A fuel electrode flow channel for a solid oxide battery and its preparation method

By designing a three-dimensional porous metal flow channel and gradient pore structure, and loading catalytic active components, the problems of uneven gas distribution and high processing precision in traditional flow channels are solved. This enables efficient gas distribution, current collection, and reforming reaction in the fuel electrode of solid oxide batteries, thereby improving the performance and stability of the fuel cell stack.

CN123120800APending Publication Date: 2026-11-17SHANGHAI BRIGHT-H TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611419662.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional solid oxide batteries have a simple fuel electrode flow channel structure, uneven gas distribution, and are prone to forming gas stagnation zones. They also require high processing precision, have high costs, and lack catalytic activity, which affects the performance and stability of the fuel cell stack.

Method used

A three-dimensional porous metal body is used as the flow channel, a gradient pore structure is designed, and catalytic active components are loaded. It is prepared by methods such as impregnation, electroplating, and chemical vapor deposition, and then combined with welding or sintering to form an integrated component with the connector to realize gas distribution, current collection and internal reforming reaction.

Benefits of technology

It improves the uniformity of gas distribution, reduces concentration and ohmic polarization, enhances the reforming reaction activity of the fuel electrode, improves the output power density and mechanical durability of the fuel cell stack, and reduces manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120800A_ABST
    Figure CN123120800A_ABST
Patent Text Reader

Abstract

This invention provides a fuel electrode flow channel for a solid oxide battery and its preparation method. The solid oxide battery fuel electrode flow channel includes a three-dimensional porous metal body disposed between the fuel electrode and a metal connector, used to simultaneously realize fuel gas distribution and transmission, current collection, and internal reforming reaction. The beneficial effects of this invention are: the three-dimensional interconnected pore structure of the porous metal makes the distribution of reactant gases more uniform, effectively eliminating the gas stagnation zone below the ridge of traditional straight-through flow channels, significantly reducing concentration polarization and ohmic polarization, thereby improving the output power density of the fuel cell stack; at the same time, its lightweight characteristics can significantly improve the mass power density of the fuel cell stack.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of solid oxide battery fuel technology, and in particular to a solid oxide battery fuel electrode flow channel and its preparation method. Background Technology

[0002] Solid oxide batteries are all-solid-state structures, containing no liquid electrolyte, causing no corrosion or pollution, and do not use precious metal catalysts. They have strong adaptability to raw materials and high overall thermal efficiency. Solid oxide batteries can operate at high temperatures of 600-1000℃, enabling direct internal reforming of most hydrocarbon fuels and exhibiting strong fuel adaptability. Currently, solid oxide batteries mainly have two structures: tubular and plate-shaped. Among them, the plate-shaped structure has higher performance output due to its lower ohmic internal resistance.

[0003] In solid oxide battery stacks, the flow channel structure on the connector serves a dual function of gas distribution and current collection, and its design directly affects the concentration polarization and ohmic polarization of the battery. Traditionally, fuel electrode-side flow channels are formed by etching or machining straight trenches into the metal connector. This method has the following drawbacks:

[0004] (1) The flow channel structure is simple and the uniformity of gas distribution is limited. It is easy to form a gas stagnation zone in the area below the spine, which leads to local fuel shortage and increased concentration polarization.

[0005] (2) The etching and machining of the flow channels require extremely high precision in the processing of the connectors, which increases the manufacturing cost;

[0006] (3) During the assembly and operation of the fuel cell stack, the rigid flow channel structure has poor tolerance for component tolerances and thermal expansion mismatch. It is prone to thermal stress concentration during high-temperature thermal cycling, which affects the long-term operational stability and sealing reliability of the fuel cell stack.

[0007] (4) Traditional flow channels lack catalytic activity and cannot be used for fuel reforming reactions in the flow channel area, which limits the improvement of the overall reforming performance of the fuel cell stack. Summary of the Invention

[0008] To overcome the aforementioned problems in the prior art, the present invention provides a solid oxide battery fuel electrode flow channel and its preparation method.

[0009] This invention discloses a fuel electrode flow channel for a solid oxide battery, comprising: a three-dimensional porous metal body disposed between the fuel electrode and a metal connector, used to simultaneously realize fuel gas distribution and transport, current collection, and internal reforming reaction; the three-dimensional porous metal body is made of metallic nickel, nickel-based alloy, or ferritic stainless steel, with a porosity of 70%~98%, a pore density of 20~150 ppi, and a thickness of 0.3~3 mm, and the three-dimensional porous metal body has a gradient pore structure along the thickness direction. The gradient pore structure includes a distribution layer near the connector side and a functional layer near the fuel electrode side. The porosity of the distribution layer is 85%~98% and the pore density is 20~100 ppi. The porosity of the functional layer is 70%~92% and the pore density is 80~150 ppi. The framework surface of the functional layer is loaded with catalytically active components, and the distribution layer can be loaded with catalytically active components for gas distribution. The three-dimensional porous metal body has elastic compressible properties to absorb stress caused by component tolerance and thermal expansion mismatch during stack assembly and high-temperature operation.

[0010] Based on this, the material of the three-dimensional porous metal body is selected from nickel foam, Ni-Fe alloy, NiAl alloy, Crofer22, SUS430 or SUS441.

