Electrode manufacturing method and electrode

By coating hollow active material particles onto the electrode and applying pressure to deform them, combined with multiple rolling processes, the problem of uniformity in the density and thickness of the active material layer in the electrode in the prior art has been solved, and high-density and low-resistance electrode manufacturing has been achieved.

CN123120645APending Publication Date: 2026-11-17TOYOTA JIDOSHA KK
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202610380486.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-15
Filing Date
2026-03-26
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies make it difficult to increase the density of active materials in the electrode active material layer by increasing the pressing pressure, and it is also difficult to achieve uniform thickness of the electrode active material layer.

Method used

A mixed material containing hollow active material particles is coated on a sheet current collector, and pressure is applied through a rolling process to deform the hollow active material particles. Combined with the first and second rolling processes, the density of the active material is increased and the ripples are corrected.

Benefits of technology

This achieved high density and uniform thickness in the electrode active material layer, reducing resistance and improving electrode performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120645A_ABST
    Figure CN123120645A_ABST
Patent Text Reader

Abstract

A method for manufacturing an electrode includes: a layer forming step, wherein a mixed material comprising hollow active material particles is coated on at least one surface of a sheet-like current collector to form an electrode active material layer; and a rolling step, wherein the electrode active material layer is rolled by applying a predetermined pressure to deform the hollow active material particles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The technology disclosed in this specification relates to a method for manufacturing an electrode and the electrode itself. Background Technology

[0002] Japanese Patent Application Publication No. 2006-128039 discloses the following method for manufacturing a bipolar battery electrode: an active material that is not easily flattened is first coated on one side of the current collector and then pressed, and then an active material that is easily flattened is coated on the remaining side and then pressed. Summary of the Invention

[0003] To increase the density or uniformity of the electrode active material layer, an electrode with an active material layer coated on the surface of a sheet-like current collector is subjected to rolling pressing using rollers. However, even with increased pressing pressure, it is difficult to increase the density of the active material in the electrode active material layer. Furthermore, Japanese Patent Application Publication No. 2006-128039 does not disclose a solution to this problem.

[0004] This specification discloses a method for manufacturing an electrode. The method includes: a layer forming step, which coats at least one surface of a sheet-like current collector with a mixed material comprising hollow active material particles to form an electrode active material layer; and a rolling step, which rolls the electrode active material layer by applying a predetermined pressure to deform the hollow active material particles.

[0005] According to the described structure, through a rolling process, a portion of the hollow active material particles are deformed and flattened or crushed. Therefore, the density of the active material in the electrode active material layer can be higher than before.

[0006] This specification discloses an electrode with the following structure: a sheet-like current collector; and an electrode active material layer formed on at least one side of the current collector, the electrode active material layer comprising hollow active material particles and active material particles in a flattened state of the hollow portion of the hollow structure.

[0007] According to the structure described, the electrode active material layer contains active material particles with a flattened hollow structure. Therefore, an electrode with a high density of active material in the electrode active material layer can be obtained. Attached Figure Description

[0008] Hereinafter, with reference to the accompanying drawings, the features, advantages, and technical and industrial significance of exemplary embodiments of the present invention will be described, in which the same reference numerals denote the same elements, and wherein:

[0009] Figure 1 This is a flowchart illustrating the electrode manufacturing process.

[0010] Figure 2 This is a cross-sectional view used to illustrate step S100.

[0011] Figure 3 This is a partial sectional view used to illustrate step S120.

[0012] Figure 4 This is a magnified view of a portion of the electrode active material layer prior to step S120, which contains hollow-structured positive electrode active material particles.

[0013] Figure 5 This is a magnified view of a portion of the electrode active material layer after step S120, which contains hollow-structured positive active material particles.

[0014] Figure 6 This is a cross-sectional view of a secondary battery.

[0015] Figure 7 This is an exploded perspective view of the electrode stack. Detailed Implementation

[0016] The following lists the main features of the illustrated embodiments. These features can be combined in any way.

[0017] According to the electrode manufacturing method disclosed in this specification, the electrode active material layer may be a positive electrode active material layer containing the active material particles as positive electrode active material.

