Photosensitive resin composition and its preparation method

The crosslinking reaction of benzotriazole adhesion promoter modified with active double bonds with alkali-soluble resin composition solves the problem of insufficient adhesion of photosensitive layer, achieving high adhesion and electroplating resistance, and improving the production efficiency and reliability of printed circuit boards.

CN123113241APending Publication Date: 2026-11-17TAICANG SIDIKE NEW MATERIALS SCI & TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611226840.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-13
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing photosensitive layer has insufficient adhesion to the substrate surface, which makes the electroplating process prone to plating problems and prolonged peeling time in the manufacturing of high-density circuit boards. In addition, existing additives have residue and delamination defects.

Method used

Benzotriazole modified with active double bonds is used as an adhesion promoter. It is combined with alkali-soluble resin, photopolymerizable monomer and photoinitiator to improve the adhesion between the photosensitive layer and the substrate and enhance the bonding force by forming coordination bonds and cross-linking reaction.

Benefits of technology

It improves the adhesion and electroplating resistance of the photosensitive layer on low-profile copper foil, reduces the defect of prolonged peeling time, improves the production efficiency and yield of PCB/FPC, and is less prone to development residue and electroplating delamination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123113241A_ABST
    Figure CN123113241A_ABST
Patent Text Reader

Abstract

This invention provides a photosensitive resin composition, comprising, by weight, the following raw material components: 45-65 parts of alkali-soluble resin, 35-55 parts of photopolymerizable monomer, 0.1-6 parts of photoinitiator, 0.5-5 parts of adhesion promoter, and 0.1-5 parts of additive; wherein the adhesion promoter is benzotriazole modified with active double bonds as shown in Formula I. This invention also provides a method for preparing the adhesion promoter and a method for preparing the photosensitive resin composition. The photosensitive resin composition of this invention can improve adhesion to low-profile copper foil and improve electroplating resistance without causing prolonged peeling time. Furthermore, it can improve the production efficiency and yield of PCB / FPC. The preparation method of this invention is simple, easy to implement, and produces stable finished products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of photoresist technology, and particularly relates to a photosensitive resin composition and its preparation method. Background Technology

[0002] Photosensitive dry film, also known as dry film photoresist, is the main material for pattern transfer in the manufacturing process of printed circuit boards (PCBs). It typically consists of a protective film, a photosensitive layer, and a carrier film, forming a photosensitive element. The photosensitive layer often comprises photosensitive resin, reactive diluent, and photoinitiator. Copper-clad laminates and other metal substrates usually consist of two or one conductive layers on one side and an insulating resin layer in the middle, hereinafter referred to as "substrate". Printed circuit boards (PCBs) use these photosensitive elements and are manufactured through the following steps: First, the protective film in the photosensitive element is removed, and the photosensitive layer with the carrier film is laminated onto a circuit-forming substrate such as a copper-clad laminate or an aluminum substrate. Next, the photosensitive layer is exposed through a mask or by direct laser imaging to form a photocurable portion. Then, after exposure, the support film is peeled off, and the area outside the photocurable portion of the photosensitive layer is removed using a developer to form the resist pattern. Next, the resist pattern is used as a resist, and etching or electroplating followed by etching is performed to form a conductor pattern. Finally, the photocured part (resist pattern) of the photosensitive layer is peeled off.

[0003] In recent years, with the increasing density of printed circuit boards (PCBs) and the refinement of conductor patterns, the contact area between the substrate used for circuit formation and the photosensitive layer acting as resist has decreased. For example, in PCBs used in high-frequency and high-speed applications, such as 5G base stations, very low profile copper foil (VLP) is required, with a surface roughness requirement of Ra ≤ 0.3µm and Rz ≤ 1.5µm. For these reasons, the photosensitive layer must maintain excellent adhesion to the substrate surface during etching or electroplating processes and possess excellent resolution characteristics in the formation of the resist pattern.