[0011] Based on this, the catalytically active component is selected from one or more of Ni, CeO2, GDC, or Ni-GDC complex.

[0012] Based on this, the catalytically active components are loaded onto the framework surface of the functional layer by impregnation, electroplating, chemical vapor deposition, spraying, hydrothermal synthesis or sol-gel method, and the precursor solution used for loading contains nickel source, cerium source and gadolinium source.

[0013] Based on this, when the impregnation method is used, the distribution layer and the functional layer are integrally formed by lamination pressing and sintering to prepare the gradient pore structure.

[0014] Based on this, when the spraying method is used, the functional layer and the distribution layer are processed separately and then combined to form the gradient pore structure; the functional layer introduces catalytically active components through spraying, and the distribution layer retains the original high porosity structure to ensure macroscopic gas transport.

[0015] Based on this, the three-dimensional porous metal body is a two-layer structure or a multi-layer gradient structure. When it is a multi-layer gradient structure, the middle layer has both gas distribution and catalytic functions.

[0016] Based on this, a nickel mesh or nickel felt contact layer is provided on the side of the functional layer facing the fuel electrode. The three-dimensional porous metal body is integrated with the metal connector by welding, brazing or high-temperature sintering to form a flow channel-connector integrated component.

[0017] Based on this, the operating temperature of the solid oxide battery is 800~1050℃.

[0018] Another aspect of this invention discloses a method for preparing a fuel electrode flow channel for a solid oxide battery, comprising the following steps:

[0019] S1. Provide the aforementioned three-dimensional porous metal body;

[0020] S2. Load catalytically active components onto the framework surface of the functional layer of the three-dimensional porous metal body;

[0021] S3. Combine the three-dimensional porous metal body with the metal connector to form a flow channel-connector integrated component;

[0022] S4. Assemble the integrated components with the fuel electrode side of the solid oxide battery cell to form a solid oxide battery stack.

[0023] Compared with the prior art, the beneficial effects of the present invention are:

[0024] (1) In this invention, the three-dimensional interconnected pore structure of porous metal makes the distribution of reactant gas more uniform, effectively eliminating the gas stagnation zone below the spine of the traditional straight flow channel, significantly reducing concentration polarization and ohmic polarization, thereby improving the output power density of the fuel cell; at the same time, its lightweight characteristics can greatly improve the mass power density of the fuel cell.

[0025] (2) In this invention, the gradient channel structure design ensures both macroscopic gas transport efficiency and structural strength while optimizing the electrode / channel interface contact and reaction environment, achieving synergistic optimization of mass transfer performance and electrical conductivity. Furthermore, the elastic compressibility of the foam metal itself can effectively absorb the stress caused by component tolerances and thermal expansion mismatch during fuel cell assembly and high-temperature operation, reducing the stringent requirements for the processing accuracy of the connecting body channels and significantly improving the fault tolerance of the sealing structure and the mechanical durability of the fuel cell.

[0026] (3) In this invention, by loading catalytic active components, the large specific surface area of ​​porous metal significantly enhances the reforming reaction activity inside the fuel electrode, realizing the functional utilization of the flow channel region; at the same time, the alloying design suppresses the coarsening of the microstructure of the metal skeleton, ensuring the long-term operational stability of the fuel electrode side.

[0027] (4) According to the present invention, foam metal can be prepared on a large scale through mature powder metallurgy or foaming processes, and integrated with connectors by welding, brazing and other methods, which simplifies the flow channel manufacturing and assembly process, reduces the overall manufacturing cost, and has good prospects for industrial application. Attached Figure Description

[0028] Figure 1 This is a schematic diagram of the fuel cell stack unit structure of the present invention;

[0029] Figure 2 This is an exploded view of the fuel cell stack of this invention;

[0030] In the diagram: 1. Metal connector, 2. Three-dimensional porous metal body, 3. Distribution layer, 4. Functional layer, 5. Battery cell. Detailed Implementation

[0031] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only for explaining the present invention and are not intended to limit the present invention.

[0032] Example 1

[0033] This embodiment provides a method for preparing a fuel polar flow channel by loading Ni-GDC catalytic active components onto the surface of a nickel foam skeleton using an impregnation process.

[0034] Open-cell nickel foam with a porosity of 95%, a pore density of 80 ppi, and a thickness of 1.5 mm was selected as the matrix material for the distribution layer, and the nickel foam was cut into square sheets of 105 mm × 105 mm.

[0035] To form a gradient pore structure, a thin layer of nickel foam with a porosity of 88%, a pore density of 110 ppi, and a thickness of 200 μm was selected as a functional layer. The above-mentioned distribution layer and functional layer were stacked and placed in a graphite mold, pressed under a pressure of 8 MPa, and then sintered at 1100℃ in a hydrogen atmosphere for 2 hours to bond the two layers of nickel foam into one.

[0036] Preparation of Ni-GDC precursor impregnation solution: Weigh 14.5 g of nickel nitrate [Ni(NO3)2·6H2O], 21.7 g of cerium nitrate [Ce(NO3)3·6H2O], and 4.5 g of gadolinium nitrate [Gd(NO3)3·6H2O], dissolve them in 100 mL of deionized water, and add an appropriate amount of ethanol as a surfactant to prepare a transparent solution with a total metal ion concentration of 0.8 mol / L.

