A proton exchange membrane for vehicle-mounted fuel cells and its preparation method
By combining modified mesoporous silica with a polyquinoxaline matrix, a stable proton transport channel was constructed, which solved the problems of easy phosphoric acid loss and resistance to impurities and contamination in high-temperature proton exchange membranes. This resulted in high phosphoric acid loading and strong load-bearing capacity of high-temperature proton exchange membranes, thereby improving the operational stability and lifespan of fuel cells.
Patent Information
- Application Number
- CN202611476870.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-22
- Publication Date
- 2026-11-17
AI Technical Summary
Existing high-temperature proton exchange membranes are prone to phosphoric acid loss and lack resistance to impurities and contamination, resulting in decreased proton conduction efficiency, fluctuating power output, and shortened service life. They are unable to meet the actual operating conditions of vehicle fuel cells and the requirements of industrial hydrogen supply.
Modified mesoporous silica is combined with a polyquinoxaline matrix, and imidazole groups are bridged by silane coupling agent residues to form Si-O-Si bonds and ether bonds, which covalently connect the polyquinoxaline molecular chains. Stable proton transport channels are constructed by phosphoric acid impregnation, thereby achieving strong fixation and anti-impurity properties of phosphoric acid.
It significantly improved the loading and stability of phosphoric acid, enhanced the high-temperature stability and impurity resistance of the membrane, and extended the service life and power output stability of the fuel cell.
Smart Images

Figure CN123120797A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of proton exchange membrane fuel cell technology, specifically to a high-temperature proton exchange membrane for vehicle-mounted fuel cells and its preparation method. Background Technology
[0002] High-temperature proton exchange membrane fuel cells (PEMFCs) effectively avoid the stringent dependence of low-temperature PEMFCs on pure water and cryogenic conditions, thanks to their core technological advantages such as eliminating the need for complex water humidification systems, excellent resistance to carbon monoxide poisoning, high waste heat recovery efficiency, and wide fuel compatibility. They not only possess significant application potential in stationary power generation and industrial backup power scenarios but have also become a core development direction for on-board fuel cell power systems, highly adaptable to the complex operating conditions, variable operating environments, and high power stability requirements of on-board applications. As a core component of on-board high-temperature fuel cells, the proton exchange membrane plays a crucial role in conducting protons, blocking anode and cathode gases, and ensuring the stable conduction of electrochemical reactions. Its material properties, structural stability, and operating condition adaptability directly determine the power output efficiency, service life, and operational safety of on-board fuel cells.
[0003] Among numerous high-temperature proton exchange membrane (PEM) materials, polyquinoxaline-based PEMs stand out due to their superior high-temperature thermal stability, excellent chemical corrosion resistance, good mechanical toughness, and processability. They are well-suited to the special operating conditions of fuel cells, including frequent start-ups and shutdowns, large temperature fluctuations, and high vibration loads, making them a mainstream research material with significant industrialization potential in the current high-temperature PEM field. These membrane materials typically employ a phosphoric acid impregnation and doping process to impart proton conductivity. A continuous and stable hydrogen bond transport network is constructed between the membrane matrix and phosphoric acid molecules, enabling efficient proton transfer under anhydrous high-temperature conditions and ensuring continuous and stable power generation from the fuel cell.
[0004] However, at present, pure polyquinoxaline membranes and conventional modified polyquinoxaline high-temperature proton exchange membranes are still insufficient to meet the actual operating conditions of fuel cells and the requirements of industrial hydrogen supply. Fuel cells often use industrial reformed hydrogen and crude hydrogen as fuel. The trace impurities, water vapor, and particulate matter contained in the fuel can continuously corrode the membrane material. At the same time, frequent start-stop cycles, sudden temperature changes, and mechanical vibrations under vehicle operating conditions further expose the inherent defects of the material. Currently, there are two major technical bottlenecks in this type of membrane material: poor stability of phosphoric acid under load and insufficient resistance to impurities and contamination. During operation, phosphoric acid is easily washed away by exhaust gas and leaked due to temperature fluctuations, causing interruption of the proton conduction channel. At the same time, crude hydrogen impurities can easily damage the membrane structure and hydrogen bond transport network, causing rapid degradation of membrane performance. These problems directly lead to a decrease in proton conduction efficiency, power output fluctuations, and a significant reduction in service life of on-board fuel cells, seriously restricting the large-scale promotion and engineering application of high-temperature proton exchange membrane fuel cells. Summary of the Invention
[0005] The purpose of this invention is to provide a high-temperature proton exchange membrane for vehicle fuel cells and its preparation method, so as to solve the problem of easy loss of phosphoric acid in current high-temperature proton exchange membranes.
