Low-temperature curing high-resolution negative photosensitive components, cured films and applications
By using low-temperature curing of high-resolution negative photosensitive components and utilizing free radical gelation and oxobutane cation ring-opening reaction, the problem of insufficient crosslinking density under low-temperature conditions in existing technologies is solved, achieving the formation of high-resolution micro-patterns and high hardness, which is suitable for the manufacture of color filters for AR/VR/XR silicon-based displays.
Patent Information
- Application Number
- CN202611504040.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-24
- Publication Date
- 2026-11-17
AI Technical Summary
Existing color photoresist technology has difficulty in forming high-resolution micro-patterns under low-temperature conditions, and suffers from problems such as insufficient cross-linking density, easy swelling and collapse during development, and poor storage stability, which cannot meet the manufacturing requirements of AR/VR/XR silicon-based displays.
By employing low-temperature curing high-resolution negative photosensitive compositions, a polyether interpenetrating network is formed through rapid free radical gelation, chemical amplification reaction initiated by photoacid-producing agents, and ring-opening reaction of oxobutane cations, achieving the formation of micro-patterns with high crosslinking density and high hardness.
Under post-baking conditions of 80-90℃, high-resolution image resolution below 5μm is achieved. It does not swell or collapse during development, exhibits high hardness and good reliability, and is suitable for the manufacture of color filters for silicon-based OLED, Micro-LED, and AR/VR/XR micro-display panels.
Smart Images

Figure SMS_1 
Figure SMS_3 
Figure SMS_4
Abstract
Description
Technical Field
[0001] This invention relates to the fields of optoelectronic display materials, semiconductor lithography and color filter manufacturing technology, and specifically proposes a low-temperature curing high-resolution negative photosensitive composition, curing film and its application. Background Technology
[0002] AR / VR / XR silicon-based displays typically have pixel densities exceeding 3000 PPI, with color filter subpixel sizes ranging from 2 to 5 μm. Unlike traditional LCD color filters, the color filters in silicon-based OLED displays are often located above or near the heat-sensitive organic light-emitting layer, severely limiting the thermal budget for back-end processes. Traditional color photoresists usually rely on baking at temperatures above 200°C to achieve full cross-linking, a process unsuitable for OLED organic light-emitting layers.
[0003] Existing color photoresist technology presents a significant contradiction when operating at low temperatures: if the post-baking temperature is lowered, the cross-linking density of the free radical acrylate system is insufficient, making it prone to swelling, peeling, or dissolution during development and subsequent solvent treatment; if the amount of monomer or thermal cross-linking agent is increased, it will lead to decreased storage stability, increased dark reactions, and distortion of pattern boundaries.
[0004] The main technical shortcomings at present are: ① Pure free radical acrylate system: It can form a preliminary pattern during exposure, but the crosslinking density is insufficient after baking at 90°C. It has poor resistance to NMP, PGMEA and alkaline solutions, and patterns below 5 μm are prone to collapse. ② Traditional melamine thermal crosslinking system: usually requires a high temperature for a full reaction, and insufficient curing during baking at low temperature, and increasing the amount can easily cause dark reaction and deterioration of storage stability; ③ Single chemical amplification system: It can improve the development difference between exposed and unexposed areas, but at 80–90°C, deprotection and crosslinking may not be complete, and acid diffusion can cause CD shift or edge blurring; ④ Single cationic epoxy or oxobutane system: It has the potential for low-temperature dark curing, but lacks the ability to lock shape during exposure. It may swell during the development process, making it difficult to achieve both ≤5 μm resolution and water-based TMAH development window.
[0005] Therefore, it is necessary to propose a low-temperature curable high-resolution negative photosensitive composition that can withstand a thermal budget of 80-90℃ while simultaneously achieving ≤5 μm micropattern resolution, no swelling or collapse during development, resistance to downstream solvents, high hardness, long-term reliability, and acceptable storage stability. Summary of the Invention
[0006] This invention proposes a low-temperature curable high-resolution negative photosensitive composition for use in color filters or black matrices, in order to at least address one of the many shortcomings of the prior art.
[0007] The technical solution of this invention is implemented as follows: The first aspect of the present invention is to provide a low-temperature curable high-resolution negative photosensitive composition, comprising, by weight percentage: 10-35 wt% acrylate copolymer resin, 5-15 wt% multifunctional acrylate monomer, 1-5 wt% free radical photoinitiator, 1-5 wt% photoacid generator, 8-30 wt% acid-instable resin, 5-18 wt% acid-instable crosslinking agent, 20-45 wt% colorant, 3-8 wt% oxetane monomer, and the balance being solvent and additives; wherein the acid-instable crosslinking agent is used for crosslinking under acid-catalyzed conditions at 80-90°C.
[0008] Furthermore, the acid value of the acrylate copolymer resin is 60-180 mgKOH / g; And / or, the weight-average molecular weight of the acrylate copolymer resin is 8000-40000; And / or, the multifunctional acrylate monomer is selected from at least one of pentaerythritol hexaacrylate and pentaerythritol triacrylate.
[0009] Furthermore, the free radical photoinitiator is selected from at least one of the following: compounds having a triazole skeleton, compounds having a diazole skeleton, compounds having an imidazole skeleton, phosphine compounds, hexaarylbisimidazole, oxime compounds, organic peroxides, sulfur compounds, ketone compounds, aromatic onium salts, α-hydroxy ketone compounds, and α-amino ketone compounds. And / or, the photo-induced acid-producing agent is selected from at least one of thionium salts, iodonium salts, sulfonyldiazomethane, N-sulfonyloxyimide and oxime-O-sulfonate acid-producing agents; And / or, the acid-unstable crosslinking agent is selected from at least one of diphenols, triphenols, benzyl ethers, polyacetals, glycoureas, or melamine derivative crosslinking agents.