[0004] The adhesion between the photosensitive layer and the substrate surface is mainly determined by the number of physical anchor points on the substrate surface and the weak chemical forces, such as hydrogen bonds and coordination bonds. Due to technological and market trends leading to a decrease in substrate surface roughness, the number of available physical anchor points has significantly decreased. Therefore, improving the chemical forces between the substrate and the photosensitive layer is crucial. However, existing technologies often improve adhesion through the design of the photosensitive resin, such as by adding hydrophobic monomers, for example, using styrene to adjust the resin's hydrophobicity to reduce swelling of the photosensitive layer during development and etching after photocuring, thus indirectly improving adhesion. However, this can lead to plating over-plating issues during electroplating and prolonged peeling time, while also posing a risk of incomplete photosensitive layer removal. Another approach involves adding benzotriazole (BTA) and its derivatives; however, currently used compounds of this type still have some drawbacks, such as insufficient addition resulting in no adhesion-promoting effect, or excessive addition causing residue and delamination of the plating layer. For example, introducing acid- or alkali-sensitive groups into the benzotriazole (BTA) framework allows for hydrolysis upon contact with acid or alkali, generating corresponding salt compounds that promote adhesion or provide protection. However, in actual PCB manufacturing, pickling or alkaline development times are very short, approximately 30-60 seconds, with temperatures not exceeding 30°C. Furthermore, the diffusion of acidic or alkaline ions within the photosensitive layer after photocuring is relatively slow, making it difficult to completely and quickly remove all sensitive groups. Simultaneously, residues remain on the copper surface, affecting the adhesion between subsequent electroplating layers and the copper substrate. Summary of the Invention

[0005] In view of this, the object of the present invention is to provide a photosensitive resin composition that can improve adhesion to low-profile copper foil, improve electroplating resistance, and at the same time avoid the defect of prolonged peeling time.

[0006] Another objective of this invention is to provide a method for preparing a photosensitive resin composition that is simple, easy to implement, and produces a product with stable performance.

[0007] To achieve the above objectives, the present invention provides a photosensitive resin composition, comprising, by weight, the following raw material components: 45-65 parts of alkali-soluble resin, 35-55 parts of photopolymerizable monomer, 0.1-6 parts of photoinitiator, 0.5-5 parts of adhesion promoter, and 0.1-5 parts of additives; The adhesion promoter is benzotriazole modified with active double bonds as shown in Formula I: Formula I; R1, R2, R3, and R4 are each independently selected from one of the substituent groups, hydrogen, C1-C12 alkyl groups, and C2-C12 unsaturated ester groups shown in Formula II and Formula III. Formula II; Formula III; R5 is selected from hydrogen or methyl.

[0008] In the above-mentioned photosensitive resin composition, the additives may be additives known in the art; preferably, the additives include one or a combination of several of leuco crystal violet, malachite green, and tribromomethylphenyl sulfone.

[0009] Preferably, the raw material components of the above-mentioned photosensitive resin composition may further include a solvent, which may include one or a combination of acetone, toluene, methanol, and methyl ethyl ketone.

[0010] In the described photosensitive resin composition, preferably, the solvent can be acetone / toluene / methanol = 6 / 10 / 6; or acetone / toluene / methanol = 7 / 10 / 5.

[0011] In the above-mentioned photosensitive resin composition, the amount of solvent can be adjusted as needed.

[0012] In the above-described photosensitive resin composition, preferably, the adhesion promoter is selected from compounds represented by the following formulas IV and / or V: Formula IV; Formula V.

[0013] In the above-mentioned photosensitive resin composition, preferably, the amount of the adhesion promoter is 1-4 parts.

[0014] In the above-described photosensitive resin composition, preferably, the photopolymerizing monomer can be an olefinic unsaturated carboxylic acid ester. More preferably, in the above-described photosensitive resin composition, the photopolymerizing monomer is a (meth)acrylate monomer.

[0015] In the above-mentioned photosensitive resin composition, more preferably, the photopolymerizable monomer is selected from one or a combination of several of the following: methoxy polyethylene glycol monoacrylate, ethoxy(propoxy)bisphenol A di(meth)acrylate, ethoxy(propoxy)di(meth)acrylate, polyethylene glycol diacrylate, polypropylene glycol diacrylate, ethoxy(propoxy)trimethylolpropane tri(meth)acrylate, di(trimethylolpropane)tetraacrylate, and polyurethane.

[0016] In the above-mentioned photosensitive resin composition, preferably, the amount of the photopolymerizable monomer is 35-55 parts by weight.

[0017] In the above-mentioned photosensitive resin composition, more preferably, the amount of the photopolymerizable monomer is 40-45 parts by weight.

[0018] In the above-mentioned photosensitive resin composition, preferably, the photoinitiator is an acridine compound and / or a hexaaryl diimidazole compound. By weight, when the photoinitiator is an acridine compound, the amount of photoinitiator is 0.1-2 parts, and when the photoinitiator is a hexaaryl diimidazole compound, the amount of photoinitiator is 3-6 parts.