[0006] To solve the above-mentioned technical problems, the present invention provides the following technical solution:
[0007] In a first aspect, the present invention provides a high-temperature proton exchange membrane for an on-board fuel cell, the high-temperature proton exchange membrane for an on-board fuel cell comprising a polyquinoxaline matrix and modified mesoporous silica dispersed in the polyquinoxaline matrix, and the proton exchange membrane is further doped with phosphoric acid.
[0008] The surface of the modified mesoporous silica is bridged with imidazole groups by silane coupling agent residues. The silane coupling agent residues are bonded to the surface of the modified mesoporous silica by Si-O-Si bonds and connected to imidazole phenoxy groups by ether bonds.
[0009] The modified mesoporous silica is covalently linked to the polyquinoxaline molecular chain via imine bonds.
[0010] Secondly, the present invention also provides a method for preparing a high-temperature proton exchange membrane for an on-board fuel cell, comprising the following steps:
[0011] S1. After heating and activating the mesoporous silica, add hydrochloric acid solution for acid activation treatment, centrifuge and filter, wash until neutral and dry; add the obtained product to anhydrous toluene, add KH560 for grafting treatment, centrifuge and dry to obtain epoxy-grafted mesoporous silica.
[0012] S2. Epoxy-grafted mesoporous silica, 4-(imidazol-1-yl)phenol and anhydrous toluene were mixed and heated under nitrogen protection. After centrifugation, washing and drying, the product was mixed with glyoxal, anhydrous ethanol and triethylamine. After a second heating reaction, centrifugation, washing and drying were performed to obtain modified mesoporous silica.
[0013] S3. Modified mesoporous silica, 1,4-bis(phenyloxoyl)benzene and 3,3'-diaminobenzidine were mixed, m-cresol was added, and the mixture was heated to react. The reaction mixture was added to ethanol, the precipitate was collected, washed and dried, and the dried product was dissolved in dimethyl sulfoxide to obtain modified polyquinoxaline casting solution.
[0014] S4. After the modified polyquinoxaline casting solution is cast and dried into a film, it is vacuum heated and cured, then cooled, and impregnated with phosphoric acid solution for adsorption. The adsorption continues until the membrane mass is constant, thus obtaining a high-temperature proton exchange membrane for vehicle fuel cells.
[0015] Furthermore, in S1, during heating activation, the temperature is increased to 500-550℃ at a rate of 2-5℃ / min and held for 2-3 hours;
[0016] For acid activation, heat to 95-100℃ and reflux with stirring for 4-6 hours; the concentration of hydrochloric acid solution is 4.5-5 mol / L.
[0017] During grafting, the temperature is raised to 80~100℃ and the reaction is stirred for 12~24 hours.
[0018] Furthermore, in S1, the mass ratio of mesoporous silica, hydrochloric acid solution and KH560 is 5:(30~50):(0.5~3).
[0019] Furthermore, in S2, the mass ratio of epoxy-grafted mesoporous silica, 4-(imidazol-1-yl)phenol, glyoxal, and triethylamine is 5: (0.1~1.2): (0.5~2): (0.1~0.3).
[0020] Furthermore, in S2, during the first heating reaction, the temperature is raised to 75~85℃, and the reaction is stirred for 8~10 hours;
[0021] During the second heating reaction, the temperature was raised to 65~68℃, and the reaction was stirred for 8~12 hours.
[0022] Furthermore, in S3, the molar ratio of 1,4-bis(phenyloxo)benzene to 3,3'-diaminobenzidine is 1:(0.8~1.05).
[0023] Furthermore, in S3, the amount of modified mesoporous silica added is 3 to 8 wt% of the total mass of 1,4-bis(phenyloxo)benzene and 3,3'-diaminobenzidine.
