Preparation method of iron-based superconducting tape

By melting iron-based superconducting precursor powder at high temperature under an inert atmosphere and coating it onto a metal substrate, iron-based superconducting tapes were prepared. This solved the problem of low engineering critical current density in existing technologies, achieved a higher superconducting core ratio and stable superconducting performance, and expanded the application range.

CN123120423APending Publication Date: 2026-11-17QILU ZHONGKE ELECTRICAL ADVANCED ELECTROMAGNETIC DRIVE TECH RES INST +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510632808.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing iron-based superconducting wires encounter bottlenecks in improving the critical current density in engineering applications due to the combination of metal sheathing and ceramic powder processing, which increases processing difficulty and easily leads to uneven core wires.

Method used

Iron-based superconducting precursor powder is subjected to high-temperature melting treatment under an inert atmosphere to form a molten precursor, which is then coated onto a metal substrate to prepare an iron-based superconducting tape. A protective layer is formed by electroplating.

Benefits of technology

It improves the density and proportion of superconducting cores, enhances the engineering critical current density of iron-based superconducting tapes, and ensures stable superconducting properties under high current loads, making it suitable for superconducting magnets, superconducting cables, and superconducting motors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120423A_ABST
    Figure CN123120423A_ABST
Patent Text Reader

Abstract

This invention relates to the field of superconducting materials technology, specifically providing a method for preparing iron-based superconducting tapes, aiming to solve the problem of low engineering current density in existing iron-based superconducting tapes. The preparation method provided by this invention includes: subjecting iron-based superconducting precursor powder to high-temperature melting treatment under an inert atmosphere to obtain a molten precursor; and coating the molten precursor onto a metal substrate to obtain the iron-based superconducting tape. Compared to superconducting wires prepared using the powder-in-tube method, the iron-based superconducting tape prepared by the method provided by this invention has the advantages of higher superconducting core density and a higher superconducting core ratio, which is beneficial for improving the engineering critical current density of iron-based superconducting tapes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of superconducting materials technology, specifically providing a method for preparing iron-based superconducting tapes. Background Technology

[0002] The groundbreaking discovery of superconductivity in iron-based superconducting materials is like a boulder thrown into a lake of science, sparking a surge of research into novel iron-based superconductors in the scientific community. Iron-based superconducting materials stand out due to their significant advantages, such as high upper critical field, low anisotropy, and low fabrication cost, and are considered a new type of superconducting material with great application potential in strong magnetic fields.

[0003] The key applications of iron-based superconducting materials lie in the mid-temperature, high-magnetic-field, and high-electricity fields. Cutting-edge fields such as magnetic confinement fusion, next-generation high-energy particle accelerators, and high-field nuclear magnetic resonance spectrometers all place high hopes on them. To meet the practical application requirements of iron-based superconducting materials in these fields, iron-based superconducting wires not only need to possess high engineering critical current densities but also excellent mechanical properties.

[0004] Currently, the critical current density of iron-based superconducting wires has reached the standard for practical application. However, the improvement of engineering critical current density has encountered a bottleneck in the composite processing of metal sheathing and ceramic powder. Specifically, superconducting wires prepared by the powder-in-tube method are easily constrained by the composite processing of metal sheathing and ceramic powder. In particular, the engineering critical current density of superconducting wires prepared by the powder-in-tube method is generally around 10... 3 A / cm 2 ~10 4 A / cm 2 (i.e., 1000 amperes / cm² to 10,000 amperes / cm²). Further increasing the proportion of superconducting cores would interfere with the plastic deformation of the composite during processing, not only significantly increasing the processing difficulty but also easily causing uneven core wires. Summary of the Invention

[0005] The present invention aims to solve the above-mentioned technical problems, namely, at least the problem of low engineering current density of existing iron-based superconducting tapes.

[0006] This invention provides a method for preparing iron-based superconducting tapes, the method comprising:

[0007] Iron-based superconducting precursor powder was subjected to high-temperature melting treatment under an inert atmosphere to obtain a molten precursor.

[0008] The molten precursor is coated onto a metal substrate to obtain an iron-based superconducting tape.