[0018] According to the structure described, it is possible to increase the density of active material in the positive electrode, which requires a higher density of active material compared to the negative electrode.

[0019] The electrode manufacturing method disclosed in this specification further includes a second rolling step, in which the electrode active material layer is rolled after the first rolling step, and the pressure applied to the electrode active material layer in the second rolling step is less than the pressure applied to the electrode active material layer in the first rolling step.

[0020] According to the structure, the density of the active material in the electrode active material layer can be further increased by the second rolling process, or the ripples generated on the electrode in the first rolling process can be reduced.

[0021] According to the electrode manufacturing method disclosed in this specification, the mixed material may contain non-hollow active material particles, the diameter of which is less than twice the wall thickness of the hollow active material particles.

[0022] According to the structure described, the electrode active material layer comprises hollow active material particles and non-hollow active material particles. The diameter of the non-hollow active material particles is less than twice the wall thickness of the hollow active material particles. Therefore, even if the hollow active material particles deform during the rolling process, excessive pressure can be avoided on the non-hollow active material particles.

[0023] The embodiments will be described with reference to the accompanying drawings. The drawings are for illustrative purposes only, and the embodiments are not limited to the content shown. Furthermore, since the drawings are illustrative, some details have been omitted.

[0024] Figure 1 The electrode manufacturing method is illustrated in the flowchart. The electrode manufacturing method generally includes a step of forming an electrode active material layer on a current collector (step S100), a step of applying a first pressure to the electrode active material layer and rolling it (step S120), and a step of applying a second pressure to the electrode active material layer and rolling it (step S140). Step S100 corresponds to the layer forming step. Step S120 corresponds to the first rolling step. Step S140 corresponds to the second rolling step. However, step S140 is not mandatory. When step S140 is omitted, step S120 is referred to as the rolling step. The electrode manufacturing method may also include steps not shown. Figure 1 The process.

[0025] Figure 2 This is a diagram illustrating step S100, simply showing a cross-section of the electrode 20. In step S100, an electrode active material layer 24 is formed by coating at least one surface of the sheet-like current collector 22 with a mixed material containing active material particles with a hollow structure.

[0026] exist Figure 2 In the diagram, a cross-section of the current collector 22 is shown from a viewpoint orthogonal to the long side direction D1 of the current collector 22. The direction D2 orthogonal to the long side direction D1 refers to the width direction D2 of the current collector 22. The current collector 22 is a metal foil. The electrode 20 is, for example, the positive electrode used in a rechargeable lithium-ion battery. The current collector 22 is, for example, an aluminum foil. A slurry containing a mixture of active materials, conductive additives, binders, solvents, etc., is applied to both sides of the current collector 22, such as... Figure 2 As shown, electrode active material layers 24 are formed on both sides of the current collector 22. When the electrode 20 is a positive electrode, the electrode active material layer 24 is equivalent to a positive electrode active material layer containing active material particles that serve as positive electrode active materials.

[0027] As positive electrode active materials, all types of active materials can be used, such as olivine-type, layered rock salt-type, and spinel-type active materials, for example, lithium iron phosphate, lithium nickel oxide, lithium cobalt oxide, and lithium manganese oxide. Positive electrode active materials can also be ternary materials containing the three elements nickel, cobalt, and manganese.

[0028] Figure 3 This is a diagram used to illustrate step S120, and... Figure 2 Similarly, a simplified cross-section of electrode 20 is shown. Figure 1 Although omitted, a drying process is performed between steps S100 and S120 to dry the electrode active material layer 24 formed on the current collector 22. The drying process may also be performed after step S120 or after step S140. In step S120, the electrode active material layer 24 is rolled by applying a predetermined pressure (first pressure) to deform the hollow active material particles. It can be understood that during the rolling of the electrode active material layer 24, both the electrode active material layer 24 and the current collector 22 are also rolled.

[0029] according to Figure 3 A pair of rollers 8 are in contact with each side of the electrode active material layer 24 coated on both sides of the electrode 20, i.e., both sides of the current collector 22. Rolling is performed using the rollers 8 to achieve high density or uniform thickness of the electrode active material layer 24. The rollers 8 have an elongated cylindrical shape along the width direction D2. Figure 3 Electrode 20 is conveyed along the long side direction D1 under a first pressure applied by a pair of rollers 8 rotatably supported around roller shaft 6.