[0010] Furthermore, the acid-instable resin is a resin containing an acid-instable functional group, wherein the acid-instable functional group is selected from at least one of tert-butoxycarbonyl, acetal, ketal or tert-ester. And / or, the oxetane monomer is selected from at least one of monofunctional, difunctional or polyfunctional oxetanes, or oxetane-containing side-chain resins.
[0011] Furthermore, the colorant is selected from at least one of organic colored pigments or dyes and carbon black dispersions; And / or, the solvent is selected from at least one of propylene glycol methyl ether acetate and cyclohexanone; And / or, the additive is selected from at least one of dispersants, leveling agents, adhesion promoters, crosslinking agents, and acid diffusion inhibitors.
[0012] A second aspect of the present invention is to provide a cured film, which is prepared by the following steps: S1. Coat the substrate with the low-temperature curing high-resolution negative photosensitive composition described in the first aspect to obtain a wet film; S2. Soft baking removes the solvent from the wet film to obtain a dry film; S3. Expose the dry film under a photomask; S4. Crosslink the exposed film at 60-70℃ for 30-180s; S5. Develop with alkaline solution to wash away unexposed areas; S6. Bake at 80-90℃ for 15-30 minutes to obtain the cured film.
[0013] Furthermore, the solid content of the photosensitive component is 18-25 wt%; And / or, the dry film thickness is 1.5-2.0 μm; And / or, the alkaline solution is selected from at least one of inorganic bases, organic amines, quaternary ammonium compounds, alkanolamines, and cyclic amines; And / or, in step S6, before post-baking, place the exposed area under a deep ultraviolet light source for re-exposure at 500-2000 millijoules per square centimeter.
[0014] A third aspect of the present invention is to provide an RGB color layer comprising the cured film described in the second aspect.
[0015] A fourth aspect of the invention is to provide a black matrix comprising the cured film described in the second aspect.
[0016] A fifth aspect of the invention is to provide the application of the RGB color layer described in the third aspect and / or the black matrix described in the fourth aspect in silicon-based OLED, silicon-based Micro-LED, and AR / VR / XR micro-display panels.
[0017] Compared with the prior art, the beneficial effects of the present invention are as follows: The low-temperature curing, high-resolution negative photosensitive composition proposed in this invention, through its specific composition, enables rapid free radical gelation to lock micro-patterns, followed by chemical amplification of the exposure area at low temperatures via a photoacid-inducing agent, and finally, dark curing via oxobutane cationic ring-opening to form a polyether interpenetrating network. This allows for simultaneous achievement of pattern resolution below 5 μm, NMP residual film rate exceeding 90%, high hardness, and good reliability under post-baking conditions at 80-90°C. This composition is particularly suitable for manufacturing RGB color layers and black matrices for silicon-based OLEDs, silicon-based Micro-LEDs, and AR / VR / XR silicon-based displays with a PPI greater than 3000. Detailed Implementation
[0018] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0019] This invention proposes a low-temperature curable, high-resolution negative photosensitive composition, comprising, by weight percentage: 10-35 wt% acrylate copolymer resin A, 5-15 wt% multifunctional acrylate monomer B, 1-5 wt% free radical photoinitiator C, 1-5 wt% photoacid-generating agent D, 8-30 wt% acid-unstable resin E, 5-18 wt% acid-unstable crosslinking agent F, 20-45 wt% colorant G, 3-8 wt% oxetane monomer H, and the balance being solvent and additives; wherein the acid-unstable crosslinking agent is used for crosslinking under acid-catalyzed conditions at 80-90℃.
[0020] The above components form the following time-coupled reactions during exposure, PEB, development, and post-baking: The first stage is instantaneous free radical lock-in during exposure: the free radical initiator absorbs ultraviolet light to generate free radicals; the multifunctional acrylate rapidly polymerizes and gels. An initial three-dimensional framework is established before the acid-catalyzed reaction fully occurs to limit developer penetration and acid diffusion, preventing the collapse of patterns below 5μm. The second stage is PEB low-temperature chemical amplification densification: the photo-induced acid generator produces acid in the exposure area, which promotes the deprotection of the acid-instable resin and causes the acid-instable crosslinking agent to react with hydroxyl / carboxyl groups. The third stage is post-baking / dark reaction cationic reinforcement: the photo-induced acid-generating agent continues to initiate the ring-opening polymerization of oxobutane, forming polyether segments or polyether crosslinking networks. Interpenetrating or semi-interpenetrating networks are formed within the existing acrylic / CA network, compensating for insufficient low-temperature CA reaction and improving NMP residual film yield, hardness, and aging color difference stability.
[0021] Since the three stages use the same exposure pattern as the basis for spatial selection and use the same photo-induced acid-generating acid source to simultaneously drive chemical amplification and cationic ring-opening reactions, the present invention forms a reaction cascade confined by the exposure region, rather than a simple mixture of three curing systems.
[0022] By using the low-temperature curing high-resolution negative photosensitive composition of the present invention, it can still form a sufficiently high crosslinking density and pattern mechanical strength under post-baking conditions of 80-90°C, and can obtain high-resolution patterns below 5μm by alkaline developer. It is suitable for manufacturing color filter RGB pixels and black matrix used in silicon-based OLED, silicon-based Micro-LED, AR / VR / XR micro-display panels.
[0023] In this invention, the acrylate copolymer resin contains carboxyl groups to provide alkali-developable properties and hydroxyl groups to provide crosslinking sites. Its acid value is preferably 60-180 mgKOH / g, and its Mw is preferably 8,000-40,000.