[0009] In some feasible embodiments of the above-mentioned method for preparing iron-based superconducting tapes, the "high-temperature melting treatment of iron-based superconducting precursor powder" includes:

[0010] The iron-based superconducting precursor powder is placed into a heat treatment furnace, and the temperature inside the heat treatment furnace is raised to a preset temperature and held for a preset time.

[0011] In some feasible embodiments of the above-described method for preparing iron-based superconducting tapes, the preset temperature is 800℃~1200℃; and / or

[0012] The preset duration is 10 min to 30 min.

[0013] In some feasible embodiments of the above-mentioned method for preparing iron-based superconducting tapes, the heat treatment furnace is provided with a liquid outlet, and the step of "coating the molten precursor onto the metal substrate" includes:

[0014] The distance between the liquid outlet and the surface of the metal base strip is maintained at a preset gap, and the metal base strip is moved along its length at a preset speed.

[0015] In some feasible embodiments of the above-described method for preparing iron-based superconducting tapes, the heat treatment furnace is in the shape of an inverted trapezoid or a funnel; and / or

[0016] The liquid outlet is located at the bottom of the heat treatment furnace, and the bottom wall of the heat treatment furnace is flat.

[0017] In some feasible embodiments of the above-described method for preparing iron-based superconducting tape, the thickness of the superconducting layer coated on the metal substrate tape is 10 μm to 100 μm.

[0018] In some feasible embodiments of the above-mentioned method for preparing iron-based superconducting tapes, the iron-based superconducting precursor powder includes one of barium potassium iron arsenic, iron selenium tellurium, calcium potassium iron arsenic, and samarium oxy iron arsenic.

[0019] In some feasible embodiments of the above-described method for preparing iron-based superconducting tapes, the metal substrate is made of one of nickel, nickel alloys, and stainless steel; and / or

[0020] The thickness of the metal substrate is 10μm to 50μm.

[0021] In some feasible embodiments of the above-described method for preparing iron-based superconducting tapes, the preparation method further includes:

[0022] The cooled iron-based superconducting tape is electroplated to form a protective layer on the surface of the iron-based superconducting tape.

[0023] In some feasible embodiments of the above-described method for preparing iron-based superconducting tapes, the thickness of the protective layer is 50 μm to 100 μm.

[0024] The beneficial effects of this invention are:

[0025] In preparing iron-based superconducting tapes, this invention first melts iron-based superconducting precursor powder at high temperature in an inert atmosphere, and then coats the molten precursor formed after high-temperature melting onto a metal substrate, thereby achieving the preparation of iron-based superconducting tapes. Compared with superconducting wires prepared by powder-packing method, the iron-based superconducting tapes prepared by the method provided by this invention have the advantages of higher superconducting core density and higher superconducting core ratio. A higher superconducting core ratio means that, under the same tape size, the tape with a higher superconducting core ratio can carry more superconducting current, that is, improve the engineering critical current density of the iron-based superconducting tape. This allows the prepared iron-based superconducting tape to transmit current more efficiently in practical applications and maintain stable superconducting characteristics under high current loads, showing broader application prospects in superconducting magnets, superconducting cables, superconducting motors, and other superconducting related technologies. Attached Figure Description

[0026] The preferred embodiments of the present invention are described below with reference to the accompanying drawings, in which:

[0027] Figure 1 A flowchart illustrating the preparation method of the iron-based superconducting tape provided in an embodiment of the present invention;

[0028] Figure 2 This is a schematic diagram of coating a molten precursor onto a metal substrate according to an embodiment of the present invention.

[0029] Explanation of reference numerals in the attached figures:

[0030] 10. Molten precursor; 20. Metal substrate; 30. Superconducting layer; 40. Heat treatment furnace. Detailed Implementation

[0031] Preferred embodiments of the present invention will now be described with reference to the accompanying drawings. Those skilled in the art should understand that these embodiments are merely illustrative of the technical principles of the invention and are not intended to limit the scope of protection of the invention. Those skilled in the art can make adjustments as needed to adapt to specific applications. Numerous specific details are set forth in the following detailed description to better illustrate the invention. Those skilled in the art should understand that the invention can be practiced without certain specific details.