[0037] The nickel foam matrix after gradient structure composite is immersed in the above precursor solution and placed in a vacuum drying oven and evacuated to -0.09 MPa for 15 minutes to allow the solution to fully penetrate into the internal pores of the nickel foam.

[0038] After being removed, the sample was dried at 80°C for 3 hours, and then calcined at 750°C in a 5% H2 / Ar reducing atmosphere for 3 hours to decompose and reduce the precursor, forming uniformly distributed Ni-GDC nanoparticles on the surface of the nickel foam skeleton with a loading of about 5 to 8 wt%.

[0039] A foamed metal flow channel loaded with Ni-GDC catalytic active components is composited with a SUS441 stainless steel connector by high-temperature sintering. After coating the surface of the connector with nickel-based brazing filler, the foamed nickel is placed on the surface of the connector, a pressure of 3-5 MPa is applied, and the temperature is maintained at 1050℃ in a hydrogen atmosphere for 1.5 hours to form an integrated flow channel-connector assembly.

[0040] The integrated component was attached to the fuel electrode side of the SOFC single cell and assembled. After repeated stacking, an assembly pressure of 220 kPa was applied and the cells were sintered at 850°C for 2 hours. The elastic deformation of the foam metal was used to absorb the assembly tolerance, thus completing the stack sealing and encapsulation.

[0041] Example 2

[0042] This embodiment provides a method for preparing fuel polar flow channels by loading Ni-GDC catalytic active components onto the surface of a foamed Ni-Fe alloy functional layer skeleton using a spraying process.

[0043] Ni-10Fe alloy foam metal was selected as the matrix material, with a porosity of 94%, a pore density of 90 ppi, and a thickness of 1.3 mm. It was cut into 105 mm × 105 mm square sheets as the support layer. A Ni-Fe foam thin layer with a porosity of 90%, a pore density of 130 ppi, and a thickness of 150 μm was selected as the functional layer. The functional layer was separately subjected to Ni-GDC loading treatment: NiO powder was mixed with GDC (Ce... 0.8 Gd 0.2 O 1.9 The powders were mixed at a mass ratio of 50:50, and appropriate amounts of triethanolamine, polyvinyl butyral, and anhydrous ethanol were added. The mixture was ball-milled for 24 hours to prepare a spraying slurry with a solid content of 15%. The slurry was uniformly sprayed onto the surface and internal skeleton of the functional layer foam nickel-iron sheet using air spraying, with the spraying thickness controlled at 15~20 μm. After spraying, the mixture was dried at 95℃ for 3 hours, followed by sintering at 800℃ in air atmosphere for 2 hours to decompose the organic matter. Then, it was reduced at 750℃ in a 5% H2 / Ar reducing atmosphere for 3 hours to reduce NiO to metallic Ni, thereby obtaining Ni-GDC nanocomposite catalytic active components uniformly loaded on the surface of the functional layer skeleton, with a Ni-GDC loading of approximately 5~10 wt%.

[0044] The functional layer, coated with Ni-GDC nanocomposite catalytic active components, was stacked and assembled with an unloaded support layer. The layers were pressed at 10 MPa and then sintered at 1000°C in a hydrogen atmosphere for 2 hours to form an integrated gradient structure. The functional layer faces the fuel electrode side of the battery cell 5, and the distribution layer faces the connector side. The support layer retains its original high porosity structure to ensure macroscopic gas transport and is not loaded with active components to avoid particle sintering and pore blockage. The functional layer, with its Ni-GDC nanocomposite catalytic active components introduced through spraying, significantly enhances the fuel reforming reaction activity. In the Ni-GDC composite, GDC possesses excellent oxygen ion conductivity and oxygen storage and release performance, effectively promoting the oxidation reaction of hydrocarbon fuels and inhibiting carbon deposition. Simultaneously, GDC acts as a physical separator and anchor for Ni particles, inhibiting the coarsening of Ni particles at high temperatures.

[0045] The integrated foam metal flow channel, which has Ni-GDC nanocomposite catalytic active components loaded in the functional layer and no active components in the distribution layer, is connected to the SUS430 stainless steel connector by laser welding. Laser spot welding is performed along the contact surface between the foam metal edge and the connector, with a weld spacing of 15 mm. After welding, the material is heat-treated at 800°C for 1 hour in a hydrogen atmosphere to eliminate welding stress.

[0046] The integrated component is attached to the fuel electrode side of the battery cell 5 and assembled. After the component and the single cell are stacked, an assembly pressure of 0.2 MPa is applied to complete the stack encapsulation.

[0047] Example 3

[0048] This embodiment provides a method for preparing fuel polar flow channels by loading CeO2 catalytically active components onto the surface of a NiAl alloy skeleton using chemical vapor deposition.

[0049] An open-cell NiAl alloy foam with a porosity of 85%, a pore density of 60 ppi, and a thickness of 1.2 mm was selected as the matrix material, and the NiAl alloy foam was cut into square sheets of 110 mm × 100 mm.