[0024] Furthermore, in S3, during the heating reaction, the temperature is raised to 60~80℃ and the reaction is carried out for 24~36h; the solid content of the modified polyquinoxaline casting solution is 5~12wt%.
[0025] Furthermore, in S4, the drying temperature during the casting and drying process is 100~125℃;
[0026] During vacuum heating curing, the temperature is raised to 350~400℃ in a vacuum environment and held for 0.5~1h;
[0027] The phosphoric acid solution concentration is 60~85wt%, and adsorption is completed after the weight becomes constant.
[0028] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0029] This invention addresses the shortcomings of traditional polyquinoxaline high-temperature proton exchange membranes, such as limited phosphate loading, easy loss of high-temperature phosphate, poor tolerance to fuel impurities, severe long-term conductivity decay, easy aggregation of inorganic fillers, and weak interfacial compatibility. It designs a preparation system for mesoporous silica through stepwise functionalization modification, covalent in-situ copolymerization, imidazole-enhanced phosphorus fixation, and a dense cross-linked anti-impurity network. First, the mesoporous silica is deeply activated by high-temperature calcination combined with concentrated hydrochloric acid reflux, significantly increasing the density of surface-active silanol groups. Then, KH560 is used to achieve controllable epoxy grafting on the silica surface, obtaining highly active epoxy-grafted mesoporous silica.
[0030] Subsequently, this invention further reacts 4-(imidazol-1-yl)phenol with epoxy-grafted mesoporous silica. The imidazolium ring in 4-(imidazol-1-yl)phenol has higher reactivity than the phenolic hydroxyl group, preferentially opening the epoxy group to introduce nitrogen-containing heterocycles and phenolic hydroxyl groups onto the filler surface. In the subsequent reaction, triethylamine can abstract the active hydrogen from the phenolic hydroxyl group of 4-(imidazol-1-yl)phenol, significantly enhancing the nucleophilicity of the generated phenoxy anion, which attacks the aldehyde carbon of the glyoxal monomer, resulting in a phenol-aldehyde addition condensation. This achieves a single-end reaction between the phenolic hydroxyl group and the glyoxal on the filler surface, while retaining the active aldehyde group at the other end. The imidazolium ring introduced in this reaction can form ionic bonds and multiple hydrogen bonds with phosphoric acid. Compared to pure polyquinoxaline relying solely on weak hydrogen bonds to support phosphoric acid, this significantly increases the phosphoric acid doping amount. Simultaneously, the imidazolium group strongly anchors phosphoric acid, significantly suppressing its volatilization, migration, and loss under high-temperature conditions, effectively solving the problem of rapid conductivity decay during long-term operation of traditional high-temperature membranes.
[0031] Based on this, the aldehyde groups on the surface of the modified mesoporous silica prepared in this invention can also undergo Schiff base copolymerization with 3,3'-diaminobenzidine and 1,4-bis(phenyloxadenyl)benzene, so that the mesoporous silica is covalently anchored inside the polyquinoxaline polymer crosslinking network, overcoming the drawbacks of traditional physical doping fillers such as numerous interface defects, easy precipitation, and easy agglomeration. Finally, after phosphoric acid impregnation, the imidazole basic sites, ordered mesoporous channels, and dense crosslinking network in the membrane synergistically construct a stable and continuous proton transport channel, achieving high phosphoric acid loading, strong phosphoric acid immobilization capacity, excellent high-temperature stability, and impurity resistance, breaking through the technical bottleneck of insufficient comprehensive performance of existing high-temperature proton exchange membranes. Attached Figure Description
[0032] Figure 1 This is a TEM image of the mesoporous silica used in Embodiment 3 of the present invention;
[0033] Figure 2 This is a TEM image of the modified mesoporous silica prepared in Example 3 of this invention;
[0034] Figure 3This is a polarization curve of the high-temperature proton exchange membrane for vehicle fuel cells prepared in Example 3 of the present invention after being applied to the membrane electrode assembly. Detailed Implementation
[0035] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0036] The mesoporous silica used in this invention is SBA-15 molecular sieve.