[0032] Currently, the critical current density of iron-based superconducting wires has reached the standard for practical application. However, the improvement of engineering critical current density has encountered a bottleneck in the composite processing of metal sheathing and ceramic powder. Specifically, superconducting wires prepared by the powder-in-tube method are easily constrained by the composite processing of metal sheathing and ceramic powder. In particular, the engineering critical current density of superconducting wires prepared by the powder-in-tube method is generally around 10... 3 A / cm 2 ~10 4 A / cm 2 (i.e., 1000 amperes / cm² to 10,000 amperes / cm²). Further increasing the proportion of superconducting cores would interfere with the plastic deformation of the composite during processing, not only significantly increasing the processing difficulty but also easily causing uneven core wires.

[0033] To address the issue of low engineering current density in superconducting wires prepared using existing powder-packing methods, this invention provides a method for preparing iron-based superconducting tapes. Please refer to [link to relevant documentation]. Figures 1 to 2 The preparation method includes:

[0034] S1. Under an inert atmosphere, the iron-based superconducting precursor powder is subjected to high-temperature melting treatment to obtain molten precursor 10.

[0035] Specifically, under an inert atmosphere, iron-based superconducting precursor powder is placed into a heat treatment furnace 40, the temperature inside the heat treatment furnace 40 is raised to a preset temperature, and held at that temperature for a preset time to obtain a molten precursor 10.

[0036] In this context, "in an inert atmosphere" refers to conducting related operations in an environment containing an inert gas. This prevents chemical reactions between the iron-based superconducting precursor powder and oxygen, water vapor, or other substances in the air. This ensures the smooth formation of the molten precursor 10 from the melted iron-based superconducting precursor powder, preventing oxidation, hydrolysis, or other side reactions that could alter the composition of the molten precursor 10 and affect the subsequent fabrication of the iron-based superconducting tape. Common inert gases include argon (Ar), helium (He), neon (Ne), krypton (Kr), and xenon (Xe).

[0037] Iron-based superconducting precursor powder serves as the initial powder raw material for preparing iron-based superconducting materials (such as iron-based superconducting tapes and wires). Its core components are the chemical elements necessary for iron-based superconductors. This iron-based superconducting precursor powder needs to be prepared through a specific synthesis process (such as solid-state reaction method) and gradually transformed into a material with superconducting properties during subsequent heat treatment and molding processes.

[0038] There is a wide variety of iron-based superconducting precursor powders, mainly due to the high diversity in the chemical composition and crystal structure of iron-based superconductors. Common types of iron-based superconducting precursor powders include barium potassium iron arsenide (BaKFeAs), iron selenium tellurium (FeSeTe), calcium potassium iron arsenide (CaKFeAs), and samarium oxy iron arsenide (SmOFFeAs) systems.

[0039] It is understood that, in addition to the types mentioned above, there are other types of iron-based superconducting precursor powders. This embodiment will not elaborate on other types of iron-based superconducting precursor powders one by one.

[0040] Furthermore, the preset melting temperature is 800℃~1200℃, and the preset holding time is 10min~30min. When preparing different iron-based superconducting tapes, different types of iron-based superconducting precursor powders will use different preset melting temperatures and durations. For example, when preparing barium potassium iron arsenic (BaKFeAs) superconducting tapes, the preset melting temperature is 1200℃, and the preset holding time is 10min; when preparing iron selenium tellurium (FeSeTe) superconducting tapes, the preset melting temperature is 800℃, and the preset holding time is 30min; when preparing calcium potassium iron arsenic (CaKFeAs) superconducting tapes, the preset melting temperature is 1200℃, and the preset holding time is 20min; and when preparing samarium oxide iron arsenic (SmOFFeAs) superconducting tapes, the preset melting temperature is 1200℃, and the preset holding time is 30min.

[0041] It should be noted that the values ​​in the above examples are merely exemplary and should not be construed as limiting the scope of protection of this invention.

[0042] The preset temperature is set to ensure that all components of the iron-based superconducting precursor powder can fully melt; that is, the specific value of the preset temperature is related to the melting point of each component of the iron-based superconducting precursor powder. Furthermore, the specific value of the preset duration is related to the diffusion rate of each component of the iron-based superconducting precursor powder, allowing the various components to mix thoroughly in the molten state, forming a chemically homogeneous molten precursor 10. Since sufficient diffusion is required for uniform distribution of each component during heating, the preset duration of the holding phase in this invention provides sufficient time for component diffusion, ensuring the quality of the molten precursor 10 and laying a solid foundation for the subsequent preparation of high-performance iron-based superconducting tapes.

