides, with a long side of 104 mm and a short side of 1 mm-2 mm.

[0033] The rectangular shape of the composite surface has one side of 104 mm and another side of 2 mm-4 mm. The composite surface is formed by connecting the surface of the strip region of one photomask blank substrate and the surface of the strip region of another photomask blank substrate such that the reference surfaces of the two surfaces overlap each other.

[0034] 8. The photomask preform substrate assembly according to Item 7, wherein the photomask preform substrate has a thickness of 6.35 mm.

[0035] 9. A method for manufacturing a photomask blank substrate, the photomask blank substrate having two main surfaces consisting of a first main surface and a second main surface, the first main surface and the second main surface each having a square shape with one side of 152 mm and the other side of 152 mm, the method comprising:

[0036] The local processing steps for the first main surface and the fine polishing steps following the local processing steps, wherein

[0037] The local processing steps include:

[0038] (A1) The step of forming one or two strip regions with a rectangular shape in a rectangular region on the first main surface of the raw material substrate, wherein the rectangular region has a center at the intersection of the diagonals of the first main surface, a short side of 104 mm, and a long side of 132 mm, the short side being parallel to the edge of the first main surface, and the rectangular shape having one or two short sides of the rectangular region as one side, the long side being 104 mm, and the short side being 1 mm-2 mm.

[0039] (B1) The steps for evaluating the flatness of the one or two strip regions, and

[0040] (C1) The step of partially processing the first main surface to make the flatness of the one or two strip regions within a predetermined range.

[0041] 10. The manufacturing method according to Item 9 further includes (D1) a step of evaluating the flatness of the one or two strip regions of the first main surface after partial processing in step (C1).

[0042] 11. The manufacturing method according to item 10, wherein when the flatness of one strip region or the flatness of one or both of the two strip regions evaluated in step (D1) is not within the predetermined range, step (C1) or steps (C1) and (D1) are performed again.

[0043] 12. A method for manufacturing a photomask preform substrate assembly, the photomask preform substrate assembly comprising two photomask preform substrates, each photomask preform substrate having two main surfaces consisting of a first main surface and a second main surface, the first main surface and the second main surface each being square in shape with one side of 152 mm and the other side of 152 mm, the method comprising:

[0044] The local processing step and the fine polishing step following the local processing step are for one or both of the first main surface of the two photomask blank substrates, wherein

[0045] The local processing steps include:

[0046] (A2) In each of the two raw material substrates, the step of forming a strip region with a rectangular shape in a rectangular region on the first main surface, wherein the rectangular region has a center at the intersection of the diagonals of the first main surface, a short side of 104 mm and a long side of 132 mm, the short side being parallel to the edge of the first main surface, and the rectangular shape having one short side as one side of the rectangular region, the long side being 104 mm, and the short side being 1 mm-2 mm.

[0047] (B2) The step of evaluating the flatness of a composite surface having a rectangular shape, wherein the rectangular shape has one side of 104 mm and another side of 2 mm-4 mm, the composite surface being formed by connecting the surface of the strip region of one photomask blank substrate and the surface of the strip region of another photomask blank substrate such that the reference surfaces of the two surfaces overlap each other; and

[0048] (C2) The step of partially processing one or two of the first main surfaces to make the flatness of the composite surface within a predetermined range.

[0049] 13. The manufacturing method according to item 12 further includes (D2) a step of evaluating the flatness of the composite surface after partial processing in step (C2).

[0050] 14. The manufacturing method according to item 13, wherein when the flatness of the composite surface evaluated in step (D2) is not within the predetermined range, step (C2) or steps (C2) and (D2) are performed again.

[0051] 15. The manufacturing method according to item 9 or 12, wherein the photomask blank substrate has a thickness of 6.35 mm.

[0052] Beneficial effects of the present invention

[0053] According to the present invention, a photomask can be provided that reduces the displacement of the transfer position during exposure and can achieve good transfer performance, especially in exposure using the photomask, particularly in exposure utilizing high NA EUVL, good stitching can be achieved. Attached Figure Description

[0054] Figure 1 This is a plan view illustrating an embodiment of a rectangular region and a strip region on the first main surface of the photomask blank substrate according to the present invention; and

[0055] Figure 2 This is a plan view illustrating an embodiment of the composite surface, wherein strip regions of two first main surfaces in the photomask blank substrate group of the present invention are connected. Detailed Implementation

[0056] The present invention will now be described in detail.

[0057] The photomask preform substrate of the present invention has two main surfaces and a predetermined thickness. The main surfaces of the photomask preform substrate of the present invention are square in shape, with one side measuring 152 mm and the other side measuring 152 mm. The thickness can be appropriately selected according to the required dimensions of the photomask to be manufactured using the photomask preform substrate. In particular, a substrate having a square main surface of 152 mm × 152 mm and a thickness of 6.35 mm is preferred; this is referred to as a so-called 6025 substrate, and is a substrate having two rectangular main surfaces of 6 inches × 6 inches and a thickness of 0.25 inches.

[0058] The material of the photomask preform substrate described in this invention can be a conventionally used material and is not particularly limited. However, when drawing fine patterns, the photomask preform substrate is exposed to high-energy exposure light; therefore, TiO2-doped quartz glass (containing 3 wt%-10 wt% TiO2) is suitable, as it exhibits very high dimensional stability at high temperatures. As the raw material substrate for the photomask preform substrate, substrates synthesized, molded, and processed according to conventional methods can be used.

[0059] Photomask preform substrates require high flatness. This is because higher flatness facilitates target exposure, and substrates with higher flatness are more suitable for fabricating fine patterns. A photomask preform substrate comprises two main surfaces: a first main surface on which exposure patterns (such as wiring patterns) are formed after film formation, and a second main surface on which no exposure patterns are formed, the second main surface being held and held by the exposure machine. State-of-the-art photomasks are primarily reflective masks, and extremely high levels of flatness are required on the first and second main surfaces. Therefore, various studies have been conducted on planarization techniques using local processing methods to improve the flatness of the first main surface.

[0060] In recent years, to meet the demand for further miniaturization of circuits, EUVL has also trended towards higher NA (Negative Atmosphere). Specifically, the NA has increased from the conventional NA of 0.33 to NA of 0.55, and in EUV exposure with NA of 0.55, a deformable optical system different from the conventional optical system is employed. Therefore, with NA of 0.33, exposure is performed on the main surface of the photomask at the same magnification in both the x and y directions, but with NA of 0.55, exposure is performed on the main surface of the photomask at different magnifications in the x and y directions. Thus, although the circuit can be further miniaturized, a single exposure can only form a circuit in a conventional half-field, while two exposures using two photomasks are needed to form the full field. Therefore, splicing techniques have been developed for precisely joining circuit patterns in half-fields. Splicing is a technique for precisely joining two interrupted circuits. Although it is difficult to precisely join extremely fine circuit patterns, in recent years, through advances in research and development, its application in mass production is being realized.