[0019] In the above-mentioned photosensitive resin composition, preferably, the amount of acridine initiator is 0.3-1.5 parts by weight. More preferably, the amount of acridine initiator is 0.5-1 parts by weight.

[0020] In the above-mentioned photosensitive resin composition, preferably, the amount of hexaaryl diimidazole initiator is 3.5-5.0 parts by weight.

[0021] In the above-mentioned photosensitive resin composition, preferably, the photoinitiator is selected from one or a combination of two of 9-phenyl-substituted acridine compounds, o-chlorohexaaryl diimidazole, and 2,2',4-tris(2-chlorophenyl)-5-(3,4-dimethoxyphenyl)-4'5'-diphenyl-1,1'-diimidazole.

[0022] In the above-mentioned photosensitive resin composition, preferably, the alkali-soluble resin is an acrylate copolymer containing aromatic groups, which is copolymerized from methacrylic acid and copolymer units, and the copolymerization ratio of comonomers with aromatic groups is 10%-50% based on the total mass of comonomers during the copolymerization process.

[0023] In the above-mentioned photosensitive resin composition, preferably, the copolymer unit is selected from one or a combination of several of methyl methacrylate, ethyl methacrylate, butyl methacrylate, benzyl methacrylate, and styrene.

[0024] In the above-mentioned photosensitive resin composition, preferably, the alkali-soluble resin has a weight-average molecular weight of 30,000-70,000, a resin acid value of 160-200 mg KOH / g, and a molecular weight distribution index of 1.0-3.0.

[0025] Preferably, in the above-described photosensitive resin composition, the adhesion promoter is prepared by the following steps: Benzotriazole is mixed with concentrated sulfuric acid and then concentrated nitric acid is added to undergo a nitration reaction to obtain benzotriazole with a nitro group on the benzene ring; Benzotriazole with a nitro group on the benzene ring was dissolved in methanol and reduced to amino-substituted benzotriazole using Pd / C and hydrogen. An adhesion promoter is obtained by dissolving an amino-substituted benzotriazole in dichloromethane, adding triethylamine, and then adding acryloyl chloride dropwise.

[0026] In the above-mentioned photosensitive resin composition, the amounts of methanol, triethylamine, and dichloromethane can be adjusted as needed. Pd / C is a commonly used substance in this field.

[0027] In the above-mentioned photosensitive resin composition, the adhesion promoter shown in Formula V is a known compound, and its synthesis method can be a conventional synthesis method.

[0028] In the above-mentioned photosensitive resin composition, preferably, the preparation step of the adhesion promoter further includes quenching the adhesion promoter obtained after the reaction with acryloyl chloride with water, extracting the crude product; then adding the crude product to an ethanol solution of KOH for reaction, quenching the reaction with HCl, extracting with a water and dichloromethane system, drying the organic phase with Na2SO4, concentrating, and separating with a silica gel column to obtain a high-purity adhesion promoter.

[0029] In the above-mentioned photosensitive resin composition, the photosensitive resin composition enhances its adhesion to the substrate through the following reaction mechanism: when the photosensitive resin composition is bonded to the substrate surface, it first forms coordination bonds and hydrogen bonds with copper atoms through the carboxyl groups in the resin and the triazole groups in the adhesion promoter; after being irradiated by ultraviolet light, the photoinitiator generates free radicals, which initiate the photopolymerization of monomers. At the same time, it reacts with the double bonds in the adhesion promoter that have already formed coordination bonds on the substrate surface to form a cross-linked body, thereby enhancing the bonding force between the entire cross-linked system and the substrate surface.

[0030] The present invention also provides a method for preparing the above-mentioned photosensitive resin composition, which is prepared by mixing an alkali-soluble resin, a photopolymerizable monomer, a photoinitiator, an adhesion promoter and an additive.

[0031] In the aforementioned photosensitive resin composition containing benzotriazole adhesion promoters modified with active double bonds, the active double bonds of the adhesion promoter are linked to an amide bond and an amine alkyl group on the benzene ring. This structure can both improve adhesion between the triazole and copper atoms on the copper substrate by forming coordinate bonds, and the active double bonds can crosslink with other active monomers in the composition to form a crosslinked system with excellent cohesive strength. If unmodified benzotriazole (BTA) is directly added to the composition, its rigid structure and small molecular size make it unable to form stronger covalent bonds with the molecules in the system, leading to its easy residue on the copper surface of the substrate, resulting in poor oxidation of the copper surface after development; it can also cause plating separation during electroplating, insufficient plating adhesion, and precipitation in the electroplating solution, causing plating solution contamination and affecting plating thickness.