[0024] In a preferred embodiment, the acrylate resin is a multi-component copolymer formed by free radical polymerization of unsaturated monomers. The molecular chain structure of this copolymer is designed to achieve an optimal balance of heat resistance, developability, adhesion, and optical properties within a single polymer. Its monomer composition is characterized by containing the following components (A) and (B), and the selection of component (B) must meet specific quantity requirements: Component (A): A carboxyl-containing unsaturated monomer refers to a monomer whose molecular structure simultaneously possesses at least one polymerizable unsaturated double bond and at least one terminal carboxylic acid group (-COOH). In one embodiment of the present invention, component (A) is methacrylic acid (MAA). The presence of component (A) endows the copolymer resin with solubility in alkaline developing solution and serves as a reaction anchor for subsequent side chain modification; Component (B): Other copolymerizable functional monomers refer to monomers other than Component (A) mentioned above that can undergo random or block copolymerization with Component (A). To precisely control the overall physical properties of the resin, Component (B) is selected from at least one or more of the following different monomers in combination: 1) Rigid alicyclic monomers: used to increase glass transition temperature (Tg) and reduce hygroscopicity. Selected from cyclohexyl methacrylate (CHMA), dicyclopentane methacrylate (DCPMA), and isobornyl methacrylate (IBOMA); 2) Heat-resistant modifying monomers: used to impart resistance to high-temperature processes to resins. Selected from N-cyclohexylmaleimide (CHMI) and N-phenylmaleimide (PMI); 3) Polar / Reactive Monomers: Used to improve substrate adhesion or provide ring-opening reaction sites. Selected from hydroxyethyl methacrylate (HEMA), hydroxypropyl methacrylate (HPMA), and glycidyl methacrylate (GMA); 4) Optical / General-Purpose Adjustment Monomers: Used to improve refractive index, leveling properties, or control costs. Selected from benzyl methacrylate (BnMA), methyl methacrylate (MMA), 4-acryloylmorpholine (ACMO), and p-isopropenylphenol.
[0025] In embodiments of the present invention, the acrylate resin polymer Resin-A has a weight-average molecular weight of 12,000 and an acid value of 110. It is a copolymer synthesized using four monomers: methacrylic acid (MAA), isobornyl methacrylate (IBOMA), benzyl methacrylate (BnMA), and hydroxyethyl methacrylate (HEMA) in a molar ratio of 2:3:4:1.
[0026] The acrylate grinding and dispersing resin was prepared by the following method: the monomer molar ratio was designed as methacrylic acid (MAA): isobornyl methacrylate (IBOMA): benzyl methacrylate (BnMA): hydroxyethyl methacrylate (HEMA) = 2:3:4:1. The synthesis steps of this quaternary methyl acrylate copolymer resin are as follows: Prepare a four-necked flask (2 liters) equipped with a stir bar, condenser, thermometer, and nitrogen inlet. Add 350g of PGMEA to the flask. Start stirring and purge with nitrogen (degassing) for at least 30 minutes to remove oxygen from the solvent. Heat to 85°C. In a separate beaker, mix 47.6g of MAA, 143.9g of IBOMA, 195.4g of BnMA, and 27.9g of HEMA. Add the remaining 235.2 g of PGMEA, along with 8.3 g of azobisisobutyronitrile (AIBN) and 2.1 g of chain transfer agent n-Dodecyl Mercaptan, to the above monomer mixture. Stir until the initiator is completely dissolved. When the temperature inside the reactor stabilizes at 85°C, begin adding the second-stage prepared mixture using a metering pump. The adding time is set to 3 hours. During the adding process, maintain the reactor temperature at 85±2°C. After the adding is complete, maintain the temperature at 85°C and continue stirring for 2 hours (this is the maturation period). Raise the temperature to 95°C and maintain it for 1 hour to completely decompose any remaining trace amounts of initiator. Stop heating and allow it to cool naturally to below 40°C. Take samples to test the solid content and acid value (target acid value approximately 75-80 mgKOH / g, molecular weight 8000±500, viscosity 6.0±0.5 cP).
[0027] In this invention, the multifunctional acrylate monomer compound belongs to the category of free radical polymerizable compounds. For example, compounds containing vinyl unsaturated groups. Groups containing vinyl unsaturated groups, such as vinyl, (meth)allyl, (meth)acryloyl, etc. The polymerizable monomer compound can be in any chemical form, such as monomers, prepolymers, and oligomers. The molecular weight of the polymerizable monomer compound is typically from 100 to 3000. The polymerizable monomer compound is a compound containing 3 to 15 vinyl unsaturated groups. Specific examples include paragraphs 0095 to 0108 of Japanese Patent Application Publication No. 2009-288705, paragraph 0227 of Japanese Patent Application Publication No. 2013-029760, paragraphs 0254 to 0257 of Japanese Patent Application Publication No. 2008-292970, paragraphs 0034 to 0038 of Japanese Patent Application Publication No. 2013-253224, paragraph 0477 of Japanese Patent Application Publication No. 2012-208494, Japanese Patent Application Publication No. 2017-048367, Japanese Patent No. 6057891, Japanese Patent No. 6031807, and the compounds described in JP 2017-194662 A. The aforementioned patent documents describe the following commercially available products: dipentanetriol triacrylate (commercially available product KAYARAD D-330, manufactured by KAYAKU Corporation, Japan) and dipentanetriol tetraacrylate (commercially available product KAYARAD D-320, manufactured by KAYAKU Corporation, Japan), pentaerythritol penta(meth)acrylate dipentane (commercially available product KAYARAD D-310, manufactured by KAYAKU Corporation, Japan), dineopentaerythritol alcohol hexa(meth)acrylate (commercially available product KAYARADDPHA, manufactured by KAYAKU Corporation, Japan, NK ester A-DPH-12E, manufactured by SHIN-NAKAMURA CHEMICAL Corporation), and these (compounds having a structure in which a methacryloyl group is linked through ethylene glycol and / or propylene glycol residues) (e.g., SR454 and SR499, commercially available from SARTOMER Company, Inc.) are preferred.In addition, as polymerizable compounds, diglyceride EO (ethylene oxide) modified (meth) acrylate (M-460 is a commercially available product manufactured by TOAGOSEI CO., LTD.), neopentyl glycerol can also be used in tetraacrylate (manufactured by SHIN-NAKAMURA CHEMICAL CO., LTD., NK ester a-TMMT), 1,6-hexanediol diacrylate (manufactured by Kayaku Corporation, KAYARAD HDDA, Japan), RP-1040 (Kayaku Corporation, Japan), ARONIX TO-2349 (TOAGOSEI Corporation), NK Oligo UA-7200 (SHIN-NAKAMURA CHEMICAL Co., Ltd.), 8UH-1006, 8UH-1012 (Taisei Fine Chemicals Co., Ltd.), light acrylate POB-A0 (Kyoisha CHEMICAL Co., Ltd.), etc.