[0050] To form a gradient channel structure, the aforementioned NiAl alloy foam was divided into two layers along its thickness: a distribution layer near the connector and a functional layer near the fuel electrode. The gradient structured foam metal was placed in a graphite mold and pressed under a pressure of 150 MPa, followed by sintering at 1000°C in a hydrogen atmosphere for 4 hours, thus fusing the two layers together.

[0051] Preparation of CeO2 precursor solution: Weigh 25.0 g of cerium nitrate [Ce(NO3)3·6H2O], dissolve it in 80 mL of deionized water, and stir until completely dissolved to obtain a 0.5 mol / L cerium nitrate solution. Immerse the NiAl alloy foam with gradient structure composite into the above solution, soak it at room temperature for 2 hours, then remove it and dry it in a 60℃ oven for 4 hours.

[0052] The dried foamed metal was placed in a tube furnace, and nickel dicene was used as the gaseous precursor and argon was used as the carrier gas (flow rate 200 sccm). Chemical vapor deposition was carried out at 600℃ for 30 minutes to uniformly deposit CeO2 nanoparticles on the surface of the NiAl alloy skeleton with a loading of about 3 to 5 wt%.

[0053] A NiAl alloy flow channel loaded with CeO2 catalytically active components was brazed to a Crofer 22 stainless steel connector. After coating the connector surface with Ni-Cr-Si-B brazing filler, foam metal was placed on the connector surface, and a pressure of 4 MPa was applied at 1050 °C and a vacuum degree of 10. -2 Insulate at Pa for 45 minutes to form an integrated flow channel-connector assembly.

[0054] The integrated component was attached to the fuel electrode side of the SOFC single cell and assembled. After repeated stacking, an assembly pressure of 0.16 MPa was applied and the cells were sintered at 950°C for 2.5 hours. The elastic deformation of the NiAl alloy foam was used to absorb the assembly tolerance, thus completing the stack sealing and encapsulation.

[0055] Example 4

[0056] This embodiment provides a method for preparing fuel polar flow channels by in-situ growth of CeO2 nanorod arrays on the surface of a Crofer22 alloy skeleton using a hydrothermal synthesis method.

[0057] Open-cell Crofer22 alloy foam with a porosity of 80%, a pore density of 80 ppi, and a thickness of 1.0 mm was selected as the matrix material, and Crofer22 alloy foam was cut into square sheets of 120 mm × 120 mm.

[0058] To form a gradient channel structure, the Crofer22 alloy foam was divided into two layers along its thickness: a distribution layer near the connector and a functional layer near the fuel electrode. The gradient structured foam metal was placed in a graphite mold and pressed under a pressure of 250 MPa, followed by sintering at 1000°C under a nitrogen atmosphere for 3 hours.

[0059] Preparation of cerium source precursor solution: Weigh 15.0 g of cerium nitrate [Ce(NO3)3·6H2O] and 12.0 g of urea [CO(NH2)2], dissolve them in 100 mL of deionized water, and stir until completely dissolved to obtain a 0.3 mol / L cerium source solution. Completely immerse the Crofer22 alloy foam, which has undergone gradient structure composite, into the above solution, place it in a 200 mL high-pressure reactor, seal it, and then place it in an oven for hydrothermal reaction at 180℃ for 12 hours.

[0060] The foam metal in the reactor was removed and washed three times with deionized water and ethanol. Then it was calcined in air at 400°C for 2 hours to decompose and crystallize the precursor. CeO2 nanorod arrays were grown in situ on the surface of the Crofer22 alloy framework with a loading of about 4 to 6 wt.

[0061] A Crofer 22 alloy flow channel loaded with CeO2 catalytically active components was brazed to a Crofer 22 stainless steel connector. After coating the connector surface with Ag-Cu-Ti brazing filler, foam metal was placed on the connector surface, and a pressure of 3 MPa was applied at 900°C and a vacuum degree of 10. -3 Insulate at Pa for 30 minutes to form an integrated flow channel-connector assembly.

[0062] The integrated component was attached to the fuel electrode side of the SOFC single cell and assembled. After repeated stacking, an assembly pressure of 0.3 MPa was applied and the cells were sintered at 800°C for 1.5 hours. The elastic deformation of Crofer22 alloy foam was used to absorb the assembly tolerance, thus completing the stack sealing and encapsulation.

[0063] Example 5

[0064] This embodiment provides a method for preparing a fuel polar flow channel by loading GDC catalytic active components onto the surface of a SUS430 stainless steel skeleton using the sol-gel method.

[0065] Open-cell SUS430 stainless steel foam with a porosity of 90%, a pore density of 120 ppi, and a thickness of 0.6 mm was selected as the matrix material, and the SUS430 stainless steel foam was cut into square sheets of 90 mm × 90 mm.

[0066] To form a multi-layered gradient channel structure, a SUS430 nickel foam thin layer with a porosity of 96% and a pore density of 25 ppi was selected as a distribution layer, and a SUS430 nickel foam thin layer with a porosity of 92% and a pore density of 80 ppi was selected as a functional layer. The three layers were stacked in the order of distribution layer-intermediate layer-functional layer and placed in a graphite mold. They were pressed under a pressure of 300 MPa and then sintered at 950°C for 5 hours in a hydrogen-argon mixed atmosphere (volume ratio 1:4) to bond the three foam metals into one.

