Separator and its preparation method, lithium-ion battery

By using polypropylene and polysulfone-based membranes in ultrathin separators and coating them with dopamine and polyalkanol ether-modified thiols, the problems of insufficient puncture resistance and mechanical strength of the separators are solved, thereby improving the safety and energy density of lithium-ion batteries.

CN123121079APending Publication Date: 2026-11-17JIANGSU ZENIO NEW ENERGY BATTERY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611290175.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing ultra-thin separators have insufficient puncture resistance and mechanical strength, leading to safety issues such as thermal runaway and internal short circuits in lithium-ion batteries.

Method used

Polypropylene and polysulfone are used as the base film, and the surface is coated with dopamine and polyalkanol ether grafted modified polythiol coating. The covalent bond between the coating and the base film is enhanced, thereby improving mechanical strength and thermal stability.

Benefits of technology

It significantly enhances the thermal stability and mechanical strength of the separator, improves the safety performance and lifespan of lithium-ion batteries, and maintains high energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention provides a separator, its preparation method, and a lithium-ion battery. The separator includes a base film, a first coating on at least one surface of the base film in its thickness direction, and a second coating on the surface of the first coating away from the base film. The base film comprises polypropylene and polysulfone, the first coating comprises dopamine, and the second coating comprises polyalkylene ether-grafted modified polythiol. The introduction of polysulfone (PSU) into the base film modifies the polypropylene (PP), enhancing the puncture strength of the base film. The polyalkylene ether-grafted modified polythiol, as the second coating of the separator, exhibits high thermal stability, contributing to enhanced mechanical strength. Simultaneously, the phenolic hydroxyl groups (-OH) and amino groups (-NH2) in dopamine can chemically react with polar groups (sulfone groups -SO2-) on the surface of the base film and thiol groups (-SH) in the second coating to form covalent bonds, resulting in an extremely strong bond between the second coating and the base film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of membrane technology, and more specifically, to a membrane and its preparation method, and a lithium-ion battery. Background Technology

[0002] As the new energy vehicle industry continues to demand longer battery range and higher safety performance, lithium batteries are being developed towards higher energy density. Among these components, the separator, as a key component for isolating the positive and negative electrodes, preventing short circuits, and ensuring ion transport, has a significant impact on the performance of high-energy-density battery cells.

[0003] Ultrathin separators can significantly increase battery energy density within the same volume. However, existing ultrathin separators suffer from insufficient puncture resistance and mechanical strength, easily leading to safety issues such as thermal runaway and internal short circuits. For example, the reduced thickness of existing ceramic coatings results in insufficient thermal stability, necessitating the development of novel polymer composite materials. Summary of the Invention

[0004] The main objective of this invention is to provide a separator and its preparation method, as well as a lithium-ion battery, to solve the safety problems of existing ultra-thin separators, such as insufficient puncture resistance and mechanical strength, which lead to thermal runaway in lithium-ion batteries.

[0005] To achieve the above objectives, according to one aspect of the present invention, a diaphragm is provided, the diaphragm comprising a base membrane, a first coating located on at least one side surface in the thickness direction of the base membrane, and a second coating located on a surface of the first coating away from the base membrane, the base membrane comprising polypropylene and polysulfone, the first coating comprising dopamine, and the second coating comprising polyalkylene ether-grafted modified polythiol.

[0006] Furthermore, the above-mentioned diaphragm satisfies at least one of the following conditions (a1) to (a5): (a1) the mass ratio of polypropylene to polysulfone is (80~90):(10~20); (a2) the thickness of the base film is 2.5 μm~5.5 μm; (a3) ​​the mass percentage of polyalkyl ether segments in the polyalkyl ether grafted modified polythiol is 18%~40%; (a4) the thickness of the second coating is 1 μm~3 μm; (a5) the thickness of the first coating is 0.1 μm~1 μm.

[0007] According to another aspect of the present invention, a method for preparing the aforementioned diaphragm is provided, comprising: step S1, mixing raw materials including polypropylene and polysulfone and coating them onto a substrate to obtain a base film; step S2, forming a first coating including dopamine on the surface of the base film; step S3, grafting polysulfone onto polyalkyl ether organic compounds to obtain polyalkyl ether grafted modified polysulfone; and step S4, coating the surface of the first coating away from the base film with polyalkyl ether grafted modified polysulfone and then drying it to obtain a diaphragm.

[0008] Further, in step S1 above, the preparation process of the base film includes: step S11, stirring and mixing raw materials including polypropylene, polysulfone, compatibilizer and first solvent to obtain a homogeneous slurry; step S12, coating the homogeneous slurry onto a glass substrate to obtain a wet film with the glass substrate as the support; step S13, immersing the wet film in the bath liquid of a coagulation bath for coagulation to obtain a coagulated base film; step S14, washing and vacuum drying the coagulated base film in sequence to obtain a base film; wherein, the mass ratio of polypropylene to polysulfone is (80~90):(10~20), and the ratio of the total mass of polypropylene and polysulfone, the mass of compatibilizer and the mass of first solvent is (20~30):(3~8):(62~77).

[0009] Further, the above preparation method satisfies at least one of the following conditions (b1) to (b7): (b1) the first solvent is a mixture of N-methylpyrrolidone and N,N-dimethylformamide, and the mass ratio of N-methylpyrrolidone to N,N-dimethylformamide is (7~8):(2~3); (b2) the compatibilizer is hydrogenated styrene-butadiene-styrene block copolymer and / or polypropylene grafted maleic anhydride; (b3) the stirring temperature is 100 ℃~150 ℃, the stirring time is 10 h~12 h, and the stirring speed is 200 rpm~400 rpm; (b4) the bath liquid is a mixture of water and ethanol, the mass concentration of ethanol is 5 wt%~10 wt%, and the temperature of the bath liquid is 20 ℃~30 ℃; (b5) the thickness of the wet film is 3 μm~7 μm, and the residence time of the wet film in the bath liquid is 1 min~3 min; (b6) the solidified base film is rinsed with water for 3 minutes. (b7) The vacuum drying temperature is 50 ℃ to 60 ℃, and the vacuum drying time is 10 h to 12 h.

[0010] Further, in step S2 above, the process of forming the first coating includes: immersing the base film in a dopamine solution and then cleaning and drying it sequentially; wherein, the dopamine solution includes dopamine and water, the mass ratio of dopamine to water is (2~5):(1~2), the immersion temperature is 29 ℃~32 ℃, and the immersion time is 24 h~36 h.

[0011] Further, step S3 includes: step S31, in a nitrogen atmosphere, a first mixture of raw materials including polythiol, polyalkyl ether organics and a second solvent is formed to obtain a first mixture; step S32, a second mixture of raw materials including an initiator and a third solvent is formed to obtain a second mixture; step S33, the first mixture and the second mixture are mixed and then subjected to ultraviolet irradiation to obtain a post-reaction system; step S34, the post-reaction system is subjected to post-treatment sequentially to obtain polyalkyl ether graft-modified polythiol; wherein, the mass ratio of polythiol, polyalkyl ether organics and the second solvent is (80~100):(50~60):(1~10); the polyalkyl ether organics are selected from any one or more of polyethylene glycol monomethyl ether, polyethylene glycol methyl ether methacrylate and polyethylene glycol ether.

[0012] Further, step S3 above satisfies at least one of the following conditions (c1) to (c6): (c1) the second solvent is the same as the third solvent, and the second solvent is selected from any one or more of tetrahydrofuran, acetone, and acetonitrile; (c2) the temperature of the first mixture is 45 ℃ to 65 ℃; (c3) the initiator is benzoyl peroxide and / or azobisisobutyronitrile; (c4) the mass ratio of the initiator to the third solvent is (1~3):(30~90); (c5) the post-treatment process includes: precipitating the reaction system in a fourth solvent and then filtering and drying it sequentially; the fourth solvent is n-hexane and / or petroleum ether, and the temperature of the fourth solvent is 0 ℃ to 5 ℃; the drying temperature is 40 ℃ to 60 ℃, and the time is 24 h to 36 h; (c6) the grafting rate of the mercapto groups in the polythiol to polyalkanol ether organic compounds is 20% to 60%.

