A high-temperature resistant FR-4 copper-clad laminate and its preparation method
By constructing a gradient distribution structure between the surface layer and the core layer in FR-4 copper clad laminate, and using an imidazoline-containing silane coupling agent and a compound epoxy resin system, combined with a gradient temperature and pressure process, the problem of high adhesion of the surface layer and low thermal expansion of the core layer in FR-4 copper clad laminate during high temperature and high pressure lamination was solved, thereby improving the interfacial bonding strength and resistance to humid heat aging.
Patent Information
- Application Number
- CN202611111459.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-24
- Publication Date
- 2026-11-17
AI Technical Summary
Existing FR-4 copper clad laminates have difficulty simultaneously achieving high surface adhesion and low thermal expansion of the core layer during high-temperature and high-pressure lamination, and the interfacial bonding strength between the resin and copper foil and its resistance to damp heat aging are also poor.
The FR-4 copper clad laminate with a gradient distribution structure is constructed by creating a gradient distribution of surface A-layer adhesive and inner B-layer adhesive on a glass fiber cloth. The A-layer adhesive contains an imidazoline-containing silane coupling agent to form stable coordination bonds with the copper foil. The B-layer adhesive uses a compound of naphthalene-type epoxy resin and biphenyl-type epoxy resin and adds a high amount of inorganic filler. Combined with gradient heating and pressurization process, the resin is fully cured.
This technology achieves a performance differentiation between high surface adhesion and low thermal expansion of the core layer in copper-clad laminates after lamination, improving interfacial bonding strength and resistance to damp heat aging, and obtaining high peel strength and excellent dimensional stability.
Abstract
Description
Technical Field
[0001] This application relates to the field of polymer composite materials and electronic circuit board manufacturing, specifically to an FR-4 copper clad laminate suitable for multilayer printed circuit board lamination process and its preparation method, and particularly to an FR-4 copper clad laminate with low resin flow characteristics during high temperature and high pressure lamination process. Background Technology
[0002] FR-4 copper-clad laminate, as a core raw material in the electronics industry, has wide applications in the field of multilayer printed circuit boards. In the lamination process of multilayer circuit boards, it is typically necessary to press and cure multilayer core boards with pre-fabricated circuitry and prepregs, which serve as interlayer adhesives, into a single unit under high temperature and pressure. During this process, the resin surrounding the prepreg melts under the influence of temperature and pressure, flows, and fills the interlayer voids, ultimately curing to achieve interlayer bonding. Therefore, the resin system and structural distribution of the prepreg have a significant impact on the overall performance of the copper-clad laminate.
[0003] Current prepregs typically employ a homogeneous structure, meaning the resin composition remains consistent throughout the fiberglass cloth surface and interior. However, homogeneous prepregs, after lamination, struggle to balance the high adhesion of the surface layer with the low coefficient of thermal expansion of the core layer, resulting in low peel strength and insufficient heat resistance. Furthermore, conventional silane coupling agents can only bond with copper foil through hydrogen bonding or physical adsorption, failing to form stable chemical bonds, leading to unsatisfactory interfacial bonding strength and resistance to damp heat aging.
[0004] Therefore, how to achieve functional differentiation between the surface layer and the core layer of the prepreg after lamination, so that the surface layer has high adhesion and the core layer has low thermal expansion, while ensuring stable and reliable interfacial bonding between the resin and the copper foil, is a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0005] To address the functional differentiation between the surface and core layers of prepreg after lamination and curing, and to ensure that the surface layer has high adhesion and the core layer has low thermal expansion, while maintaining a stable and reliable interfacial bond between the resin and the copper foil, this application aims to provide a high-temperature resistant FR-4 copper clad laminate and its preparation method.