[0030] For example, a description of the hollow active material particles contained in the electrode active material layer 24 can be found in the positive electrode active material particles disclosed in Japanese Patent Application Publication No. 2020-35671. Figure 4 A portion of the electrode active material layer 24, including hollow-structured positive electrode active material particles 40, is shown under magnification. Figure 4 and the following Figure 5 The cross-section of positive electrode active material particles 40 is schematically shown in the figure. Figure 4 This refers to the electrode active material layer 24 formed on the current collector 22 in step S100, i.e., the electrode active material layer 24 before the rolling process based on step S120.

[0031] exist Figure 4 , 5In this paper, the particle shape of the positive electrode active material particle 40 is simply represented by a circle or the like, but the particle shape can be a shape including distortion or unevenness as disclosed in Japanese Patent Application Publication No. 2020-35671. The positive electrode active material particle 40 has a shell portion 42 integrally formed by multiple primary particles and a hollow portion 44 formed inside the shell portion 42. As disclosed in Japanese Patent Application Publication No. 2020-35671, a through hole extending to the hollow portion 44 can be formed in a part of the shell portion 42.

[0032] The thickness of the shell 42 of the positive electrode active material particle 40 is equivalent to the wall thickness T of the hollow active material particle. The wall thickness T can be calculated by (outer diameter A1 of the positive electrode active material particle 40 - inner diameter B of the positive electrode active material particle 40) / 2. The inner diameter B is the diameter of the hollow part 44. When observing multiple positive electrode active material particles 40, of course, the outer diameter A1 and inner diameter B will vary, so the wall thickness T can be a statistically obtained average value.

[0033] Figure 5 and Figure 4 Similarly, a portion of the electrode active material layer 24, including hollow-structured positive active material particles 40, is shown under magnification. Figure 5 The electrode active material layer 24 shown is the electrode active material layer 24 after rolling based on step S120. Therefore, the positive electrode active material particles 40 are deformed. Figure 5 In this designation, the positive electrode active material particle 40 deformed through step S120 is represented by the symbol 40a. The positive electrode active material particle 40a may, for example, have its hollow portion 44 flattened and deformed into a flat shape, or be further deformed to the point of breaking or crushing. The degree of flattening of the hollow portion 44 also varies depending on the positive electrode active material particle 40a. The positive electrode active material particle 40a includes particles whose hollow portion 44 has completely disappeared and is thus flattened, and particles whose hollow portion 44 is flattened to the point of maintaining an elliptical or oblong shape, etc.

[0034] like Figure 5 As shown, the electrode active material layer 24 also contains undeformed positive electrode active material particles 40. That is, the electrode active material layer 24 after step S120 is in a state containing positive electrode active material particles 40 (40a) that maintain a hollow structure and whose hollow portions 44 are flattened. Therefore, the first pressure applied to the electrode active material layer 24 in step S120 is set to a value that can deform at least a portion of the positive electrode active material particles 40. The first pressure is, for example, a value preset through experimentation or simulation. Furthermore, the first pressure can be, for example, set to a pressure corresponding to an appropriate porosity of the electrode active material layer 24, referring to Japanese Patent Application Laid-Open No. 2006-128039.

[0035] Thus, according to this embodiment, the electrode active material layer 24 formed on the current collector 22 in step S100 contains hollow positive electrode active material particles 40. Then, in step S120, a portion of the hollow positive electrode active material particles 40 is deformed and flattened or crushed. Therefore, the density of active material in the electrode active material layer 24 can be higher than before. In particular, in the manufacturing process of the electrode 20 as the positive electrode, by applying steps S100 and S120 of this embodiment, a positive electrode with increased active material density can be obtained. In addition, in the negative electrode (referring to the negative electrode) having a negative electrode current collector and a negative electrode active material layer formed on the negative electrode current collector... Figure 6 , 7 This embodiment can also be applied to the manufacturing process of the negative electrode 30.