[0028] In addition, trifunctional (meth)acrylate compounds, such as trimethylolpropane tri(meth)acrylate, trimethylolpropane propoxy-modified tri(meth)acrylate, trimethylolpropane ethoxylate-modified trifunctional (meth)acrylate compounds, such as tri(meth)acrylate, isocyanuric acid ethoxy-modified tri(meth)acrylate, neopentylglycerol tri(meth)acrylate, etc. Commercial products of trifunctional (meth)acrylate compounds include ARONIX M-309, M-310, M-321, M-350, M-360, M-313, M-315, M-306, M-305, M-303, M-452, M-450 (manufactured by TOAGOSEI Co., Ltd.), NK ester A9300, A-GLY-9E, A-GLY-20E, A-TMM-3, A-TMM-3L, A-TMM-3LM-N, A-TMPT, TMPT, TMPT (manufactured by SHIN-NAKAMURA Chemical Co., Ltd.), KAYARAD-GPO-303, TMPTA, THE-330, TPA-330, PET-30 (Kayaku Co., Ltd., Japan), etc.
[0029] Polymerizable monomer compounds can also contain acid groups, which effectively remove polymerizable monomer compounds from unexposed portions during development, thus inhibiting the formation of development residues. These acid groups can be carboxyl, sulfonic, phosphate, etc. Examples of commercially available polymerizable monomer compounds containing acid groups include ARONIX M-305, M-510, M-520, and ARONIX TO-2349 (manufactured by TOAGOSEI Ltd.). The acid values of these polymerizable monomer compounds are typically from 0.1 to 40 mg KOH / g.
[0030] Polymerizable monomeric compounds can also be compounds having a caprolactone structure. Examples include the KAYARAD DPCA series, such as DPCA-20, DPCA-30, DPCA-60, and DPCA-120, which are available from NIPPONKAYAKU CO., Ltd.
[0031] Polymerizable monomer compounds can also be compounds having 4 to 20 vinyl alkoxy groups. Examples include polymerizable monomer compounds with vinyl oxides and / or vinyl oxides. Commercially available examples of such compounds include SR-494 manufactured by Sartomer Company, tetrafunctional (meth)acrylic acid with 3 isobutyl and 4 ethoxy groups, and KAYARADTPA-330, etc.
[0032] Polymerizable monomer compounds can also be compounds with a fusiform skeleton. Commercially available products include OGSOL EA-0200 and EA-0300 (manufactured by Osaka Gas Chemicals Co., Ltd.).
[0033] In this invention, the free radical photoinitiator is a compound that is photosensitive to light from the ultraviolet to the visible region, and common photoradical polymerization initiators are selected. Examples include, but are not limited to, haloalkanes derivatives (e.g., compounds with a triazole skeleton, compounds with a diazole skeleton, compounds with an imidazole skeleton, etc.), phosphine compounds and hexaarylbisimidazoles, carbazole oxime esters, organic peroxides, sulfur compounds, ketone compounds, aromatic onium salts, α-hydroxy ketone compounds, α-amino ketone compounds, etc. Examples may include BASF Irgacure OXE01, OXE02 and ADEKA Co., Ltd. N-1919.
[0034] In this invention, the photoacid-generating agent is applied to a negative photosensitive composition. After a photoacid-promoted crosslinking reaction, the exposed portion of the resist coating exhibits lower solubility in the developer compared to the unexposed portion. Ester groups having tertiary noncycloalkyl or tertiary alicyclic carbons covalently bonded to the carbonyl oxygen of the ester, as well as acetal groups, are generally preferred photoacid-instantaneous groups of the resin used in the photoresist of this invention. These can be selected from Irgacure PAG103, Irgacure PAG121, Irgacure PAG169, Irgacure PAG250, and Irgacure PAG103, Irgacure PAG121, Irgacure PAG169, Irgacure PAG250, and Irgacure PAG169. PAG290, Diphenyliodonium hexafluorophosphate, Tri-p-Tolylsulfonium hexafluorophosphate, Di(3-methylphenyl)hexafluorophosphate, Bis(4-tert-butylphenyl)iodonium hexafluorophosphate, 4,4'-Dimethyliodonium hexafluorophosphate, Di(4-tert-butylphenyl)hexafluorophosphate, (2-naphthyl)(2,4,6-trimethylphenyl)hexafluorophosphate, (4-biphenyl)(2,4,6-trimethylphenyl)hexafluorophosphate 1, bis(3-methylphenyl)hexafluorophosphate iodine, bis(2-methylphenyl)hexafluorophosphate iodine, 4-octyloxydiphenyliodohexafluoroantimonate, diphenyliodonitrate, diphenyl(trifluoromethyl)sulfonium trifluoromethanesulfonate, tri-p-tolylsulfonium trifluoromethanesulfonate, (4-methoxyphenyl)diphenylsulfonium trifluoromethanesulfonate, 1-naphthyldiphenylsulfonium trifluoromethanesulfonate, tris(4-tert-butylphenyl)sulfonium trifluoromethanesulfonate, (4-phenoxyphenyl) Diphenylsulfonium trifluoromethanesulfonate, (4-phenylthiophenyl)diphenylsulfonium trifluoromethanesulfonate, bis[4-(1,1-dimethylethyl)phenyl]iodonium trifluoromethanesulfonate, (2-tolyl)(2,4,6-trimethylphenyl)iodonium trifluoromethanesulfonate, phenyl(2,4,6-trimethoxyphenyl)iodonium p-toluenesulfonate, bis(4-tert-butylphenyl)iodonium p-toluenesulfonate, diphenyliodonium p-toluenesulfonate, N-hydroxy The mixture contains at least one of the following: naphthaleneimide trifluoromethanesulfonic acid, 2,4-bis(trichloromethyl)-6-p-methoxystyryl-S-triazine, N-hydroxy-5-norbornene-2,3-diamide nonafluorobutanesulfonic acid, perfluorobutylsulfonic acid triphenylsulfonium salt, bis(4-tert-butylphenyl)iodonium perfluoro-1-butanesulfonic acid, diphenyliodoacyl chloride, and a weak acid salt composed of iodonium salt, sulfonium salt, phosphonium salt, ammonium salt, and diazonium salt; wherein Irgacure PAG 103, Irgacure PAG 121, Irgacure PAG 169, Irgacure PAG250, and Irgacure PAG290 are purchased from BASF AG and are trade names.