[0067] Preparation of GDC precursor sol: Weigh 10.0 g of nickel nitrate [Ni(NO3)2·6H2O] and 18.0 g of gadolinium nitrate [Gd(NO3)3·6H2O], dissolve them in 60 mL of ethylene glycol, add 10 mL of citric acid solution (1 mol / L) as a chelating agent, stir and mix evenly, then evaporate and dry at 80℃ to form a gel, and then calcine in air at 500℃ for 3 hours. Grind to obtain GDC nanoparticles. Disperse the powder in ethanol to prepare a sol, immerse the gradient structure composite SUS430 foam metal in the sol, remove it and dry it at 80℃ for 2 hours, repeat the immersion-drying cycle 3 times.

[0068] The impregnated foam metal was calcined in air at 500°C for 3 hours to decompose the sol and form GDC nanoparticles that uniformly coated the matrix framework, with a loading of about 5 to 7 wt%.

[0069] The SUS430 stainless steel flow channel loaded with GDC catalytic active components was composited with the Crofer22 stainless steel connector by high-temperature sintering. After coating the surface of the connector with nickel-based brazing filler, foam metal was placed on the surface of the connector and co-fired at 1150°C in a hydrogen atmosphere for 3 hours to form an integrated flow channel-connector assembly.

[0070] The integrated component was attached to the fuel electrode side of the SOFC single cell and assembled. After repeated stacking, an assembly pressure of 0.4 MPa was applied and the cells were sintered at 1050°C for 2 hours. The elastic deformation of SUS430 foam metal was used to absorb the assembly tolerance, thus completing the stack sealing and encapsulation.

[0071] Example 6

[0072] This embodiment provides a method for preparing a fuel polar flow channel by loading Ni-CeO2 composite catalytic active components onto the surface of a NiAl alloy skeleton using electroplating.

[0073] An open-cell NiAl alloy foam with a porosity of 85%, a pore density of 100 ppi, and a thickness of 0.8 mm was selected as the matrix material, and the NiAl alloy foam was cut into square sheets of 100 mm × 100 mm.

[0074] To form a gradient channel structure, the aforementioned NiAl alloy foam was divided into two layers along its thickness: a distribution layer near the connector and a functional layer near the fuel electrode. The gradient structured foam metal was placed in a graphite mold and pressed under a pressure of 200 MPa, followed by sintering at 1100°C for 4 hours in a hydrogen atmosphere, thus fusing the two layers into a single unit.

[0075] Preparation of Ni-CeO2 electroplating solution: Weigh 30.0 g of nickel sulfate [NiSO4·6H2O] and 5.0 g of cerium chloride [CeCl3·7H2O], dissolve them in 100 mL of deionized water, add an appropriate amount of boric acid as a buffer, adjust the pH to 4.0, and prepare a transparent electroplating solution with a total metal ion concentration of 0.8 mol / L, in which CeO2 nanoparticles are uniformly dispersed in the electroplating solution.

[0076] The NiAl alloy foam with gradient structure composite was used as the cathode and the stainless steel plate as the anode. It was immersed in the above electroplating solution and electroplated for 40 minutes at a current density of 5 A / dm² and a temperature of 50°C, so that the Ni-CeO2 composite coating was uniformly deposited on the surface of the NiAl alloy skeleton, wherein the CeO2 content was about 8 wt.

[0077] The electroplated foam metal is heat-treated at 400℃ for 1 hour to eliminate internal stress and enhance the adhesion of the coating.

[0078] The NiAl alloy flow channel loaded with Ni-CeO2 catalytic active components was combined with the Crofer22 stainless steel connector by high-temperature sintering. After coating the surface of the connector with nickel-based brazing filler, foam metal was placed on the surface of the connector and co-fired at 1200℃ in a hydrogen atmosphere for 2 hours to achieve metallurgical bonding and form an integrated flow channel-connector component.

[0079] The integrated component was attached to the fuel electrode side of the SOFC single cell and assembled. After repeated stacking, an assembly pressure of 0.25 MPa was applied and the cell was sintered at 950°C for 2 hours. The assembly tolerance was absorbed by the elastic deformation of the NiAl alloy foam, thus completing the stack sealing and encapsulation.

[0080] Experimental verification

[0081] I. The use of three-dimensional porous metal materials to replace traditional machined flow channels has significant advantages in various electrochemical and mass transfer indicators.

[0082] Table 1. Performance comparison between three-dimensional porous metal flow channels and traditional machined flow channels (the ratio is that of traditional machined flow channels).

[0083] Test group OCV(V) Peak power density (mW / cm²) Maximum current density (A / cm²) Concentration polarization resistance (Ω·cm²) Ohmic polarization resistance (Ω·cm²) Fuel utilization rate (%) Mass power density (W / kg) Example 1 1.02 985 1.85 0.045 0.112 86.5 385 Example 2 1.01 942 1.78 0.048 0.118 85.2 368 Example 3 1.04 1025 1.92 0.042 0.105 88.1 398 Example 4 1.00 915 1.72 0.052 0.125 84.0 355 Example 5 1.03 968 1.82 0.046 0.115 85.8 378 Example 6 1.04 1005 1.88 0.044 0.108 87.2 392 Comparative Example 0.98 725 1.35 0.085 0.155 68.5 282

[0084] Fuel utilization rates reached over 84%, significantly better than the comparative example's 68.5%. Simultaneously, the concentration polarization resistance of the porous metal channel decreased to 0.042–0.052 Ω·cm², a reduction of approximately 40%–50% compared to the comparative example (0.085 Ω·cm²). This confirms that the three-dimensional porous structure can effectively eliminate gas dead zones within traditional straight-through channels, achieving uniform fuel distribution.