[0043] Furthermore, melting and holding the iron-based superconducting precursor powder in an inert atmosphere allows for precise control of temperature and time parameters during the heat treatment process, which is crucial for ensuring the performance consistency of each batch of products. For example, by setting fixed heating rates, holding temperatures, and holding times, it can be ensured that each batch of molten precursor 10 has similar quality and performance. This allows for standardized process parameters during production, improving production efficiency and product quality while reducing production costs, thus facilitating large-scale, industrialized production.

[0044] S2. Coat the molten precursor 10 onto the metal substrate 20 to obtain an iron-based superconducting tape.

[0045] Specifically, the heat treatment furnace 40 is provided with a liquid outlet. During coating, the distance between the liquid outlet and the surface of the metal substrate 20 is kept at a preset gap, and the metal substrate 20 is moved along its length at a preset speed, thereby coating the molten precursor 10 onto the metal substrate 20 to obtain an iron-based superconducting tape.

[0046] The preset gap and preset speed are interrelated. If the preset gap is large and the preset speed is too fast, the molten precursor 10 may not adequately cover the baseband surface; conversely, if the preset gap is small and the preset speed is too slow, the molten precursor 10 may accumulate on the baseband surface. Therefore, the optimal combination of the two needs to be determined through experiments and optimization. Specifically, the preset gap ranges from 0.05 mm to 0.1 mm, and the preset speed ranges from 1 m / min to 10 m / min. For example, the preset gap is 0.1 mm, and the preset speed is 1 m / min.

[0047] It should be noted that the values ​​in the above examples are merely exemplary and should not be construed as limiting the scope of protection of this invention.

[0048] After multiple experimental optimizations, when the metal substrate 20 moves at a preset fixed speed and the distance between the liquid outlet and the surface of the metal substrate 20 is maintained at a preset fixed gap, the amount of liquid coated on a unit area of ​​the metal substrate 20 per unit time remains basically consistent, thereby ensuring the uniform thickness of the superconducting coating coated on the metal substrate 20. In addition, a suitable gap and moving speed can prevent defects such as accumulation, flow, or bubbles in the superconducting layer 30 coated on the surface of the metal substrate 20. Controlling the distance between the liquid outlet of the heat treatment furnace 40 and the metal substrate 20 to a moderate level can ensure that the molten precursor 10 flows out at an appropriate pressure and flow rate and uniformly covers the surface of the metal substrate 20. At the same time, using a suitable moving speed can prevent the molten precursor 10 from becoming uneven due to excessive residence time.

[0049] like Figure 2As shown, the metal substrate 20 is a thin strip material made from a metal or metal alloy as the matrix material through a specific process. Furthermore, the metal substrate 20 is made of a high-strength metal, such as nickel, nickel alloy, or stainless steel. Because high-strength metals possess excellent yield strength and tensile strength, they can withstand significant external forces without significant plastic deformation or fracture. In practical applications of superconducting tapes, such as large superconducting magnet systems, which are subjected to various forces including electromagnetic forces and mechanical vibrations, the high-strength metal substrate 20 ensures the structural integrity of the superconducting tape and maintains its stable superconducting performance. Moreover, the high-strength metal substrate 20 also possesses good toughness, absorbing energy when subjected to impact or vibration, preventing brittle fracture. During the transportation, installation, and use of superconducting tapes, collisions or vibrations are inevitable; good toughness ensures that the substrate will not be easily damaged, thus protecting the internal superconducting layer 30.

[0050] The thickness of the metal substrate 20 is 10 μm to 50 μm, and the thickness of the superconducting layer 30 coated on the metal substrate 20 is 10 μm to 100 μm. For example, when preparing barium potassium iron arsenide (BaKFeAs) superconducting tape, a stainless steel substrate with a thickness of 50 μm is used, and the thickness of the superconducting layer coated on the stainless steel substrate is 10 μm; when preparing iron selenium tellurium (FeSeTe) superconducting tape, a nickel alloy substrate with a thickness of 30 μm is used, and the thickness of the superconducting layer coated on the nickel alloy substrate is 50 μm; when preparing calcium potassium iron arsenide (CaKFeAs) superconducting tape, a nickel metal substrate with a thickness of 10 μm is used, and the thickness of the superconducting layer coated on the nickel metal substrate is 30 μm; when preparing samarium oxy iron arsenide (SmOFFeAs) superconducting tape, a nickel metal substrate with a thickness of 10 μm is used, and the thickness of the superconducting layer coated on the nickel metal substrate is 100 μm.