[0035] In this invention, the acid-unstable resin comprises repeating units (a) and optionally repeating units (b), (c), (d), and / or (e). The acid-unstable resin can be synthesized by any desired method, for example, by dissolving one or more monomers selected from those corresponding to the repeating units above in an organic solvent, adding a free radical polymerization initiator thereto, and then heating for polymerization. Examples of organic solvents suitable for polymerization include toluene, benzene, tetrahydrofuran, diethyl ether, and dioxane. Examples of polymerization initiators used herein include 2,2'-azobisisobutyronitrile (AIBN), 2,2'-azobis(2,4-dimethylpentanonitrile), dimethyl 2,2-azobis(2-methylpropionate), benzoyl peroxide, and lauroyl peroxide. Preferably, the system is heated at 50-80°C to induce polymerization. The reaction time is preferably 2-100 hours, more preferably 5-20 hours. When copolymerizing monomers containing hydroxyl groups, the hydroxyl groups can be replaced with acetal groups, typically ethoxyethoxy, which are easily deprotected by acid, before polymerization, and the protection can be removed by a weak acid and water after polymerization. Alternatively, the hydroxyl groups can be replaced with acetyl, formyl, neopentyl, or similar groups before polymerization, and alkaline hydrolysis can be performed after polymerization. Another method can be used when copolymerizing hydroxystyrene or hydroxyvinylnaphthalene. Specifically, acetoxystyrene or acetoxyvinylnaphthalene is used instead of hydroxystyrene or hydroxyvinylnaphthalene, and the acetoxy group is deprotected by alkaline hydrolysis after polymerization, thereby converting the polymer product into hydroxystyrene or hydroxyvinylnaphthalene. For alkaline hydrolysis, alkalis such as ammonia or triethylamine can be used. Preferably, the reaction temperature is -20°C to 100°C, more preferably 0°C to 60°C, and the reaction time is 0.2-100 hours, more preferably 0.5-20 hours. The acid-unstable resin preferably has a weight-average molecular weight (Mw) in the range of 1,000-500,000, more preferably 2,000-30,000, which is determined by GPC using tetrahydrofuran (THF) solvent relative to a polystyrene standard.
[0036] The repeating unit (a) has the following structure:
[0037] Where R A Each can be either hydrogen or methyl. R 21 and R 22 Each is an acid-labile group. Y 1 It is a single bond, a phenylene or naphthylene group, or a C1-C12 linker containing at least one part selected from ester bonds and lactone rings. 2 It consists of a single bond or an ester bond.
[0038] Typical acid-unstable groups may be selected from those groups described in JP-A2013-080033 (USP 8,574,817) and JP-A 2013-083821 (USP 8,846,303), including but not limited to at least one of t-BOC, acetal, ketal or tertiary ester protecting groups.
[0039] Repeating unit (b) may be selected from phenolic hydroxyl groups.
[0040] The repeating unit (c) is selected from hydroxyl (other than the phenolic hydroxyl group mentioned above), lactone ring, ether bond, ester bond, carbonyl group, cyano group and carboxyl group.
[0041] The repeating unit (d) comprises a compound selected from indene, benzofuran, benzothiophene, acenaphthene, chromone, coumarin and norbornene, or derivatives thereof.
[0042] The repeating unit (e) is derived from styrene, vinylnaphthalene, vinylanthracene, vinylpyrene, methylene indene, vinylpyridine, and vinylcarbazole.
[0043] In a preferred embodiment, the acid-unstable resin is selected from at least one of polymer 1 and polymer 2: .
[0044] In this invention, the acid-instantaneous crosslinking agent is a crosslinking agent that uses acid as a catalyst to form crosslinks between polymeric compounds and makes the polymeric compounds insoluble in the aforementioned developing solution. It includes, but is not limited to, at least one of diphenols, triphenols, benzyl ethers, polyacetals, glycoureas, or melamine derivative crosslinking agents. Among these compounds, 2-nucleophenols such as 4,4'-diphenylmethylene bisphenol, 4,4'-diphenylethylidene bisphenol, and bisphenol A are preferred; 3-nucleophenols such as 4,4',4"-methylenetriphenol and 4,4'-[1-[4-[1-(4-hydroxyphenyl)-1-methylethyl]phenyl]ethylidene]bisphenol are also preferred.