[0013] Further, step S4 above includes: step S41, mixing the raw materials including polyalkyl ether grafted modified polythiol and a fifth solvent in a third mixing process to obtain a third mixture; step S42, mixing the raw materials including the third mixture, a dispersant, and a binder to obtain a slurry; step S43, coating the slurry onto the surface of the first coating away from the base film and then drying it to obtain a diaphragm; wherein, step S4 satisfies at least one of the following conditions (d1) to (d7): (d1) the mass ratio of polyalkyl ether grafted modified polythiol to the fifth solvent is (1~5): (d2) The fifth solvent is ethanol and / or isopropanol; (d3) The dispersant is a mixture of alcohol dispersant and ammonium salt dispersant, with a mass ratio of (5~10):(1~3), the alcohol dispersant being selected from any one or more of ethanol, isopropanol, n-propanol, n-butanol and isobutanol, and the ammonium salt dispersant being ammonium polyacrylate and / or ammonium phosphate; (d4) The binder is selected from any one or more of polyacrylic acid, waterborne polyurethane dispersion and PVB resin; (d5) The temperature of the third mixture is 40 ℃~60 ℃; (d6) The mass ratio of the third mixture, dispersant and binder is (10~15):(1~2):(1~2); (d7) The coating method is selected from any one or more of roller coating, blade coating and spray coating.

[0014] According to another aspect of the present invention, a lithium-ion battery is provided, comprising a negative electrode, a separator, and a positive electrode, wherein the separator is the aforementioned separator or a separator prepared by the aforementioned preparation method.

[0015] By applying the technical solution of this invention, the diaphragm of this application solves the problems of insufficient puncture resistance and mechanical strength of ultra-thin diaphragms in the prior art. In particular, after introducing the modified coating, the thermal stability and mechanical strength of the diaphragm are significantly enhanced. Specifically, the polysulfone (PSU) backbone contains benzene rings (-C6H4-) and sulfone groups (-SO2-). These groups endow polysulfone with excellent heat resistance, chemical stability, and mechanical properties. Therefore, the addition of polysulfone can significantly improve the toughness, impact resistance, and heat resistance of polypropylene (PP). The second coating uses polyalkanol ether-grafted modified polythiol. This material combines the high thermal stability of polythiol with the flexibility and lithium-ion conductivity of polyalkanol ether. By introducing flexible polyethylene glycol ether segments into the polythiol backbone, not only is an efficient path for lithium-ion transport provided, but the rigidity of the coating structure is also maintained, thereby enhancing the overall performance of the diaphragm. In the first coating, dopamine covalently bonds with the polar groups (sulfone groups -SO2-) on the surface of the base membrane (PP / PSU composite base membrane). The phenolic hydroxyl groups (-OH) and amino groups (-NH2) in dopamine can chemically react with the thiol groups (-SH) in the second coating to form covalent bonds. These covalent bonds result in an extremely strong bond between the second coating and the base film, making it less prone to separation or detachment due to external factors (such as temperature and solvents). This avoids the risk of traditional coatings peeling off under extreme conditions such as high temperatures or solvent environments, significantly improving the mechanical strength and stability of the second coating. Simultaneously, it enhances the puncture resistance and tensile strength of the separator, ensuring battery safety during assembly and use. Therefore, the separator of this application, while maintaining high energy density, significantly improves battery safety performance and lifespan, achieving a significant breakthrough in ultra-thin separator technology. Detailed Implementation

[0016] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. The present invention will now be described in detail with reference to the embodiments.

[0017] As analyzed in the background section, ultrathin separators have insufficient puncture resistance and mechanical strength, leading to safety issues such as thermal runaway in lithium-ion batteries. To solve this problem, the present invention provides a separator, its preparation method, and a lithium-ion battery.

[0018] In a typical embodiment of this application, a diaphragm is provided, the diaphragm comprising a base membrane, a first coating located on at least one side surface of the base membrane in the thickness direction, and a second coating located on a surface of the first coating away from the base membrane, the base membrane comprising polypropylene and polysulfone, the first coating comprising dopamine, and the second coating comprising polyalkylene ether-grafted modified polythiol.

[0019] The diaphragm of this application solves the problems of insufficient puncture resistance and mechanical strength in existing ultrathin diaphragms. In particular, the thermal stability and mechanical strength of the diaphragm are significantly enhanced after the introduction of a modified coating. Specifically, the polysulfone (PSU) backbone contains benzene rings (-C6H4-) and sulfone groups (-SO2-). These groups endow polysulfone with excellent heat resistance, chemical stability, and mechanical properties. Therefore, the addition of polysulfone can significantly improve the toughness, impact resistance, and heat resistance of polypropylene (PP). The second coating uses polyalkanol ether-grafted modified polythiol. This material combines the high thermal stability of polythiol with the flexibility and lithium-ion conductivity of polyalkanol ether. By introducing flexible polyethylene glycol ether segments into the polythiol backbone, not only is an efficient pathway for lithium-ion transport provided, but the rigidity of the coating structure is also maintained, thereby enhancing the overall performance of the diaphragm. In the first coating, dopamine covalently bonds with the polar groups (sulfone groups -SO2-) on the surface of the base membrane (PP / PSU composite base membrane). The phenolic hydroxyl groups (-OH) and amino groups (-NH2) in dopamine can chemically react with the thiol groups (-SH) in the second coating to form covalent bonds. These covalent bonds result in an extremely strong bond between the second coating and the base film, making it less prone to separation or detachment due to external factors (such as temperature and solvents). This avoids the risk of traditional coatings peeling off under extreme conditions such as high temperatures or solvent environments, significantly improving the mechanical strength and stability of the second coating. Simultaneously, it enhances the puncture resistance and tensile strength of the separator, ensuring battery safety during assembly and use. Therefore, the separator of this application, while maintaining high energy density, significantly improves battery safety performance and lifespan, achieving a significant breakthrough in ultra-thin separator technology.

[0020] In one embodiment of this application, the diaphragm satisfies at least one of the following conditions (a1) to (a5): (a1) the mass ratio of polypropylene to polysulfone is (80~90):(10~20); (a2) the thickness of the base film is 2.5 μm~5.5 μm; (a3) ​​the mass percentage of polyalkyl ether segments in the polyalkyl ether grafted modified polythiol is 18%~40%; (a4) the thickness of the second coating is 1 μm~3 μm; (a5) the thickness of the first coating is 0.1 μm~1 μm.

[0021] By adjusting the ratio of polypropylene to polysulfone, the modification effect of the benzene ring (-C6H4-) and sulfone group (-SO2-) in the polysulfone (PSU) main chain on polypropylene is greatly improved, optimizing the overall performance of the base film, enhancing the puncture strength and thermal stability of the separator, while maintaining good lithium-ion permeability. The preferred thickness range of the base film not only helps to improve the energy density of the battery but also improves the mechanical strength and thermal stability of the separator, effectively reducing the risk of internal short circuits in the battery. The preferred mass percentage of polyalkylol ether segments in the polythiol grafted with polyalkylol ether not only improves the lithium-ion transport path through the introduced flexible segments but also enhances the flexibility and adhesion of the coating material, resulting in a tighter bond between the coating and the base film. Controlling the thickness of the second coating provides the necessary protection and thermal stability without excessively increasing the separator thickness, which would affect the thinner and lighter design of the battery. Controlling the thickness of the first coating allows the thin and robust dopamine coating to improve the hydrophilicity and mechanical properties of the separator while reducing the overall thickness of the separator, which has a positive effect on improving the overall energy density of the battery.

