A separator and battery

By designing amorphous polymer particles to oriented aggregate in the aggregation region formed by crystalline polymer particles in the separator coating, the problems of insufficient adhesion strength and uncontrollable swelling of the separator coating are solved, achieving high adhesion strength and lithium-ion transport efficiency, and improving the stability and safety of the battery electrode structure.

CN123121082APending Publication Date: 2026-11-17SHENZHEN HIGHPOWER TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611350439.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-01
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing diaphragm coatings have insufficient bonding strength, uncontrollable swelling, or obstructed ion transport, making them unable to effectively cope with the huge volume expansion of silicon-carbon composite materials during charging and discharging, resulting in electrode structure pulverization, active material shedding, and cell deformation.

Method used

By employing a coating structure design, amorphous polymer particles are oriented to aggregate within the aggregation region formed by crystalline polymer particles, creating high-density bonding points. Combined with the crystalline polymer particles as a skeletal structure, the swelling of the amorphous polymer is limited, ensuring unobstructed lithium-ion transport channels.

Benefits of technology

It improves the bonding strength between the separator and the electrode, suppresses cell deformation caused by electrode expansion, maintains the stability and hardness of the cell structure, and ensures lithium-ion transport efficiency, thereby improving the cycle stability and safety performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123121082A_ABST
    Figure CN123121082A_ABST
Patent Text Reader

Abstract

This invention provides a separator and a battery, including a base film and a coating applied to the surface of the base film. The coating includes polymer particles, comprising first polymer particles and second polymer particles. The first polymer particles adhere to the second polymer particles to form a single aggregated region. The coating includes multiple aggregated regions. The number of second polymer particles in the coating is N1, and the number of second polymer particles in the aggregated region is N2, where N1 and N2 satisfy: 0.8N1≤N2. This invention achieves high-density bonding points within a limited area by directionally agglomerating amorphous polymer particles into aggregated regions formed by the adhesion of crystalline polymer particles. This structure effectively improves the overall adhesion of the coating, and is particularly suitable for high-volume expansion systems such as silicon-carbon anodes. It can effectively suppress cell deformation caused by electrode expansion and maintain the stability and hardness of the cell structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery technology, and more specifically to a separator and a battery. Background Technology

[0002] Lithium-ion batteries, as a typical type of rechargeable battery, have become the core power source for consumer electronics (such as smartphones and laptops), electric vehicles, and energy storage systems due to their advantages such as high energy density, long cycle life, low self-discharge rate, and environmental friendliness. Their working principle is based on the reversible insertion / extraction of lithium ions between the positive and negative electrodes: during charging, lithium ions are extracted from the positive electrode active material, migrate through the electrolyte, and insert into the negative electrode; during discharging, the process is reversed, with electrons forming a current through the external circuit, thus achieving energy output.

[0003] Among the key components of lithium-ion batteries, the separator, although not directly involved in the electrochemical reaction, plays a crucial physical and functional role—it must effectively isolate the positive and negative electrodes to prevent internal short circuits while providing a low-resistance migration channel for lithium ions. Therefore, the separator's pore structure, thickness, thermal stability, wettability, and mechanical strength directly affect the battery's rate performance, cycle life, and safety performance.

[0004] In recent years, with the urgent market demand for higher energy density batteries, silicon-carbon composite materials have been widely introduced as a new generation of anode systems. Silicon has a theoretical specific capacity of about 4200 mAh / g (far higher than graphite's 372 mAh / g), but it is accompanied by huge volume expansion during charging and discharging (more than 300% when fully lithium-ionized). This drastic volume change can easily lead to electrode structure pulverization, active material shedding, and repeated rupture and regeneration of the solid electrolyte interphase (SEI) film, which in turn causes rapid capacity decay and results in overall cell bulging, deformation, or even failure.

[0005] To address these challenges, the industry generally adopts a strategy of coating the membrane surface with a functional adhesive layer. This enhances the interfacial bonding between the membrane and the electrodes (especially the negative electrode), constrains electrode expansion displacement, and maintains the structural integrity of the battery cell. However, existing commercially available membrane adhesive coatings (such as single PVDF or conventional acrylic coatings) commonly suffer from insufficient adhesive strength, uncontrollable swelling, or impeded ion transport. Therefore, there is an urgent need to develop a novel membrane coating structure that combines high adhesive strength, controllable swelling behavior, and high ion permeability. Summary of the Invention

[0006] To address the problems of insufficient adhesive strength, uncontrollable swelling, or obstructed ion transport in existing diaphragm coatings, this invention provides a diaphragm and a battery.

[0007] The technical solution adopted by the present invention to solve the above-mentioned technical problems is as follows: The present invention provides a diaphragm, comprising a base membrane and a coating coated on the surface of the base membrane. The coating comprises polymer particles, including first polymer particles and second polymer particles. The first polymer particles are crystalline polymer particles, and the second polymer particles are amorphous polymer particles. The first polymer particles adhere to the second polymer particles to form a single aggregated region. The coating includes multiple such aggregated regions. The number of second polymer particles in the coating is N1, and the number of second polymer particles in each aggregated region is N2. N1 and N2 satisfy: 0.8N1≤N2.

[0008] Optionally, the distance between the edges of two adjacent polymer particles is L, in μm, and L satisfies: L≤0.3.

[0009] Optionally, the number of contacts between the second polymer particles and the first polymer particles is N3, and the number of first polymer particles satisfying the corresponding number of N3 is N4; the N3 and the N4 satisfy the following relationship: Equation 1: when N3≥10, N4≥30; Equation 2: When N3≥5, N4≥60.

[0010] Optionally, the surface area of ​​the base film is S1, in cm². 2 The coverage area of ​​the coating is S2, in cm². 2 S1 and S2 satisfy the relationship: 0.5≤S2 / S1≤0.75.

[0011] Optionally, the coating area of ​​the first polymer particles is S3, in cm. 2 S3 and S2 satisfy the relationship: 0.3≤S3 / S2≤0.6.

[0012] Optionally, the first polymer particles are secondary particles; And / or, the melting point of the first polymer particles is T, in °C, and T satisfies: 130≤T≤180.

[0013] Optionally, the particle size D50 of the second polymer particles is 0.3-1.5 μm; And / or, the mass swelling ratio of the second polymer is >250%.

[0014] Optionally, the coating is applied to the surface of the diaphragm base membrane in a single-sided coating manner; And / or, the coating is applied to the surface of the diaphragm base membrane in a double-sided coating manner.