[0032] As can be seen from the above, the technical solution provided by the present invention has the following significant beneficial effects: The photosensitive resin composition of this invention can improve adhesion to low-profile copper foil and enhance electroplating resistance without causing prolonged peeling time. Furthermore, it can improve the production efficiency and yield of PCB / FPCs. The preparation method of this invention is simple, easy to implement, and produces stable finished products. Attached Figure Description

[0033] Figure 1 A schematic diagram of the process route for the adhesion promoter BPEM; Figure 2 The image shows the 1H-NMR spectrum of the adhesion promoter BPEM. Detailed Implementation

[0034] To provide a clearer understanding of the technical features, objectives, and beneficial effects of this disclosure, the technical solution of this disclosure is described in detail below, but this should not be construed as limiting the scope of implementation of this disclosure. Unless otherwise specified, the experimental methods described in the following embodiments are conventional methods; the reagents and materials described, unless otherwise specified, are commercially available.

[0035] Example 1: This embodiment provides a photosensitive resin composition, comprising the following raw material components in parts by weight: Alkali-soluble resins, photopolymerizable monomers, photoinitiators, adhesion promoters, additives, and solvents; The adhesion promoter is a compound represented by Formula IV.

[0036] Formula IV.

[0037] This embodiment also provides a method for preparing an adhesion promoter (BPEM), such as... Figure 1 As shown, it is prepared through the following steps: In the first step, 1H-benzotriazole (25 g, 209.87 mmol) was mixed with concentrated sulfuric acid (80 mL) at 0 °C to form a mixture. Concentrated nitric acid (44.76 g, 461.70 mmol) was then added dropwise to the mixture to initiate a nitration reaction. The mixture was then stirred at 60 °C for 8 hours. After cooling to room temperature, the reaction mixture was slowly poured into crushed ice, resulting in the precipitation of a white solid. The white solid precipitate was washed with ethanol and dried to obtain benzotriazole with a nitro group on the benzene ring: 4-nitro-1H-benzo[d][1,2,3]triazole (20 g, 121.86 mmol, yield 58.07%).

[0038] spectral data: 1H NMR (400 MHz, DMSO-d6) δ = 8.58 (d, J = 8.1 Hz, 1H), 8.45(d, J = 7.8 Hz, 1H), 7.63 (t, J = 8.0 Hz, 1H) The 1H-NMR spectrum confirmed that it was 4-nitro-1H-benzo[d][1,2,3]triazole.

[0039] In the second step, under a nitrogen atmosphere, Pd / C (3.24 g, 3.05 mmol) was added to a methanol (40 mL) solution of 4-nitro-1H-benzotriazole (5 g, 30.47 mmol). The suspension was degassed and purged three times with hydrogen. The reaction mixture was then stirred for 1 hour under a hydrogen atmosphere at 40°C. After filtration, the filtrate was concentrated under reduced pressure to obtain a yellow solid, namely amino-substituted benzotriazole: 1H-benzo[d][1,2,3]triazole-4-amine (4 g, 29.82 mmol, yield 97.88%), which could be used directly in the next step without further purification. spectral data: 1 H NMR (400 MHz, DMSO-d6) δ = 7.12 (t, J = 7.8 Hz, 1H), 6.82 (d, J = 8.1 Hz, 1H), 6.39 (d, J = 7.5 Hz, 1H), 5.86 (s, 2H) The 1H-NMR spectrum confirmed that it was 1H-benzo[d][1,2,3]triazol-4-amine.