[0006] In the first aspect, this application provides a high-temperature resistant FR-4 copper-clad laminate, which adopts the following technical solution: A high-temperature resistant FR-4 copper clad laminate includes a fiberglass cloth and a resin solution impregnated on the fiberglass cloth, wherein the resin solution includes an A-resin distributed on the surface of the fiberglass cloth and a B-resin distributed inside the fiberglass cloth. The A-type adhesive comprises, by weight, 80-120 parts of bisphenol A type epoxy resin, 5-15 parts of silane coupling agent containing imidazoline, 5-20 parts of toughening agent, 2-6 parts of curing agent, 1-3 parts of accelerator, 10-30 parts of first inorganic filler, and 5-15 parts of flame retardant. The B-type adhesive comprises, by weight: 20-60 parts of naphthalene-type epoxy resin, 40-80 parts of biphenyl-type epoxy resin, 20-40 parts of linear phenolic resin, 100-200 parts of the second inorganic filler, 1-3 parts of coupling agent, 1-3 parts of dispersant, and 10-25 parts of flame retardant. The viscosity of adhesive A at 25°C is 200-600 mPa·s, and the viscosity of adhesive B at 25°C is 600-1500 mPa·s, with the viscosity of adhesive A being lower than that of adhesive B.
[0007] By employing the above technical solution, a gradient distribution structure of surface A-layer adhesive and internal B-layer adhesive was constructed within the fiberglass cloth. Adhesive A has a low viscosity and easily accumulates on the surface of the fiberglass cloth during impregnation. Its formulation contains imidazoline-containing silane coupling agents that can form stable coordination bonds with the copper foil surface, enhancing interfacial bonding strength. Simultaneously, the toughening agent in adhesive A improves interfacial toughness and reduces interfacial stress concentration. Adhesive B has a higher viscosity and accumulates within the fiberglass cloth. It is a blend of naphthalene-type epoxy resin and biphenyl-type epoxy resin, with a high filler content of a second inorganic filler, effectively reducing the thermal expansion coefficient of the core layer and improving dimensional stability and heat resistance. Through the synergistic effect of adhesives A and B, the copper-clad laminate achieves a performance differentiation between high surface adhesion and low thermal expansion of the core layer after lamination and curing.
[0008] Optionally, the imidazoline-containing silane coupling agent is a silane coupling agent with an amino group and / or an unsaturated double bond on the imidazoline ring.
[0009] Further optionally, the imidazoline-containing silane coupling agent is a silane coupling agent with an amino group and an unsaturated double bond on the imidazoline ring.
[0010] By employing the above technical solution, the imidazoline-containing silane coupling agent has an amino group and / or an unsaturated double bond on the imidazoline ring. The amino group can form a multidentate chelate structure with the copper foil surface, enhancing the interfacial coordination bond density and thus improving the interfacial bonding strength; the unsaturated double bond can participate in the resin crosslinking reaction during the curing process, forming chemically bonded flexible segments, further improving the interfacial toughness and resistance to humid heat aging.
[0011] Optionally, the imidazoline-containing silane coupling agent is prepared by reacting fatty acids with diethylenetriamine through amidation, cyclization and dehydration to generate an amino-imidazoline intermediate, which is then grafted onto the silane coupling agent. The molar ratio of the fatty acid to diethylenetriamine is 1:0.8-1.5; the molar ratio of the aminoimidazoline intermediate to the silane coupling agent is 1:0.5-2.0.
[0012] Further optionally, the molar ratio of the fatty acid to diethylenetriamine is 1:1.0-1.2; and the molar ratio of the aminoimidazoline intermediate to the silane coupling agent is 1:0.8-1.5.
[0013] By employing the above technical solution, the imidazoline-containing silane coupling agent is prepared by reacting fatty acids and diethylenetriamine through amidation, cyclization, and dehydration to generate an amino-imidazoline intermediate, which is then grafted onto the silane coupling agent. Furthermore, the molar ratios of fatty acids to diethylenetriamine and the intermediate to the silane coupling agent are optimized. By controlling the reaction ratios, the amino group content and silane group density in the coupling agent molecule can be adjusted, thereby specifically optimizing the interfacial crosslinking density and interfacial flexibility to meet the interfacial performance requirements of different application scenarios.
[0014] Optionally, the toughening agent is selected from at least one of carboxyl-terminated butadiene nitrile rubber or polyethersulfone.
[0015] Alternatively, the toughening agent may be carboxyl-terminated nitrile butadiene rubber.