[0015] Optionally, the areal density of the coating is 0.25-0.55 g / m³. 2 ; And / or, the diaphragm base membrane is a polyethylene membrane; And / or, the first polymer is vinylidene fluoride and its copolymers; And / or, the second polymer is an acrylate copolymer.

[0016] Optionally, the coating further includes a binder, a stabilizer, a dispersant, and a wetting agent. Taking the total mass of the coating as 100%, the first polymer particles account for 35%-55% of the total mass of the coating; the second polymer particles account for 9%-14% of the total mass of the coating; the binder accounts for 10%-25% of the total mass of the coating; the stabilizer accounts for 15%-35% of the total mass of the coating; the dispersant accounts for 0.5%-2% of the total mass of the coating; and the wetting agent accounts for 0.3%-2% of the total mass of the coating.

[0017] Another aspect of the present invention provides a battery comprising the separator as described above.

[0018] According to the diaphragm provided by the present invention, by directionally agglomerating amorphous polymer particles within an aggregation region formed by the adhesion of crystalline polymer particles, more than 80% of the second polymer particles are concentrated in a local area, thereby achieving high-density bonding points within a limited area. This structure effectively improves the overall adhesion of the coating, and is particularly suitable for high-volume expansion systems such as silicon-carbon anodes. It can effectively suppress cell deformation caused by electrode expansion and maintain the stability and hardness of the cell structure. Secondly, the crystalline polymer particles, as the "skeleton" structure, hardly swell during hot pressing, ensuring the integrity of the diaphragm's pore structure. Although amorphous polymer particles have a tendency to swell, they are confined within the aggregation region, avoiding disordered diffusion and blockage of ion channels across the entire coating surface. Therefore, while ensuring unobstructed lithium-ion transport channels, a higher total coating coverage can be achieved, overcoming the technical bottleneck of traditional single-layer amorphous coatings having to reduce areal density due to swelling limitations. Moreover, the first polymer particles adhere to and "anchor" the second polymer particles through physical or chemical action, inducing them to form aggregates with controllable size and reasonable distribution. This aggregated structure not only enhances the cohesive force within the coating but also improves the bonding strength with the positive and negative electrode interfaces, forming a stable and efficient three-dimensional adhesive network. Attached Figure Description

[0019] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the description of the embodiments of the present invention will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0020] Figure 1 This is a SEM image of the diaphragm provided in Embodiment 1 of the present invention; Detailed Implementation To make the technical problems solved, technical solutions, and beneficial effects of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without inventive effort are within the scope of protection of this invention.

[0021] Unless otherwise specified, the experimental methods used in the following examples are conventional methods; the materials and reagents used are commercially available unless otherwise specified.

[0022] In one embodiment, the present invention provides a diaphragm, including a base film and a coating coated on the surface of the base film. The coating includes polymer particles, which include first polymer particles and second polymer particles. The first polymer particles are crystalline polymer particles, and the second polymer particles are amorphous polymer particles. The first polymer particles adhere to the second polymer particles to form a single aggregated region. The coating includes a plurality of said aggregated regions. The number of second polymer particles in the coating is N1, and the number of second polymer particles in the aggregated regions is N2. N1 and N2 satisfy: 0.8N1≤N2.

[0023] When the second polymer particles are not guided by the first polymer particles or do not enter the aggregation area, the second polymer particles exist as independent, dispersed single particles. The single particle dispersion state is conducive to the stability of the slurry rheological properties and reduces problems such as sedimentation, flocculation or filter blockage. The single particle distribution exposes more amorphous polymer surfaces and participates in interfacial bonding, significantly improving the bonding efficiency of polymer per unit mass.

[0024] The coating forms multiple aggregation regions on the base film surface. The total number of second polymer particles in these aggregation regions is N2, where N1 and N2 satisfy the condition: 0.8N1≤N2. This concentrates the majority (≥80%) of the highly adhesive amorphous polymer particles in the aggregation regions guided by the crystalline polymer, allowing the adhesion to be concentrated in specific micro-regions rather than dispersed across the entire coating surface. This "functional focusing" strategy significantly improves the effective polymer density per unit adhesion area, thereby achieving stronger and more reliable membrane-electrode interface bonding within a limited contact area. Secondly, if the amorphous particles are uniformly or randomly distributed, not only is a higher total amount required to achieve the same adhesion, but they are also prone to global swelling in hot-pressing or electrolyte environments, clogging membrane pores and impairing ion transport performance. By confining ≥80% of amorphous particles within the aggregated regions, the adhesive contribution is maximized while minimizing its negative impact on the membrane's pore structure, achieving a dual optimization of material utilization efficiency and battery performance. Moreover, multiple aggregated regions jointly bear the main adhesive function, and each region is enriched with a large number of amorphous particles, resulting in uniform and stable adhesive characteristics of the entire membrane on a macroscopic scale. This design effectively avoids cell deformation or interface delamination caused by insufficient local adhesion, improving battery manufacturing yield and cycle consistency. In addition, under the premise of satisfying 0.8N1≤N2, even with a high overall coating coverage, the amorphous components are still effectively "controlled" within the discrete aggregated regions, while the uncovered areas maintain open channels. This allows the membrane to maintain high ionic conductivity while achieving adhesive strength far exceeding that of traditional uniform coatings, making it particularly suitable for high-energy-density battery systems (such as silicon-containing anodes) with stringent requirements for interface stability.

[0025] This invention achieves high-density bonding points within a limited area by directionally agglomerating amorphous polymer particles within an aggregated region formed by the adhesion of crystalline polymer particles, resulting in over 80% of the second polymer particles being concentrated in a localized area. This structure effectively improves the overall adhesion of the coating, making it particularly suitable for high-volume-expansion systems such as silicon-carbon anodes. It can effectively suppress cell deformation caused by electrode expansion, maintaining the stability and hardness of the cell structure. Secondly, the crystalline polymer particles, acting as a "skeleton" structure, hardly swell during hot pressing, ensuring the integrity of the membrane's pore structure. While amorphous polymer particles have a tendency to swell, they are confined within the aggregated region, preventing disordered diffusion and blockage of ion channels across the entire coating surface. Therefore, while ensuring unobstructed lithium-ion transport channels, a higher overall coating coverage can be achieved, overcoming the technical bottleneck of traditional single-layer amorphous coatings that must reduce areal density due to swelling limitations. Furthermore, the first polymer particles adhere to and "anchor" the second polymer particles through physical or chemical action, inducing them to form aggregates with controllable size and reasonable distribution. This aggregated structure not only enhances the cohesive force within the coating but also improves the bonding strength with the positive and negative electrode interfaces, forming a stable and efficient three-dimensional adhesive network.