[0022] According to another aspect of the present invention, a method for preparing the aforementioned diaphragm is provided, comprising: step S1, mixing raw materials including polypropylene and polysulfone and coating them onto a substrate to obtain a base film; step S2, forming a first coating including dopamine on the surface of the base film; step S3, grafting polysulfone onto polyalkyl ether organic compounds to obtain polyalkyl ether grafted modified polysulfone; and step S4, coating the surface of the first coating away from the base film with polyalkyl ether grafted modified polysulfone and then drying it to obtain a diaphragm.

[0023] This application addresses the issues of insufficient puncture resistance and mechanical strength faced by ultrathin separators in battery applications. By modifying a polypropylene (PP) base film with polysulfone (PSU), the toughness, impact resistance, and heat resistance of the base film are improved. Subsequently, a first coating containing dopamine is formed on the base film surface. The phenolic hydroxyl groups (-OH) and amino groups (-NH2) in dopamine covalently bond with the polar groups (-SO2-) on the base film surface, increasing the adhesion between the coating and the base film. Further treatment with polyalkylene ethers is used to graft-modified polythiol. This modification not only retains the rigid portion of the polythiol but also introduces flexible segments, providing channels for lithium-ion transport and optimizing lithium-ion conductivity. Specifically, the introduced polyalkylene ether organic segments replace a portion of the -SH group in polythiol, providing a channel for lithium-ion transport and optimizing lithium-ion conductivity. Simultaneously, the rigid portion of polythiol is retained as a framework, and the remaining -SH can form covalent bonds with the phenolic hydroxyl (-OH) and amino (-NH2) groups in dopamine, enhancing the adhesion between the polythiol coating and the base film. Finally, drying treatment yields the final separator. This series of steps effectively improves the separator's thermal stability, mechanical strength, and lithium-ion conductivity, especially significantly enhancing its puncture resistance and reducing thermal shrinkage, thereby improving safety during battery charging and discharging while maintaining high energy density and capacity retention.

[0024] In one embodiment of this application, the preparation process of the base film in step S1 includes: step S11, mixing raw materials including polypropylene, polysulfone, compatibilizer and first solvent to obtain a homogeneous slurry; step S12, coating the homogeneous slurry onto a glass substrate to obtain a wet film with the glass substrate as the support; step S13, immersing the wet film in the bath liquid of a coagulation bath for coagulation to obtain a coagulated base film; step S14, washing and vacuum drying the coagulated base film in sequence to obtain a base film; wherein, the mass ratio of polypropylene to polysulfone is (80~90):(10~20), and the ratio of the total mass of polypropylene and polysulfone, the mass of compatibilizer and the mass of first solvent is (20~30):(3~8):(62~77).

[0025] Step S11 involves mixing polypropylene (PP), polysulfone (PSU), a compatibilizer, and a first solvent in a specific ratio to form a homogeneous slurry. The mass ratio of PP to PSU is between 80-90:10-20, and the total mass ratio of the three is 20-30:3-8:62-77. This ratio effectively promotes the compatibility of PP and PSU in the solvent, forming a stable and uniform slurry, laying the foundation for subsequent film formation. Step S12 involves coating the homogeneous slurry onto a glass substrate. Utilizing the flatness and stability of the glass substrate, a wet film is obtained on the support. The thickness of the wet film can be precisely controlled using coating tools such as a doctor blade, thus affecting the performance of the final base film. In Step S13, after the wet film is immersed in the coagulation bath, the temperature and residence time of the bath directly affect the film's structure and porosity. Adding an appropriate amount of ethanol reduces surface tension and closed pores, resulting in a more uniform film structure and a reasonable pore distribution, ensuring the film's ion conductivity. The washing and vacuum drying in step S14 not only remove residual solvents but also improve the dryness and stability of the base film, which is beneficial to improving the safety performance of the battery. Through the series of steps in the base film preparation in the above preferred scheme, precise control of the base film performance is achieved. Combined with the first coating of dopamine and the second coating of polyalkylene ether grafted modified polythiol, the thermal stability and mechanical strength of the separator are effectively improved, while ensuring the internal resistance, energy density and capacity retention of the lithium-ion battery.

[0026] In one embodiment of this application, the above preparation method satisfies at least one of the following conditions (b1) to (b7): (b1) the first solvent is a mixture of N-methylpyrrolidone and N,N-dimethylformamide, and the mass ratio of N-methylpyrrolidone to N,N-dimethylformamide is (7~8):(2~3); (b2) the compatibilizer is hydrogenated styrene-butadiene-styrene block copolymer and / or polypropylene grafted maleic anhydride; (b3) the stirring temperature is 100 ℃~150 ℃, the stirring time is 10 h~12 h, and the stirring speed is 200 rpm~400 rpm; (b4) the bath liquid is a mixture of water and ethanol, the mass concentration of ethanol is 5 wt%~10 wt%, and the temperature of the bath liquid is 20 ℃~30 ℃; (b5) the thickness of the wet film is 3 μm~7 μm, and the residence time of the wet film in the bath liquid is 1 min~3 min. (b6) Rinse the solidified base film with water 3 to 5 times, each rinse lasting 3 to 5 minutes; (b7) Vacuum drying temperature is 50 ℃ to 60 ℃, and vacuum drying time is 10 h to 12 h.

[0027] Optimizing specific solvent ratios can improve the solubility and uniformity of polypropylene (PP) and polysulfone (PSU) during the blending process, promoting the formation of a more stable and uniform composite base film, thereby enhancing the mechanical strength and thermal stability of the base film. Optimized compatibilizers can improve the compatibility between PP and PSU, making the base film structure denser, reducing porosity, and improving the puncture resistance of the separator. The above stirring and mixing conditions promote the complete dissolution and uniform mixing of the polymer, further optimizing the microstructure of the composite material and enhancing its mechanical properties. Optimized bath composition and conditions, and the addition of ethanol, can reduce surface tension and promote wet film formation. A suitable bath temperature helps control the uniformity of porosity and film thickness, optimizing the ion conductivity of the separator. Controlling the wet film thickness and residence time promotes the uniform distribution of membrane pores, improving the mechanical strength and thermal stability of the separator. Optimized rinsing and solidification of the base film by the number of times and time helps remove residual solvent, reducing the risk of adverse reactions between the electrolyte and the separator, and improving battery safety. The above vacuum drying conditions allow the base film to dry completely, reducing the risk of battery performance degradation due to residual moisture.

[0028] In one embodiment of this application, the process of forming the first coating in step S2 includes: immersing the base film in a dopamine solution and then cleaning and drying it sequentially; wherein the dopamine solution includes dopamine and water, the mass ratio of dopamine to water is (2~5):(1~2), the immersion temperature is 29 ℃~32 ℃, and the immersion time is 24 h~36 h.

[0029] The optimal dopamine-to-water mass ratio in the dopamine solution promotes good dispersion of dopamine in the aqueous solution, facilitating uniform adsorption of dopamine molecules onto the substrate membrane surface. The optimal immersion temperature accelerates the penetration of the dopamine solution into the substrate membrane without causing excessive oxidation of the dopamine, thus improving the stability and reliability of the coating. The chosen immersion time allows dopamine to fully react with the functional groups on the substrate membrane, forming a robust covalent bond network and enhancing the adhesion of the first coating to the substrate membrane. Furthermore, the first coating, obtained through washing (preferably 5-8 times) and drying, not only significantly strengthens the bond strength between the substrate membrane and the first coating but also optimizes the thermal stability and mechanical strength of the membrane. This is because the phenolic hydroxyl groups (-OH) and amino groups (-NH2) in dopamine chemically react with the polar groups (sulfone groups -SO2-) on the substrate membrane, forming stable covalent bonds, thereby reinforcing the interface between the coating and the substrate membrane. Meanwhile, during the coating process, dopamine undergoes self-polymerization to generate a small amount of polydopamine. This process further increases the complexity and functionality of the coating material, which helps to improve the overall performance of the diaphragm, especially its stability under high temperature conditions and its ability to resist external mechanical stress.