[0061] The displacement of the transfer position during exposure is a factor that directly affects the exposure quality. The displacement of the transfer position during exposure (Image Placement Error: IPE) can be expressed by the following formula:

[0062] IPE = d × tanθ / M

[0063] Where d represents the flatness of the exposure surface of the photomask, θ represents the incident angle of the exposure light, and M represents the reduction ratio.

[0064] IPE is inversely proportional to the shrinkage ratio.

[0065] In optical systems using morphing lenses, the reduction ratio varies depending on the orientation of the photomask because the circuit pattern is asymmetrically reduced, and thus the IPE also varies. Since EUV light is emitted at a predetermined angle θ (e.g., 6 degrees), which is tilted relative to a direction orthogonal to the main surface of the substrate of the photomask, a positional displacement of the exposure pattern occurs on the wafer depending on the surface shape of the photomask, and a smaller IPE results in a smaller positional displacement during exposure, which is preferable. Therefore, similarly, in areas that can be spliced, a higher flatness (a smaller flatness value) results in a lower IPE, which is advantageous for bonding circuit patterns.

[0066] Regarding the relationship between IPE and magnification M, M=4 is independent of the photomask orientation in a conventional EUV exposure machine with NA 0.33, but in an EUV exposure machine with NA 0.55, there are directions with M=4 and M=8. Therefore, IPE varies depending on the photomask orientation, and IPE is relatively more affected in directions with lower magnification M. Therefore, to evaluate IPE while taking into account the photomask orientation, it is effective to consider each of the x and y directions separately.

[0067] Here, if the direction of the lower magnification M (M=4) (the tangent direction of the two halves (the direction of one edge of the main surface)) is represented by the x-direction, and the direction of the higher magnification M (M=8) (the arrangement direction of the two halves (the direction of the other edge of the main surface)) is represented by the y-direction, the flatness obtained by decomposing the flatness d in the x-direction is represented by (dx), and the flatness obtained by decomposing the flatness d in the y-direction is represented by (dy), then the IPE (IPEx) in the x-direction and the IPE (IPEy) in the y-direction can be expressed by the following formulas:

[0068] IPEx = dx × tanθ / 4 and

[0069] IPEy = dy × tanθ / 8, and

[0070] IPE is represented by the following formula:

[0071] IPE = ((IPEx) 2 + (IPEy) 2 ) 0.5 .

[0072] Therefore, since the IPE is higher in the x-direction at lower magnification M than in the y-direction at higher magnification M, the flatness in the x-direction must be given more weight than the flatness in the y-direction when considering the flatness of the area that can be used as a splicing target. Furthermore, regarding the displacement of the two halves in the alignment direction (the direction of the other side of the main surface), the circuit can overlap at the junction of the two halves and breakage can be relatively easily avoided. However, displacement of the two halves in the tangential direction (the direction of one side of the main surface) results in a shortage of linewidth at the junction of the circuit, and if the displacement exceeds the linewidth, a breakage occurs. Therefore, the flatness in the tangential direction must be given more weight.

[0073] In the photomask blank substrate of the present invention, when a strip region with a rectangular shape is formed on the long side end of the rectangular region in the first main surface, the flatness of the strip region is 10 nm or less. The rectangular region has a center at the intersection of the diagonals of the first main surface, a short side of 104 mm, and a long side of 132 mm. The short side is parallel to the edge of the first main surface. The rectangular shape has a short side that is one side, a long side of 104 mm, and a short side of 1 mm-2 mm. Photomasks including this photomask blank substrate can achieve good splicing, wherein the displacement of the transfer position during exposure is reduced when using high-NA EUVL exposure.

[0074] Figure 1 This is a plan view illustrating an embodiment of a rectangular region and a strip region on the first main surface of the photomask blank substrate according to the present invention. The rectangular region 2 has a short side of 104 mm and a long side of 132 mm, and is centered at the intersection of the diagonals of the first main surface 1, located where the short side is parallel to the edge of the first main surface (the four sides of the rectangular region 2 are parallel to the four sides of the first main surface 1). On the other hand, the strip region 3 has a rectangular shape, with one or both short sides of the rectangular region 2 as one side, a long side of 104 mm and a short side of 2 mm, and one or two strip regions 3 and 3 can be disposed within the rectangular region 2.

[0075] The strip region is a region that can be a target for splicing. From the viewpoint of effectively suppressing the influence of flatness in splicing while reliably reducing the influence of flatness in the tangential direction (the direction of one side of the main surface) of the two halves, the width of each of the two halves in the tangential direction (the direction of one side of the main surface) is the same as the width of the rectangular region, and the arrangement direction of the two halves (the direction of the other side of the main surface) is a part of the width of the rectangular region, which is effective. In this invention, the length of the short side of the strip region is 1 mm-2 mm, preferably 1 mm, more preferably 1.5 mm, and even more preferably 2 mm.

[0076] When two strip regions are set at both ends of the long side of a rectangular region, the flatness of each of the two strip regions is preferably 10 nm or less, wherein each of the two strip regions has a rectangular shape, wherein each of the two short sides of the rectangular region is taken as a side, the long side is 104 mm, and the short side is 1 mm-2 mm. A height map from surface shape measurement can be applied to the shape of the strip regions. In this case, two strip regions along one side (located at both ends of the other side of the first main surface) can be set as regions that can be spliced ​​together. Note that the main surface can have two rectangular regions orthogonal to each other, and the strip region of one rectangular region or the strip regions of both rectangular regions can be the target.

[0077] The flatness of the strip region is 10 nm or less. When the flatness of the strip region is 10 nm or less, if the magnification M satisfies M=4 and the incident angle is 6 degrees, the displacement (IPE) of the transfer position in the strip region that can become the stitching target during exposure is about 0.26 nm or less, and is about 1.9% or less of the EUV exposure wavelength of 13.5 nm. The flatness of the strip region is preferably 7 nm or less, and more preferably 5 nm or less.

[0078] In the photomask blank substrate described in this invention, the ratio of the flatness of the strip region to the flatness of the rectangular region is preferably 0.3 or less (30% or less), and more preferably 0.25 or less (25% or less). When two, three, or four strip regions are used as targets, the ratio of the flatness of each strip region to the flatness of the rectangular region is preferably 0.3 (30% or less), and more preferably 0.25 or less (25% or less). If the flatness ratio is within this range, the strip region that can be the stitching target is significantly flatter than the entire rectangular region containing the strip region, and the substrate is more suitable as a photomask blank substrate for photomasks that are effective for exposures using high NA EUVL.

[0079] In a photomask blank substrate, the flatness of not only the strip region that can serve as the stitching target, but also the flatness of the entire main surface, especially the flatness of the entire exposure target area of ​​the main surface, is important. The rectangular region corresponds to the half-field range in EUV exposure at NA 0.55, and the flatness of the rectangular region affects the IPE of the entire pattern formed in that half-field. In the photomask blank substrate described in this invention, the flatness of the rectangular region (the flatness of the entire rectangular region) is preferably 30 nm or less, and more preferably 25 nm or less. Height maps in surface shape measurements can be applied to the shape of the rectangular region. If the flatness of the rectangular region is within this range, not only the strip region that can serve as the stitching target but also the entire exposure target area of ​​the main surface is flat, and the substrate is more suitable as a photomask blank substrate for photomasks that are effective for exposures using high NA EUVL. Note that the flatness of the rectangular region is ideally 0 nm, but is typically greater than 0 nm.