[0040] In the third step, 1H-benzotriazol-4-amine (8 g, 59.64 mmol), triethylamine (12.07 g, 119.28 mmol, 16.60 mL), and anhydrous dichloromethane (80 mL) were stirred and mixed at 0°C. Acryloyl chloride (11.88 g, 131.21 mmol, 10.66 mL) was added dropwise to the solution at 0°C. The reaction mixture was then stirred at 25°C for 1 hour to obtain the adhesion promoter, which was crude. The reaction was quenched by adding water (20 mL). The reaction mixture was diluted with water (300 mL) and extracted with dichloromethane (300 mL × 3). The combined organic phases were washed three times with saturated brine (50 mL), dried over anhydrous sodium sulfate, filtered, and concentrated under reduced pressure to obtain the residue. The crude product was stirred with potassium hydroxide (4.02 g) in methanol (60 mL) at room temperature for 10 minutes. At 0°C, the pH was adjusted to 5-6 with 1 mol / L hydrochloric acid aqueous solution to quench the reaction, followed by dilution with water (400 mL) and extraction with dichloromethane (400 mL × 8). The combined organic phases were dried over anhydrous sodium sulfate, filtered, and concentrated under reduced pressure to obtain the residue. The residue was purified by rapid silica gel column chromatography (ISCO®; 120 g SepaFlash® silica gel column, eluent gradient of 0-30% ethyl acetate / petroleum ether, flow rate 80 mL / min). The crude product was milled at room temperature with dichloromethane (10 mL) and petroleum ether (200 mL) for 5-10 min, followed by filtration to obtain the active double-bond modified benzotriazole: N-(1H-benzotriazol-4-yl)acrylamide (3 g, 15.94 mmol, yield 26.73%) as a white solid.

[0041] The diagram is as follows Figure 2 As shown, its data is: 1 H NMR (400 MHz, DMSO-d6) δ = 15.6 (br s, 1H),10.69 (br s, 1H), 8.00 (s, 1H), 7.70 - 7.27 (m, 2H), 6.97 - 6.61 (m, 1H),6.36 - 6.31 (m, 1H), 5.94 - 5.73 (m, 1H) The 1H-NMR spectrum confirmed that it was N-(1H-benzotriazol-4-yl)acrylamide.

[0042] This embodiment provides a set of photosensitive resin compositions, which are prepared in comparison with control substances. The compositions include the following raw material components: alkali-soluble resin, photopolymerizable monomer, photoinitiator, adhesion promoter, additives, and solvent; the amounts of each component are shown in Table 1 below.

[0043] Table 1

[0044] Note: All weights in Table 1 are calculated based on solid weight and do not include solvent components.

[0045] As shown in Table 1, the embodiments in this specification use three parallel example samples and five comparative sample samples for control experiments. The samples in this embodiment (including example samples and comparative sample samples) are prepared by mixing alkali-soluble resin, photopolymerizable monomer, photoinitiator, adhesion promoter and additives.

[0046] In the examples of this specification, alkali-soluble resin a is an acrylate copolymer, polymerized by solution polymerization in a mass ratio of methacrylic acid / methyl methacrylate / styrene / butyl acrylate = 25 / 50 / 20 / 5; the solvent is butanone; the solid content is 45%, the weight average molecular weight is 60,000, the dispersity is 2.3, and the acid value is 163 mg KOH / g. (Provided by Jiangsu Sidike New Material Technology Co., Ltd.)

[0047] Photopolymerizable monomer b (available from Migen Special Chemicals Co., Ltd.): Composed of the following raw material components: 23g of 10(ethoxy)bisphenol A dimethacrylate, 8g of 4-(ethoxy)nonylphenol acrylate, 8g of 3(ethoxy)trimethylolpropane triacrylate, and 3g of ethylene oxide polypropylene glycol dimethacrylate.

[0048] Photoinitiator C (available from Shanghai McLean Biochemical Technology Co., Ltd.): 9-Phenylacetidine 0.6g.

[0049] Adhesion promoter: The compound represented by Formula IV (abbreviated as BPEM) was prepared by the method described in Example 1. In an alternative embodiment, the compound represented by Formula V produces similar effect data.

[0050] Additive e (available from Shanghai Maclean Biochemical Technology Co., Ltd.) consists of the following components: 1.0 g of leuco crystal violet, 0.03 g of malachite green, and 1 g of tribromomethylphenyl sulfone. In another alternative embodiment, the components in the additive may be adjusted as needed.

[0051] Solvent: Composed of the following components: 6g acetone, 10g toluene, and 6g methanol. Alternatively, the solvent in this embodiment may be 7g acetone, 10g toluene, and 5g methanol.

[0052] Example 2:

[0053] A comparative experiment was conducted on the three example samples and five comparative sample samples obtained in Example 1.