[0030] In one embodiment of this application, step S3 includes: step S31, in a nitrogen atmosphere, raw materials including polythiol, polyalkyl ether organics and a second solvent are first mixed to obtain a first mixture; step S32, raw materials including an initiator and a third solvent are second mixed to obtain a second mixture; step S33, the first mixture and the second mixture are mixed and then irradiated with ultraviolet light to obtain a post-reaction system; step S34, the post-reaction system is post-treated sequentially to obtain polyalkyl ether graft-modified polythiol; wherein, the mass ratio of polythiol, polyalkyl ether organics and the second solvent is (80~100):(50~60):(1~10); the polyalkyl ether organics are selected from any one or more of polyethylene glycol monomethyl ether, polyethylene glycol methyl ether methacrylate and polyethylene glycol ether.

[0031] In step S31, a nitrogen atmosphere ensures an inert environment for the system, preventing oxygen from interfering with the reaction. Polythiol, polyalkanol ether organics, and the second solvent are mixed in the above proportions to form a first mixture. This provides a uniform reaction medium for the subsequent grafting reaction, facilitating the uniform grafting of polyalkanol ether organics onto polythiol. In step S32, the preparation of the second mixture of the initiator and the third solvent effectively controls the dissolution and activity of the initiator, ensuring its stability and efficiency in the grafting reaction. In step S33, the first mixture and the second mixture are mixed and then... Ultraviolet irradiation initiates a grafting reaction between polythiol and polyalkanol ether organic compounds, forming a post-reaction system. The selectivity of ultraviolet irradiation improves the controllability of the reaction, promotes the grafting reaction between -SH groups and polyalkanol ether organic compounds under mild conditions, and reduces the use of high temperature or strong oxidants and the occurrence of side reactions. In step S34, the post-reaction system is post-treated, including precipitation, filtration, and drying, to obtain polyalkanol ether graft-modified polythiol. This process not only removes unreacted raw materials and byproducts, but also improves the quality and purity of the modified polythiol.

[0032] In addition, in step S33, the wavelength range of ultraviolet irradiation is 320~400nm. Samples are taken every 10 minutes, and the concentration of -SH is determined by iodometric titration. Irradiation is stopped when the -SH conversion rate reaches (20~60)±5% (reaction time is about 45~60 minutes).

[0033] Iodometric titration is a method that uses the reducing power of thiol groups (-SH) to determine their content. Iodine (I₂) can oxidize thiols to disulfides, while iodine itself is reduced to iodide ions (I₂). - The reaction equation is as follows:

[0034] 2R-SH+I2 →RSS-R+2HI

[0035] Excess iodine can be titrated with a standard sodium thiosulfate solution to calculate the thiol content.

[0036] Iodometric method operation steps:

[0037] Dissolve polythiol in a suitable solvent (such as benzene or acetonitrile) at a ratio of (1-5):(5-10), ensuring complete dissolution. In a 250 mL iodine flask, add the dissolved polythiol sample solution and 50 mL of water. Add iodine solution (I₂ / KI solution) dropwise, 2-3 mL at a time, stirring constantly until the brown color of the mixture no longer disappears. Stop adding iodine solution when the brown color of the organic layer persists for more than 5 minutes. Add 10-20 mL of starch solution as an indicator. Titrate the excess iodine with sodium thiosulfate solution until the blue color of the aqueous layer disappears and does not return after stirring for 2-3 minutes.

[0038] Calculate the thiol content using the following formula:

[0039] F ( g ) = 0.1 × ( V 0- V ) / 1000× m

[0040] Where: V0 is the volume of sodium thiosulfate solution consumed in the blank experiment (mL); V is the volume of sodium thiosulfate solution consumed when titrating the polythiol sample (mL); m is the mass of the sample (g).

[0041] In one embodiment of this application, step S3 above satisfies at least one of the following conditions (c1) to (c6): (c1) the second solvent is the same as the third solvent, and the second solvent is selected from any one or more of tetrahydrofuran, acetone, and acetonitrile; (c2) the temperature of the first mixture is 45 ℃ to 65 ℃; (c3) the initiator is benzoyl peroxide and / or azobisisobutyronitrile; (c4) the mass ratio of the initiator to the third solvent is (1~3):(30~90); (c5) the post-treatment process includes: precipitating the reaction system in a fourth solvent and then filtering and drying it sequentially; the fourth solvent is n-hexane and / or petroleum ether, and the temperature of the fourth solvent is 0 ℃ to 5 ℃; the drying temperature is 40 ℃ to 60 ℃, and the time is 24 h to 36 h; (c6) the grafting rate of the mercapto groups in the polythiol to polyalkanol ether organic compounds is 20% to 60%.

[0042] First, by using the same second and third solvents, uniform mixing of polypropylene, polysulfone, and the initiator can be promoted, thereby improving the uniformity of the coating and the compatibility of the composite material. A preferred specific temperature range accelerates the decomposition of the initiator, effectively promoting the grafting reaction while reducing the risk of material decomposition due to excessively high temperatures, thus enhancing the stability and effectiveness of the modified polythiol coating. Second, using benzoyl peroxide or azobisisobutyronitrile as the initiator not only promotes the grafting reaction between polythiol and polyalkylene ether organic compounds but also promotes the reaction under mild conditions, improving reaction controllability. A preferred mass ratio of initiator to third solvent improves the effective dissolution of the initiator while reducing the risk of reduced reaction efficiency due to excessive solvent. In the post-treatment process, precipitation in hexane or petroleum ether, followed by filtration and low-temperature drying, effectively removes unreacted substances and solvents, maintaining the purity and structural integrity of the coating. Low-temperature drying also reduces the risk of thermal degradation of the coating material. Grafting rates in polythiol within the above range can balance the mechanical strength and lithium-ion transport performance of the coating, enhancing the toughness of the coating while preserving the lithium-ion conduction channels, thus improving the safety and efficiency of the battery at high energy densities.

[0043] In one embodiment of this application, step S4 includes: step S41, mixing the raw materials comprising polyalkylene ether-grafted modified polythiol and a fifth solvent in a third mixture to obtain a third mixture; step S42, mixing the raw materials comprising the third mixture, a dispersant, and a binder to obtain a slurry; step S43, coating the slurry onto the surface of the first coating away from the base film and then drying it to obtain a diaphragm; wherein, step S4 satisfies at least one of the following conditions (d1) to (d7): (d1) the mass ratio of polyalkylene ether-grafted modified polythiol to the fifth solvent is (1~5): (d2) The fifth solvent is ethanol and / or isopropanol; (d3) The dispersant is a mixture of alcohol dispersant and ammonium salt dispersant, with a mass ratio of (5~10):(1~3), the alcohol dispersant being selected from any one or more of ethanol, isopropanol, n-propanol, n-butanol and isobutanol, and the ammonium salt dispersant being ammonium polyacrylate and / or ammonium phosphate; (d4) The binder is selected from any one or more of polyacrylic acid, waterborne polyurethane dispersion and PVB resin; (d5) The temperature of the third mixture is 40 ℃~60 ℃; (d6) The mass ratio of the third mixture, dispersant and binder is (10~15):(1~2):(1~2); (d7) The coating method is selected from any one or more of roller coating, blade coating and spray coating.