[0080] In stitching, the half-fields (circuits) must be precisely joined together. Even if the flatness of the strip regions of each of the two photomask blank substrates is good, the overall shape where the two strip regions are joined may not be flat enough in some cases, and in these cases, there is a possibility that a good stitching cannot be achieved. Therefore, it is useful to combine two photomask blank substrates that can achieve good stitching to join the circuits of the strip regions of the two photomasks and perform exposure using high NA EUVL. To date, the advantages of stitching in the case of combining two photomask blank substrates have not been studied based on the shape of the main surfaces of the two photomask blank substrates, especially the strip regions.

[0081] The photomask preform substrate assembly of the present invention comprises two photomask preform substrates. In the photomask preform substrate assembly of the present invention, in each of the two photomask preform substrates, when a strip region with a rectangular shape is formed in a rectangular region on a first main surface, the flatness of the composite surface is preferably 10 nm or less. The rectangular region has a center at the intersection of the diagonals of the first main surface, a short side of 104 mm, and a long side of 132 mm. The short side is parallel to the edge of the first main surface. The rectangular shape has one side as the short side of the rectangular region, and its long side is 104 mm. The short side is 1 mm-2 mm. The rectangular shape of the composite surface has one side of 104 mm and another side of 2 mm-4 mm. The composite surface is formed by connecting the surface of the strip region of one photomask preform substrate and the surface of the strip region of the other photomask preform substrate, such that the reference surfaces of the two surfaces overlap each other. The flatness of the composite surface is preferably 7 nm or less, more preferably 5 nm or less.

[0082] For the strip regions to be connected, it is only required to connect any one strip region of one photomask preform substrate and any one strip region of another photomask preform substrate. The composite surface consists of the surface of a strip region of one photomask preform substrate (one strip region) and the surface of a strip region of another photomask preform substrate (the other strip region). This composite surface is a virtual surface obtained by combining the shapes of the two surfaces. The other side of the composite surface is preferably 2 mm, more preferably 3 mm, and even more preferably 4 mm.

[0083] When connecting the surfaces of one strip region to the surface of another strip region, if necessary and with the application of splicing, one or the other strip region is rotated 90, 180, or 270 degrees along a reference surface, and a 104 mm edge on the side furthest from the center of the first main surface of one strip region is connected to a 104 mm edge on the side furthest from the center of the first main surface of the other strip region. A height map from surface shape measurements can be applied to the shape of the strip region. Additionally, as the reference surface when connecting the surfaces of the strip regions, the least-squares surface of the rectangular region of each of the two photomask substrates connecting the strip regions, or the least-squares surface of each of the strip regions to be connected, can be applied.

[0084] Figure 2 This is a plan view illustrating an embodiment of the composite surface, wherein strip regions connect two first main surfaces in the photomask preform substrate group according to the present invention. A composite surface 4 is formed by strip regions 3 and 3 connecting rectangular regions 2 and 2 of the first main surfaces of the two photomask preform substrates, at a 104 mm edge on one side away from the center of the first main surface of the strip region 3 of one photomask preform substrate and at a 104 mm edge on one side away from the center of the first main surface of the strip region 3 of the other photomask preform substrate. The composite surface has a rectangular shape with one side measuring 104 mm and the other side measuring 4 mm.

[0085] In this photomask substrate set, the overall shape obtained by joining strip regions that can serve as stitching targets is sufficiently flat, the difference in displacement of the transfer positions in the two strip regions that can serve as stitching targets during exposure is small, and the circuit patterns of the two halves can be joined more precisely. The photomask blank substrate set is suitable as a photomask blank substrate set for photomasks that are effective for high-NA EUVL exposure.

[0086] The following describes a method for manufacturing the photomask preform substrate and photomask preform substrate assembly according to the present invention. The method for manufacturing the photomask preform substrate according to the present invention includes a local processing step on a first main surface and a fine polishing step following the local processing step. The method for manufacturing the photomask preform substrate according to the present invention may include a local processing step on a second main surface and a fine polishing step following the local processing step.

[0087] In the fabrication of photomask preform substrates, a raw material substrate for the photomask preform substrate is prepared from a glass ingot before local processing steps. This raw material substrate is typically prepared by first cutting the glass ingot into a predetermined shape and then machining its outline, followed by polishing the main surface and end faces. The polishing can be performed in several stages, such as coarse polishing, fine polishing, and ultra-fine polishing. This polishing can be done using polishing cloths and polishing agents. The polishing agent is not particularly limited, but for example, an aqueous dispersion of cerium oxide with an average primary particle size of 10 nm–100 nm, or an aqueous dispersion of silica nanoparticles with an average primary particle size of 10 nm–100 nm (colloidal silica aqueous dispersion) can be used.

[0088] The shape of a surface obtained solely through local processing is not flat and is typically a shape that offsets changes in surface shape during subsequent fine polishing (typically, a centrally protruding shape (a shape where the central portion of the main surface protrudes), a centrally recessed shape (a shape where the central portion of the main surface is recessed), etc.). Even if the flatness of the surface shape obtained solely through local processing is evaluated, the evaluation may only deviate from the evaluation result of the final obtained photomask blank substrate's main surface shape. The change in the main surface shape caused by fine polishing under predetermined polishing conditions after local processing is reproducible. By understanding the change in the main surface shape after fine polishing under predetermined polishing conditions and applying this change to the main surface shape after local processing, the surface shape after fine polishing under predetermined polishing conditions can be predicted. Therefore, before fine polishing, the shape of the surface obtained after fine polishing can be evaluated during the local processing stage, and the quality of the main surface shape obtained by fine polishing can be evaluated. The change in the main surface shape after fine polishing under predetermined polishing conditions can be obtained by pre-processing and evaluating a substrate (the substrate having a surface shape similar to the surface shape of the substrate to be processed). The local processing steps can be repeated until the predetermined shape is obtained.

[0089] In the method for manufacturing photomask blank substrate described in this invention,

[0090] The preferred local processing steps include:

[0091] (A1) The step of forming one or two strip regions with a rectangular shape in a rectangular region on the first main surface of the raw material substrate, wherein the rectangular region has a center at the intersection of the diagonals of the first main surface, a short side of 104 mm, and a long side of 132 mm, the short side being parallel to the edge of the first main surface, and the rectangular shape having one or both of the short sides of the rectangular region as one side, the long side being 104 mm, and the short side being 1 mm-2 mm.

[0092] (B1) The steps for evaluating the flatness of the one or two strip regions, and

[0093] (C1) The step of partially processing the first main surface to make the flatness of the one or two strip regions within a predetermined range.