[0016] By adopting the above technical solution, the toughening agent is selected from at least one of carboxyl-terminated nitrile butadiene rubber or polyethersulfone, with carboxyl-terminated nitrile butadiene rubber being more preferred. Carboxyl-terminated nitrile butadiene rubber can form a block copolymer with epoxy resin, improving interfacial toughness; polyethersulfone can form an interpenetrating network structure during epoxy curing, maintaining or increasing the glass transition temperature while improving toughness.
[0017] Optionally, the first inorganic filler is selected from at least one of spherical silica, molten silica micro powder, and boron nitride.
[0018] Optionally, the first inorganic filler is spherical silica.
[0019] Optionally, the first inorganic filler comprises spherical silica with a particle size of 1-2 μm.
[0020] Optionally, the second inorganic filler comprises spherical silica, fused silica micropowder, and boron nitride; wherein the weight ratio of the spherical silica to the fused silica micropowder is 2-4:1, and the weight ratio of the total amount of the spherical silica and the fused silica micropowder to the boron nitride is 8-20:1.
[0021] By adopting the above technical solution, the first inorganic filler is selected from at least one of spherical silica, fused silica micropowder, and boron nitride, with spherical silica being more preferred. Spherical silica has good dispersibility and flowability, which is beneficial for maintaining a moderate viscosity of the surface adhesive while not excessively affecting the bonding performance. When the first inorganic filler contains spherical silica with a particle size of 1-2 μm, it can form a good dispersion state in the surface adhesive, further optimizing the rheological properties of the adhesive. The second inorganic filler contains spherical silica, fused silica micropowder, and boron nitride, and the weight ratio of spherical silica to fused silica micropowder and the weight ratio of their total amount to boron nitride are further defined. The compound use of inorganic fillers with different particle sizes and morphologies can form a densely packed structure in the B adhesive, effectively reducing the thermal expansion coefficient of the core layer; at the same time, boron nitride has good thermal conductivity, which helps to improve the heat dissipation performance of the copper clad laminate.
[0022] Secondly, this application provides a method for preparing a high-temperature resistant FR-4 copper-clad laminate as described in the first aspect, comprising the following steps: S1. Prepare the A glue and the B glue; S2. Impregnate the fiberglass cloth with the B adhesive and blow it with hot air to form a semi-cured barrier layer in the semi-gelled state, thus obtaining a first-processed fiberglass cloth. S3. Impregnate the primary treated fiberglass cloth with adhesive A, so that adhesive A is enriched on the surface of the primary treated fiberglass cloth; S4. The glass fiber cloth obtained in step S3 is baked and cured to obtain the semi-cured sheet; S5. The multilayer prepreg and copper foil are stacked together and pressed and cured to obtain the copper-clad laminate.
[0023] By employing the above technical solution, first impregnating with adhesive B and then subjecting it to hot air blowing treatment, adhesive B forms a semi-cured barrier layer in a semi-gelled state. This barrier layer effectively prevents the subsequent impregnation of adhesive A from excessively penetrating into the interior of the fiberglass cloth, thereby ensuring a clear and stable gradient structure where adhesive A is enriched on the surface and adhesive B is enriched inside. This process is simple and controllable, facilitating the stable industrial production of gradient structures.
[0024] Optionally, the pressing and curing process is carried out using a gradient heating and gradient pressurization process.
[0025] Optionally, the gradient heating and gradient pressurization process includes: a first stage of heating from room temperature to 100°C at a pressure of 0.4-0.6 MPa; a second stage of holding at 100°C at a pressure of 0.7-0.9 MPa; a third stage of heating from 100°C to 150°C at a pressure of 1.3-1.7 MPa; a fourth stage of holding at 150°C at a pressure of 1.3-1.7 MPa; a fifth stage of heating from 150°C to 190°C at a pressure of 2.3-2.7 MPa; a sixth stage of holding at 190°C at a pressure of 2.8-3.2 MPa; and a seventh stage of cooling while maintaining a pressure of 2.8-3.2 MPa.