[0037] Example 1
[0038] A method for preparing a high-temperature proton exchange membrane for an on-board fuel cell includes the following steps:
[0039] S1. Mesoporous silica was heated to 500℃ at a rate of 2℃ / min and calcined for 3h to remove the template agent. Then, it was added to a 4.5mol / L hydrochloric acid solution and ultrasonically dispersed. The mixture was then heated to 95℃ and refluxed and stirred for 6h. After centrifugation and filtration, it was washed with deionized water until neutral and dried under vacuum at 300℃ for 4h. Then, it was added to anhydrous toluene, KH560 was added, the mixture was heated to 80℃ and stirred for 24h. After centrifugation, it was washed with anhydrous toluene and dried to obtain epoxy-grafted mesoporous silica.
[0040] The mass ratio of mesoporous silica, hydrochloric acid solution and KH560 is 5:30:0.5.
[0041] S2. Epoxy-grafted mesoporous silica and 4-(imidazol-1-yl)phenol were added to anhydrous toluene under a nitrogen atmosphere, heated to 75°C, and stirred for 10 h. The precipitate was separated by centrifugation, washed with anhydrous toluene, and the dried product was mixed with glyoxal and anhydrous ethanol. Triethylamine was added, the temperature was raised to 65°C, and the reaction was stirred for 12 h. The mixture was then separated by centrifugation, washed with anhydrous ethanol, and vacuum dried to obtain modified mesoporous silica.
[0042] The mass ratio of epoxy-grafted mesoporous silica, 4-(imidazol-1-yl)phenol, glyoxal, and triethylamine is 5:0.1:0.5:0.1.
[0043] S3. Modified mesoporous silica, 1,4-bis(phenyloxoyl)benzene and 3,3'-diaminobenzidine were mixed and dispersed evenly. Then, m-cresol was added and heated to 60°C. After reacting for 36 hours, the heating was stopped, and the mixture was added to ethanol. The precipitate was collected, washed, and vacuum dried. The dried product was dissolved in dimethyl sulfoxide to obtain a modified polyquinoxaline casting solution with a solid content of 5 wt%.
[0044] The molar ratio of 1,4-bis(phenyloxylated)benzene to 3,3'-diaminobenzidine is 1:0.8, and the amount of modified mesoporous silica added is 3 wt% of the total mass of 1,4-bis(phenyloxylated)benzene and 3,3'-diaminobenzidine.
[0045] S4. The modified polyquinoxaline casting solution was cast into a film, dried at 100°C, heated to 350°C under vacuum, kept at that temperature for 1 hour and cooled, and then immersed in a 60wt% phosphoric acid solution at an immersion temperature of 120°C. After adsorption until the weight was constant, a high-temperature proton exchange membrane for vehicle fuel cells was obtained.
[0046] Example 2
[0047] A method for preparing a high-temperature proton exchange membrane for an on-board fuel cell includes the following steps:
[0048] S1. Mesoporous silica was heated to 530℃ at a rate of 4℃ / min and calcined for 2.5h to remove the template agent. Then, it was added to a 4.8mol / L hydrochloric acid solution and ultrasonically dispersed. The mixture was then heated to 98℃ and refluxed with stirring for 5h. After centrifugation and filtration, it was washed with deionized water until neutral and dried under vacuum at 300℃ for 4h. Then, it was added to anhydrous toluene, KH560 was added, the mixture was heated to 90℃ and stirred for 20h. After centrifugation and separation, it was washed with anhydrous toluene and dried to obtain epoxy-grafted mesoporous silica.
[0049] The mass ratio of mesoporous silica, hydrochloric acid solution and KH560 is 5:40:2.
[0050] S2. Epoxy-grafted mesoporous silica and 4-(imidazol-1-yl)phenol were added to anhydrous toluene under a nitrogen atmosphere, heated to 80°C, and stirred for 9 hours. The precipitate was separated by centrifugation, washed with anhydrous toluene, and the dried product was mixed with glyoxal and anhydrous ethanol. Triethylamine was added, the temperature was raised to 68°C, and the reaction was stirred for 10 hours. The mixture was then separated by centrifugation, washed with anhydrous ethanol, and vacuum dried to obtain modified mesoporous silica.