[0094] In step (A1), for the strip-shaped region, on the first main surface of the raw material substrate, only a predetermined region is required to be set as the strip-shaped region within a predetermined rectangular region. For example, rectangular regions and strip-shaped regions can be set in a height map obtained by measuring the shape of the first main surface. In this invention, the shapes of the first main surface, its rectangular region, its strip-shaped region, and its composite surface can be measured, for example, by a laser interferometer.

[0095] In step (B1), it is preferable not to directly use the shape of the first main surface before fine polishing, but to evaluate the flatness of the strip region from the shape of the first main surface after local processing, which incorporates the surface shape changes caused by fine polishing. In this case, when the shape of the strip region of the first main surface after local processing is represented by S0, and the surface shape change caused by fine polishing is represented by ΔS, the shape S0' of the first main surface after fine polishing, represented by S0 + ΔS = S0', can be applied and evaluated in the strip region. Therefore, the shape of the strip region obtained after fine polishing can be evaluated, and further, the flatness can be evaluated (calculated) from the shape of the strip region. ΔS can be obtained by pre-polishing another substrate having a surface shape similar to the substrate to be processed.

[0096] In step (C1), the first main surface is locally machined so that the flatness of the strip region evaluated in step (B1) is within a predetermined range. The local machining of the first main surface can be performed on the entire first main surface, only on the rectangular region, or only on the strip region.

[0097] In this invention, during localized processing, selective removal of relatively protruding portions is performed on a first main surface. Localized processing can be performed by polishing using a polishing cloth and a polishing agent. The polishing agent is not particularly limited, but for example, an aqueous dispersion of cerium oxide with an average primary particle size of 10 nm-100 nm, or an aqueous dispersion of silica nanoparticles with an average primary particle size of 10 nm-100 nm (colloidal silica aqueous dispersion) can be used. For localized processing, methods such as magnetorheological polishing (MRF) can also be applied.

[0098] The method for manufacturing photomask blank substrate according to the present invention preferably further includes (D1) a step of evaluating the flatness of one or two strip regions of the first main surface after local processing in step (C1).

[0099] In step (D1), similar to step (B1), it is preferable not to directly use the shape of the first main surface before fine polishing, but to evaluate the flatness of the strip region from the shape of the first main surface after local processing, which incorporates the surface shape changes caused by fine polishing. Similarly, in this case, similar to step (B1), the shape S0' of the first main surface after fine polishing can be applied to and evaluated within the strip region. Therefore, the shape of the strip region obtained after fine polishing can be evaluated, and furthermore, the flatness can be evaluated (calculated) from the shape of the strip region.

[0100] Note that the flatness of the rectangular region can be evaluated in conjunction with either step (B1) or step (D1). Similarly, in this case, similar to the strip region, the above method is preferably used to superimpose the surface shape change caused by fine polishing onto the first main surface shape after local processing, thereby evaluating the flatness of the resulting rectangular region. Therefore, the shape of the rectangular region obtained after fine polishing can be evaluated, and furthermore, the flatness can be evaluated (calculated) from the shape of the rectangular region. Furthermore, the ratio of the flatness of the strip region to the flatness of the rectangular region can be calculated from the flatness of the strip region and the flatness of the rectangular region.

[0101] If the flatness of one or two strip regions, or the ratio of the flatness of a strip region to the flatness of a rectangular region, and / or the flatness of a strip region to the flatness of a rectangular region, as evaluated in step (D1) meets a predetermined range, a fine polishing step can be performed. Conversely, if the flatness of one or two strip regions, or the ratio of the flatness of a strip region to the flatness of a rectangular region, and / or the flatness of a strip region to the flatness of a rectangular region, as evaluated in step (D1) does not meet a predetermined range, it is preferable to repeat step (C1) or steps (C1) and (D1). Note that step (C1) or steps (C1) and (D1) can be repeated until the flatness of the strip region, or the ratio of the flatness of a strip region to the flatness of a rectangular region, and / or the flatness of a strip region to the flatness of a rectangular region, meets a predetermined range.

[0102] In the method for manufacturing the photomask blank substrate group described in this invention...

[0103] The preferred local processing steps include:

[0104] (A2) The step of setting a strip region with a rectangular shape in a rectangular region on the first main surface of each of the two raw material substrates, wherein the rectangular region has a center at the intersection of the diagonals of the first main surface, a short side of 104 mm and a long side of 132 mm, the short side being parallel to the edge of the first main surface, and the rectangular shape having the short side of the rectangular region as one side, the long side being 104 mm, and the short side being 1 mm-2 mm.

[0105] (B2) The step of evaluating the flatness of a composite surface having a rectangular shape, wherein the rectangular shape has one side of 104 mm and another side of 2 mm-4 mm, and the composite surface is formed by connecting the surfaces of one strip region and the surfaces of another strip region such that the reference surfaces of the two surfaces overlap each other; and

[0106] (C2) The step of partially processing one or two of the first main surfaces to make the flatness of the composite surface within a predetermined range.

[0107] In step (A2), for the strip-shaped region, on the first main surface of the raw material substrate, only a predetermined region is required to be set as the strip-shaped region within a predetermined rectangular region. For example, rectangular and strip-shaped regions can be set in a height map obtained by measuring the shape of the first main surface. The shape of the first main surface can be measured, for example, by a laser interferometer.

[0108] In step (B2), it is preferable not to use the shape of the first main surface before fine polishing, but to use the shape obtained by superimposing the surface shape change caused by fine polishing onto the shape of the first main surface after partial processing, to evaluate the flatness of the composite surface. In this case, when the shape of the composite surface of the first main surface after partial processing is represented by S0, and the surface shape change caused by fine polishing is represented by ΔS, the shape S0' of the first main surface after fine polishing, represented by S0 + ΔS = S0', can be applied and evaluated in the composite surface. Therefore, the shape of the composite surface obtained after fine polishing can be evaluated, and further, the flatness can be evaluated (calculated) from the shape of the composite surface. ΔS can be obtained by pre-polishing another substrate having a surface shape similar to the substrate to be processed.

[0109] In step (C2), one or two of the first main surfaces are locally machined so that the flatness of the composite surface evaluated in step (B2) is within a predetermined range. The local machining of the first main surface may be performed on the entire first main surface, only on a rectangular area, or only on a strip area.

[0110] The method for manufacturing the photomask blank substrate group of the present invention preferably further includes (D2) a step of evaluating the flatness of the composite surface after local processing in step (C2).

[0111] In step (D2), similar to step (B2), preferably, instead of using the shape of the first main surface before fine polishing, the shape obtained by superimposing the surface shape change caused by fine polishing onto the shape of the first main surface after local processing is used to evaluate the flatness of the composite surface. Similarly, in this case, similar to step (B2), the shape S0' of the first main surface after fine polishing can be applied and evaluated in the composite surface. Therefore, the shape of the composite surface obtained after fine polishing can be evaluated, and furthermore, the flatness can be evaluated (calculated) from the shape of the composite surface.

[0112] If the flatness of the composite surface evaluated in step (D2) meets the predetermined range, a fine polishing step can be performed. On the other hand, if the flatness of the composite surface evaluated in step (D2) is not within the specified range, it is preferable to repeat step (C2) or steps (C2) and (D2). Note that step (C2) or steps (C2) and (D2) can be repeated until the flatness of the composite surface meets the predetermined range.