[0026] By adopting the above technical solution, the lamination and curing process employs gradient heating and gradient pressurization, further defining the temperature and pressure parameters at each stage. This gradient heating and gradient pressurization process allows the resin to gradually soften, flow, and fully fill the interlayer voids during lamination, avoiding excessive resin flow or interlayer bubble residue caused by excessively rapid heating or pressurization. Simultaneously, it ensures complete resin curing, resulting in a copper-clad laminate with a dense internal structure and good interfacial bonding.
[0027] In summary, this application includes at least one of the following beneficial technical effects: 1. By constructing a gradient distribution structure between the surface A-layer adhesive and the internal B-layer adhesive, and combining it with the preparation process of first impregnating the B-layer adhesive to form a semi-cured barrier layer and then impregnating the A-layer adhesive, the copper-clad laminate can simultaneously possess the performance advantages of high surface adhesion and low thermal expansion of the core layer after lamination and curing, thereby obtaining high peel strength and excellent dimensional stability. Moreover, the gradient structure is clear and stable, and the process is controllable. 2. The A adhesive uses an imidazoline-containing silane coupling agent, which can form stable coordination bonds with the copper foil surface, enhance the interfacial bonding strength, and at the same time, by controlling the molecular structure of the coupling agent to optimize the interfacial crosslinking density and interfacial toughness, the resistance to humid heat aging is significantly improved. 3. Glue B uses a blend of naphthalene-type epoxy resin and biphenyl-type epoxy resin, and adds a high amount of inorganic filler to form a tightly packed structure, which effectively reduces the thermal expansion coefficient of the core layer and improves heat resistance and heat dissipation performance. Detailed Implementation
[0028] The present application will be further described in detail below with reference to various embodiments.
[0029] The following is some information about the raw materials: Bisphenol A type epoxy resin: EEW = 180-200 g / eq; Naphthalene-type epoxy resin: EEW = 250-270 g / eq; Biphenyl-type epoxy resin: EEW = 280-300 g / eq; Linear phenolic resin: CAS: 9003-35-4, hydroxyl equivalent 105-115 g / eq; Carboxyl-terminated acrylonitrile butadiene rubber (CTBN): Carboxyl content 0.4-0.6 meq / g, number average molecular weight 3000-5000; Spherical silica: for use in A-type adhesive, particle size 1-2μm; for use in B-type adhesive, particle size 3-5μm. Fused silica micropowder: average particle size 0.3-0.8 μm, Boron nitride: average particle size 5-10 μm; Halogen-free phosphorus-containing flame retardant: CAS 225789-38-8.
[0030] Preparation Example 1: Silane Coupling Agent Containing Imidazoline 1. Preparation of alkyl imidazoline intermediates Add 100g (0.35mol) of stearic acid, 40g (0.38mol) of diethylenetriamine, and 50mL of xylene to a container, purge with nitrogen for protection, heat to 150℃, and react for 2 hours to carry out the amidation reaction. Heat to 220℃ and carry out cyclization and dehydration reaction until no more water comes out of the water separator; Xylene and excess diethylenetriamine were removed by vacuum distillation to obtain the intermediate.
[0031] 2. Grafting with silane coupling agents Dissolve 50g of the intermediate obtained in the previous step in anhydrous ethanol, and slowly add 35.4g of KH-560 type silane coupling agent dropwise, controlling the dropping rate and keeping the reaction temperature below 60℃. After the addition is complete, raise the temperature to 85℃ and reflux for 5 hours. After the reaction is complete, remove the solvent by vacuum distillation to obtain the product, which is the silane coupling agent containing imidazoline.
[0032] Preparation Example 2 The difference from Preparation Example 1 is that in step (1), the amount of stearic acid added is 100g and the amount of diethylenetriamine is 54g, and in step (2), the amount of KH-560 type silane coupling agent added is 35.4g. The other reaction conditions are the same as those in Preparation Example 1.
[0033] Preparation Example 3 The difference from Preparation Example 1 is that the amount of KH-560 silane coupling agent added in step (2) is 53.1 g, and the other reaction conditions are the same as in Preparation Example 1.
[0034] Preparation Example 4 The difference from Preparation Example 1 is that the amount of KH-560 silane coupling agent added in step (2) is 17.7g, and the other reaction conditions are the same as those in Preparation Example 1.