[0051] The mass ratio of epoxy-grafted mesoporous silica, 4-(imidazol-1-yl)phenol, glyoxal, and triethylamine is 5:1:1.5:0.2.
[0052] S3. Modified mesoporous silica, 1,4-bis(phenyloxoyl)benzene and 3,3'-diaminobenzidine were mixed and dispersed evenly. The mixture was then added to m-cresol, heated to 70°C, and reacted for 30 h. Heating was then stopped, and the mixture was added to ethanol. The precipitate was collected, washed, and vacuum dried. The dried product was dissolved in dimethyl sulfoxide to obtain a modified polyquinoxaline casting solution with a solid content of 10 wt%.
[0053] The molar ratio of 1,4-bis(phenyloxylated)benzene to 3,3'-diaminobenzidine is 1:1, and the amount of modified mesoporous silica added is 5 wt% of the total mass of 1,4-bis(phenyloxylated)benzene and 3,3'-diaminobenzidine.
[0054] S4. The modified polyquinoxaline casting solution was cast into a film, dried at 120°C, heated to 370°C under vacuum, held for 0.8 h and cooled, and then immersed in a 70 wt% phosphoric acid solution at 130°C. After adsorption until the weight was constant, a high-temperature proton exchange membrane for vehicle fuel cells was obtained.
[0055] Example 3
[0056] A method for preparing a high-temperature proton exchange membrane for an on-board fuel cell includes the following steps:
[0057] S1. Mesoporous silica was heated to 550℃ at a rate of 5℃ / min and calcined for 2 hours to remove the template agent. Then, it was added to a 5 mol / L hydrochloric acid solution and ultrasonically dispersed. The mixture was then heated to 100℃ and refluxed with stirring for 4 hours. After centrifugation and filtration, the silica was washed with deionized water until neutral and dried under vacuum at 300℃ for 4 hours. The silica was then added to anhydrous toluene, KH560 was added, and the mixture was heated to 100℃ and stirred for 12 hours. After centrifugation, the silica was washed with anhydrous toluene and dried to obtain epoxy-grafted mesoporous silica.
[0058] The mass ratio of mesoporous silica, hydrochloric acid solution and KH560 is 5:50:3.
[0059] S2. Epoxy-grafted mesoporous silica and 4-(imidazol-1-yl)phenol were added to anhydrous toluene under a nitrogen atmosphere, heated to 85°C, and stirred for 8 hours. The precipitate was separated by centrifugation, washed with anhydrous toluene, and the dried product was mixed with glyoxal and anhydrous ethanol. Triethylamine was added, the temperature was raised to 68°C, and the reaction was stirred for 8 hours. The mixture was then separated by centrifugation, washed with anhydrous ethanol, and vacuum dried to obtain modified mesoporous silica.
[0060] The mass ratio of epoxy-grafted mesoporous silica, 4-(imidazol-1-yl)phenol, glyoxal, and triethylamine is 5:1.2:2:0.3.
[0061] S3. Modified mesoporous silica, 1,4-bis(phenyloxoyl)benzene and 3,3'-diaminobenzidine were mixed and dispersed evenly. The mixture was then added to m-cresol, heated to 80°C, and reacted for 24 hours. Heating was then stopped, and the mixture was added to ethanol. The precipitate was collected, washed, and vacuum dried. The dried product was dissolved in dimethyl sulfoxide to obtain a modified polyquinoxaline casting solution with a solid content of 8 wt%.
[0062] The molar ratio of 1,4-bis(phenyloxylated)benzene to 3,3'-diaminobenzidine is 1:1.05, and the amount of modified mesoporous silica added is 8 wt% of the total mass of 1,4-bis(phenyloxylated)benzene and 3,3'-diaminobenzidine.
[0063] S4. The modified polyquinoxaline casting solution was cast into a film, dried at 125°C, heated to 400°C under vacuum, held for 0.5 h and cooled, and then immersed in a phosphoric acid solution with a concentration of 85 wt% at an immersion temperature of 140°C. After adsorption until the weight was constant, a high-temperature proton exchange membrane for vehicle fuel cells was obtained.