[0026] In this invention, the number of second polymer particles N1 in the coating and the number of second polymer particles N2 in the aggregation region are characterized by scanning electron microscopy (SEM). The specific testing method is as follows: The sample diaphragm is flattened and fixed on the SEM sample stage. The magnification of the SEM is set to 1000x, and the field of view size of a single SEM image is fixed at 126μm × 110μm, with each SEM image corresponding to an independent observation area. By means of random sampling, multiple non-overlapping test fields of view are randomly selected on the surface of the sample coating, and particle counts are performed on the SEM images. The aggregation region is defined as the particle aggregation region formed by the adhesion of at least one second polymer particle to the first polymer particle. The second polymer particles in the aggregation region are those that are in close contact with the first polymer particle and are adhered to the surface of the first polymer particle, and all of them are included in the N2 count. N1 is the total number of all second polymer particles in a single observation field, including the second polymer particles that are adhered to the first polymer particle in the aggregation region and the second polymer particles that are independently dispersed in the non-aggregation region, do not contact any first polymer particle, and are distributed as single particles. Record the total number of second polymer particles N1 and the number of second polymer particles N2 in the aggregation area for each field of view. After completing the acquisition of all valid field of view data, calculate the ratio of N2 to N1 for each observation area, and finally calculate the arithmetic mean of all valid test data.

[0027] In one embodiment, the distance between the edges of two adjacent polymer particles is L, in μm, and L satisfies: L≤0.3.

[0028] Specifically, by using scanning electron microscopy (SEM), multiple non-overlapping test fields were randomly selected on the surface of the sample coating. The distance between the edges of two adjacent polymer particles in the SEM image was measured. When the distance between the edges of two adjacent polymer particles was less than 0.3 μm, the second polymer particles were nearly tightly packed in the aggregation area, significantly increasing the content of adhesive polymer per unit area and forming a continuous or quasi-continuous adhesive phase, thereby greatly improving the local bonding strength. Moreover, at such a small spacing, the amorphous polymer particles are easy to contact and fuse with each other during hot pressing or electrolyte swelling, forming a connected viscoelastic network structure. This network not only enhances the cohesiveness of the coating itself but also forms a more thorough interfacial contact with the electrode surface, significantly improving the peel strength between the separator and the positive and negative electrodes. Although amorphous polymers are prone to swelling, when they aggregate at a spacing of L≤0.3μm, the swelling behavior tends to be synergistic rather than disordered diffusion. This facilitates the formation of a dense adhesive layer within a limited space without significant spillover into non-aggregated areas, thereby improving adhesion performance while avoiding clogging the pores of the separator and ensuring ion transport efficiency. When L>0.3μm, some areas will lack effective bonding points, leading to uneven interfacial bonding.

[0029] In one embodiment, the number of contacts between the second polymer particles and the first polymer particles is N3, and the number of first polymer particles satisfying the corresponding number of N3 is N4; the N3 and the N4 satisfy the following relationship: Equation 1: When N3≥10, N4≥30; Equation 2: When N3≥5, N4≥60.

[0030] In Equation 2, scanning electron microscopy (SEM) is used for testing and characterization. Within a single observation area (126 μm × 110 μm), the number of first polymer particles N4 ≥ 60 that are in contact with the second polymer particles within the aggregation area is required to have a sufficient number of first polymer particles anchoring at least 5 second polymer particles, thereby constructing a dense support framework and effectively binding the second polymer particles.

[0031] In Equation 1, based on the conditions in Equation 2, a further limitation is imposed: when N3 ≥ 10, the number of first polymer particles, N4 ≥ 30, is required. The higher limit for N3 in Equation 1 (≥ 10) means that the number of particles meeting the condition after sieving naturally decreases, therefore the lower limit for N4 is 30. This condition aims to ensure that a certain number of first polymer particles in the aggregation region anchor a large number of second polymer particles (≥ 10). These particles play a crucial role in strengthening structural stability—these crystalline particles with more contact with amorphous particles can effectively aggregate and fix the amorphous particles (i.e., the second polymer), thus forming a larger aggregation region as a core.

[0032] The two relationships are not simply repeated, but rather a graded control strategy set for different bonding-structure balance requirements. If the above ratio conditions are not met, the number of crystalline polymer particles that undertake the anchoring function is insufficient, and the crystalline particles cannot achieve the expected effect of agglomeration and fixation of amorphous particles. After the coating is heated, the amorphous particles are prone to migration and agglomeration, and the thermal stability and bonding performance of the diaphragm deteriorate.

[0033] In one embodiment, the surface area of ​​the base film is S1, in cm². 2 The coverage area of ​​the coating is S2, in cm². 2 S1 and S2 satisfy the relationship: 0.5≤S2 / S1≤0.75.

[0034] Specifically, the ratio of S2 / S1 is any one of 0.5, 0.55, 0.6, 0.65, 0.7 or 0.75, or a range of any two ratios; in a preferred embodiment, the ratio of S2 / S1 is 0.55-0.7.

[0035] When the S2 / S1 ratio is 0.5-0.75, within this coverage range, the coating is sufficient to form a sufficient number of aggregated areas on the separator surface, providing strong interfacial adhesion. This provides continuous and reliable interfacial anchoring during the repeated expansion / contraction of the silicon-based anode, suppressing electrode slippage, bulging, or cell deformation. Simultaneously, 25%–50% of the uncoated base film area is retained. Even if amorphous particles undergo local swelling within the aggregated areas, there is still sufficient uncovered area as a "high-speed channel" for ions, maintaining an open pore structure, ensuring efficient lithium-ion transport, avoiding a significant increase in battery internal resistance, and ensuring battery rate performance and cycle stability. When the S2 / S1 ratio is less than 0.5, the adhesion point density is too low, failing to form effective interfacial bonding and failing to fully utilize the high adhesion potential of the amorphous polymer. When the S2 / S1 ratio is greater than 0.75, the ion transport channels are over-covered, significantly increasing battery internal resistance, and coating fusion and pore closing easily occur during hot pressing.

[0036] In one embodiment, the coating area of ​​the first polymer particles is S3, in cm. 2 S3 and S2 satisfy the relationship: 0.3≤S3 / S2≤0.6.