[0044] In step S41 above, the set mass ratio of polyalkylene ether-grafted modified polythiol to the fifth solvent ensures the slurry has suitable viscosity and flowability, facilitating subsequent coating processes. The fifth solvent, due to its good volatility, aids in rapid drying without damaging the coating material. The dispersant, a mixture of alcohol and ammonium salt dispersants, and its specific mass ratio effectively enhance the stability of the coating slurry and improve the uniform distribution of the coating on the diaphragm. The preferred binder improves the adhesion between the coating and the diaphragm, enhancing the overall mechanical properties of the diaphragm. The preferred preparation temperature helps maintain the ideal rheological properties of the slurry, facilitating coating. By adjusting the mass ratio of the third mixture, dispersant, and binder, the slurry can achieve a better coating effect, neither too thick nor too thin, resulting in a controllable and uniform coating thickness. The above coating method provides a wider range of process options, which can be flexibly adjusted according to actual needs to achieve optimal coating quality.

[0045] According to another aspect of the present invention, a lithium-ion battery is provided, comprising a negative electrode, a separator, and a positive electrode, wherein the separator is the aforementioned separator or a separator prepared by the aforementioned preparation method.

[0046] As mentioned above, the separator of this application has both excellent puncture resistance and tensile strength. The lithium-ion battery prepared using this separator can improve battery safety, reduce thermal shrinkage, and optimize the conduction performance of lithium ions while ensuring high energy density, thereby improving the battery capacity retention rate.

[0047] The separator prepared in this application has a porosity of 9%~14% at 120°C, a puncture strength of 402 gf~450 gf, and a thermal shrinkage rate of 1.0%~1.5% at 120°C. The lithium-ion battery including this separator has a battery energy density of 149 Wh / kg~160 Wh / kg, a capacity retention rate of 92%~94% after 500 cycles, and an internal resistance of 13.6~14.9 Ω.

[0048] Furthermore, it should be noted that the negative electrode sheet of the application includes a negative electrode current collector (specifically, it can be copper foil) and a negative electrode active material layer coated on the negative electrode current collector. Specifically, the negative electrode active material layer may include a negative electrode active material, a conductive agent, and a binder, wherein the negative electrode active material may include at least one of graphite, hard carbon, soft carbon, silicon-based materials, and lithium metal; the conductive agent may include at least one of conductive carbon black, carbon nanotubes, and acetylene black; and the binder may include sodium carboxymethyl cellulose (CMC), etc. The positive electrode sheet includes a positive electrode current collector (specifically, it can be aluminum foil) and a positive electrode active material layer coated on the positive electrode current collector. Specifically, the positive electrode active material layer may include a positive electrode active material, a conductive agent, and a binder, wherein the positive electrode active material may include at least one of lithium iron phosphate, lithium manganese iron phosphate, and high-nickel ternary materials; the conductive agent may include at least one of conductive carbon black, carbon nanotubes, and acetylene black; and the binder may include polyvinylidene fluoride (PVDF), etc.

[0049] The beneficial effects of this application will be explained below with reference to specific embodiments.

[0050] Example 1

[0051] 1. Preparation of negative electrode sheet: The prepared negative electrode active material (graphite), conductive agent (conductive carbon black) and binder (CMC) are mixed in a mass ratio of 90:2:8 to obtain a mixed material. The mixed material is thoroughly stirred in deionized water to obtain a negative electrode slurry. The obtained negative electrode slurry is coated on conventional copper foil, and after drying and rolling, a negative electrode sheet is obtained.

[0052] 2. Preparation of positive electrode sheet: The positive active material (lithium iron phosphate), conductive agent (conductive carbon black) and binder (PVDF) are mixed in a mass ratio of 95:3:2 to obtain a mixed material. The mixed material is thoroughly stirred in NMP to obtain a positive electrode slurry. The obtained positive electrode slurry is coated on conventional aluminum foil, and after drying and rolling, a positive electrode sheet is obtained.

[0053] 3. Preparation of the separating membrane:

[0054] 3.1 Preparation of PP / PSU (polypropylene / polysulfone) blend base film

[0055] (1) Prepare raw materials: Mix PP and PSU in a ratio of 80:20, blending solvent (NMP / DMF volume ratio = 7:3), compatibilizer (SEBS).

[0056] (2) Preparation of blending solvent: Mix the mixture of PP and PSU, compatibilizer and solvent in a ratio of 25:3:72, and heat and stir at 120°C until a clear homogeneous solution is formed. The stirring time is 12h to ensure that the polymer is completely dissolved.

[0057] (3) Film formation process (phase inversion method)

[0058] The solution was coated onto the glass substrate using a doctor blade, with a wet film thickness set to 5 μm. Coagulation bath conditions: the wet film was immersed in a 25°C water bath (non-solvent) for 3 min, with 5 wt% ethanol added to the bath solution (to reduce surface tension and minimize closed pores).

[0059] (4) Post-treatment and drying: Rinse with deionized water 5 times (5 min each time) to remove residual solvent (NMP residue must be <0.1 wt%). Vacuum dry at 55℃ for 10 h to obtain PP / PSU (polypropylene / polysulfone) blend base film with a film thickness of 3 μm.

[0060] 3.2 Preparation of dopamine coating (PDA)

[0061] A dopamine solution was prepared by mixing dopamine hydrochloride and deionized water at a mass ratio of 3:1. The PP / PSU composite base membrane was then immersed in the dopamine solution and reacted at 32°C for 36 hours. The base membrane was then removed, washed with distilled water 5-8 times, and allowed to air dry, forming a 0.2 μm thick dopamine coating on the base membrane surface.

[0062] 3.3 Preparation of polythiol modification (glove box operation, isolated from water and oxygen)

[0063] 1. Raw material preparation

[0064] Polythiol, polyethylene glycol monomethyl ether (MPEG), anhydrous acetonitrile, benzoyl peroxide (BPO), anhydrous ethanol.

[0065] 2. Flexible grafting segment

[0066] Polythiol, MPEG, and acetonitrile were added to a reactor in a ratio of 85:50:3. Nitrogen gas was purged for 30-50 minutes to remove oxygen, and the mixture was stirred and heated to 55°C to ensure uniform dissolution. Benzoyl peroxide (BPO) and acetonitrile were mixed at a mass ratio of 1:50 to dissolve the BPO initiator. The BPO initiator was added to the mixture (at a ratio of 1:150), and the mixture was irradiated with ultraviolet light at a wavelength of 360 nm. Samples were taken every 10 minutes, and the concentration of -SH was determined by iodometric titration. Irradiation was stopped when the -SH conversion rate reached 40% (approximately 55 minutes of reaction time). The reaction solution was injected into cold diethyl ether to precipitate the precipitate, filtered, and then vacuum dried at 55°C for 24 hours.

[0067] Iodometric titration is a method that uses the reducing properties of thiols (-SH) to determine their content. Iodine (I₂) can oxidize thiols to disulfides, while iodine itself is reduced to iodide ions (I₂). - The reaction equation is as follows:

[0068] 2R-SH+I2 →RSS-R+2HI

[0069] Excess iodine can be titrated with a standard sodium thiosulfate solution to calculate the thiol content.

[0070] Iodometric method operation steps:

[0071] Dissolve 2g of modified polythiol in an appropriate amount of solvent (acetonitrile) at a ratio of 1:10, ensuring complete dissolution. In a 250 mL iodine flask, add the dissolved polythiol sample solution and 50 mL of water. Add iodine solution (I₂ / KI solution) dropwise, 3 mL at a time, stirring constantly until the brown color of the mixture no longer disappears. Stop adding iodine solution when the brown color of the organic layer persists for more than 5 minutes. Add 10 mL of starch solution as an indicator. Titrate the excess iodine with 800 mL of sodium thiosulfate solution until the blue color of the aqueous layer disappears and becomes transparent. At this point, 80 mL of sodium thiosulfate solution has been consumed.