[0113] Especially in photomask preform substrates used in cutting-edge products, the defect level on the substrate surface obtained through localized processing alone may be insufficient. Therefore, in the manufacturing of photomask preform substrates, a fine polishing step is performed after the localized processing steps. Additionally, if necessary, the shape of the first main surface, its rectangular region, its stripe region, and its composite surface of the photomask preform substrate obtained after fine polishing can be evaluated, and the flatness can be assessed (calculated). In this case, since fine polishing is performed, the surface shape change (ΔS) caused by fine polishing need not be considered.

[0114] The flatness of the strip-shaped area, the flatness of the rectangular area, and the ratio of the flatness of the strip-shaped area to the flatness of the rectangular area after fine polishing can be evaluated to see if they meet the predetermined range. If the flatness of the strip-shaped area, the flatness of the rectangular area, and the ratio of the flatness of the strip-shaped area to the flatness of the rectangular area after fine polishing are not within the predetermined range, a local processing step can be performed again, and fine polishing can be performed again.

[0115] The photomask blank substrate and photomask blank substrate assembly manufactured in this manner can achieve good splicing, wherein the displacement of the transfer position during exposure is reduced when using high NA EUVL exposure.

[0116] Example

[0117] The present invention will now be described in detail with reference to the embodiments, but the present invention is not limited to the following embodiments.

[0118] Example 1

[0119] Ten glass substrates were prepared, made of SiO2 and TiO2 (TiO2 concentration: approximately 7% by weight). The dimensions and shape of each of the first and second main surfaces were 152 mm × 152 mm squares with a thickness of 6.35 mm. The end faces of the glass substrates (the four surfaces other than the main surfaces) were chamfered and ground, and further rough and fine polished using a polishing slurry containing cerium oxide abrasive grains.

[0120] Next, ten glass substrates (substrate 1-1 to substrate 1-10) were placed in a carrier of a double-sided polishing apparatus using a velvety soft polishing cloth, and the first and second main surfaces were ultra-precisely polished using a polishing slurry containing colloidal silica abrasive particles. After ultra-precision polishing, the glass substrates were washed with a washing solution containing KOH to remove silica nanoparticles therefrom, and then dried.

[0121] Next, on the first main surface, two strip regions with rectangular shapes are provided in a rectangular region, wherein the rectangular region has a center at the intersection of the diagonals of the first main surface, a short side of 104 mm and a long side of 132 mm, the short side being parallel to the edge of the first main surface, and the rectangular shape having the short side of the rectangular region as one side, the long side being 104 mm and the short side being 2 mm ((A1) step).

[0122] Next, the shape (S0) of the rectangular region of the first main surface is measured using a surface shape measuring device (Ultraflat, manufactured by Tropel). A substrate with a similar surface shape to the substrate to be processed is pre-processed, and the pre-measured surface shape change (ΔS) caused by fine polishing is added. The surface shape (S0') obtained by superimposing the surface shape change caused by fine polishing is then calculated. Next, the surface shapes of portions of two strip regions are extracted from the surface shape (S0') of the rectangular region, and the flatness of the strip regions is evaluated (calculated) (step (B1)). The results are shown in Table 1.

[0123] Table 1

[0124]

[0125] In any one of the ten glass substrates (substrates 1-1 to 1-10), the flatness of two strip regions is not within the predetermined range (10 nm or less). Therefore, the strip regions are locally processed so that the flatness of the strip regions is within the predetermined range (step (C1)).

[0126] As a local processing apparatus, the local processing apparatus described in JP-A 2010-194705 (Patent Document 3) is used. Local processing using this apparatus polishes the entire surface of the substrate while controlling the movement speed of the fine polishing tool, and the target shape can be obtained by slowly moving the polishing tool in relatively protruding portions and quickly moving it in relatively recessed portions. As the processing tool for the local processing apparatus, a felt polishing wheel is used, and as the polishing slurry, silica nanoparticles (AJ-3540, manufactured by Nissan Chemical Corporation) mixed with a small amount of defoamer (Shin-Etsu Silicone KS-537, manufactured by Shin-Etsu Chemical Co., Ltd.) are used.

[0127] Next, the shape (S0) of a rectangular region on the first main surface is measured using a surface shape measuring device (Ultraflat, manufactured by Tropel). A substrate with a similar surface shape to the substrate to be processed is pre-processed, and the pre-measured surface shape change (ΔS) caused by fine polishing is superimposed. The surface shape (S0') obtained by superimposing the surface shape change caused by fine polishing is then calculated. Next, the surface shapes of two strip regions are extracted from the surface shape (S0') of the rectangular region, and the flatness of the strip regions is evaluated (calculated) (step (D1)). The results are shown in Table 2.

[0128] Table 2

[0129]

[0130] In each of the ten glass substrates (substrates 1-1 to 1-10), the flatness of the two strip regions is within a predetermined range (10 nm or less). Therefore, the flatness of the two strip regions is evaluated to be within the predetermined range after fine polishing, and the local processing step is terminated.

[0131] Next, the glass substrate, after the local processing steps, is placed in the carrier of a polishing apparatus using a velvety soft polishing cloth, and finely polished using a polishing slurry containing colloidal silica. After polishing, the glass substrate is washed with a washing solution containing KOH to remove the colloidal silica, and then dried to obtain a photomask blank substrate.

[0132] Next, the shape of the rectangular region of the first main surface was measured using a surface shape measuring device (Ultraflat, manufactured by Tropel). Then, the surface shapes of portions of the two strip regions were extracted from the surface shape of the rectangular region, and the flatness of the strip regions was evaluated (calculated). The results are shown in Table 3.

[0133] Table 3

[0134]

[0135] In each of the ten photomask blank substrates (substrates 1-1 to 1-10), the flatness of the two strip regions was confirmed to be within a predetermined range (10 nm or less).

[0136] Example 2

[0137] Five glass substrates were prepared, made of SiO2 and TiO2 (TiO2 concentration: approximately 7% by weight). The dimensions and shape of each of the first and second main surfaces were 152 mm × 152 mm squares with a thickness of 6.35 mm. The end faces of the glass substrates (the four surfaces other than the main surfaces) were chamfered and ground, and further rough and fine polished using a polishing slurry containing cerium oxide abrasive grains.

[0138] Next, five glass substrates (substrates 2-1 to 2-5) were placed in a carrier of a double-sided polishing apparatus using a velvety soft polishing cloth, and the first and second main surfaces were ultra-precisely polished using a polishing slurry containing colloidal silica abrasive particles. After ultra-precision polishing, the glass substrates were washed with a washing solution containing KOH to remove the silica nanoparticles therefrom, and then dried.

[0139] Next, on the first main surface, two strip regions with rectangular shapes are provided in a rectangular region, wherein the rectangular region has a center at the intersection of the diagonals of the first main surface, a short side of 104 mm and a long side of 132 mm, the short side being parallel to the edge of the first main surface, and the rectangular shape having the short side of the rectangular region as one side, the long side being 104 mm and the short side being 2 mm ((A1) step).