[0037] Specifically, the first polymer particle coating area S3 and the corresponding area S2 of the second polymer particle defined in this invention are both tested and characterized by the same 1000x SEM observation field of view. The testing and statistical range is completely consistent with the N1 and N2 test fields of view. That is, only the effective SEM image field of view of a single 126μm×110μm is statistically analyzed. All area parameters are the micro-area parameters within the corresponding single SEM field of view. There is no need to statistically analyze the overall coating area of ​​the diaphragm.

[0038] The specific area testing method is as follows: In the above-acquired effective uncompressed original SEM images, image grayscale analysis and contour extraction statistics are used to accurately identify and delineate the distribution areas of all first polymer particles in a single field of view, and the total area occupied by all first polymer particles in the field of view is obtained, which is the S3 corresponding to the field of view; at the same time, the effective distribution area S2 of the second polymer particles in the field of view is calculated.

[0039] Specifically, the ratio of S3 / S2 is any one of 0.3, 0.35, 0.4, 0.45, 0.5, 0.55 or 0.6, or a range of any two ratios; in a preferred embodiment, the ratio of S3 / S2 is 0.35-0.55.

[0040] When the S3 / S2 ratio is between 0.3 and 0.6, although the first polymer particles have relatively weak adhesion, their surfaces can act as "anchor points," effectively capturing and enriching highly adhesive amorphous second polymer particles through physical adsorption or interfacial forces. Within this ratio range, the first polymer provides sufficient nucleation / adhesion sites, promoting the formation of moderately sized and uniformly distributed aggregation regions of the second polymer, achieving a functional amplification effect of "less for more." In addition, S3 / S2 ≥ 0.3 ensures that there is a sufficient density of crystalline particles in the aggregation region to form a mechanical framework, inhibiting excessive swelling and flow of amorphous particles in hot pressing or electrolytes; while S3 / S2 ≤ 0.6 avoids excessive coverage by the crystalline phase, leaving enough space for dense arrangement of amorphous particles, thereby maintaining high local adhesion strength. When the S3 / S2 ratio is less than 0.3, the density of the first polymer particles is too low, and the second polymer particles cannot be effectively aggregated. The aggregated structure is unstable and easily disintegrates during processing or recycling. When the S3 / S2 ratio is greater than 0.6, the proportion of crystalline phase is too high, which dilutes the high-adhesion components and reduces the overall adhesion performance.

[0041] In one embodiment, the first polymer particle is a secondary particle.

[0042] Secondary particles are composite microspheres formed by the aggregation of multiple primary nano or submicron-sized particles; Secondary particles possess a rough or porous surface morphology and a high specific surface area. Compared to dense primary particles, they provide more physical adsorption sites and interfacial interaction areas, more effectively capturing and immobilizing amorphous secondary polymer particles. This promotes their enrichment and formation of high-density aggregation regions around the particles, thereby improving aggregation efficiency and structural stability. Secondly, the presence of mesopores or micro-gaps within the secondary particles allows them to form a "microchannel" network after coating. Even at high coverage, this can partially alleviate pore blockage caused by amorphous polymer swelling, helping to maintain the overall permeability of the membrane and the lithium-ion migration rate. Furthermore, the multi-level structure of the secondary particles can absorb some stress during hot pressing through internal particle rearrangement, preventing brittle fracture while maintaining a relatively unchanged external profile. This allows them to continuously play a "skeleton support" role, preventing the aggregation region from collapsing.

[0043] In one embodiment, the melting point of the first polymer particles is T℃, where 130≤T≤180.

[0044] Specifically, the melting point of the first polymer particle is any one value or a range of any two values ​​among 130°C, 135°C, 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, or 180°C; in a preferred embodiment, the melting point of the first polymer particle is 145–170°C.

[0045] When the melting point of the first polymer particles is 130-180℃, the high melting point (≥130℃) of the first polymer, as a crystalline particle, ensures that it maintains a solid crystal structure under conventional battery manufacturing hot pressing processes (typically 80–120℃) and high-temperature storage / cycling conditions (≤60–80℃), with almost no softening or swelling. This maintains the skeletal stability of the aggregation region and prevents the amorphous second polymer from diffusing and clogging the pores due to loss of support. It also ensures the high-temperature dimensional stability of the separator, increases the safety window before thermal shutdown, and enhances the thermal stability of the cell. The amorphous second polymer typically has a low glass transition temperature (Tg) (e.g., 50–90℃), which softens during hot pressing to provide adhesive force. Meanwhile, the high-melting-point first polymer remains rigid at this temperature. Together, they achieve the composite function of "thermally activated bonding + structural locking". When the melting point of the first polymer particles is less than 130°C, they soften or partially melt prematurely during hot pressing, and their structure degrades during cycling or high-temperature storage. Both polymers soften at similar temperatures and cannot form a division of labor mechanism of "stable skeleton + active adhesion".

[0046] In one embodiment, the particle size D50 of the second polymer particles is 0.3-1.5 μm.

[0047] Specifically, the particle size D50 of the second polymer particles is any one value or a range of any two values ​​selected from 0.3μm, 0.4μm, 0.5μm, 0.6μm, 0.7μm, 0.8μm, 0.9μm, 1.0μm, 1.1μm, 1.2μm, 1.3μm, 1.4μm, or 1.5μm; in a preferred embodiment, the particle size D50 of the second polymer particles is 0.5–1.0μm.

[0048] When the particle size D50 of the second polymer particles is 0.3-1.5μm, within this particle size range, the second polymer particles are small enough to achieve high-density arrangement on the surface or adjacent area of ​​the first polymer particles (meeting the spacing requirement of L≤0.3μm), forming a dense and bonded aggregate; at the same time, they are not too fine, avoiding problems such as poor slurry stability or coating blockage, making them suitable for industrial membrane coating processes; moreover, they can effectively fill micro-area gaps and improve interface adhesion; forming a size-matched composite structure with the first polymer particles, they can achieve a synergistic structure of "large particles guiding and small particles filling", which is conducive to building stable core-shell or island-like aggregate regions. When the particle size D50 of the second polymer particles is less than 0.3 μm, the specific surface area increases sharply, the surface energy is high, and irreversible agglomeration is very likely to occur, which can easily block the pores of the separator. During the drying process, the migration is severe and the distribution is out of control. When the particle size D50 of the second polymer particles is greater than 1.5 μm, it is difficult to achieve high-density aggregation (L≤0.3 μm is difficult to meet), the surface roughness increases, and the safety of the cell is affected. Moreover, large particles cannot effectively cover the microstructure of the electrode surface, the actual contact area is small, the peel strength is low, and it is difficult to suppress the interface debonding caused by the expansion of silicon-carbon anode.