[0072] The mass of thiol groups in the modified polythiol is 12%, and the thiol groups in 2g of modified polythiol are 0.24g. At this time, the thiol content in the thiol is 0.144g. Substituting into formula (2), the conversion rate of thiol groups is calculated to be 40%.

[0073] The thiol group content in the modified polythiol was calculated using the following formulas (1) and (2):

[0074] (1) F(g)=[0.1×(V0-V) / 1000]×m=[0.1×(800-80) / 1000]×2=0.144g

[0075] Substituting into formula (2): R(%) = (1 - F / 0.12m) × 100% = (1 - 0.144 / 0.24) × 100% = 40%

[0076] Where: V0 is the initial sodium thiosulfate solution volume (mL); V is the volume of sodium thiosulfate solution consumed during the titration of the polythiol sample (mL); m is the sample mass (g); F is the mass of -SH in the modified polythiol; and R is the conversion rate of -SH.

[0077] 3.4 Preparation of polythiol coating

[0078] (1) Raw material preparation

[0079] Modified polythiol; solvent: ethanol; dispersant: a mixture of alcohol (ethanol) and ammonium salt dispersant (ammonium polyacrylate); binder: polyacrylic acid.

[0080] (2) Preparation of coating slurry

[0081] The modified polythiol and ethanol were mixed at a ratio of 1:2 (by mass), heated to 40°C, and stirred until homogeneous. The resulting alcohol mixture, dispersant, and binder were then mixed at a ratio of 10:1:1 and stirred until homogeneous.

[0082] (3) Preparation of polythiol coating

[0083] The polythiol coating slurry is uniformly coated onto the surface of the dopamine coating away from the base film using a roller coating method.

[0084] The coated diaphragm was dried in an oven (40°C) to remove the solvent and control the thickness of the polythiol coating to 1.5 μm.

[0085] 4. Preparation of electrolyte:

[0086] Ethylene carbonate (EC) and dimethyl carbonate (DMC) were mixed in a volume ratio of 1:1 to obtain a mixed organic solvent. Then, fully dried lithium salt LiPF6 was dissolved in the mixed organic solvent at a ratio of 1 mol / L to prepare an electrolyte. 0.4 wt% of silicon dioxide (SiO2) was added to the electrolyte.

[0087] 5. Lithium-ion battery manufacturing:

[0088] After weighing, the electrode sheets are directly used as the negative electrode of the lithium-ion battery. The 2032 coin cell is assembled in a glove box filled with Ar. The assembly sequence of the battery from top to bottom is: negative electrode shell, gasket, pad, lithium sheet, separator, self-supporting electrode sheet, positive electrode shell. The resulting coin cell is further tested on a charge and discharge tester.

[0089] Examples 2-4

[0090] The difference from Example 1 is that in the preparation steps of the separator, the thickness of the PP / PSU (polypropylene / polysulfone) blend base film in Examples 2, 3 and 4 is 4.5 μm, 5 μm and 5.5 μm respectively, while the other steps are the same as in Example 1.

[0091] The preparation of the negative electrode, positive electrode, electrolyte, and battery is the same as in Example 1.

[0092] Examples 5-6

[0093] The difference from Example 1 is that in the preparation steps of the separator, the thickness of the polythiol coating in Examples 5 and 6 is 2 μm and 3 μm respectively, while the rest of the steps are the same as in Example 1.

[0094] The preparation of the negative electrode, positive electrode, electrolyte, and battery is the same as in Example 1.

[0095] Examples 7-8

[0096] The difference from Example 1 is that in the preparation steps of the separator, the reaction time for preparing the dopamine coating (PDA) in Examples 7 and 8 is set to 24h and 30h respectively, and the corresponding thicknesses of the dopamine coating are 0.1μm and 0.3μm respectively. The remaining steps are the same as in Example 1.

[0097] The preparation of the negative electrode, positive electrode, electrolyte, and battery is the same as in Example 1.

[0098] Examples 9-10

[0099] The difference from Example 1 is that in the preparation of polythiol modification, the reaction time of the grafted flexible segment in Example 9 and Example 10 is changed to 27 min and 82 min respectively, and the corresponding conversion rates of thiol groups are 20% and 60% respectively. The remaining steps are the same as in Example 1.

[0100] The preparation of the negative electrode, positive electrode, electrolyte, and battery is the same as in Example 1.

[0101] Example 11

[0102] The difference from Example 10 is that in the preparation of polythiol modification, the reaction time of grafting flexible segments is changed to 20 min, and the corresponding conversion rate of thiol groups is 15%. The remaining steps are the same as in Example 1.

[0103] The preparation of the negative electrode, positive electrode, electrolyte, and battery is the same as in Example 1.

[0104] Example 12

[0105] The difference from Example 5 is that the thickness of the polythiol coating is 0.8 μm, while the rest of the steps are the same as in Example 1.

[0106] The preparation of the negative electrode, positive electrode, electrolyte, and battery is the same as in Example 1.

[0107] Example 13

[0108] The difference from Example 7 is that dopamine hydrochloride and deionized water were mixed at a mass ratio of 6:1 to form a dopamine solution, and the reaction time for preparing the dopamine coating (PDA) was set to 40h, corresponding to a dopamine coating thickness of 0.8μm. The remaining steps were the same as in Example 1.

[0109] The preparation of the negative electrode, positive electrode, electrolyte, and battery is the same as in Example 1.

[0110] Example 14

[0111] The difference from Example 7 is that the mass ratio of polypropylene to polysulfone is 90:10, and the remaining steps are the same as in Example 1.

[0112] The preparation of the negative electrode, positive electrode, electrolyte, and battery is the same as in Example 1.

[0113] Example 15

[0114] The difference from Example 7 is that the mass ratio of polypropylene to polysulfone is 70:30, and the remaining steps are the same as in Example 1.

[0115] The preparation of the negative electrode, positive electrode, electrolyte, and battery is the same as in Example 1.

[0116] Example 16

[0117] The difference from Example 1 is that polythiol, MPEG, and acetonitrile are added in a ratio of 100:60:10, while the remaining steps are the same as in Example 1.

[0118] The preparation of the negative electrode, positive electrode, electrolyte, and battery is the same as in Example 1.

[0119] Example 17

[0120] The difference from Example 1 is that polythiol, MPEG, and acetonitrile were added in a ratio of 70:45:10, while the remaining steps were the same as in Example 1.

[0121] The preparation of the negative electrode, positive electrode, electrolyte, and battery is the same as in Example 1.

[0122] Example 18

[0123] The difference from Example 1 is that the polyalkyl alcohol ether organic compound is polyethylene glycol ether, and the remaining steps are the same as in Example 1.

[0124] The preparation of the negative electrode, positive electrode, electrolyte, and battery is the same as in Example 1.

[0125] Comparative Example 1:

[0126] The difference from Example 1 is that the separator is prepared using pure PP base film, while the preparation of the negative electrode, positive electrode, electrolyte and battery is the same as in Example 1.

[0127] Comparative Example 2:

[0128] The difference from Example 1 is that the preparation of the dopamine coating (PDA) is omitted in the preparation of the separator, while the preparation of the negative electrode, positive electrode, electrolyte and battery is the same as in Example 1.

[0129] Comparative Example 3:

[0130] The difference from Example 1 is that a PP / PSU composite base film is used directly as the separator, while the preparation of the negative electrode, positive electrode, electrolyte and battery is the same as in Example 1.

[0131] Comparative Example 4:

[0132] The difference from Example 1 is that the preparation of the polythiol coating is omitted in the preparation of the separator, while the preparation of the negative electrode, positive electrode, electrolyte and battery is the same as in Example 1.