[0054] Preparation of photosensitive dry film: The photosensitive resin composition listed in Table 1 of Example 1 was used to prepare a photosensitive dry film, including the following steps: using experimental equipment (model: Elcometer 4340, UK), the photosensitive composition slurry prepared according to Table 1 was coated onto a 15μm thick polyethylene terephthalate (PET) support film; the solvent was removed by baking at 100°C for 5 minutes, and the thickness of the photosensitive layer was controlled at 38μm after baking. Then, a polyethylene film (PE) was covered for protection to obtain the photosensitive dry film.

[0055] Fabrication of resist-patterned substrates: Substrates with resist patterns were prepared using the photosensitive compositions of samples 1-3 and comparative samples 1-5 of the present invention shown in Table 1, as follows: (1) Photosensitive layer bonding process: A double-sided copper-clad laminate with a total thickness of 1.0 mm was used. After being pickled with 3% H2SO4, washed with water and dried, a bright copper surface with a surface roughness Ra of (0.1-0.3) μm and Rz of (1.0-1.5) μm was obtained. After being heated to 80°C, while peeling off the PE protective film of the photosensitive dry film obtained from each example or comparative example, the above photosensitive resin composition was laminated onto the copper-clad laminate using a hot roller laminator (CSL-M25E type manufactured by Zhisheng Technology Co., Ltd.) at a roller temperature of 110°C, an air pressure of 0.4 MPa and a lamination speed of 2.0 m / min to obtain a test substrate.

[0056] (2) Exposure process: A laser direct imaging device (Fine 10 model provided by Orbotech, using dual-wavelength mode, 50% 405nm, 50% 375nm) is used to irradiate a portion of the above photosensitive layer with active light of a specific wavelength, so that the above area is photocured to form a cured area. The sensitivity is tested using a Stouffer 41-level exposure scale, and the number of exposure grids is controlled between 17 and 23.

[0057] (3) Development process: The portion of the photosensitive layer, excluding the cured area, is removed from the substrate, forming a resist pattern on the substrate. After exposure, the PET support film is peeled off, and a dry film developing machine (manufactured by Dongguan Universe Circuit Board Equipment Co., Ltd.) equipped with a 1wt% Na2CO3 alkaline aqueous solution is used to spray and dissolve the unexposed portion of the photosensitive resin layer at a development point speed of 50%. After development, the substrate is rinsed with tap water for 1.5 times the development time, dehydrated using an air knife, and then dried with hot air to obtain a substrate with the cured photosensitive layer.

[0058] Evaluation Project 1. Sensitivity Evaluation On the above-mentioned film-coated test substrate, a Stouffer 41-level exposure scale was placed for photosensitivity testing. After the exposure process, the test substrate was left to stand for more than 15 minutes, then the PET film layer was peeled off, and a 1.0 wt% sodium carbonate aqueous solution was sprayed at 30°C to remove the unexposed resist layer, with a development point of 50%. After the above operation, a cured film obtained by curing the photosensitive resin composition was formed on the substrate surface. The exposure energy (mJ / cm2) when the number of residual segments on the exposure scale obtained through the cured film was 20 segments was used to evaluate the photosensitivity of the photosensitive resin composition; the lower the value, the better the photosensitivity.

[0059] 2. Adhesion Evaluation On the aforementioned test substrate after coating, photomask data with a wiring pattern of n:400 (unit: μm) was used to expose the substrate at an energy level that ensured a residual stage number of 20 after development using a Stouffer 41 exposure scale. After the development process, the resist pattern was observed using an optical microscope. The minimum linewidth at which a complete cured resist line was formed was used as the adhesion value to evaluate adhesion (μm). The smaller this value, the better the adhesion.

[0060] 3. Resolution Evaluation On the aforementioned test substrate after coating, photomask data with a wiring pattern of linewidth / spacing width of n:n (unit: μm) was used to expose the substrate at an energy level that ensures a residual stage number of 20 after development using a Stouffer 41 exposure ruler. After the development process, the resist pattern was observed using an optical microscope. The minimum line spacing that formed the complete cured resist lines was used as the adhesion value to evaluate the resolution (μm). The smaller this value, the better the resolution.

[0061] 4. Evaluation of residues after development The aforementioned test substrates with photosensitive layers were developed directly without prior exposure. After development, a fluorescence microscope was used to observe whether any residual substances emitted blue light upon ultraviolet irradiation.

[0062] ◎: Completely black, no blue light; ○: There are a few blue glowing spots; ×: There is a large area of ​​blue light.