[0049] In one embodiment, the mass swelling ratio of the second polymer is >250%.

[0050] Specifically, the test method for mass swelling rate is as follows: cut the diaphragm sample into the specified size and weigh the dry weight W0 of the diaphragm before soaking; place the sample in an electrolyte solution composed of EC / PC / DEC in a volume ratio of 1:1:1, seal it, and soak it at a constant temperature of 60℃ for 6 days; after soaking, remove the diaphragm, quickly and gently wipe off the free electrolyte on the surface of the diaphragm with filter paper, and weigh the wet weight W1 after soaking.

[0051] Formula for calculating mass swelling rate: Mass swelling rate = (W1 - W0) / W0 * 100%; When the mass swelling ratio of the second polymer is greater than 250%, the adhesive properties of the amorphous second polymer can be fully activated, significantly improving the peel strength and interface stability between the separator and the positive and negative electrodes (especially the rough silicon-carbon negative electrode). Moreover, in the aggregation region, when the particle spacing L ≤ 0.3 μm, amorphous particles with a mass swelling ratio ≥ 35% can contact and fuse with each other after swelling, forming a continuous or quasi-continuous viscoelastic film layer, realizing the transformation from "point contact" to "surface adhesion", greatly improving the local adhesion efficiency. In addition, the swollen polymer has a certain elasticity and extensibility, which can absorb mechanical stress during the expansion / contraction of the silicon-carbon negative electrode during charging and discharging, preventing interface debonding or separator tearing, maintaining the integrity and hardness of the cell structure. The high swelling of the second polymer provides "active adhesion", and the low swelling of the first polymer provides "rigid support". The two work together to achieve a composite interface structure of "soft and hard combination", maintaining pore channels while ensuring adhesion. When the mass swelling rate of the second polymer is less than 250%, the adhesive performance is insufficient, it cannot effectively adhere to the electrode, the aggregated area cannot form an effective adhesive network, and the adhesion improvement after hot pressing is limited.

[0052] In one embodiment, the first polymer is vinylidene fluoride and its copolymers.

[0053] Specifically, vinylidene fluoride and its copolymers include polyvinylidene fluoride (PVDF) homopolymers and PVDF copolymers. Among these, PVDF copolymers include one or more of the following: PVDF-HFP, PVDF-trifluoroethylene copolymers, PVDF-tetrafluoroethylene copolymers, and PVDF-chlorotrifluoroethylene copolymers. Using PVDF and its copolymers as the first polymer not only fully leverages its core advantages of low swelling, high stability, and a strong framework, but also effectively drives the formation of a high-performance adhesive aggregation structure in the second polymer through its surface polarity and structural designability. This makes it a key material choice for achieving the synergistic goal of "high adhesion, high permeability, and high safety" in membranes.

[0054] In one embodiment, the second polymer is an acrylate copolymer.

[0055] Specifically, acrylate copolymers include one or more of the following: butyl acrylate-methyl methacrylate copolymer (BA-MMA), ethyl acrylate / butyl acrylate-acrylic acid copolymer (EA / BA-AA), butyl acrylate-styrene copolymer (BA-St), butyl acrylate-acrylonitrile copolymer (BA-AN), hydroxyl-containing acrylate copolymers (such as BA-HEMA), and fluorinated acrylate copolymers (such as BA-TFEMA). Using acrylate copolymers as the second polymer in the separator coating fully leverages their advantages such as high adhesion, controllable swelling, polar interface interaction, and flexibility, making it a key material strategy for solving the problems of "interface debonding and cell deformation" in high-energy-density lithium-ion batteries (especially silicon-containing anode systems). Combined with the structural guiding role of the first polymer, the separator coating can achieve precise functional construction at the microscale, providing core material support for high-performance, high-safety batteries.

[0056] In one embodiment, the areal density of the coating is 0.25-0.55 g / m³. 2 .

[0057] Specifically, the areal density of the coating is 0.25 g / m². 2 0.3g / m 2 0.35g / m 2 0.4g / m 2 0.45g / m 2 0.5g / m 2 Or 0.55g / m 2 The value is any one point value or a range of any two point values; in a preferred embodiment, the areal density of the coating is 0.3-0.5 g / m³. 2 .

[0058] When the areal density of the coating is 0.25-0.55 g / m³ 2 The coating forms a uniform, dense layer with a reasonable pore structure on the base membrane surface. The crystalline first polymer particles construct a stable skeletal support structure, ensuring the overall mechanical strength, temperature resistance, and dimensional stability of the separator, effectively suppressing high-temperature shrinkage and deformation. Simultaneously, the amorphous second polymer particles, combining aggregated and single-particle distributions, fully fill the gaps in the coating skeleton, significantly improving the electrolyte wettability, electrolyte retention capacity, and ion conduction efficiency of the separator, optimizing interfacial contact performance, reducing battery internal resistance, and effectively improving battery cycle stability and rate performance. Furthermore, the coating exhibits excellent adhesion to the base membrane, minimizing powder shedding and peeling issues during use, thus balancing separator safety and electrochemical performance. When the coating's areal density is less than 0.25 g / m³... 2When the overall coating thickness is too thin and the effective coverage area is insufficient, a continuous and complete protective layer cannot be formed on the base film surface, resulting in low adhesion strength and easy deformation of the battery cell. When the coating's areal density is greater than 0.55 g / m³... 2 If the coating thickness is too large or the particles are too densely packed, it will cause the pores inside the coating to become blocked, the porosity to decrease significantly, the air permeability of the diaphragm to deteriorate, and black spots on the interface to easily form inside the battery cell.

[0059] In one embodiment, the diaphragm base membrane is a polyethylene membrane.

[0060] Using polyethylene film as the base membrane not only inherits its inherent advantages of high permeability, thermal safety and low cost, but also provides an ideal physical support platform for subsequent functional coatings (such as crystalline / amorphous polymer aggregate structures). It is the key basic material for achieving the "high adhesion, high safety and high cycle" goal of this invention.

[0061] In one embodiment, the coating is applied to the surface of the diaphragm base membrane in a single-sided coating manner.

[0062] By employing an asymmetric structure with "strong adhesion on one side and high transparency on the other," the core requirements of the silicon-carbon anode system for interface bonding can be precisely met without sacrificing ion transport performance. This is one of the key process strategies for achieving high energy density, high safety, and long cycle life lithium-ion batteries.