[0133] Comparative Example 5:

[0134] The difference from Example 1 is that polyalkylol ether organic compounds were not used to graft and modify polythiol in the preparation of the separator, while the preparation of the negative electrode, positive electrode, electrolyte and battery were the same as in Example 1.

[0135] Performance testing:

[0136] The performance of the separators and batteries obtained in the above embodiments and comparative examples was tested.

[0137] (1) Internal resistance test: The internal resistance of different groups of batteries is obtained by using a battery internal resistance meter.

[0138] (2) Battery energy density test: First, weigh the battery and record the weight as m. Then, at 25°C, charge the battery with a constant current of 0.33C to 3.65V, and then charge it with a constant voltage of 3.65V until the current is ≤0.05C. After standing for 5 minutes, discharge it with a constant current of 0.33C to 2.0V to obtain the discharge energy Q. The battery energy density is calculated as Q / m.

[0139] (3) Capacity retention test

[0140] At 25℃, with initial and cutoff voltages of 2.2V and 3.65V respectively, the battery is first charged at 1C to 3.65V, then charged at a constant voltage of 3.65V until the current decreases to 0.05C, followed by a 0.5C discharge to 2.2V. This cycle of charging and discharging is repeated. The specific capacity of the first discharge cycle is recorded as C1, the specific capacity of the 100th discharge cycle as C100, the specific capacity of the 500th discharge cycle as C500, and the specific capacity of the nth discharge cycle as Cn. The capacity retention rate of the nth cycle is calculated as Cn / C1 × 100%.

[0141] (4) Thermal response test of the isolation membrane

[0142] The membrane was kept in a constant temperature chamber at 60℃ for 30 minutes, and then the temperature was raised to 120℃ to test the porosity of the membrane.

[0143] Cut at least three representative circular or square samples from the diaphragm to be tested. Place the samples in a vacuum drying oven and vacuum dry at 120°C for at least 2 hours to thoroughly remove moisture and residual solvent. Transfer the dried samples to a desiccator to cool to room temperature (approximately 20-25°C). Weigh each dried sample in air and record it as m1 (in g). Turn on the high-temperature constant temperature chamber and density measuring device to heat and stabilize the impregnation solution at 120±2°C. Immerse the dried and weighed (m1) sample in the 120°C impregnation solution. To ensure that the impregnation solution completely fills the diaphragm pores, evacuate the container containing the sample and impregnation solution for 5-10 minutes until no air bubbles escape. Using the special support of the high-temperature densitometer, completely immerse the sample saturated with the impregnation solution in the 120°C impregnation solution (high-boiling-point silicone oil) (but without contacting the container walls and bottom). After the reading stabilizes, record the mass at this point as m2 (in g). This is equivalent to the buoyancy force experienced by a saturated sample in a high-temperature impregnation solution. The average value of at least three parallel sample test results should be taken as the final test value, and the test temperature should be noted as 120℃.

[0144] Calculate apparent density (ρ) a ): ρ a = (m1 / (m1-m2)) ρ li q

[0145] ρ a m1: Apparent density of the sample at 120℃ (g / cm³); m2: Apparent mass of the dried sample in air (g); m3: Apparent mass of the saturated sample in the impregnation solution (g); ρ li q: Density of the impregnation solution at 120℃ (g / cm³);

[0146] Calculate porosity (P, %): P = (1-ρ a / ρ i ) 100%

[0147] P: Porosity of the sample (%); ρ a : Calculated apparent density (g / cm³); ρ i : Spatial density of the diaphragm material (g / cm³), ρ of polypropylene (PP) i The ρ of polyethylene (PE) is 0.91 g / cm³. i It is 0.96 g / cm³.

[0148] (5) Puncture strength test

[0149] Cut a sample of suitable size from the diaphragm material to be tested, typically circular with a diameter of 50 mm. The sample surface should be flat, without wrinkles or damage. Install the puncture clamp on the upper and lower clamp seats of the electronic tensile testing machine, ensuring the clamp is securely installed and centered. Install the puncture needle on the clamp, ensuring it is perpendicular to the clamp plane. Place the diaphragm sample flat on the lower clamp of the puncture clamp and use the clamp to hold the sample tightly with moderate clamping force. Set the test parameters on the operating interface of the electronic tensile testing machine, such as test speed (50 mm / min), test stroke, and data acquisition frequency (50 Hz). Start the testing machine; the puncture needle moves downward at the set speed, penetrating the diaphragm sample. The machine's sensors will collect force and displacement data in real time and display the force-displacement curve. When the puncture needle has completely penetrated the diaphragm, record the maximum force value, which is the puncture resistance strength of the diaphragm.

[0150] (6) Heat shrinkage rate test

[0151] Cut three 100mm × 100mm square samples from the diaphragm. One edge of the sample should be parallel to the longitudinal edge of the diaphragm, with a deviation angle not exceeding 5° to ensure the accuracy of the test results. Mark the longitudinal and transverse sides of the samples for subsequent dimensional changes. Place a stainless steel plate and two sheets of quantitative filter paper in a blower-type constant temperature chamber and heat to 130±1℃. Use a high-precision measuring tool to record the initial longitudinal and transverse dimensions of the samples. Maintain the temperature at 130℃ for 1 hour (±6 minutes). After heating, remove the samples and allow them to return to room temperature before measuring the longitudinal and transverse dimensions again. Take the average of the three test data as the final heat shrinkage rate of the diaphragm, i.e., shrinkage rate (%) = [(initial length - length after heating) / initial length] × 100%.

[0152] The test results are listed in Table 1.

[0153] Table 1

[0154]

[0155] Based on the test results of the examples and comparative examples, the puncture strength and heat shrinkage rate in Example 1 are both very good. The introduction of polysulfone (PSU) to modify the polypropylene (PP) base film and the polythiol coating effectively improve the thermal stability of the diaphragm and enhance its mechanical strength.

[0156] The thickness of the composite base film and the polythiol coating affect the properties of the separator. Test data shows that increasing the thickness of both the base film and the coating slightly improves the puncture strength of the separator, but this increased thickness leads to a decrease in the battery's energy density. Conversely, as the conversion rate of the thiol groups increases, the puncture strength of the separator decreases, the lithium-ion transport capacity increases, and the capacity retention rate slightly improves.

[0157] Therefore, the ultrathin diaphragm prepared in Example 1 of the present invention can maintain excellent electrical properties while ensuring excellent needle penetration strength and thermal shrinkage rate.

[0158] As can be seen from the above description, the embodiments of the present invention achieve the following technical effects:

[0159] The diaphragm of this application solves the problems of insufficient puncture resistance and mechanical strength in existing ultrathin diaphragms. In particular, the thermal stability and mechanical strength of the diaphragm are significantly enhanced after the introduction of a modified coating. Specifically, the polysulfone (PSU) backbone contains benzene rings (-C6H4-) and sulfone groups (-SO2-). These groups endow polysulfone with excellent heat resistance, chemical stability, and mechanical properties. Therefore, the addition of polysulfone can significantly improve the toughness, impact resistance, and heat resistance of polypropylene (PP). The second coating uses polyalkanol ether-grafted modified polythiol. This material combines the high thermal stability of polythiol with the flexibility and lithium-ion conductivity of polyalkanol ether. By introducing flexible polyethylene glycol ether segments into the polythiol backbone, not only is an efficient pathway for lithium-ion transport provided, but the rigidity of the coating structure is also maintained, thereby enhancing the overall performance of the diaphragm. In the first coating, dopamine covalently bonds with the polar groups (sulfone groups -SO2-) on the surface of the base membrane (PP / PSU composite base membrane). The phenolic hydroxyl groups (-OH) and amino groups (-NH2) in dopamine can chemically react with the thiol groups (-SH) in the second coating to form covalent bonds. These covalent bonds result in an extremely strong bond between the second coating and the base film, making it less prone to separation or detachment due to external factors (such as temperature and solvents). This avoids the risk of traditional coatings peeling off under extreme conditions such as high temperatures or solvent environments, significantly improving the mechanical strength and stability of the second coating. Simultaneously, it enhances the puncture resistance and tensile strength of the separator, ensuring battery safety during assembly and use. Therefore, the separator of this application, while maintaining high energy density, significantly improves battery safety performance and lifespan, achieving a significant breakthrough in ultra-thin separator technology.