[0036] The positive electrode active material particles 40 before deformation are larger in shape than the positive electrode active material particles 40a after deformation. That is, in the electrode active material layer 24 coated on the current collector 22, the specific surface area of ​​the positive electrode active material particles 40 is relatively small. Therefore, the amount of binder included as a binder in the electrode active material layer 24 can be reduced. By reducing the amount of binder, the resistance within the electrode active material layer 24 can be reduced.

[0037] To further increase the density of active material in the electrode active material layer 24, the number of deformed positive electrode active material particles 40a is preferably greater than the number of undeformed positive electrode active material particles 40. Therefore, the first pressure can be set to a value that can deform at least half of the number of positive electrode active material particles 40 contained in the electrode active material layer 24.

[0038] The aforementioned mixed material coated on the current collector 22 to form the electrode active material layer 24 may contain non-hollow, i.e., solid active material particles. Figure 4 , 5 In this text, the symbol 46 represents the positive electrode active material particles contained in the electrode active material layer 24, i.e., non-hollow positive electrode active material particles. Thus, hollow positive electrode active material particles 40 and non-hollow positive electrode active material particles 46 can coexist in the electrode active material layer 24. Positive electrode active material particles 40 and 46 can be active materials of the same type (composition) or different types. For example, the diameter (outer diameter) A2 of the positive electrode active material particle 46 is less than twice the wall thickness T of the positive electrode active material particle 40. If the outer diameter A2 is less than twice the wall thickness T, when the electrode active material layer 24 is rolled in step S120 and the positive electrode active material particles 40 are deformed, it is easier to avoid applying excessive pressure to the positive electrode active material particles 46, and to suppress the breakage of the positive electrode active material particles 46.

[0039] according to Figure 1 Step S140 is performed on the electrode 20, which has been rolled in step S120 to form the electrode active material layer 24. In step S140, as... Figure 3 As shown, the electrode 20, conveyed along the long side direction D1, is subjected to rolling, and the electrode active material layer 24 is further rolled. In this embodiment, the second pressure applied to the electrode active material layer 24 in step S140 is set to a value less than the first pressure applied to the electrode active material layer 24 in step S120.

[0040] In step S120, when the electrode active material layer 24 is pressed with a higher pressure (first pressure) that can deform the hollow structure of the positive electrode active material particles 40, wavy ripples sometimes occur on the electrode 20. In step S140, by pressing the electrode active material layer 24 with a second pressure lower than the first pressure, the density of the active material in the electrode active material layer 24 is further increased, and the aforementioned ripples are corrected, resulting in a reduction in ripples.

[0041] For example, such as Figure 6 and Figure 7 As shown, the electrode 20 manufactured by the manufacturing method of this embodiment is used as part of the structure of the secondary battery 10. Figure 6 A cross-section of the secondary battery 10 is shown in a simplified manner. The secondary battery 10 is a lithium-ion battery. The secondary battery 10 includes an electrode stack 16, which is formed by sandwiching a separator 14 between electrodes 20 (hereinafter, positive electrode 20) and negative electrode 30 and stacking them alternately in a first direction. Figure 7 The electrode stack 16 is simply shown in an exploded perspective view. The secondary battery 10 has a flexible outer casing (not shown), to which the electrode stack 16 is sealed. An electrolyte (not shown) is sealed inside the outer casing. The outer casing is, for example, a laminate. Figure 6 , 7 For ease of explanation, the X, Y, and Z axes are shown as mutually orthogonal. The Z-axis direction corresponds to the first direction. The first direction can also be referred to as the stacking direction. Figure 6 It is a sectional view based on a section orthogonal to the Y-axis.

[0042] like Figure 6 , 7 As shown, the electrode stack 16 is formed by alternately stacking generally rectangular positive electrodes 20 and generally rectangular negative electrodes 30 via a separator 14, which is a strip-shaped structure with alternating zigzag bends and folds. In this configuration, each of the plurality of positive electrodes 20 is sandwiched between one of the two sides of the separator 14, and each of the plurality of negative electrodes 30 is sandwiched between the other of the two sides of the separator 14. The positive electrodes 20 and negative electrodes 30 extend along the X-axis and Y-axis directions, respectively.