[0045] In this invention, the colorant is an organic molecular colored pigment or dye, or a carbon black dispersion; for pigments, see Japanese Patent Application Publication No. 2013-077009, Japanese Patent Application Publication No. 2014-130338, and International Publication No. 2015 / 166779, etc. The colorant can be at least one of the following: diammonium compounds, squaric acid monium salt compounds, anthocyanin compounds, phthalocyanine compounds, naphthyl phthalocyanine compounds, tetrachlorobenzene compounds, ammonium compounds, ammonium compounds, azo compounds, anthraquinone compounds, porphyrin compounds, pyrrolopyrrole compounds, oxacyanine compounds, ketone compounds, hexaporin compounds, metal dithiols, copper compounds, tungsten compounds, and metal borides. Colored dyes include pyrazole azo compounds, aniline azo compounds, triarylmethyl alkyl compounds, anthraquinone compounds, anthraquinone compounds, benzyl compounds, oxacyanine compounds, pyrazolotriazole azo compounds, pyridone azo compounds, anthocyanin compounds, phenanthrene compounds, pyrrolopyrazole azomethine compounds, phthalocyanine compounds, benzopiperanone compounds, indigo compounds, and pyrrole methylene compounds.
[0046] In this invention, if only monofunctional 3-ethyl-3-hydroxymethyloxetane (commonly known as OXT-101, CAS 3047-32-3) is used as the oxetane monomer, its main function is to dilute the reaction and adjust flexibility. To more effectively support the interpenetrating network and increase the crosslinking density, this invention preferably uses compounds containing two or more oxetane groups, or uses monofunctional oxetanes in combination with difunctional / polyfunctional oxetanes (such as 3,3'-(oxybis(methylene)bis(3-ethyl)oxetane, also known as OXT-221, CAS 18934-00-4), preferably a combination of OXT-101 and OXT-221 in a 1:1 molar ratio.
[0047] In this invention, the additives include at least one of dispersants, leveling agents, adhesion promoters, crosslinking agents, and acid diffusion inhibitors. The surfactants include fluorinated surfactants, nonionic surfactants, cationic surfactants, anionic surfactants, polysiloxane surfactants, etc., or are described in paragraphs 0238-0245 of International Publication No. 2015 / 166779 and paragraphs 0166-0167 of International Publication No. 2016 / 158818. The leveling agent can be selected from BYK-UV3510 and BYK-307, purchased from BYK Chemical Company, and are trade names.
[0048] In this invention, the organic solvent may be a compound listed in Japanese Patent Application Publication No. 2011-232632 or at least one compound from the group consisting of the following compounds.
[0049] In this invention, the acid diffusion inhibitor is generally an amine or a weak acid onium salt. For example, compounds listed in Japanese Patent Application Publication No. 2011-232632, or triethylamine, triisobutylamine, triisooctylamine, trioctylamine, diethanolamine, triethanolamine, benzylamine, allylamine, ethanolamine, tributylamine, tetrabutylammonium hydroxide, tetramethylammonium hydroxide, trimethylsulfonium hydroxide, triphenylsulfonium hydroxide, dimethyldodecylamine, aniline, p-toluidine, etc.
[0050] Suitable crosslinking agents include epoxy compounds, melamine compounds, guanidine compounds, glyceryl compounds and urea compounds, isocyanate compounds, azide compounds, and compounds having double bonds such as alkenyl ether groups, which are substituted therewith at least one group selected from hydroxymethyl, alkoxymethyl, and acyloxymethyl groups. Examples of epoxy compounds include tris(2,3-epoxypropyl)isocyanurate, trimethylolpropane triglycidyl ether, trimethylolpropane triglycidyl ether, and trimethylolethyl ethane triglycidyl ether. Examples of melamine compounds include hexamethylol melamine, hexamethoxymethyl melamine, hexamethylol melamine compounds with 1-6 hydroxymethyl groups methoxymethylated, and mixtures thereof, hexamethoxyethyl melamine, hexaacyloxymethyl melamine, hexamethylol melamine compounds with 1-6 hydroxymethyl groups acyloxymethylated, and mixtures thereof. Examples of guanidine compounds include tetrahydroxymethylguanidine, tetramethoxymethylguanidine, tetrahydroxymethylguanidine compounds with 1-4 hydroxymethyl groups methoxymethylated, and mixtures thereof, tetramethoxyethylguanidine, tetraacyloxyguanidine, tetrahydroxymethylguanidine compounds with 1-4 hydroxymethyl groups acyloxymethylated, and mixtures thereof. Examples of urea compounds include tetrahydroxymethylurea, tetramethoxymethylurea, tetramethoxymethylurea, tetrahydroxymethylurea compounds with 1-4 hydroxymethyl groups methoxymethylated, and mixtures thereof, and tetrahydroxymethylurea compounds with 1-4 hydroxymethyl groups acyloxymethylated, and mixtures thereof. Examples of urea compounds include tetrahydroxymethylurea, tetramethoxymethylurea, tetrahydroxymethylurea compounds with 1-4 hydroxymethyl groups methoxymethylated, mixtures thereof, and tetramethoxyethylurea.
[0051] Suitable isocyanate compounds include toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, and cyclohexane diisocyanate.
[0052] Suitable azide compounds include 1,1'-biphenyl-4,4'-diazide, 4,4'-methylidene diazide, and 4,4'-oxybisazide. Examples of compounds containing an alkenyl ether group include ethylene glycol divinyl ether, triethylene glycol divinyl ether, 1,2-propanediol divinyl ether, 1,4-butanediol divinyl ether, tetramethylene glycol divinyl ether, neopentyl glycol divinyl ether, trimethylolpropane trivinyl ether, hexanediol divinyl ether, 1,4-cyclohexanediol divinyl ether, pentaerythritol trivinyl ether, pentaerythritol tetravinyl ether, sorbitol tetravinyl ether, sorbitol pentavinyl ether, and trimethylolpropane trivinyl ether.
[0053] The crosslinking agent is preferably added in an amount of 0.1-50 parts by weight, more preferably 1-40 parts by weight, relative to 100 parts by weight of the acid-instable resin.