[0035] Preparation Example 5 The difference from Preparation Example 1 is that 99g of oleic acid was used instead of stearic acid in step (1), and the other reaction conditions were the same as in Preparation Example 1.
[0036] Example 1 Preparation of resin solution The surface adhesive (hereinafter referred to as Glue A) contains the following components by weight: 100 parts of bisphenol A type epoxy resin, 10 parts of the imidazoline-containing silane coupling agent obtained in Preparation Example 1 (hereinafter referred to as imidazoline silane), 15 parts of carboxyl-terminated butadiene-acrylonitrile rubber (CTBN), 4 parts of dicyandiamide, 2 parts of substituted urea accelerator, 20 parts of spherical silica, 12 parts of halogen-free phosphorus-containing flame retardant, and an appropriate amount of methyl ethyl ketone.
[0037] Bisphenol A type epoxy resin, imidazoline silane and CTBN are added to a reaction vessel, stirred and heated to 110°C, and kept at the temperature for 2 hours to allow the carboxyl groups of CTBN to react with the epoxy groups of epoxy resin to form a block copolymer. Cool to 60℃, add dicyandiamide, substituted urea accelerator and halogen-free phosphorus flame retardant, and stir until dissolved. After adding spherical silica and dispersing at high speed for 1 hour, the mixture is ground using a grinder until the fineness is ≤15μm. Add methyl ethyl ketone (MEK) to adjust the solid content to 70%, and continue stirring for 30 minutes to obtain glue A. The viscosity of glue A at 25°C is 400±50 mPa.s.
[0038] The core layer adhesive (hereinafter referred to as B adhesive) contains the following components by weight: 40 parts of naphthalene-type epoxy resin, 60 parts of biphenyl-type epoxy resin, 32 parts of linear phenolic resin, 120 parts of spherical silica, 40 parts of fused silica micro powder, 10 parts of boron nitride, 2 parts of wetting and dispersing agent, 1.5 parts of KH-560 type silane coupling agent, 18 parts of halogen-free phosphorus-containing flame retardant, and an appropriate amount of methyl ethyl ketone.
[0039] Naphthalene-type epoxy resin, biphenyl-type epoxy resin, linear phenolic resin, halogen-free phosphorus-containing flame retardant and KH-560 type silane coupling agent are added to the reaction vessel and stirred until dissolved. Add wetting and dispersing agent, stir evenly, then add spherical silica, molten silica micro powder and boron nitride, disperse at high speed for 1.5 hours, and grind until the fineness is ≤20μm; Add methyl ethyl ketone (MEK) to adjust the solid content to 80%, and continue stirring for 30 minutes to obtain glue B. The viscosity of glue B at 25°C is 1000±100 mPa·s.
[0040] Electronic-grade glass fiber cloth is passed through a glue tank containing B glue at a linear speed of 2.0 m / min. The temperature of the glue tank is controlled at 25℃ to ensure that the glue fully penetrates into the glass fiber bundle. The amount of glue applied is controlled by a pressure roller so that the B glue accounts for 25-35% of the mass of the glass fiber bundle. After the fiberglass cloth exits the adhesive tank, it enters the hot air knife system. The system parameters are: hot air temperature 120℃, wind speed 25m / s, air knife at a 40° angle to the cloth surface, and air knife spacing 5cm. Hot air is used to remove excess B adhesive and air bubbles from the surface. On the other hand, it rapidly heats the B adhesive on the cloth surface to a semi-gel state, while controlling the degree of B-level curing at about 25%, forming a semi-cured barrier layer. The fiberglass cloth obtained after the previous step is cooled to 35°C and immersed in a glue tank containing adhesive A. Due to capillary action and concentration difference, adhesive A will be preferentially adsorbed on the surface layer of the fiberglass cloth, thus forming a gradient distribution with adhesive A enriched on the surface and adhesive B enriched in the interior. The amount of adhesive applied is controlled by a pressure roller so that the total resin content accounts for 45±2% of the mass of the fiberglass cloth. The impregnated fiberglass cloth was then placed into a six-section vertical drying oven, and the temperature profile was set as follows: Zones 1-2: 120℃; Zones 3-4: 150℃; Zones 5-6: 170℃; The total baking time was set to 8 minutes to obtain a semi-cured sheet.