[0063] 5. Evaluation of electroplating resistance On the above-mentioned test substrate after film application, exposure was performed using photomask data with a wiring pattern of 3 / 3 linewidth / line spacing (unit: mil) to achieve an energy level of 20 for the residual level after development by a Stoutffer 41 exposure ruler. After the development process, copper plating pretreatment was performed in the following sequence: immersion in degreasing solution (Baikal M404, 4%) for 5 min (38°C) → water rinsing for 1 min → micro-etching (5% sodium persulfate solution) for 1 min → acid pickling with dilute sulfuric acid (10%) for 1 min. The substrate was then immersed in copper sulfate electroplating solution (copper sulfate 75 g / L, sulfuric acid 210 g / L, chloride ion 50 ppm, bath starter CU603BK 10 ml / L, brightener CU603B 5 ml / L) and copper plating was performed for 30 minutes at room temperature and 3.0 A / dm2. Afterwards, a pre-tin plating treatment was performed in the following sequence: water rinse for 1 min → methanesulfonic acid (10%) pickling for 1 min. Then, the sample was immersed in a stannous methanesulfonate plating solution (stannous methanesulfonate 160 mL / L, B14WA14 wetting agent 70 mL / L, B14BR14 wetting agent 3 mL / L, B14RX14 wetting agent 3 mL / L, SB stabilizer) and tin-plated for 20 minutes at 22°C and 2.0 A / dm². Following this, a water rinse → film stripping (3.0% sodium hydroxide solution, 50°C) → water rinse → drying was performed. Additionally, after the cured photosensitive layer was peeled off, the presence of excess copper in the original photosensitive layer was observed from above using an optical microscope, and further confirmation of plating penetration was performed using a scanning electron microscope. Evaluation was conducted according to the following criteria: ◎: No plating seepage; ○: Slight plating penetration; ×: Severe plating penetration.

[0064] 6. Evaluation of electroplating layering Samples were taken from the electroplating resistance evaluation samples and analyzed using FIB-SEM to determine the electroplating cross-section. The evaluation was based on the size and number of voids at the copper plating interface, according to the following evaluation criteria: ◎: Longest dimension < 200nm; ○: The longest dimension is ≥200nm and <800nm, and the number within a 0.2mm length range is less than 5; ×: Longest dimension ≥ 800nm.

[0065] The test results for evaluation items 1-6 are summarized in Table 2 below: Table 2

[0066] The results in Table 2 show that the photosensitive resin compositions of Examples 1-3, with the adhesion promoter of this invention as the core, are comparable in exposure energy and resolution to those without BPEM (Comparative Example 3) and those with BTA (Comparative Examples 4, 5). However, Examples 1-3 have a significant advantage in adhesion and electroplating resistance on low-profile copper foil surfaces, with no residue after development and no obvious delamination of the plating layer. This provides an effective method to improve adhesion and electroplating resistance while also enhancing the reliability and dependability of PCB processing. Comparative Example 3, without BPEM, tends to have poor adhesion and electroplating resistance. Comparative Examples 4 and 5, with BTA added, are prone to development residue and electroplating delamination. Furthermore, experimental data from Comparative Example 1 show that as the amount of BPEM added is adjusted to 0.2g, electroplating resistance is insufficient, and severe plating penetration occurs. Experimental data from Comparative Example 2 show that as the amount of BPEM added is adjusted to 6g, a small amount of development residue and electroplating delamination begin to appear.

[0067] It is evident that the adhesion promoter of this invention, through the triazole group in the promoter, can form coordination bonds with copper, while simultaneously introducing flexible active double bonds that can participate in photoreactions onto the benzotriazole molecule. These active double bonds can polymerize with other active monomers in the photosensitive layer, forming a bidirectional connection between coordination bonds with the copper atoms of the substrate and covalent bonds within the internal molecular chains. This increases the number of coordination bonds between the photosensitive resin composition and the copper substrate, while simultaneously allowing the "anchoring molecules" to cross-link with other photocurable monomers in the composition, forming a link between the substrate interface and the photosensitive layer, resulting in a more stable and robust adhesion system and improving the overall adhesion of the photosensitive resin composition. Furthermore, it is precisely the strong interfacial bonding force of the promoter to the copper atoms of the substrate that makes it difficult for brighteners and wetting agents in the copper plating solution to penetrate between the cured photosensitive layer and the copper substrate, thus preventing electroplating penetration. Additionally, within a suitable addition range, no residue remains on the substrate after development, increasing the reliability of the PCB electroplating layer.