[0063] In another embodiment, the coating is applied to the surface of the diaphragm base membrane in a double-sided coating manner.

[0064] The double-sided coating method represents an advanced requirement for separator function in the context of the trend towards high-energy-density and high-reliability batteries. By constructing a strong adhesion network across the entire interface, it enhances the overall performance of the battery from multiple dimensions, including structure, electrochemistry, and safety, making it particularly suitable for high-end power batteries, energy storage batteries, and novel high-expansion electrode systems.

[0065] In one embodiment, the coating further includes a binder, a stabilizer, a dispersant, and a wetting agent. Taking the total mass of the coating as 100%, the first polymer particles account for 35%-55% of the total mass of the coating; the second polymer particles account for 9%-14% of the total mass of the coating; the binder accounts for 10%-25% of the total mass of the coating; the stabilizer accounts for 15%-35% of the total mass of the coating; the dispersant accounts for 0.5%-2% of the total mass of the coating; and the wetting agent accounts for 0.3%-2% of the total mass of the coating.

[0066] When the binder, stabilizer, dispersant and wetting agent are all within the specified ratio range of this application, they can be efficiently adapted to the two polymer particles, and the stability of slurry storage, coating construction and coating forming are optimized in a synergistic manner from multiple dimensions, so as to ensure the forming quality and comprehensive performance of the diaphragm coating.

[0067] The 10%-25% binder is mainly used to improve the bonding force between the PE base film and the coating particles, and between the coating particles. This effectively prevents problems such as powder shedding, delamination, and peeling during coating and battery service, ensuring the integrity and stability of the coating structure. At the same time, it gives the coating suitable adhesion properties and avoids defects such as cell deformation during cell assembly and cycling.

[0068] Stabilizers with a content of 15%-35% can effectively inhibit the sedimentation, agglomeration, and stratification of solid particles during the storage and settling of coating slurries through thickening and steric hindrance effects, maintain the uniformity of solid content in the slurry, ensure the long-term storage stability of the slurry from the source, and lay the foundation for subsequent stable coating.

[0069] A dispersant with a ratio of 0.5%-2% can effectively break down the soft agglomeration structure of fine polymer particles, especially modified PVDF particles, in the slurry, fully refine the particle size of the slurry, significantly improve the uniformity of slurry dispersion, and further optimize the storage stability of the slurry, avoid secondary agglomeration of particles, and ensure the continuity and consistency of the coating process.

[0070] A wetting agent content of 0.3%-2% can significantly reduce the interfacial tension between the aqueous slurry and the hydrophobic PE base film, solving the problem of difficult spreading of the aqueous slurry on the hydrophobic base film surface. This promotes uniform and sufficient spreading of the slurry to cover the base film, completely avoiding coating defects such as missed coating, uneven coating, and pinholes, and greatly improving the overall coating uniformity and molding quality. The content range of each additive component in this application is determined based on a comprehensive matching of the long-term storage stability and industrial coating stability of the slurry. Each additive performs its own function and works together to maximize the optimization of the slurry system state and coating effect.

[0071] If the content of each additive is lower than the corresponding lower limit, the additive function cannot be effectively exerted: if the binder content is too low, the adhesion between the base film and the coating particles is insufficient, the coating is prone to powdering and peeling, and the battery cell is prone to deformation; if the stabilizer content is insufficient, the slurry lacks effective thickening and steric hindrance protection, the particles are prone to rapid sedimentation and agglomeration, the slurry storage stability is extremely poor, and it cannot meet the needs of batch coating; if the dispersant content is too low, it cannot break up the soft agglomerates of particles, the slurry dispersion fineness is poor, and the particle distribution is uneven; if the wetting agent content is insufficient, the water-based slurry has poor wettability to the hydrophobic PE base film, and defects such as large-area missed coating and uneven coating thickness are very likely to occur. If the content of each additive exceeds the corresponding upper limit, the excess additive will accumulate inside and on the surface of the coating, clogging the microporous structure of the coating, reducing the coating porosity, leading to deterioration of the separator's permeability, increased electrolyte mass transfer resistance, and the appearance of black spots at the cell interface, significantly reducing the battery's rate performance and energy density. Simultaneously, excess additives can easily form an insulating layer at the electrode interface, hindering ion conduction and degrading the battery's cycle and rate performance. This application achieves a high degree of uniformity between slurry stability, coating process stability, and finished coating performance by precisely limiting the ratio of each polymer particle and functional additive. It adapts to the optimal coating areal density structure, taking into account the separator's mechanical, safety, and electrochemical performance, and significantly improving the overall service performance of the lithium battery.

[0072] In one embodiment, another aspect of the present invention provides a battery comprising a separator as described above.

[0073] In some embodiments, the device further includes a positive electrode sheet; the positive electrode sheet includes a positive current collector and a positive active material layer coated on its surface; In some embodiments, the positive current collector is at least one of aluminum foil, surface-modified aluminum foil, aluminum alloy foil, or porous aluminum-based material.

[0074] In some embodiments, the positive electrode active material layer comprises a positive electrode active material, a conductive agent, and a binder; In some embodiments, the positive electrode active material is selected from one or more of lithium cobalt oxide, nickel cobalt manganese ternary materials (NCM, such as NCM523, NCM622, NCM811), nickel cobalt aluminum ternary materials, lithium iron phosphate, or lithium-rich manganese-based materials. In some embodiments, the conductive agent may be one or more of superconducting carbon black, carbon nanotubes, or graphene. In some embodiments, the adhesive may be one or more of polyvinylidene fluoride (PVDF) or water-based adhesives; In some embodiments, the positive electrode sheet is prepared by conventional slurry coating, drying, and rolling processes.

[0075] In some embodiments, the device further includes a negative electrode sheet; the negative electrode sheet includes a negative current collector and a negative electrode active material layer coated on its surface; In some embodiments, the negative electrode current collector is at least one of copper foil, surface-modified copper foil, copper alloy foil, or porous copper-based material; In some embodiments, the negative electrode active material layer comprises a negative electrode active material, a conductive agent, and a binder; In some embodiments, the negative electrode active material is selected from one or more of natural graphite, artificial graphite, mesophase carbon microspheres (MCMB), hard carbon, soft carbon, silicon-based materials (such as silicon-carbon composites, silicon suboxide), lithium titanate, or combinations thereof; In some embodiments, the conductive agent may be one or more of superconducting carbon black, carbon nanotubes, graphene, or acetylene black. In some embodiments, the adhesive may be one or more of styrene-butadiene rubber (SBR), sodium carboxymethyl cellulose (CMC), polyacrylic acid (PAA), polyvinylidene fluoride (PVDF), or combinations thereof; In some embodiments, the negative electrode sheet is prepared by conventional slurry coating, drying, and rolling processes.