[0041] Take eight of the above-mentioned semi-cured sheets, stack them together, and cover each with a copper foil on the top and bottom. Place them in a vacuum hot press and use a gradient temperature / pressure program. The first stage temperature is set to rise from room temperature to 100°C, the pressure to 0.5 MPa, the time to 50 minutes, and the heating rate to 1.5°C / min; the second stage temperature is set to 100°C, the pressure to 0.8 MPa, and the time to 10 minutes; the third stage temperature is set to rise from 100°C to 150°C, the pressure to 1.5 MPa, and the time to 20 minutes, with a heating rate to 1.5 MPa. The heating rate is 2.7℃ / min; the fourth stage maintains 150℃ at 1.5MPa for 20 minutes; the fifth stage increases the temperature from 150℃ to 190℃ at 2.5MPa for 15 minutes; the sixth stage maintains 190℃ at 3.0MPa for 90 minutes; and the seventh stage decreases the temperature from 190℃ to 50℃ at 3.0MPa for the time required to cool to room temperature, while maintaining pressure during the cooling process.
[0042] Example 2 The difference between this embodiment and Example 1 is that the imidazoline silane coupling agent prepared in Preparation Example 2 is used in Glue A instead of the product obtained in Preparation Example 1, while the remaining components and preparation process are the same as in Example 1.
[0043] Example 3 The difference between this embodiment and Example 1 is that the imidazoline silane coupling agent prepared in Preparation Example 3 is used in Glue A instead of the product obtained in Preparation Example 1, while the remaining components and preparation process are the same as in Example 1.
[0044] Example 4 The difference between this embodiment and Example 1 is that the imidazoline silane coupling agent prepared in Preparation Example 4 is used in gel A instead of the product obtained in Preparation Example 1, while the remaining components and preparation process are the same as in Example 1.
[0045] Example 5 The difference between this embodiment and Example 1 is that the imidazoline silane coupling agent prepared in Preparation Example 5 is used in colloid A instead of the product obtained in Preparation Example 1, while the remaining components and preparation process are the same as in Example 1.
[0046] Example 6 The difference between this embodiment and Embodiment 1 is that polyethersulfone is used instead of CTBN as a toughening agent in adhesive A. Specifically: Add 8 parts of polyethersulfone to replace CTBN along with epoxy resin, heat to 120°C and stir to dissolve, forming a homogeneous solution before proceeding with subsequent operations.
[0047] Example 7 The difference between this embodiment and Example 1 is that the amount of methyl ethyl ketone is reduced and the viscosity of adhesive A is controlled at 600±50 mPa.s. The remaining components and preparation process are the same as in Example 1.
[0048] Example 8 The difference between this embodiment and Example 1 is that the amount of methyl ethyl ketone is increased, and the viscosity of glue A is controlled to be 200±30 mPa.s. The remaining components and preparation process are the same as in Example 1.
[0049] Example 9 The difference between this embodiment and Example 1 is that the amount of methyl ethyl ketone is increased, and the viscosity of the B glue is controlled to be 600±50 mPa.s. The remaining components and preparation process are the same as in Example 1.
[0050] Example 10 The difference between this embodiment and Example 1 is that the amount of methyl ethyl ketone is reduced and the viscosity of the B glue is controlled at 1500±150 mPa.s. The remaining components and preparation process are the same as in Example 1.
[0051] Example 11 The difference between this embodiment and Embodiment 1 is that the amount of spherical silica added in colloid B is adjusted from 120 parts to 80 parts, and the amount of molten silica micro powder is adjusted from 40 parts to 30 parts. The remaining components and preparation process are the same as in Embodiment 1.
[0052] Comparative Example 1 The difference between this comparative example and Example 1 is that a homogeneous semi-cured sheet was prepared using a single-tank impregnation process without hot air purging. The remaining components and pressing process are the same as in Example 1.