[0064] Comparative Example 1
[0065] This comparative example provides a method for preparing a high-temperature proton exchange membrane for an on-board fuel cell. Compared with Example 3, this comparative example uses unmodified mesoporous silica in an equal amount to replace modified mesoporous silica, and the remaining steps and parameters are the same as in Example 3.
[0066] Comparative Example 2
[0067] This comparative example provides a method for preparing a high-temperature proton exchange membrane for an on-board fuel cell. Compared with Example 3, this comparative example only prepares epoxy-grafted mesoporous silica in an equal amount to replace the modified mesoporous silica. The remaining steps and parameters are the same as in Example 3.
[0068] Comparative Example 3
[0069] This comparative example provides a method for preparing a high-temperature proton exchange membrane for a vehicle-mounted fuel cell. Compared with Example 3, this comparative example only uses an equal amount of nano-silica to replace mesoporous silica, while the remaining steps and parameters are the same as in Example 3.
[0070] Comparative Example 4
[0071] This comparative example provides a method for preparing a high-temperature proton exchange membrane for an on-board fuel cell. Compared with Example 3, this comparative example does not add modified mesoporous silica, and the remaining steps and parameters are the same as in Example 3.
[0072] Detection method:
[0073] Phosphoric acid adsorption rate: After film formation in step S4, the film weight is measured before and after immersion in phosphoric acid solution. The calculation formula is as follows:
[0074]
[0075] Tensile strength: The high-temperature proton exchange membranes for vehicle fuel cells prepared in Examples 1-3 and Comparative Examples 1-4 were prepared into test samples with a thickness of 90±5μm and a length and width of 10cm×40mm. Tensile strength was tested using a universal electronic testing machine at a tensile speed of 0.5mm / min.
[0076] Electrical conductivity: The electrical conductivity of the high-temperature proton exchange membranes for vehicle fuel cells prepared in Examples 1-3 and Comparative Examples 1-4 was tested using an electrochemical impedance spectroscopy instrument at a temperature of 160°C.
[0077] Anti-attenuation performance test: Using H2 + 1000ppm CO + 5ppm H2S to simulate mixed impurity gas, after continuous operation for 100h, the conductivity retention rate before and after simulation was tested.
[0078] The test results are shown in Table 1 below.
[0079] Table 1. Experimental performance results of Examples 1-3 and Comparative Examples 1-4
[0080] Phosphoric acid adsorption rate (%) Tensile strength (MPa) Electrical conductivity (mS / cm) Conductivity retention rate (%) Example 1 406 21 89.6 97.1 Example 2 430 24 91.2 97.9 Example 3 453 25 91.8 98.3 Comparative Example 1 386 18 87.5 90.8 Comparative Example 2 391 21 87.3 90.2 Comparative Example 3 357 22 79.2 93.1 Comparative Example 4 306 15 72.2 85.9
[0081] TEM analysis was performed on the mesoporous silica prepared in Example 3 before and after modification. The images are shown below. Figure 1 , Figure 2 .Depend on Figure 1 As can be seen, the unmodified SBA-15 type mesoporous silica has clear and regular edges with parallel stripes, and is a typical two-dimensional hexagonal ordered mesoporous structure with uniform pore size; while the modified mesoporous silica retains its pore structure after the modification process, and the pore walls are coated with an organic amine layer without pore collapse.
[0082] Furthermore, as can be seen from the data in Comparative Example 1, compared with Example 3, its phosphoric acid adsorption rate, conductivity, and conductivity retention rate all decreased significantly. This indicates that although the introduction of unmodified mesoporous silica can improve the phosphoric acid adsorption and mechanical properties to a certain extent, due to the lack of imidazole functional sites and covalent interface binding, the phosphoric acid anchoring ability, impurity shielding ability, and conduction stability are still significantly weaker than those of the present invention.
[0083] Comparative Example 2 data shows that only epoxy grafting was completed without imidazoleization and aldehyde modification, which cannot achieve strong phosphate anchoring and covalent copolymerization reinforcement, making it difficult to fundamentally solve the problems of phosphate loss and impurity tolerance.