[0140] Next, the shape (S0) of the rectangular region of the first main surface is measured using a surface shape measuring device (Ultraflat, manufactured by Tropel). A substrate with a similar surface shape to the substrate to be processed is pre-processed, and the pre-measured surface shape change (ΔS) caused by fine polishing is superimposed, and the surface shape (S0') obtained by superimposing the surface shape change caused by fine polishing is calculated. Then, the surface shapes of two strip regions are extracted from the surface shape (S0') of the rectangular region, and the flatness of the strip regions is evaluated (calculated) (step (B1)). Additionally, the flatness of the rectangular region is evaluated (calculated) using the surface shape (S0') of the rectangular region, and the ratio of the flatness of the strip regions to the flatness of the rectangular region is calculated. The results are shown in Table 4.

[0141] Table 4

[0142]

[0143] In any of the five glass substrates (substrates 2-1 to 2-5), the flatness of neither of the two strip regions is within a predetermined range (10 nm or less), and in one or both of the two strip regions, the ratio of the flatness of the strip region to the flatness of the rectangular region is not within a predetermined range (0.3 or less (30% or less)). Therefore, the rectangular region comprising the strip region is locally processed such that the flatness of the strip region and the ratio of the flatness of the strip region to the flatness of the rectangular region are within a predetermined range (step (C1)).

[0144] As a local processing apparatus, the local processing apparatus described in JP-A 2010-194705 (Patent Document 3) is used. Local processing using this apparatus polishes the entire surface of the substrate while controlling the movement speed of the fine polishing tool, and the target shape can be obtained by slowly moving the polishing tool in relatively protruding portions and quickly moving it in relatively recessed portions. As the processing tool for the local processing apparatus, a felt polishing wheel is used, and as the polishing slurry, silica nanoparticles (AJ-3540, manufactured by Nissan Chemical Corporation) mixed with a small amount of defoamer (Shin-Etsu Silicone KS-537, manufactured by Shin-Etsu Chemical Co., Ltd.) are used.

[0145] Next, the shape (S0) of the rectangular region of the first main surface is measured using a surface shape measuring device (Ultraflat, manufactured by Tropel). A substrate with a similar surface shape to the substrate to be processed is pre-processed, and the pre-measured surface shape change (ΔS) caused by fine polishing is superimposed. The surface shape (S0') obtained by superimposing the surface shape change caused by fine polishing is then calculated. Next, the surface shapes of two strip regions are extracted from the surface shape (S0') of the rectangular region, and the flatness of the strip regions is evaluated (calculated) (step (D1)). Furthermore, the flatness of the rectangular region is evaluated (calculated) using the surface shape (S0') of the rectangular region, and the ratio of the flatness of the strip regions to the flatness of the rectangular region is calculated. The results are shown in Table 5.

[0146] Table 5

[0147]

[0148] In each of the five glass substrates (substrates 2-1 to 2-5), the flatness of the two strip regions is within a predetermined range (10 nm or less), and the ratio of the flatness of the strip region to the flatness of the rectangular region in both strip regions is within a predetermined range (0.3 or less (30% or less)). Therefore, if the flatness of the two strip regions and the ratio of the flatness of the two strip regions to the flatness of the rectangular region after fine polishing are both within the predetermined range, the local processing step is terminated.

[0149] Next, the glass substrate, after the local processing steps, is placed in the carrier of a polishing apparatus using a velvety soft polishing cloth, and finely polished using a polishing slurry containing colloidal silica. After polishing, the glass substrate is washed with a washing solution containing KOH to remove the colloidal silica, and then dried to obtain a photomask blank substrate.

[0150] Next, the shape of the rectangular region of the first main surface was measured using a surface shape measuring device (Ultraflat, manufactured by Tropel). Then, the surface shapes of two strip regions were extracted from the surface shape of the rectangular region, and the flatness of the strip regions was evaluated (calculated). Additionally, the flatness was evaluated (calculated) based on the surface shape of the rectangular region, and the ratio of the flatness of the strip regions to the flatness of the rectangular region was calculated. The results are shown in Table 6.

[0151] Table 6

[0152]

[0153] In each of the five photomask blank substrates (substrates 2-1 to 2-5), the flatness of the two strip regions was confirmed to be within a predetermined range (10 nm or less). Furthermore, in each of the five photomask blank substrates (substrates 2-1 to 2-5), the ratio of the flatness of the two strip regions to the flatness of the rectangular region was confirmed to be within a predetermined range (0.3 or less (30% or less)).

[0154] Example 3

[0155] Five glass substrates were prepared, made of SiO2 and TiO2 (TiO2 concentration: approximately 7% by weight). The dimensions and shape of the first and second main surfaces were 152 mm × 152 mm squares with a thickness of 6.35 mm. The end faces of the glass substrates (the four surfaces other than the main surfaces) were chamfered and ground, and then further rough and fine polished using a polishing slurry containing cerium oxide abrasive grains.

[0156] Next, five glass substrates (substrates 3-1 to 3-5) were placed in a carrier of a double-sided polishing apparatus using a velvety soft polishing cloth, and the first and second main surfaces were ultra-precisely polished using a polishing slurry containing colloidal silica abrasive particles. After ultra-precision polishing, the glass substrates were washed with a washing solution containing KOH to remove the silica nanoparticles therefrom, and then dried.

[0157] Next, on the first main surface, two strip regions with rectangular shapes are provided in a rectangular region, wherein the rectangular region has a center at the intersection of the diagonals of the first main surface, a short side of 104 mm and a long side of 132 mm, the short side being parallel to the edge of the first main surface, and each of the two short sides of the rectangular region is a side, with the long side being 104 mm and the short side being 2 mm ((A1) step).

[0158] Next, the shape (S0) of the rectangular region of the first main surface is measured using a surface shape measuring device (Ultraflat, manufactured by Tropel). A substrate with a similar surface shape to the substrate to be processed is pre-processed, and the pre-measured surface shape change (ΔS) caused by fine polishing is added. The surface shape (S0') obtained by superimposing the surface shape change caused by fine polishing is then calculated. Next, the surface shapes of two strip regions are extracted from the surface shape (S0') of the rectangular region, and the flatness of the strip regions is evaluated (calculated) (step (B1)). Additionally, the flatness of the rectangular region is evaluated (calculated) using the surface shape (S0') of the rectangular region. The results are shown in Table 7.

[0159] Table 7

[0160]

[0161] In any of the five glass substrates (substrates 3-1 to 3-5), the flatness of both strip regions is outside the predetermined range (10 nm or less), and the flatness of the rectangular region is outside the predetermined range (30 nm or less). Therefore, the local processing includes the rectangular region of the strip region, such that the flatness of the strip region and the flatness of the rectangular region are within the predetermined range (step (C1)).