[0054] The present invention also proposes a cured film, which is prepared by the following steps: (1) Dissolve the aforementioned resins A and E in a solvent, add components B, C, D, F, and H and necessary additives, stir thoroughly, add pre-dispersed pigment or carbon black dispersion, and filter through a 0.1–0.2 μm filter membrane to obtain the color photoresist composition. (2) Coating the aforementioned low-temperature curing high-resolution negative photosensitive composition onto the substrate to obtain a wet film; (3) Soft baking removes the solvent from the wet film to obtain a dry film; (4) Expose the dry film under a photomask; (5) Crosslink the exposed film at 60-70℃ for 30-180s; (6) Use alkaline solution for development and wash away the unexposed areas; (7) The cured film is obtained by baking at 80-90℃ for 15-30 minutes.
[0055] The cured film of this invention, under the same exposure event, first rapidly establishes a micro-pattern framework through free radical polymerization, then triggers low-temperature chemical amplification crosslinking within the framework's confined region by acid generated by PAG, and finally, continuously initiates ring-opening dark curing of oxobutane from the same acid source, forming a cured film with interpenetrating network characteristics. Under a tolerable thermal budget of 80-90℃, it simultaneously achieves ≤5 μm micro-pattern resolution, no swelling or collapse during development, resistance to downstream solvents, high hardness, long-term reliability, and acceptable storage stability.
[0056] Specifically, in some embodiments, the cured film possesses properties such as ≤5 μm resolution, NMP residual film rate ≥90% (N-methylpyrrolidone soaked at 60°C for 10 min), hardness ≥3H, and aging ΔE ≤3. The cured film obtained through the above steps can be used in the manufacture of silicon-based OLED / Micro-LED color filters or black matrices with PPI >3000.
[0057] It is particularly noteworthy that the negative photoresist curing process of this invention employs three key aspects: first, DPHA rapid gelation to initially limit acid diffusion and developer penetration; second, PAG simultaneously driving the reaction of acid-unstable resin / crosslinking agent and the ring-opening polymerization of oxetane; and third, the formation of a low-shrinkage cured film with interpenetrating acrylic / CA and polyether networks under post-baking conditions at 80-90°C. These synergistic processes produce non-linear effects that cannot be expected through simple addition: the free radical stage improves pattern retention, the CA stage enhances developer selectivity and low-temperature insolubility, and the Oxetane stage supplements chemical resistance and aging stability. Together, these three factors enable the composition to achieve high resolution and high reliability within the OLED thermal budget, a set of performance characteristics that cannot be simultaneously achieved by any single mechanism or any two mechanisms.
[0058] In a preferred embodiment, the solid content of the photosensitive component is 18-25 wt%, the viscosity is adjusted according to the spin-coated film thickness, and the preferred dry film thickness is 1.5-2.0 μm.
[0059] In a preferred embodiment, the alkaline compound contained in the alkaline developer is not particularly limited and can be appropriately selected based on the solubility characteristics of the photosensitive resin composition, film thickness, development rate, and pattern morphology requirements. Examples of alkaline compounds include inorganic bases, organic amines, quaternary ammonium compounds, alkanolamines, and cyclic amines. Among them, inorganic bases may be, for example, sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium silicate, sodium metasilicate, or ammonia; organic amines may be, for example, primary amines such as ethylamine and n-propylamine, secondary amines such as diethylamine and di-n-propylamine, or tertiary amines such as triethylamine and methyldiethylamine; quaternary ammonium compounds may be, for example, tetramethylammonium hydroxide or choline-based quaternary ammonium salts; alcoholic amines may be, for example, triethanolamine, diethanolamine, monoethanolamine, dimethylamine ethanol, or diethylamine ethanol; cyclic amines may be, for example, pyrrole, piperidine, 1,8-diazabicyclo[5,4,0]-7-undecene, 1,5-diazabicyclo[4,3,0]-5-nonene, or morpholine. The content of the above-mentioned basic compounds in the developer solution is usually 0.01 to 50% by mass, preferably 0.02 to 1% by mass. To improve the edge shape, residue removal, wettability, or uniformity of the developed pattern, the alkaline developer may further contain a surfactant, such as a nonionic surfactant, at a concentration of 0.1–5% by mass. Furthermore, when the developer is an alkaline aqueous solution, a water-soluble organic solvent, such as ethanol, γ-butyrolactone, dimethylformamide, or N-methyl-2-pyrrolidone, may be added as needed. The developing process is not particularly limited and can be performed by immersion, spraying, or coating. The resulting patterned film can be further rinsed with pure water or other suitable cleaning solutions to remove residual developer and dissolved components.
[0060] The following formulations are expressed as solids by mass fraction. Examples 1-3 correspond to blue, green, and red color filters, respectively, and Example 4 corresponds to the black matrix. All examples were baked at 90℃ for 10 min. Specific compositions are shown in Table 1, and curing methods are shown in Table 2.
[0061] Table 1:
[0062] Note: In Table 1, when component G is a pigment dispersion and is a mixed pigment, it is the mass ratio of the two pigments; component H is the molar ratio of the two monomers, and the same applies to Tables 3-1 and 3-2 below.
[0063] Table 2:
[0064] Meanwhile, comparative examples as shown in Tables 3-1 and 3-2 are set up, and the only difference between the curing methods shown in Table 2 and the curing methods is the post-baking method.
[0065] Table 3-1:
[0066] Table 3-2:
[0067] The above embodiments and comparative examples were tested according to the indicators shown in Table 4.
[0068] Table 4:
[0069] The test results are shown in Table 5.
[0070] Table 5:
[0071] The results show that the cured films prepared in Examples 1-5 possess properties such as ≤5 μm resolution, NMP residual film rate ≥90% (N-methylpyrrolidone soaked at 60°C for 10 min), hardness ≥3H, and aging ΔE ≤3. They can be used in the manufacture of silicon-based OLED / Micro-LED color filters or black matrices with PPI >3000.
[0072] Comparative Example 3 maintained a certain resolution after the removal of Oxetane, indicating that free radical + CA can provide basic mapping capabilities; however, its NMP residual film rate and aging ΔE were significantly worse than those of the Example, proving that Oxetane is not a common additive, but a key reinforcing mechanism to achieve high chemical resistance and long-term stability under low-temperature baking conditions.