[0051] It should be noted that the values ​​in the above examples are merely exemplary and should not be construed as limiting the scope of protection of this invention.

[0052] In addition, the heat treatment furnace 40 is in the shape of an inverted trapezoid or funnel. This not only helps the molten precursor 10 to gather at the bottom of the heat treatment furnace 40 and be discharged through the outlet to better adapt to the coating operation, but also improves the gas flow, so that the protective gas can be evenly diffused and quickly exchanged in the furnace, reducing flow dead zones and avoiding problems such as oxidation in local areas due to insufficient gas.

[0053] Furthermore, the liquid outlet is located at the bottom of the heat treatment furnace 40, and the bottom wall of the heat treatment furnace 40 is flat. When coating the molten precursor 10, the flat bottom wall reduces disturbance and turbulence during liquid flow, allowing the molten precursor 10 to be evenly spread on the surface of the metal substrate 20. This helps to avoid local coatings that are too thick or too thin, and also helps to reduce liquid flow deviation or splashing, thereby improving the uniformity of coating.

[0054] S3. Electroplating is performed on the cooled iron-based superconducting tape to form a protective layer on the surface of the iron-based superconducting tape.

[0055] Furthermore, the thickness of the protective layer is 50 μm to 100 μm. For example, the thickness of the protective layer is 50 μm when preparing barium potassium iron arsenic (BaKFeAs) superconducting tapes; 50 μm when preparing iron selenium tellurium (FeSeTe) superconducting tapes; 100 μm when preparing calcium potassium iron arsenic (CaKFeAs) superconducting tapes; and 50 μm when preparing samarium oxide iron arsenic (SmOFFeAs) superconducting tapes. In addition, the material of the protective layer can be copper, silver, etc. In iron-based superconducting tapes, the protective layer can effectively shield external electromagnetic interference, reduce eddy current losses, and also provide mechanical protection, preventing damage to the superconducting layer 30 from external forces.

[0056] It should be noted that the values ​​in the above examples are merely exemplary and should not be construed as limiting the scope of protection of this invention.

[0057] Example 1: Preparation of Barium-Potassium-Iron-Arsenic (BaKFeAs) Superconducting Tape

[0058] In an argon atmosphere glove box, Ba shavings, K blocks, Fe powder, and As powder are mixed according to the chemical formula Ba 0.5 K 0.5 The molar ratio of Fe2As2(Ba122) was thoroughly and uniformly mixed to obtain Ba122 superconducting precursor powder. The Ba122 superconducting precursor powder was placed in an inert atmosphere heating furnace with a liquid outlet and heated to 1200℃, and held for 10 minutes. The molten Ba122 liquid was coated onto a stainless steel substrate with a thickness of 50 micrometers, and the thickness of the superconducting layer was controlled at 10 micrometers. The cooled substrate coated with the Ba122 superconducting layer was electroplated with copper, and the copper layer thickness was 50 micrometers.

[0059] Experimental tests revealed that the critical transition temperature of this superconducting tape is 37K, and the engineering critical current density is 60,000 amperes per square centimeter (A / cm²). 2 The tensile strength is 400 MPa, while the engineering critical current density of existing superconducting wires prepared by the powder-packing method is generally around 10 MPa. 3 A / cm 2 ~104 A / cm 2 (i.e., 1000 amperes / cm² to 10,000 amperes / cm²), it can be seen that the engineering critical current density of the barium potassium iron arsenic (BaKFeAs) superconducting tape prepared by the preparation method provided by the present invention is greater than that of the iron-based superconducting wire prepared by the existing powder packing method.