[0043] The separator 14 is formed of a material that combines the properties of permeability (allowing for the movement of charge carriers, in this case, lithium ions, during charging and discharging) with insulation (preventing short circuits caused by contact between the positive electrode 20 and the negative electrode 30). Examples of materials for the separator 14 include polypropylene and polyethylene. Figure 6 , 7 As shown, the structure of a series of serrated, tortuous partitions 14 sandwiched between electrodes is only one example. The partitions 14 sandwiched between electrodes can be separated from each other.

[0044] like Figure 7 As shown, the positive electrode 20 includes a current collector 22 (hereinafter, positive current collector 22) and an electrode active material layer 24 (hereinafter, positive active material layer 24) formed on the positive current collector 22. The negative electrode 30 includes a negative current collector 32 and a negative active material layer 34 formed on the negative current collector 32. The negative active material layer 34 is formed on both sides of the negative current collector 32, for example. The negative current collector 32 is, for example, a copper foil. The negative active material layer 34 contains a negative active material. Examples of negative active materials include, for example, carbon materials such as graphite, hard carbon, and soft carbon, materials that form alloys with lithium such as silicon (Si), and lithium alloys.

[0045] The positive electrode 20 and the negative electrode 30 each have uncoated portions 22a and 32a protruding in a direction intersecting the first direction. The uncoated portion 22a of the positive electrode 20 is the area in the positive current collector 22 where the positive active material layer 24 is not coated. The uncoated portion 32a of the negative electrode 30 is the area in the negative current collector 32 where the negative active material layer 34 is not coated. For example, the Y-axis direction (Y-axis + direction and Y-axis - direction) corresponds to the direction intersecting the first direction. According to... Figure 7 The uncoated portion 22a of the positive electrode 20 protrudes in the Y-axis + direction, and the uncoated portion 32a of the negative electrode 30 protrudes in the Y-axis - direction. Although not shown in the figure, the uncoated portions 22a of each of the plurality of positive electrodes 20 are electrically connected to the positive terminal outside the area held by the separator 14, for example, via current collectors. Similarly, although not shown in the figure, the uncoated portions 32a of each of the plurality of negative electrodes 30 are electrically connected to the negative terminal even further outside the area held by the separator 14, for example, via current collectors.

[0046] The above provides a detailed description of specific examples of the technology disclosed in this specification. However, these are merely illustrative and do not limit the scope of the claims. The technology described in the claims includes various modifications and alterations to the specific examples illustrated above. Furthermore, the technical elements described in this specification or drawings are technically useful individually or in various combinations, and are not limited to the combinations described in the claims at the time of application. Moreover, the technology illustrated in this specification or drawings is technology that simultaneously achieves multiple objectives, and is technically useful even if it achieves only one objective.

Claims

1. A method for manufacturing an electrode, characterized in that, include: In the layer formation process, an electrode active material layer is formed by coating at least one surface of a sheet-like current collector with a mixed material containing hollow active material particles. and The rolling process involves applying a predetermined pressure to the electrode active material layer to deform the active material particles in the hollow structure, thereby rolling the electrode active material layer.

2. The method for manufacturing the electrode according to claim 1, characterized in that, The electrode active material layer is a positive electrode active material layer containing the active material particles that serve as positive electrode active materials.

3. The method for manufacturing the electrode according to claim 1, characterized in that, Also includes: The second rolling process involves rolling the electrode active material layer after the first rolling process. The pressure applied to the electrode active material layer in the second rolling process is less than the pressure applied to the electrode active material layer in the first rolling process.

4. The method for manufacturing an electrode according to claim 1, characterized in that, The hybrid material contains active material particles with a non-hollow structure. The diameter of the non-hollow active material particles is less than twice the wall thickness of the hollow active material particles.

5. An electrode, characterized in that, have: Plate-shaped current collector; and An electrode active material layer is formed on at least one surface of the current collector. The electrode active material layer includes hollow active material particles and active material particles in a flattened state of the hollow part of the hollow structure.

Citation Information

Patent Citations

  • Manufacturing method of battery electrode

    JP2006128039A

  • Positive electrode for non-aqueous electrolyte secondary battery

    JP2020035671A