[0084] Comparative Example 3 uses non-mesoporous nano-silica. Compared with Example 3, the ordered pore structure of mesoporous silica provides better phosphoric acid adsorption, proton transport and impurity sieving capabilities than the non-porous structure of nano-silica, making it more suitable as a functional filler for high-temperature proton exchange membranes.
[0085] In contrast, no modified mesoporous silica was added in Comparative Example 4, and the data showed a comprehensive decline. This indicates that the introduction of modified mesoporous silica in this invention can simultaneously achieve a comprehensive improvement in phosphoric acid immobilization capacity, mechanical properties, proton conduction properties, and impurity resistance.
[0086] Using the high-temperature proton exchange membrane for vehicle fuel cells prepared in Example 3 as raw material, membrane electrode assemblies were prepared according to the following method:
[0087] A. Catalyst slurry preparation;
[0088] Based on an anode catalyst loading of 0.5 mg Pt / cm³ 2 The cathode catalyst loading is 1.0 mg Pt / cm³. 2 The catalyst slurry was prepared in proportion, using Zhongzi Technology 60-120D as the catalyst raw material and isopropanol aqueous solution as the solvent. The volume ratio of isopropanol to water was 3:1. After mixing the catalyst with isopropanol aqueous solution, it was ultrasonically dispersed in an ice-water bath for 0.5 h. Then, 20% of the total mass of PTFE was added, and ultrasonic dispersion was continued for another 0.5 h to obtain the catalyst slurry.
[0089] B. Preparation of gas diffusion electrode;
[0090] Carbon cloth was used as raw material and cut to prepare a gas diffusion layer of 5.5cm×5.5cm. The catalyst slurry was sprayed onto the surface of the gas diffusion layer using a spray gun. After the solvent was evaporated by heating at 65°C, it was placed in a tube furnace and heated at 350°C for 0.5h under a nitrogen atmosphere to obtain a gas diffusion electrode.
[0091] C. Hot pressing;
[0092] After cutting the insulating frame and the high-temperature proton exchange membrane for vehicle fuel cells prepared in Example 3, they are stacked in the order of gas diffusion electrode - insulating frame - high-temperature proton exchange membrane for vehicle fuel cells - insulating frame - gas diffusion electrode. After hot pressing for 5 minutes at a hot pressing temperature of 150°C and a hot pressing pressure of 1MPa, the membrane electrode assembly is obtained.
[0093] Polarization curves were tested on the above-mentioned membrane electrode assembly under operating conditions of 175℃ and 0% relative humidity. The test results are shown below. Figure 3 .
[0094] Depend on Figure 3As can be seen from the above, the high-temperature proton exchange membrane for vehicle fuel cells prepared in Example 3 of this invention operates stably in a dry, unhumidified environment at 175°C, eliminating the need for a complex water management system and not relying on hydrated proton conduction. It is naturally suited for scenarios involving reformed hydrogen, waste heat coupling, and the absence of a complex water management system. The high-temperature proton exchange membrane prepared by this invention significantly outperforms pure polyquinoxaline membranes, unmodified mesoporous silica-doped membranes, epoxy-grafted mesoporous silica-doped membranes, and nano-silica-doped membranes in terms of phosphoric acid adsorption rate, tensile strength, conductivity, and conductivity retention. This demonstrates that this invention, through stepwise functionalization modification of mesoporous silica, covalent in-situ copolymerization, imidazole-strengthened phosphorus fixation, and the design of a dense cross-linked anti-impurity network, effectively overcomes the technical defects of traditional high-temperature proton exchange membranes, such as weak phosphoric acid fixation capacity, poor mechanical properties, low proton conductivity, and insufficient impurity resistance.
[0095] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A high temperature proton exchange membrane for vehicular fuel cells, characterized by: The high-temperature proton exchange membrane for vehicle-mounted fuel cells comprises a polyquinoxaline matrix and modified mesoporous silica dispersed in the polyquinoxaline matrix; the proton exchange membrane is also doped with phosphoric acid; The surface of the modified mesoporous silica is bridged with imidazole groups via silane coupling agent residues. The silane coupling agent residues are bonded to the surface of the modified mesoporous silica via Si-O-Si bonds and connected to imidazole phenoxy groups via ether bonds. The modified mesoporous silica is covalently linked to the molecular chain of polyquinoxaline via imine bonds.