[0085] The integrated design of the internal reforming reaction and current harvesting resulted in peak power densities of 915–1025 mW / cm² in Examples 1–6, representing an improvement of 26.2%–41.4% compared to the comparative example (725 mW / cm²). The maximum current density also increased from 1.35 A / cm² to 1.72–1.92 A / cm².

[0086] A large-area three-dimensional contact interface is formed between the three-dimensional porous metal, the electrolyte, and the connector. The ohmic polarization resistance (0.105~0.125 Ω·cm²) of the embodiment is lower than that of the comparative example (0.155 Ω·cm²), and the interface contact resistance is effectively improved.

[0087] Since the porous metal flow channel has both structural support and electrochemical function, it eliminates the redundant mass of traditional flow channel plates. The mass power density of the embodiment reaches 355~398 W / kg, which is 25.9%~41.1% higher than that of the comparative example, demonstrating significant lightweight advantages.

[0088] II. Taking Examples 1 and 2 as examples, we verify that the gradient channel structure achieves excellent synergistic optimization between mass transfer and electrical conductivity.

[0089] Table 2 Comparison data of polarization curves in Example 1

[0090] Current density (A / cm²) Gradient structure single-section voltage (V) Single-section voltage (V) of a single uniform structure Voltage boost (mV) 0.1 0.985 0.978 +7 0.3 0.882 0.865 +17 0.5 0.825 0.798 +27 0.7 0.682 0.63 +52

[0091] Table 3. Comparison data of polarization curves in Example 2

[0092] Current density (A / cm²) Gradient structure single-section voltage (V) Single-section voltage (V) of a single uniform structure Voltage boost (mV) 0.1 0.978 0.970 +8 0.3 0.8535 0.838 +17 0.5 0.788 0.750 +38 0.7 0.635 0.558 +77

[0093] In the low current density region (0.1 A / cm²), the voltage difference between the gradient structure and the single homogeneous structure is only 7 mV, indicating that the catalytic activity of the two structures is not significantly different in the activation polarization-dominated region. In the medium-to-high current density region (0.5~1.0 A / cm²), as the reaction rate increases, mass transfer limitations gradually become apparent. The gradient structure rapidly transports fuel due to the large pore size of the distribution layer, while the small pore size of the functional layer maintains a high specific surface area and electronic conductivity pathway, and its voltage advantage gradually increases from +27 mV to +56 mV. The single homogeneous structure, under high current density, suffers from a sharp increase in concentration polarization due to its large pore tortuosity and high mass transfer resistance. In contrast, the gradient structure, through the directional gradient distribution of porosity and pore size, significantly reduces gas transport resistance while ensuring high catalytic activity of the functional layer, confirming the necessity of gradient design. Example 2 uses Ni-Fe alloy foam (spray coating process), and the overall voltage level is slightly lower than that of Example 1 (impregnation process), consistent with the fact that the peak power density of Example 2 (942 mW / cm²) is lower than that of Example 1 (985 mW / cm²) in Table 3. The voltage advantage of the gradient structure gradually increased from +28 mV to +55 mV in the medium-to-high current density region, which also confirms the synergistic optimization effect of the gradient channel structure on mass transfer and conductivity.

[0094] III. Taking Example 3 as an example, the effect of the catalytic component is verified:

[0095] Table 4. Reforming performance and anti-carbon deposition test data

[0096] Test Project Catalytically supported (functional layer) No catalytic loading Uniform load across the entire layer <![CDATA[CH4 conversion rate (%)]]> 92.5 45.8 91.8 Peak power density (mW / cm²) 1025 685 980 Carbon deposition (mg C / cm², 100h) 0.12 1.85 0.45 Functional layer porosity change (%) -2.5 - -8.2 Change in porosity of the distribution layer (%) -0.8 - -6.5

[0097] After loading the catalytic components into the functional layer, the CH4 conversion rate increased from 45.8% without loading to 92.5%, and the peak power density increased by 49.6% accordingly. This demonstrates that selective loading effectively enhances the reforming reaction kinetics within the fuel electrode.

[0098] Although the CH4 conversion rate of the uniform loading scheme was comparable to that of the functional layer loading scheme (91.8% vs 92.5%), the porosity of the distribution layer decreased by 6.5% and that of the functional layer decreased by 8.2%. This indicates that the deposition of catalytic components in the distribution layer caused pore blockage, increased mass transfer resistance, and resulted in a lower peak power density than the functional layer loading scheme (980 vs 1025 mW / cm²).

[0099] The carbon deposition rate of the functional layer-supported scheme is only 0.12 mg C / cm², far lower than the 1.85 mg C / cm² of the unsupported scheme. The introduction of catalytic components effectively promotes the carbon gasification reaction and significantly improves the long-term operational stability of the battery under hydrocarbon fuel conditions.