[0162] As a local processing apparatus, the local processing apparatus described in JP-A 2010-194705 (Patent Document 3) is used. Local processing using this apparatus polishes the entire surface of the substrate while controlling the movement speed of the fine polishing tool, and the target shape can be obtained by slowly moving the polishing tool in relatively protruding portions and quickly moving it in relatively recessed portions. As the processing tool for the local processing apparatus, a felt polishing wheel is used, and as the polishing slurry, silica nanoparticles (AJ-3540, manufactured by Nissan Chemical Corporation) mixed with a small amount of defoamer (Shin-Etsu Silicone KS-537, manufactured by Shin-Etsu Chemical Co., Ltd.) are used.

[0163] Next, the shape (S0) of the rectangular region of the first main surface is measured using a surface shape measuring device (Ultraflat, manufactured by Tropel). A substrate with a similar surface shape to the substrate to be processed is pre-processed, and the pre-measured surface shape change (ΔS) caused by fine polishing is superimposed, and the surface shape (S0') obtained by superimposing the surface shape change caused by fine polishing is calculated. Then, the surface shapes of two strip regions are extracted from the surface shape (S0') of the rectangular region, and the flatness of the strip regions is evaluated (calculated) (step (D1)). Additionally, the flatness of the rectangular region is evaluated (calculated) using the surface shape (S0') of the rectangular region. The results are shown in Table 8.

[0164] Table 8

[0165]

[0166] In each of the five glass substrates (substrates 3-1 to 3-5), the flatness of the two strip regions is within a predetermined range (10 nm or less), and the flatness of the rectangular region is within a predetermined range (30 nm or less). Therefore, the flatness of the two strip regions and the flatness of the rectangular region after fine polishing are evaluated and found to be within the predetermined range, and the local processing step is terminated.

[0167] Next, the glass substrate, after the local processing steps, is placed in the carrier of a polishing apparatus using a velvety soft polishing cloth, and finely polished using a polishing slurry containing colloidal silica. After polishing, the glass substrate is washed with a washing solution containing KOH to remove the colloidal silica, and then dried to obtain a photomask blank substrate.

[0168] Next, the shape of the rectangular region of the first main surface was measured using a surface shape measuring device (Ultraflat, manufactured by Tropel). Then, the surface shapes of portions of the two strip regions were extracted from the surface shape of the rectangular region, and the flatness of the strip regions was evaluated (calculated). Additionally, the flatness was evaluated (calculated) based on the surface shape of the rectangular region. The results are shown in Table 9.

[0169] Table 9

[0170]

[0171] In each of the five photomask blank substrates (substrates 3-1 to 3-5), the flatness of the two strip regions was confirmed to be within a predetermined range (10 nm or less). In addition, in each of the five photomask blank substrates (substrates 3-1 to 3-5), the flatness of the rectangular region was confirmed to be within a predetermined range (30 nm or less).

[0172] Example 4

[0173] Three glass substrate groups were prepared. Each glass substrate group consisted of two glass substrates made of SiO2 and TiO2 (TiO2 concentration: approximately 7% by weight). The dimensions and shape of the first and second main surfaces were 152 mm × 152 mm squares with a thickness of 6.35 mm. The end faces of the glass substrates (the four surfaces other than the main surfaces) were chamfered and ground, and further rough and fine polished using a polishing slurry containing cerium oxide abrasive grains.

[0174] Next, six glass substrates from three glass substrate groups (substrate groups 4-1 to 4-3) were placed in a carrier of a double-sided polishing apparatus using a velvety soft polishing cloth, and the first and second main surfaces were ultra-precisely polished using a polishing slurry containing colloidal silica abrasive particles. After ultra-precision polishing, the glass substrates were washed with a washing solution containing KOH to remove silica nanoparticles, and then dried.

[0175] Next, in each of the two glass substrates in each glass substrate group, two strip regions with rectangular shapes are formed in a rectangular region on the first main surface, wherein the rectangular region has a center at the intersection of the diagonals of the first main surface, a short side of 104 mm and a long side of 132 mm, the short side being parallel to the edge of the first main surface, and the rectangular shape having the short side of the rectangular region as one side, the long side being 104 mm and the short side being 2 mm ((A2) step).

[0176] Next, in each of the two glass substrates in each glass substrate group, the shape (S0) of the rectangular region of the first main surface is measured by a surface shape measuring device (Ultraflat, manufactured by Tropel). The substrate with a similar surface shape to the substrate to be processed is pre-processed, and the pre-measured surface shape change (ΔS) caused by fine polishing is superimposed, and the surface shape (S0') obtained by superimposing the surface shape change caused by fine polishing is calculated.

[0177] Next, in each of the two glass substrates in each glass substrate group, a portion of the surface shape of a strip region is extracted from the surface shape of the rectangular region (S0'), and the surface of one strip region is connected to the surface of the other strip region such that the least-squares surfaces of the rectangular regions of the two photomask blank substrates to be connected overlap each other, thereby setting a composite surface having a rectangular shape with one side of 104 mm and the other side of 4 mm. The composite surface is an imaginary surface, which is obtained by connecting the 104 mm side of the two glass substrates on the side away from the center of the first main surface of one strip region and the 104 mm side on the side away from the center of the first main surface of the other strip region. Next, the flatness of the composite surface is evaluated (calculated) (step (B2)). The results are shown in Table 10.

[0178] Table 10

[0179]

[0180] In any of the three glass substrate groups (substrate groups 4-1 to 4-3), the flatness of the composite surface is not within a predetermined range (10 nm or less). Therefore, the strip regions of the two glass substrates are locally processed to make the flatness of the composite surface within the predetermined range (step (C2)).

[0181] As a local processing apparatus, the local processing apparatus described in JP-A 2010-194705 (Patent Document 3) is used. Local processing using this apparatus polishes the entire surface of the substrate while controlling the movement speed of the fine polishing tool, and the target shape can be obtained by slowly moving the polishing tool in relatively protruding portions and quickly moving it in relatively recessed portions. As the processing tool for the local processing apparatus, a felt polishing wheel is used, and as the polishing slurry, silica nanoparticles (AJ-3540, manufactured by Nissan Chemical Corporation) mixed with a small amount of defoamer (Shin-Etsu Silicone KS-537, manufactured by Shin-Etsu Chemical Co., Ltd.) are used.

[0182] Next, in each of the two glass substrates in each glass substrate group, the shape (S0) of a rectangular region on the first main surface is measured by a surface shape measuring device (Ultraflat, manufactured by Tropel). A substrate with a similar surface shape to the substrate to be processed is pre-processed, and the pre-measured surface shape change (ΔS) caused by fine polishing is superimposed. The surface shape (S0') obtained by superimposing the surface shape change caused by fine polishing is then calculated. Next, the surface shape (S0') of a portion of the strip region is extracted from the surface shape (S0') of the rectangular region, a composite surface is set, and the flatness of the composite surface is evaluated (calculated) (step (D2)). The results are shown in Table 11.

[0183] Table 11

[0184]

[0185] In each of the three glass substrate groups (substrate groups 4-1 to 4-3), the flatness of the composite surface is within a predetermined range (10 nm or less). Therefore, the flatness of the composite surface after fine polishing is evaluated to be within the predetermined range, and the local processing step is terminated.