[0060] Example 2: Preparation of iron selenium tellurium (FeSeTe) superconducting tape

[0061] In an argon atmosphere glove box, Fe shavings, Se powder, and Te powder are mixed according to the chemical formula FeSe. 0.5 Te 0.5 The FST superconducting precursor powder was prepared by thoroughly and uniformly mixing the powders according to the molar ratio shown in the figure. The FST superconducting precursor powder was placed in an inert atmosphere heating furnace with a lower outlet and heated to 800°C for 30 minutes. The molten FST liquid was coated onto a nickel alloy substrate with a thickness of 30 micrometers, and the thickness of the superconducting layer was controlled at 50 micrometers. The cooled nickel alloy substrate coated with the FST superconducting layer was then electroplated with copper, and the copper layer thickness was 50 micrometers.

[0062] Experimental tests revealed that the critical transition temperature of this superconducting tape is 14K, and the engineering critical current density is 40,000 amperes per square centimeter (A / cm²). 2 The tensile strength is 300 MPa, while the engineering critical current density of existing superconducting wires prepared by the powder-packing method is generally around 10 MPa. 3 A / cm 2 ~10 4 A / cm 2 (i.e., 1000 amperes / cm² to 10,000 amperes / cm²), it can be seen that the engineering critical current density of the iron selenium tellurium (FeSeTe) superconducting tape prepared by the preparation method provided by the present invention is greater than that of the iron-based superconducting wire prepared by the powder packing method.

[0063] Example 3: Preparation of calcium-potassium-iron-arsenic (CaKFeAs) superconducting tape

[0064] In an argon atmosphere glove box, Ca shavings, K blocks, Fe powder, and As powder are arranged according to the chemical formula Ca... 0.5 K 0.5The Ca1144 superconducting precursor powder was prepared by thoroughly and uniformly mixing Fe2As2 (Ca1144) at the indicated molar ratio. The Ca1144 superconducting precursor powder was placed in an inert atmosphere furnace with a lower outlet and heated to 1200℃ for 20 minutes. The molten Ca1144 liquid was coated onto a nickel metal substrate with a thickness of 10 micrometers, and the thickness of the superconducting layer was controlled at 30 micrometers. The cooled nickel metal substrate coated with the superconducting layer was then electroplated with copper, and the copper layer thickness was 100 micrometers.

[0065] Experimental tests revealed that the critical transition temperature of this superconducting tape is 30K, and the engineering critical current density is 20,000 amperes per square centimeter (A / cm²). 2 The tensile strength is 200 MPa, while the engineering critical current density of existing superconducting wires prepared by the powder-packing method is generally around 10 MPa. 3 A / cm 2 ~10 4 A / cm 2 (i.e., 1000 amperes / cm² to 10,000 amperes / cm²), it can be seen that the engineering critical current density of the calcium potassium iron arsenic (CaKFeAs) superconducting tape prepared by the preparation method provided by the present invention is greater than that of the iron-based superconducting wire prepared by the existing powder-packing method.

[0066] Example 4: Preparation of Samarium Oxide Iron Arsenic (SmOFFeAs) Superconducting Tape

[0067] In an argon atmosphere glove box, SmF3 powder, Fe2O3 powder, Fe powder, As powder, Sm powder, etc., are mixed according to the chemical formula SmO 0.7 F 0.3 The FeAs(Sm1111) molar ratio was thoroughly and uniformly mixed to obtain Sm1111 superconducting precursor powder. The Sm1111 superconducting precursor powder was placed in a high-temperature heating furnace with a lower outlet and heated to 1200℃, and held for 30 minutes. The molten Sm1111 liquid was coated onto a nickel alloy substrate with a thickness of 10 micrometers, and the thickness of the superconducting layer was controlled at 100 micrometers. The cooled nickel alloy substrate coated with the superconducting layer was electroplated with copper, and the copper layer thickness was 50 micrometers.

[0068] Experimental tests revealed that the critical transition temperature of this superconducting tape is 55K, and the engineering critical current density is 30,000 amperes per square centimeter (A / cm²). 2 The tensile strength is 300 MPa, while the engineering critical current density of existing superconducting wires prepared by the powder-packing method is generally around 10 MPa. 3 A / cm 2 ~10 4 A / cm 2(i.e., 1000 amperes / cm² to 10,000 amperes / cm²), it can be seen that the engineering critical current density of the samarium oxide iron arsenide (SmOFFeAs) superconducting tape prepared by the preparation method provided by the present invention is greater than the engineering critical current density of the iron-based superconducting wire prepared by the powder packing method.