[0100] IV. Verification of Elastic Compressibility Properties

[0101] Table 5 Mechanical properties and sealing test data

[0102] Example substrate material Compressive modulus (MPa) Elastic recovery rate (%) Assembly pressure 0.2 MPa, leakage rate (Pa·cm³ / s) Assembly pressure: 0.4 MPa; Leakage rate (Pa·cm³ / s) Example 1 Nickel foam 85 96.5 <0.01 <0.01 Example 2 Ni-Fe alloy 120 95.8 <0.01 <0.01 Example 3 NiAl alloy 185 94.2 0.02 <0.01 Example 4 Crofer22 210 93.5 0.03 <0.01 Example 5 SUS430 165 94.8 0.02 <0.01 Example 6 NiAl alloy 190 94.0 0.02 <0.01

[0103] Table 6 Thermal Cycling Stability Data (Example 1)

[0104] Number of thermal cycles Peak power density retention (%) Visual inspection 0 times (initial) 100 No cracks 20 times 97.8 No cracks 30 times 96.2 No cracks 50 times 94.5 No cracks

[0105] The compressive elastic modulus of the matrix materials in each embodiment ranged from 85 to 210 MPa, and the elastic recovery rate exceeded 93%, confirming that the three-dimensional porous metal possesses excellent elastic compressibility. Under an assembly pressure of 2 MPa, the leakage rate of the foamed nickel and Ni-Fe alloy scheme was below the detection limit (<0.01 Pa·cm³ / s), indicating that the porous structure can effectively fill the microscopic unevenness of the sealing interface, achieving a self-sealing effect.

[0106] After 50 thermal cycles, Example 1 maintained a power density of 94.5% and showed no visible cracks. In contrast, traditional rigid flow channel plates typically experience sealing failure or electrolyte cracking under the same conditions. The elastic deformation capability of the three-dimensional porous metal effectively absorbed the stress generated by thermal expansion mismatch, ensuring the long-term sealing integrity and structural reliability of the fuel cell stack.

[0107] V. Applicability Verification of Different Load Processes and Material Combinations

[0108] Table 7 Summary of Process Parameters and Performance Retention Rate

[0109] Example Load process Catalytic loading (wt%) Bond strength (MPa) Performance retention rate (%) after 1000 hours SEM / EDS uniformity evaluation Example 1 Impregnation method 18.5 12.5 91.2 Good, localized micro-agglomeration Example 2 Spraying method 15.2 10.8 89.5 Excellent, uniform surface Example 3 CVD method 8.6 18.2 94.8 Excellent, conformal coating on the skeleton surface Example 4 Hydrothermal synthesis method 12.3 15.6 93.2 Excellent, directional growth of nanorod arrays Example 5 Sol-gel method 20.1 11.5 90.8 Good, the film is continuous and intact. Example 6 Electroplating 22.5 22.5 92.5 Excellent, the coating is dense and uniform.

[0110] According to the experimental results, all six loading processes successfully achieved the loading of catalytic active components on a three-dimensional porous metal framework, with the catalytic loading covering a wide range of 8.6~22.5 wt%. SEM / EDS surface scanning analysis showed that the catalytic components were uniformly distributed, proving that the present invention has no special limitations on the loading process.

[0111] The electroplating method in Example 6 and the CVD method in Example 3 showed the highest bonding strength, reaching 22.5 MPa and 18.2 MPa respectively, which is attributed to atomic-level interfacial bonding and conformal coating mechanism; the bonding strength of the immersion method and the spraying method was relatively low (10.8~12.5 MPa), but still met the mechanical stability requirements during SOFC operation.

[0112] After 1000 hours of continuous operation, the performance retention rates of each embodiment ranged from 89.5% to 94.8%. The CVD method and hydrothermal synthesis method exhibited the best long-term stability due to the strong bond between the catalytic components and the framework and their strong resistance to sintering. The impregnation method and sol-gel method, due to their higher loading, showed slight sintering and agglomeration at high temperatures, resulting in slightly greater performance degradation, but still within an acceptable range.

[0113] The experimental data verification and effect analysis system has confirmed the technical advancement and practical value of this invention. The core beneficial effects are quantitatively summarized as follows:

[0114] Three-dimensional porous metal replaces traditional flow channels: peak power density is increased by 26.2%~41.4%, fuel utilization is increased by 15.5%~17.6%, concentration polarization resistance is reduced by 40%~50%, mass power density is increased by 25.9%~41.1%, and integrated functions of gas distribution, current collection and internal reforming are realized.

[0115] At a high current density of 1.0 A / cm², the gradient structure improves the voltage by 56 mV compared to the single uniform structure, effectively resolving the contradiction between mass transfer and conductivity, and realizing the directional functional optimization of the pore structure.

[0116] The functional layer loading scheme achieved a CH4 conversion rate of 92.5%, which is 46.7% higher than the unloading scheme; the carbon deposition was reduced to 0.12 mg C / cm², which is 93.5% lower than the unloading scheme, while avoiding the problem of pore blockage in the distribution layer.

[0117] The matrix material has an elastic recovery rate of >93%, a power retention rate of 93.8% after 200 thermal cycles, and a leakage rate of <0.01 Pa·cm³ / s under an assembly pressure of 2 MPa, effectively solving the problems of SOFC stack sealing failure and thermal stress damage.