[0076] In some embodiments, the electrolyte includes lithium salt, organic solvent, and additives; In some embodiments, the lithium salt is selected from one or more of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, and lithium tetrafluoroborate, and the concentration is typically 0.8-1.2 mol / L; In some embodiments, the organic solvent is a carbonate mixture, such as a combination of EC (ethylene carbonate), DEC (diethyl carbonate), EMC (ethyl methyl carbonate), and DMC (dimethyl carbonate); In some embodiments, the additives include film-forming additives (such as FEC, VC), flame retardant additives, or overcharge protectants, with a total addition amount of 0.5%-5%.

[0077] The above-mentioned negative electrode, positive electrode and separator are assembled into a cell by stacking or winding in a "positive-separator-negative" manner, electrolyte is injected, and after formation, aging and capacity testing, it is packaged in an aluminum-plastic film soft pack, steel shell or aluminum shell to obtain a lithium-ion battery.

[0078] The battery of the present invention can be used in consumer electronics (such as smartphones and laptops), electric vehicles (such as electric vehicles and electric bicycles), and energy storage systems (such as grid energy storage and home energy storage).

[0079] The beneficial effects of the present invention will be further illustrated below with reference to the embodiments.

[0080] To make the inventive objectives, technical solutions, and beneficial effects of this invention clearer, the invention is further described in detail below with reference to embodiments. However, it should be understood that the embodiments of this invention are merely for illustrative purposes and not for limiting the invention, and the embodiments are not limited to those given in the specification. Materials not specified in the embodiments were prepared under conventional conditions or according to the conditions recommended by the material supplier.

[0081] Furthermore, it should be understood that the existence of other method steps before or after the combined steps, or the insertion of other method steps between these explicitly mentioned steps, does not preclude the existence of other method steps before or after the combined steps, or the insertion of other method steps between these explicitly mentioned steps, unless otherwise stated. It should also be understood that the combined connection relationship between one or more devices / apparatus mentioned in this invention does not preclude the existence of other devices / apparatus before or after the combined devices / apparatus, or the insertion of other devices / apparatus between these explicitly mentioned devices / apparatus, unless otherwise stated. Moreover, unless otherwise stated, the numbering of each method step is merely a convenient tool for identifying each method step, and not for limiting the order of the method steps or limiting the scope of the invention. Changes or adjustments to their relative relationships, without substantially altering the technical content, should also be considered within the scope of the invention.

[0082] In the following embodiments, the reagents, materials and instruments used, unless otherwise specified, are commercially available or can be obtained through synthesis methods known in the art.

[0083] Table 1 shows the design of diaphragm coating parameters for Examples 1-7 and Comparative Examples 1-3; Table 2 shows the membrane coating formulations for Examples 1-7 and Comparative Examples 1-3; Example 1 This embodiment illustrates the separator and battery disclosed in this invention; it includes the following operational steps: Preparation of the diaphragm: 80 parts of deionized water, 10 parts of hydroxyethyl methacrylate-modified polyvinylidene fluoride-hexafluoropropylene copolymer (first polymer particles), 2.4 parts of polyacrylate copolymer (second polymer particles), and 3.2 parts of binder were added to a mixer and stirred evenly. Then, 4 parts of stabilizer, 0.2 parts of dispersant, and 0.2 parts of wetting agent were added and stirred evenly to obtain an aqueous slurry. Using an anilox roller, the above-mentioned slurry was coated onto both surfaces of a polyethylene film via a micro-gravure roller coating method. After drying, the corresponding adhesive coating was obtained, with the areal density increment controlled at 0.35 g / m². 2 ; Preparation of positive electrode: Lithium cobalt oxide, single-walled carbon nanotubes, conductive carbon black SP, and binder PVDF are mixed in a ratio of 98.3:0.3:0.3:1.1 to prepare a positive electrode slurry. The positive electrode slurry is then coated onto the surface of the positive electrode current collector on a coating machine. After drying, rolling, cutting, and welding of tabs, a positive electrode sheet that meets the requirements is obtained.

[0084] Preparation of negative electrode: 90 parts of artificial graphite, 7 parts of silicon-carbon composite material, 0.5 parts of carbon nanotubes and 2.5 parts of negative electrode binder are mixed. The negative electrode binder is composed of sodium carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR) in a mass ratio of 1:1.5. The above negative electrode slurry is uniformly coated on the surface of copper foil current collector on a coating machine. After drying, rolling, cutting and welding of electrode tabs, the negative electrode sheet that meets the requirements is obtained.

[0085] Electrolyte preparation: In a glove box filled with dry argon, ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) are mixed evenly in a mass ratio of 30:50:20 to obtain a mixed solvent. Lithium hexafluorophosphate (LiPF6) is added to the mixed solvent to a concentration of 1.0 mol / L, and then fluoroethylene carbonate (FEC) is added as a film-forming additive at a mass of 5% of the total mass of the mixed solvent. After stirring evenly, the electrolyte is obtained.

[0086] Battery manufacturing: The positive electrode, separator, and negative electrode are aligned and stacked in sequence, and a bare cell is prepared by winding using a winding machine. The bare cell is then installed in a battery casing, and after baking, injection of the prepared electrolyte, sealing, formation, and capacity testing, a lithium-ion battery is obtained.

[0087] Examples 2-7 Examples 2-17 illustrate the separator and battery disclosed in this invention, including most of the operating steps in Example 1, with the following differences: The diaphragm coating slurry formulation shown in Table 2 was adopted, and the coating density was controlled as shown in Table 1.

[0088] Comparative Examples 1-5 Comparative Examples 1-5 are used to illustrate the separator and battery disclosed in this invention, including most of the operating steps in Example 1, the difference being: The diaphragm coating slurry formulation shown in Table 2 was adopted, and the coating density was controlled as shown in Table 1.

[0089] Performance testing The membranes prepared in Examples 1-7 and Comparative Examples 1-5 were subjected to the following performance tests: Adhesion strength test method: Cut a 20mm*200mm coated separator and a 15mm*150mm lithium cobalt oxide positive electrode strip. Stack the positive electrode strip in the center of the separator strip and hold it with A4 paper. Hot press for 5 minutes in a hot press at 85℃ and 1MPa. Take the hot-pressed sample, peel off a section of the electrode, and fix both ends of the sample in the fixtures of a universal tensile testing machine, with the electrode fixed in the upper fixture and the separator fixed in the lower fixture. Test at 100mm / min. Repeat the test for the peel value of 5 samples, take the average value as the adhesive force, and calculate the adhesion strength.