[0068] In this embodiment, the amount of adhesion promoter was changed by using 1 part by weight and 4 parts by weight. It was found that it has excellent performance in balancing adhesion and no residue after development, and no plating penetration occurred.

[0069] As can be seen, the photosensitive resin composition of the present invention can improve adhesion to low-profile copper foil and enhance electroplating resistance without causing prolonged peeling time. Furthermore, it can improve the production efficiency and yield of PCB / FPC. The preparation method of the present invention is simple, easy to implement, and produces stable finished products.

[0070] Those skilled in the art should understand that the discussion of any of the above embodiments is merely exemplary and is not intended to imply that the scope of this disclosure (including the claims) is limited to these examples; within the framework of this disclosure, the technical features of the above embodiments or different embodiments can also be combined, the steps can be implemented in any order, and there are many other variations of different aspects of the embodiments of this disclosure as described above, which are not provided in detail for the sake of brevity.

[0071] This disclosure is intended to cover all such substitutions, modifications, and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this disclosure should be included within the scope of protection of this disclosure.

Claims

1. A photosensitive resin composition, comprising, by weight, the following raw material components: 45-65 parts of alkali-soluble resin, 35-55 parts of photopolymerizable monomer, 0.1-6 parts of photoinitiator, 0.5-5 parts of adhesion promoter, and 0.1-5 parts of additives; The adhesion promoter is benzotriazole modified with active double bonds as shown in Formula I: Equation I; in, R1, R2, R3, and R4 are each independently selected from one of the substituent groups, hydrogen, C1-C12 alkyl groups, and C2-C12 unsaturated ester groups shown in Formula II and Formula III; Formula II; Formula III; R5 is selected from hydrogen or methyl.

2. The photosensitive resin composition according to claim 1, characterized in that, The adhesion promoter is selected from the compounds represented by Formula IV and / or Formula V: Formula IV; Formula V.

3. The photosensitive resin composition according to claim 1, characterized in that: The amount of the adhesion promoter is 1-4 parts by weight.

4. The photosensitive resin composition according to claim 1, characterized in that: The photopolymerizable monomer is a (meth)acrylate monomer.

5. The photosensitive resin composition according to claim 4, characterized in that: The photopolymerizable monomer is selected from one or a combination of several of the following: methoxy polyethylene glycol monoacrylate, ethoxy(propoxy)bisphenol A di(meth)acrylate, ethoxy(propoxy)di(meth)acrylate, polyethylene glycol diacrylate, polypropylene glycol diacrylate, ethoxy(propoxy)trimethylolpropane tri(meth)acrylate, di(trimethylolpropane)tetraacrylate, and polyurethane.

6. The photosensitive resin composition according to claim 1, characterized in that: The photoinitiator is an acridine compound and / or a hexaaryl diimidazole compound. By weight, when the photoinitiator is an acridine compound, the amount of photoinitiator is 0.1-2 parts, and when the photoinitiator is a hexaaryl diimidazole compound, the amount of photoinitiator is 3-6 parts.

7. The photosensitive resin composition according to claim 6, characterized in that: The photoinitiator is selected from one or a combination of two of the following: 9-phenyl-substituted acridine compounds, o-chlorohexaaryl diimidazole, and 2,2',4-tris(2-chlorophenyl)-5-(3,4-dimethoxyphenyl)-4'5'-diphenyl-1,1'-diimidazole.

8. The photosensitive resin composition according to claim 1, characterized in that: The alkali-soluble resin is an acrylate copolymer containing aromatic groups, which is copolymerized from methacrylic acid and copolymer units. The copolymerization ratio of comonomers with aromatic groups is 10%-50% based on the total mass of comonomers during the copolymerization process. Preferably, the copolymer units are selected from one or a combination of several of methyl methacrylate, ethyl methacrylate, butyl methacrylate, benzyl methacrylate, and styrene.

9. The photosensitive resin composition according to claim 1 or 2, characterized in that, The adhesion promoter is prepared by the following steps: Benzotriazole is mixed with concentrated sulfuric acid and then concentrated nitric acid is added to undergo a nitration reaction to obtain benzotriazole with a nitro group on the benzene ring; Benzotriazole with a nitro group on the benzene ring was dissolved in methanol and reduced to amino-substituted benzotriazole using Pd / C and hydrogen. An adhesion promoter is obtained by dissolving an amino-substituted benzotriazole in dichloromethane, adding triethylamine, and then adding acryloyl chloride dropwise.