[0073] Comparative Examples 5 and 6 are used to demonstrate, respectively, that free radical lock-in and CA low-temperature densification cannot be replaced by Oxetane alone. Comparative Example 7 is used to demonstrate that Oxetane is not an arbitrarily added additive, but rather that there exists an optimal dosage window that balances crosslinking reinforcement, acid diffusion, shrinkage, and storage stability. These comparative examples together form a complete chain of evidence: the absence of any mechanism or deviation from the specified window prevents the simultaneous achievement of 90°C low-temperature processing, ≤5 μm resolution, and NMP residual film rate ≥90%.
[0074] The above comparison illustrates: 1) If free radicals are lacking for rapid gelation, although PAG acid production and cationic reaction can occur, the film in the exposed area before development lacks sufficient skeleton, and the developer can easily penetrate, causing swelling and CD shift.
[0075] 2) Without CA low-temperature densification, it is difficult to establish sufficient exposure / unexposed area difference in aqueous alkaline development by relying solely on free radicals and oxetane, and the low-temperature crosslinking reaction is insufficient.
[0076] 3) If oxobutane cationic dark curing is lacking, even if a pattern of ≤5 μm can be formed, the cured film will still show a decrease in residual film rate and deterioration in color difference under NMP and 85°C high temperature aging due to the non-dense network.
[0077] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A low-temperature curable, high-resolution negative photosensitive composition, characterized in that, The composition by weight percentage includes: 10-35 wt% acrylate copolymer resin, 5-15 wt% multifunctional acrylate monomer, 1-5 wt% free radical photoinitiator, 1-5 wt% photoacid generator, 8-30 wt% acid-instable resin, 5-18 wt% acid-instable crosslinking agent, 20-45 wt% colorant, 3-8 wt% oxetane monomer, and the balance being solvent and additives; the acid-instable crosslinking agent is used for crosslinking under acid catalysis at 80-90℃.
2. The low-temperature curable high-resolution negative photosensitive composition as described in claim 1, characterized in that, The acid value of the acrylate copolymer resin is 60-180 mgKOH / g; And / or, the weight-average molecular weight of the acrylate copolymer resin is 8000-40000; And / or, the multifunctional acrylate monomer is selected from at least one of pentaerythritol hexaacrylate and pentaerythritol triacrylate.
3. The low-temperature curable high-resolution negative photosensitive composition as described in claim 1, characterized in that, The free radical photoinitiator is selected from at least one of the following: compounds having a triazole skeleton, compounds having a diazole skeleton, compounds having an imidazole skeleton, phosphine compounds, hexaarylbisimidazole, oxime compounds, carbazole oxime esters, organic peroxides, sulfur compounds, ketone compounds, aromatic onium salts, α-hydroxy ketone compounds, and α-amino ketone compounds. And / or, the photo-induced acid-producing agent is selected from at least one of thionium salts, iodonium salts, sulfonyldiazomethane, N-sulfonyloxyimide and oxime-O-sulfonate acid-producing agents; And / or, the acid-unstable crosslinking agent is selected from at least one of diphenols, triphenols, benzyl ethers, polyacetals, glycoureas, or melamine derivative crosslinking agents.
4. The low-temperature curable high-resolution negative photosensitive composition as described in claim 1, characterized in that, The acid-instable resin is a resin containing an acid-instable functional group, wherein the acid-instable functional group is selected from at least one of tert-butoxycarbonyl, acetal, ketal or tert-ester. And / or, the oxetane monomer is selected from at least one of monofunctional, difunctional or polyfunctional oxetanes, or oxetane-containing side-chain resins.
5. The low-temperature curable high-resolution negative photosensitive composition as described in claim 1, characterized in that, The colorant is selected from at least one of organic color pigments or dyes and carbon black dispersions; And / or, the solvent is selected from at least one of propylene glycol methyl ether acetate and cyclohexanone; And / or, the additive is selected from at least one of dispersants, leveling agents, adhesion promoters, crosslinking agents, and acid diffusion inhibitors.
6. A cured film, characterized in that, It is prepared by the following steps: S1. Coating a substrate with the low-temperature curing high-resolution negative photosensitive composition according to any one of claims 1-5 to obtain a wet film; S2. Soft baking removes the solvent from the wet film to obtain a dry film; S3. Expose the dry film under a photomask; S4. Crosslink the exposed film at 60-70℃ for 30-180s; S5. Develop with alkaline solution to wash away unexposed areas; S6. Bake at 80-90℃ for 15-30 minutes to obtain the cured film.
7. The cured film as described in claim 6, characterized in that, The solid content of the photosensitive component is 18-25 wt%; And / or, the dry film thickness is 1.5-2.0 μm; And / or, the alkaline solution is selected from at least one of inorganic bases, organic amines, quaternary ammonium compounds, alkanolamines, and cyclic amine solutions; And / or, in step S6, before post-baking, place the exposed area under a deep ultraviolet light source for re-exposure at 500-2000 millijoules per square centimeter.
8. An RGB color layer, characterized in that, Includes the cured film as described in claim 6 or 7.
9. A black matrix, characterized in that, Includes the cured film as described in claim 6 or 7.
10. The application of the RGB color layer of claim 8 and / or the black matrix of claim 9 in silicon-based OLED, silicon-based Micro-LED, and AR / VR / XR micro-display panels.
Citation Information
Patent Citations
Filtering method
JP1985031807A
Bold-faced display system for line drawing display
JP1985057891A
Compound and its tautomer, metal complex compound, colored photosensitive curing composition, color filter, and method for producing the same
JP2008292970A
Colored curable composition, color filter, method of manufacturing the same, and solid-state image pickup device
JP2009288705A
Positive radiation-sensitive composition, interlayer insulation film and method for producing the same
JP2011232632A