[0160] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A diaphragm, characterized by The diaphragm includes a base membrane, a first coating on at least one surface of the base membrane in the thickness direction, and a second coating on a surface of the first coating away from the base membrane. The base membrane includes polypropylene and polysulfone, the first coating includes dopamine, and the second coating includes polyalkylene ether-grafted modified polythiol.

2. The separator according to claim 1, characterized in that The diaphragm satisfies at least one of the following conditions (a1) to (a5): (a1) The mass ratio of the polypropylene to the polysulfone is (80~90):(10~20); (a2) The thickness of the base film is 2.5 μm to 5.5 μm; (a3) The mass percentage of polyalkanol ether segments in the polyalkanol ether grafted modified polythiols is 18%~40%; (a4) The thickness of the second coating is 1 μm to 3 μm; (a5) The thickness of the first coating is 0.1 μm to 1 μm.

3. A method of producing the separator according to claim 1 or 2, characterized by, The preparation method includes: Step S1: Mix raw materials including polypropylene and polysulfone and coat them onto a substrate to obtain a base film; Step S2, forming a first coating comprising dopamine on the surface of the base film; Step S3: Polyalkanol ether organic compounds are used to graft and modify polythiol to obtain polyalkanol ether graft-modified polythiol. Step S4: After coating the surface of the first coating away from the base film with the polyalkyl ether-grafted modified polythiol, the coating is dried to obtain the diaphragm.

4. The production method according to claim 3, characterized by, In step S1, the preparation process of the base film includes: Step S11: The raw materials including the polypropylene, the polysulfone, the compatibilizer and the first solvent are stirred and mixed to obtain a homogeneous slurry; Step S12: After the homogeneous slurry is coated onto the glass substrate, a wet film with the glass substrate as the support is obtained. Step S13: Immerse the wet film in the bath liquid of the coagulation bath for coagulation to obtain a coagulated base film; Step S14: The solidified base film is washed and vacuum dried sequentially to obtain the base film; The mass ratio of polypropylene to polysulfone is (80~90):(10~20), and the mass ratio of the total mass of polypropylene and polysulfone, the mass of the compatibilizer and the mass of the first solvent is (20~30):(3~8):(62~77).

5. The preparation method according to claim 4, characterized in that, The preparation method satisfies at least one of the following conditions (b1) to (b7): (b1) The first solvent is a mixture of N-methylpyrrolidone and N,N-dimethylformamide, wherein the mass ratio of N-methylpyrrolidone to N,N-dimethylformamide is (7~8): (2~3); (b2) The compatibilizer is a hydrogenated styrene-butadiene-styrene block copolymer and / or polypropylene grafted with maleic anhydride; (b3) The mixing temperature is 100 ℃~150 ℃, the mixing time is 10 h~12 h, and the mixing speed is 200 rpm~400 rpm; (b4) The bath liquid is a mixture of water and ethanol, wherein the mass concentration of ethanol is 5 wt% to 10 wt%, and the temperature of the bath liquid is 20 ℃ to 30 ℃; (b5) The thickness of the wet film is 3 μm to 7 μm, and the residence time of the wet film in the bath liquid is 1 min to 3 min; (b6) The solidified base film is rinsed with water 3 to 5 times, with each rinsing time being 3 to 5 minutes; (b7) The vacuum drying temperature is 50 ℃~60 ℃, and the vacuum drying time is 10 h~12 h.

6. The production method according to claim 4 or 5, characterized by, In step S2, the process of forming the first coating includes: The base film was immersed in a dopamine solution and then washed and dried sequentially. The dopamine solution comprises dopamine and water, wherein the mass ratio of dopamine to water is (2~5):(1~2), the immersion treatment temperature is 29 ℃~32 ℃, and the immersion treatment time is 24 h~36 h.

7. The production method according to any one of claims 4 to 6, characterized by, Step S3 includes: Step S31: In a nitrogen atmosphere, the raw materials including the polythiol, the polyalkanol ether organic compound, and the second solvent are first mixed to obtain a first mixture; Step S32: The raw materials including the initiator and the third solvent are mixed for the second time to obtain a second mixture; Step S33: Mix the first mixture with the second mixture and then irradiate with ultraviolet light to obtain the reaction system; Step S34: The post-reaction system is subjected to sequential post-processing to obtain the polyalkylol ether grafted modified polythiol; The mass ratio of the polythiol, the polyalkylol ether organic compound, and the second solvent is (80~100):(50~60):(1~10); the polyalkylol ether organic compound is selected from any one or more of polyethylene glycol monomethyl ether, polyethylene glycol methyl ether methacrylate, and polyethylene glycol ether.

8. The production method according to claim 7, characterized by, Step S3 satisfies at least one of the following conditions (c1) to (c6): (c1) The second solvent is the same as the third solvent, wherein the second solvent is selected from any one or more of tetrahydrofuran, acetone and acetonitrile; (c2) The temperature of the first mixture is 45 ℃~65 ℃; (c3) The initiator is benzoyl peroxide and / or azobisisobutyronitrile; (c4) The mass ratio of the initiator to the third solvent is (1~3):(30~90); (c5) The post-processing includes: precipitating the reaction system in the fourth solvent and then filtering and drying it sequentially; the fourth solvent is n-hexane and / or petroleum ether, and the temperature of the fourth solvent is 0 ℃~5 ℃; the drying temperature is 40 ℃~60 ℃, and the time is 24 h~36 h; (c6) The grafting rate of the thiol groups in the polythiol to the polyalkyl ether organic compounds is 20% to 60%.

9. The production method according to claim 3 or 4, characterized by, Step S4 includes: Step S41: The raw materials including the polyalkylol ether grafted modified polythiol and the fifth solvent are mixed in a third mixture to obtain a third mixture; Step S42: Mix the raw materials including the third mixture, dispersant and binder to obtain a slurry; Step S43: The slurry is coated onto the surface of the first coating away from the base film and then dried to obtain the diaphragm; Wherein, step S4 satisfies at least one of the following conditions (d1) to (d7): (d1) The mass ratio of the polyalkylol ether grafted modified polythiol to the fifth solvent is (1~5): (2~15); (d2) The fifth solvent is ethanol and / or isopropanol; (d3) The dispersant is a mixture of alcohol dispersant and ammonium salt dispersant, wherein the mass ratio of alcohol dispersant to ammonium salt dispersant is (5~10):(1~3), wherein the alcohol dispersant is selected from any one or more of ethanol, isopropanol, n-propanol, n-butanol and isobutanol, and the ammonium salt dispersant is ammonium polyacrylate and / or ammonium phosphate. (d4) The adhesive is selected from any one or more of polyacrylic acid, water-based polyurethane dispersion, and PVB resin; (d5) The temperature of the third mixture is 40 ℃~60 ℃; (d6) The mass ratio of the third mixture, the dispersant and the binder is (10~15): (1~2): (1~2); (d7) The coating method is selected from any one or more of roller coating, blade coating and spray coating.

10. A lithium ion battery comprising a negative electrode sheet, a separator, and a positive electrode sheet, characterized by The diaphragm is the diaphragm according to claim 1 or 2, or the diaphragm prepared by the preparation method according to any one of claims 3 to 9.