[0186] Next, in each of the two glass substrates in each glass substrate group, the glass substrate after the local processing step is placed in the carrier of a polishing apparatus using a velvety soft polishing cloth, and finely polished using a polishing slurry containing colloidal silica. After polishing, the glass substrate is washed with a washing solution containing KOH to remove the colloidal silica, and then dried to obtain a photomask blank substrate group.

[0187] Next, the shape of the rectangular region of the first main surface was measured using a surface shape measuring device (Ultraflat, manufactured by Tropel). Then, the surface shape of a portion of the strip region was extracted from the surface shape of the rectangular region, a composite surface was constructed, and the flatness of the composite surface was evaluated (calculated). The results are shown in Table 12.

[0188] Table 12

[0189]

[0190] In each of the three photomask preform substrate groups (substrate groups 4-1 to 4-3), the flatness of the composite surface was confirmed to be within a predetermined range (10 nm or less).

[0191] In the photomask blank substrate and photomask blank substrate group obtained in the embodiments, the flatness of the area that can be used as a splicing target is very good, and in the exposure using high NA EUVL, it can provide a mask with reduced displacement of the transfer position during exposure, good splicing, and high exposure performance. Good exposure results can be expected from such a photomask.

Claims

1. A photomask blank substrate having two main surfaces, each consisting of a first main surface and a second main surface, wherein the first main surface and the second main surface are each square with one side of 152 mm and the other side of 152 mm. When a strip region with a rectangular shape is provided in a rectangular region on the first main surface, the flatness of the strip region is 10 nm or less, wherein the rectangular region has a center at the intersection of the diagonals of the first main surface, a short side of 104 mm and a long side of 132 mm, the short side being parallel to the edge of the first main surface, and the rectangular shape having one short side as one side, the long side being 104 mm, and the short side being 1 mm-2 mm.

2. The photomask blank substrate according to claim 1, wherein the ratio of the flatness of the strip region to the flatness of the rectangular region is 0.3 or less.

3. The photomask blank substrate according to claim 1, wherein... When two strip regions are set in the rectangular region, the flatness of each of the two strip regions is 10 nm or less, wherein each strip region has a rectangular shape, and the rectangular shape has each of the two short sides of the rectangular region as one side, the long side being 104 mm and the short side being 1 mm - 2 mm.

4. The photomask blank substrate according to claim 3, wherein the flatness ratio of each of the two strip regions to the flatness of the rectangular region is 0.3 or less.

5. The photomask blank substrate according to claim 1 or 3, wherein the flatness of the rectangular region is 30 nm or less.

6. The photomask blank substrate according to claim 1 or 3, having a thickness of 6.35 mm.

7. A photomask preform substrate assembly, comprising two photomask preform substrates, each having two main surfaces consisting of a first main surface and a second main surface, wherein the first main surface and the second main surface are each square in shape with one side of 152 mm and the other side of 152 mm. In each of the two photomask blank substrates, When a strip region with a rectangular shape is formed in a rectangular region on the first main surface, the flatness of the composite surface with the rectangular shape is 10 nm or less. The rectangular region has a center at the intersection of the diagonals of the first main surface, a short side of 104 mm, and a long side of 132 mm. The short side is parallel to the edge of the first main surface. The rectangular shape of the strip region is defined by one of its short sides, with a long side of 104 mm and a short side of 1 mm-2 mm. The rectangular shape of the composite surface has one side of 104 mm and another side of 2 mm-4 mm. The composite surface is formed by connecting the surface of the strip region of one photomask blank substrate and the surface of the strip region of another photomask blank substrate such that the reference surfaces of the two surfaces overlap each other.

8. The photomask preform substrate assembly according to claim 7, wherein the photomask preform substrate has a thickness of 6.35 mm.

9. A method for manufacturing a photomask blank substrate, the photomask blank substrate having two main surfaces consisting of a first main surface and a second main surface, the first main surface and the second main surface each having a square shape with one side of 152 mm and the other side of 152 mm, the method comprising: The local processing steps for the first main surface and the fine polishing steps following the local processing steps, wherein The local processing steps include: (A1) The step of forming one or two strip regions with a rectangular shape in a rectangular region on the first main surface of the raw material substrate, wherein the rectangular region has a center at the intersection of the diagonals of the first main surface, a short side of 104 mm, and a long side of 132 mm, the short side being parallel to the edge of the first main surface, and the rectangular shape having one or two short sides of the rectangular region as one side, the long side being 104 mm, and the short side being 1 mm-2 mm. (B1) The steps for evaluating the flatness of the one or two strip regions, and (C1) The step of partially processing the first main surface to make the flatness of the one or two strip regions within a predetermined range.

10. The manufacturing method according to claim 9, further comprising (D1) evaluating the flatness of the one or two strip regions of the first main surface after partial processing in step (C1).

11. The manufacturing method according to claim 10, wherein when the flatness of one strip region or the flatness of one or both of the two strip regions evaluated in step (D1) is not within the predetermined range, step (C1) or steps (C1) and (D1) are performed again.

12. A method for manufacturing a photomask preform substrate assembly, the photomask preform substrate assembly comprising two photomask preform substrates, each photomask preform substrate having two main surfaces consisting of a first main surface and a second main surface, the first main surface and the second main surface each having a square shape with one side of 152 mm and the other side of 152 mm, the method comprising: The local processing step and the fine polishing step following the local processing step are for one or both of the first main surface of the two photomask blank substrates, wherein The local processing steps include: (A2) In each of the two raw material substrates, the step of forming a strip region with a rectangular shape in a rectangular region on the first main surface, wherein the rectangular region has a center at the intersection of the diagonals of the first main surface, a short side of 104 mm and a long side of 132 mm, the short side being parallel to the edge of the first main surface, and the rectangular shape having one short side as one side of the rectangular region, the long side being 104 mm, and the short side being 1 mm-2 mm. (B2) The step of evaluating the flatness of a composite surface having a rectangular shape, wherein the rectangular shape has one side of 104 mm and another side of 2 mm-4 mm, the composite surface being formed by connecting the surface of the strip region of one photomask blank substrate and the surface of the strip region of another photomask blank substrate such that the reference surfaces of the two surfaces overlap each other; and (C2) The step of partially processing one or two of the first main surfaces to make the flatness of the composite surface within a predetermined range.

13. The manufacturing method according to claim 12, further comprising (D2) evaluating the flatness of the composite surface after partial processing in step (C2).

14. The manufacturing method according to claim 13, wherein when the flatness of the composite surface evaluated in step (D2) is not within the predetermined range, step (C2) or steps (C2) and (D2) are performed again.

15. The manufacturing method according to claim 9 or 12, wherein the photomask blank substrate has a thickness of 6.35 mm.

Citation Information

Patent Citations

  • Method of processing synthetic quartz glass substrate for semiconductor

    JP2010194705A

  • Photomask-forming glass substrate and method of manufacturing the same

    JP2011141536A

  • Glass substrate for EUVL mask blank, and manufacturing method thereof

    JP2017044758A