[0069] In preparing iron-based superconducting tapes, this invention first melts iron-based superconducting precursor powder at high temperature in an inert atmosphere, and then coats the molten precursor 10 formed after high-temperature melting onto a metal substrate 20, thereby achieving the preparation of iron-based superconducting tapes. Compared with superconducting wires prepared by powder-packing method, the iron-based superconducting tapes prepared by the method provided by this invention have the advantages of higher superconducting core density and higher superconducting core ratio. A higher superconducting core ratio means that, under the same tape size, the tape with a higher superconducting core ratio can carry more superconducting current, that is, improve the engineering critical current density of the iron-based superconducting tape. This allows the prepared iron-based superconducting tape to transmit current more efficiently in practical applications and maintain stable superconducting characteristics under high current loads, thus having broader application prospects in superconducting magnets, superconducting cables, superconducting motors, and other superconducting related technologies.

[0070] Furthermore, the superconducting layer 30 of the iron-based superconducting tape prepared by the present invention can be adjusted to different thicknesses as needed. At the same time, the thickness of the metal substrate 20 and the outer protective layer can also be adjusted as needed, thereby ensuring that the manufactured iron-based superconducting tape has an extremely high engineering critical current density, and the metal substrate 20 and the protective layer can be customized according to the actual application requirements such as the mechanical strength and thermal conductivity of the superconducting tape.

[0071] The technical solution of the present invention has been described above with reference to the preferred embodiments shown in the accompanying drawings. However, it will be readily understood by those skilled in the art that the scope of protection of the present invention is obviously not limited to these specific embodiments. Without departing from the principles of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after such changes or substitutions will all fall within the scope of protection of the present invention.

Claims

1. A method for preparing an iron-based superconducting tape, characterized in that, The preparation method includes: Iron-based superconducting precursor powder was subjected to high-temperature melting treatment under an inert atmosphere to obtain a molten precursor (10); The molten precursor (10) is coated onto the metal substrate (20) to obtain an iron-based superconducting tape.

2. The method for preparing iron-based superconducting tape according to claim 1, characterized in that, The "high-temperature melting treatment of iron-based superconducting precursor powder" includes: The iron-based superconducting precursor powder is placed into a heat treatment furnace (40) to raise the temperature inside the heat treatment furnace (40) to a preset temperature and hold it for a preset time.

3. The method for preparing iron-based superconducting tape according to claim 2, characterized in that, The preset temperature is 800℃~1200℃; and / or The preset duration is 10 min to 30 min.

4. The method for preparing iron-based superconducting tape according to claim 2, characterized in that, The heat treatment furnace (40) is provided with a liquid outlet, and the "coating of the molten precursor (10) onto the metal substrate (20)" includes: The distance between the liquid outlet and the surface of the metal base strip (20) is kept at a preset gap, and the metal base strip (20) is moved along its length at a preset speed.

5. The method for preparing the iron-based superconducting tape according to claim 4, characterized in that, The heat treatment furnace (40) is in the shape of an inverted trapezoid or a funnel; and / or The liquid outlet is located at the bottom of the heat treatment furnace (40), and the bottom wall of the heat treatment furnace (40) is flat.

6. The method for preparing the iron-based superconducting tape according to claim 4, characterized in that, The thickness of the superconducting layer (30) coated on the metal substrate (20) is 10 μm to 100 μm.

7. The method for preparing iron-based superconducting tape according to claim 1, characterized in that, The iron-based superconducting precursor powder includes one of barium potassium iron arsenic, iron selenium tellurium, calcium potassium iron arsenic, and samarium oxygen iron arsenic.

8. The method for preparing iron-based superconducting tape according to claim 1, characterized in that, The metal base strip (20) is made of one of nickel, nickel alloy, and stainless steel; and / or The thickness of the metal substrate (20) is 10 μm to 50 μm.

9. The method for preparing iron-based superconducting tape according to any one of claims 1-8, characterized in that, The preparation method further includes: The cooled iron-based superconducting tape is electroplated to form a protective layer on the surface of the iron-based superconducting tape.

10. The method for preparing the iron-based superconducting tape according to claim 9, characterized in that, The thickness of the protective layer is 50μm to 100μm.