2. A method for producing a high-temperature proton exchange membrane for a vehicle-mounted fuel cell as claimed in claim 1, characterized by, Includes the following steps: S1. Activate mesoporous silica by heating, add hydrochloric acid solution, acid-activate, centrifuge and filter, wash until neutral, and then dry. The obtained product was added to anhydrous toluene, then KH560 was added for grafting treatment, centrifuged and dried to obtain epoxy-grafted mesoporous silica. S2. Epoxy-grafted mesoporous silica, 4-(imidazol-1-yl)phenol and anhydrous toluene were mixed and heated under nitrogen protection. After centrifugation, washing and drying, the product was mixed with glyoxal, anhydrous ethanol and triethylamine, heated and reacted again, centrifuged, washed and dried to obtain modified mesoporous silica. S3. Modified mesoporous silica, 1,4-bis(phenyloxoyl)benzene and 3,3'-diaminobenzidine are mixed, m-cresol is added, the mixture is heated and reacted, the mixture is added to ethanol, the precipitate is collected, washed and dried, and the dried product is dissolved in dimethyl sulfoxide to obtain modified polyquinoxaline casting solution. S4. The modified polyquinoxaline casting solution is cast and dried to form a film, which is then cured by vacuum heating and cooled. The film is then immersed in a phosphoric acid solution for adsorption to obtain a high-temperature proton exchange membrane for vehicle fuel cells.
3. The method for preparing the high-temperature proton exchange membrane for vehicle-mounted fuel cells according to claim 2, characterized in that: In S1, during heating activation, the temperature is increased to 500-550℃ at a rate of 2-5℃ / min and held for 2-3 hours; For acid activation, heat to 95-100℃ and reflux with stirring for 4-6 hours; the concentration of hydrochloric acid solution is 4.5-5 mol / L. During grafting, the temperature is raised to 80~100℃ and the reaction is stirred for 12~24 hours.
4. The method for preparing the high-temperature proton exchange membrane for vehicle-mounted fuel cells according to claim 2, characterized in that: In S1, the mass ratio of mesoporous silica, hydrochloric acid solution and KH560 is 5:(30~50):(0.5~3).
5. The method for preparing a high-temperature proton exchange membrane for an on-board fuel cell according to claim 2, characterized in that: In S2, the mass ratio of epoxy-grafted mesoporous silica, 4-(imidazol-1-yl)phenol, glyoxal, and triethylamine is 5: (0.1~1.2): (0.5~2): (0.1~0.3).
6. The method for preparing the high-temperature proton exchange membrane for vehicle-mounted fuel cells according to claim 2, characterized in that: In S2, during the first heating reaction, the temperature is raised to 75~85℃ and the reaction is stirred for 8~10 hours; during the second heating reaction, the temperature is raised to 65~68℃ and the reaction is stirred for 8~12 hours.
7. The method for preparing a high-temperature proton exchange membrane for an on-board fuel cell according to claim 2, characterized in that: In S3, the molar ratio of 1,4-bis(phenyloxo)benzene to 3,3'-diaminobenzidine is 1:(0.8~1.05).
8. The method for preparing a high-temperature proton exchange membrane for an on-board fuel cell according to claim 2, characterized in that: In S3, the amount of modified mesoporous silica added is 3 to 8 wt% of the total mass of 1,4-bis(phenyloxo)benzene and 3,3'-diaminobenzidine.
9. The method for preparing a high-temperature proton exchange membrane for an on-board fuel cell according to claim 2, characterized in that: In S3, during the heating reaction, the temperature is raised to 60~80℃ and the reaction is carried out for 24~36h; the solid content of the modified polyquinoxaline casting solution is 5~12wt%.
10. The method for preparing a high-temperature proton exchange membrane for an on-board fuel cell according to claim 2, characterized in that: In S4, the drying temperature during the casting and drying process is 100~125℃. During vacuum heating curing, the temperature is raised to 350~400℃ in a vacuum environment and held for 0.5~1h; The phosphoric acid solution concentration is 60~85wt%, and phosphoric acid adsorption is completed after the membrane weight is constant.