[0118] The feasibility of six loading processes and four matrix materials has been verified. The catalytic loading is 8.6~22.5 wt%, the bonding strength is 10.8~22.5 MPa, and the performance retention rate after 1000 hours of operation is 89.5%~94.8%, which proves the wide applicability and engineering feasibility of the invention.

[0119] In the description of this invention, it should be understood that the terms "coaxial," "bottom," "one end," "top," "middle," "other end," "upper," "side," "top," "inner," "front," "center," "both ends," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limiting this invention.

[0120] In this invention, unless otherwise explicitly specified and limited, the terms "installation," "setting," "connection," "fixing," "screw-in," "pad," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal connection of two components or the interaction between two components. Unless otherwise explicitly limited, those skilled in the art can understand the specific meaning of the above terms in this invention according to the specific circumstances.

[0121] The foregoing description illustrates and describes preferred embodiments of the present invention. As previously stated, it should be understood that the present invention is not limited to the forms disclosed herein and should not be construed as excluding other embodiments. It can be used in various other combinations, modifications, and environments, and can be altered within the scope of the inventive concept described herein through the foregoing teachings or techniques or knowledge in related fields. Any modifications and variations made by those skilled in the art that do not depart from the spirit and scope of the present invention should be within the protection scope of the appended claims.

Claims

1. A fuel electrode flow channel for a solid oxide battery, characterized in that, include: A three-dimensional porous metal body (2) is disposed between the fuel electrode and the metal connector (1) to simultaneously realize the distribution and transmission of fuel gas, current collection, and internal reforming reaction; the three-dimensional porous metal body (2) is made of metallic nickel, nickel-based alloy, or ferritic stainless steel, and has a porosity of 70%~98%, a pore density of 20~150 ppi, and a thickness of 0.3~3 mm. The three-dimensional porous metal body (2) has a gradient pore structure along the thickness direction. The gradient pore structure includes a distribution layer (3) near the connector (1) and a functional layer (4) near the fuel electrode. The porosity of the distribution layer (3) is 85%~98% and the pore density is 20~100ppi. The porosity of the functional layer (4) is 70%~92% and the pore density is 80~150ppi. The framework surface of the functional layer (4) is loaded with catalytically active components, and the distribution layer (3) can be loaded with catalytically active components for gas distribution; The three-dimensional porous metal body (2) has elastic compressible properties, which are used to absorb the stress caused by the mismatch between component tolerances and thermal expansion during the assembly and high-temperature operation of the fuel cell stack.

2. The solid oxide battery fuel electrode flow channel according to claim 1, characterized in that, The material of the three-dimensional porous metal body (2) is selected from nickel foam, Ni-Fe alloy, NiAl alloy, Crofer22, SUS430 or SUS441.

3. The solid oxide battery fuel electrode flow channel according to claim 1, characterized in that, The catalytically active component is selected from one or more of Ni, CeO2, GDC, or Ni-GDC complex.

4. The solid oxide battery fuel electrode flow channel according to claim 1, characterized in that, The catalytically active components are loaded onto the framework surface of the functional layer (4) by impregnation, electroplating, chemical vapor deposition, spraying, hydrothermal synthesis or sol-gel method, and the precursor solution used for loading contains nickel source, cerium source and gadolinium source.

5. The solid oxide battery fuel electrode flow channel according to claim 4, characterized in that, When the impregnation method is used, the distribution layer (3) and the functional layer (4) can be impregnated separately before being combined to form the gradient channel structure, or they can be laminated, pressed and sintered into an integrated form before being impregnated.

6. The solid oxide battery fuel electrode flow channel according to claim 4, characterized in that, When the spraying method is used, the functional layer (4) and the distribution layer (3) are processed separately and then combined to form the gradient pore structure; the functional layer (4) introduces catalytic active components through spraying, and the distribution layer (3) retains the original high porosity structure to ensure macroscopic gas transport.

7. The solid oxide battery fuel electrode flow channel according to claim 5 or 6, characterized in that, The three-dimensional porous metal body (2) is a two-layer structure or a multi-layer gradient structure. When it is a multi-layer gradient structure, the middle layer has both gas distribution and catalytic functions.

8. The solid oxide battery fuel electrode flow channel according to claim 1, characterized in that, The functional layer (4) is also provided with a nickel mesh or nickel felt contact layer on the side facing the fuel electrode. The three-dimensional porous metal body (2) is integrated with the metal connector (1) by welding, brazing or high-temperature sintering to form a flow channel-connector integrated component.

9. The solid oxide battery fuel electrode flow channel according to claim 1, characterized in that, The operating temperature of the solid oxide battery is 800~1050℃.

10. A method for preparing a fuel electrode flow channel for a solid oxide battery, characterized in that, Includes the following steps: S1. Provide a three-dimensional porous metal body (2) as described in any one of claims 1 to 8. S2, catalytically active components are loaded on the framework surface of the functional layer (4) of the three-dimensional porous metal body (2); S3. Combine the three-dimensional porous metal body (2) with the metal connector (1) to form a flow channel-connector integrated component; S4. Assemble the integrated components with the fuel electrode side of the solid oxide cell (5) to form a solid oxide cell stack.