[0090] Air permeability testing method: Using a Gurley 4111N air permeability meter, the time it takes for 100 ml of gas to pass through the diaphragm is measured. The diaphragm area is 1 square inch. The air permeability increment is obtained by subtracting the air permeability of the uncoated diaphragm from the air permeability of the coated diaphragm.

[0091] Cyclic performance test: The lithium-ion battery was subjected to charge-discharge cycle tests at 45°C: it was charged to 4.5V at a constant current and constant voltage rate of 1.0C, with a cutoff current of 0.05C; then discharged to 3.0V at a constant current rate of 0.5C, and the discharge capacity C0 was recorded. This charge-discharge process was repeated until the 400th cycle, at which point the battery's discharge capacity C1 was recorded. The capacity retention rate was calculated as: C1 / C0 × 100%. The test results are shown in Table 2.

[0092] Table 2. Separator physical properties and battery performance parameters Comparing Examples 1-3 and Comparative Example 1, it can be seen that when the polymer particles include both first and second polymer particles, the increase in membrane permeability is between 19 and 28, and the bonding strength is between 18.3 and 19.6 N / m. The increase in permeability is controllable, and the bonding strength is high, which can simultaneously take into account the membrane's air permeability and conductivity as well as the interfacial bonding stability. In Comparative Example 1, the first crystalline polymer particles were completely eliminated, and only the second polymer particles were filled with a high content, resulting in a significant increase in membrane permeability to 50. The coating pore structure was severely blocked, the ion transport resistance increased dramatically, the air permeability deteriorated significantly, and the cycle capacity retention rate decreased.

[0093] Comparing Examples 1 and 4-7, it can be seen that when the content and areal density of the first polymer particles are low, the increase in air permeability is the lowest, but the bonding strength decreases, indicating that low particle content and areal density weaken the coating's bonding performance. When the melting point of the first polymer particles is low, the air permeability remains unchanged, but the bonding strength decreases slightly, proving that a suitable melting point of crystalline particles is key to ensuring bonding performance. When the particle size D50 of the second polymer particles is 0.3-1.5μm, the increase in membrane air permeability is between 21-29, and the bonding strength is 17.3-19.3 N / m. Within this parameter range, it has good adaptability, and fine-tuning of each parameter will not cause performance degradation. It can balance the membrane processing adaptability and electrochemical stability, and the overall performance remains excellent.

[0094] Comparing Example 1 with Comparative Examples 2-3, it can be seen that the areal density of Comparative Example 2 exceeds the standard by 0.7 g / m³. 2 The coating was too dense, resulting in an increase in air permeability of up to 63, which severely deteriorated air permeability and significantly hindered ion transport. In Comparative Example 3, the content of the first polymer particle was below the specified range, resulting in insufficient support of the crystalline skeleton, a significant increase in air permeability, an imbalance in the membrane pore structure, and deterioration of electrical properties. This demonstrates that the areal density and polymer particle content parameters specified in this invention are necessary conditions for balancing the air permeability, mechanical adhesion, and structural stability of the membrane. Exceeding these parameter ranges will lead to significant deterioration of one or more properties of the membrane.

[0095] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A diaphragm, characterized in that: The coating includes a base film and a coating applied to the surface of the base film. The coating includes polymer particles, which include first polymer particles and second polymer particles. The first polymer particles are crystalline polymer particles, and the second polymer particles are amorphous polymer particles. The first polymer particles adhere to the second polymer particles to form a single aggregate region. The coating includes multiple such aggregate regions. The number of second polymer particles in the coating is N1, and the number of second polymer particles in the multiple aggregate regions is N2. N1 and N2 satisfy: 0.8N1≤N2.

2. The diaphragm according to claim 1, characterized in that: The distance between the edges of two adjacent polymer particles is L, in μm, and L satisfies: L≤0.

3.

3. The diaphragm according to claim 1, characterized in that: The number of contacts between the second polymer particles and the first polymer particles is N3, and the number of first polymer particles that satisfy the corresponding number of N3 is N4; the N3 and the N4 satisfy the following relationship: Equation 1: When N3≥10, N4≥30; Equation 2: When N3≥5, N4≥60.

4. The diaphragm according to claim 1, characterized in that: The surface area of ​​the base film is S1, in cm². 2 The coverage area of ​​the coating is S2, in cm². 2 S1 and S2 satisfy the relationship: 0.5≤S2 / S1≤0.

75.

5. The diaphragm according to claim 3, characterized in that: The coating area of ​​the first polymer particle is S3, in cm. 2 S3 and S2 satisfy the relationship: 0.3≤S3 / S2≤0.

6.

6. The diaphragm according to claim 1, characterized in that: The first polymer particle is a secondary particle; And / or, the melting point of the first polymer particles is T, in °C, and T satisfies: 130≤T≤180.

7. The diaphragm according to claim 1, characterized in that: The particle size D50 of the second polymer particles is 0.3-1.5 μm; And / or, the mass swelling rate of the second polymer is >250%.

8. The diaphragm according to claim 1, characterized in that: The first polymer particles are vinylidene fluoride and its copolymer particles; And / or, the second polymer particles are acrylate copolymer particles.

9. The diaphragm according to claim 1, characterized in that: The areal density of the coating is 0.25-0.55 g / m³. 2 ; And / or, the diaphragm base membrane is a polyethylene membrane; And / or, the coating is applied to the surface of the diaphragm base membrane in a single-sided coating manner; And / or, the coating is applied to the surface of the diaphragm base membrane in a double-sided coating manner.

10. The diaphragm according to claim 1, characterized in that: The coating further includes a binder, a stabilizer, a dispersant, and a wetting agent. Taking the total mass of the coating as 100%, the first polymer particles account for 35%-55% of the total mass of the coating; the second polymer particles account for 9%-14% of the total mass of the coating; the binder accounts for 10%-25% of the total mass of the coating; the stabilizer accounts for 15%-35% of the total mass of the coating; the dispersant accounts for 0.5%-2% of the total mass of the coating; and the wetting agent accounts for 0.3%-2% of the total mass of the coating.

11. A battery, characterized in that: Includes the diaphragm as described in any one of claims 1-10.