[0053] The specific preparation method is as follows: After mixing and stirring A and B at a mass ratio of 1:1, a mixed adhesive solution is obtained. Electronic-grade glass fiber cloth is impregnated once through the adhesive tank. The impregnated glass fiber cloth is then placed in a vertical drying oven, and the subsequent steps are the same as in Example 1.
[0054] Comparative Example 2 The difference between this comparative example and Example 1 is that ordinary aminosilane (i.e., KH-550 type silane coupling agent) is used in glue A instead of the imidazoline silane coupling agent prepared in Example 1. The remaining components and preparation process are the same as in Example 1.
[0055] Comparative Example 3 The difference between this comparative example and Example 1 is that the viscosity of glue A and glue B is adjusted to 600±50 mPa·s, while the remaining components and preparation process are the same as in Example 1.
[0056] Comparative Example 4 The difference between this comparative example and Example 1 is that hot air purging is not performed after the first impregnation with B glue, while the remaining components and preparation process are the same as in Example 1.
[0057] Performance testing To further verify the overall performance of the embodiments and comparative examples, tests were conducted on peel strength, Z-axis CTE, solderability at 288℃, and Tg, among other aspects. Tg data are presented in the order of surface Tg / core Tg, while Comparative Example 1 only contains a single-layer structure.
[0058] The test results are summarized in Table 1. Table 1 Peel strength (N / mm) Z-axis CTE (%) Solderability at 288℃ (seconds) Tg (°C) PCT peel retention rate (%) Example 1 1.73 2.3 >360 156 / 184 92 Example 2 1.89 2.3 >360 156 / 184 91 Example 3 1.78 2.3 >360 156 / 184 94 Example 4 1.65 2.4 >300 155 / 183 88 Example 5 1.70 2.3 >360 155 / 183 90 Example 6 1.62 2.3 >360 165 / 184 89 Example 7 1.58 2.4 240 155 / 183 83 Example 8 1.55 2.4 180 154 / 182 78 Example 9 1.62 2.9 210 154 / 182 80 Example 10 1.52 2.5 180 155 / 183 75 Example 11 1.68 3.1 210 154 / 180 82 Comparative Example 1 1.05 3.4 90 165 65 Comparative Example 2 1.28 2.4 210 155 / 183 75 Comparative Example 3 1.35 2.7 150 154 / 182 70 Comparative Example 4 1.48 2.5 180 154 / 182 72 Based on the various embodiments and comparative examples and Table 1, the copper-clad laminate prepared in Example 1 uses an imidazoline-containing silane coupling agent for interfacial chemical bonding. Through the gradient structure, it achieves a synergistic effect of high adhesion of the surface layer and low expansion of the core layer. A clear component transition zone is formed through a hot air purging process. The copper-clad laminate prepared in this way exhibits excellent performance in all performance indicators.
[0059] Examples 2 to 5 employed imidazoline silane coupling agents with different structural types to verify the influence of different functional groups on the imidazoline ring on interfacial properties. Example 2 used a high-amine coordination imidazoline silane; the additional amine groups retained in the molecule could form a multidentate chelate structure with the copper foil surface, enhancing the interfacial coordination bond density and thus further improving peel strength. Example 3 used a high-silane grafted imidazoline silane; the higher density of silane groups enabled the formation of a denser interfacial crosslinking network with the resin matrix, thereby improving resistance to damp heat aging. Example 4 used a low-grafting-rate imidazoline silane; the free amine groups retained in the molecule acted as latent curing accelerators, moderately reducing the interfacial layer crosslinking density and increasing interfacial flexibility, thus exhibiting superior interfacial stability under thermal shock conditions. Example 5 used an oleic acid-type imidazoline silane; the unsaturated double bonds introduced into the molecule participated in resin crosslinking during curing, forming chemically bonded flexible segments, thereby improving interfacial toughness. The above embodiments demonstrate that the interface performance of copper-clad laminates can be specifically optimized by controlling the molecular structure of imidazoline silanes.
[0060] In Example 6, polyethersulfone was used instead of CTBN as a toughening agent. As a high heat-resistant thermoplastic resin, polyethersulfone forms an interpenetrating network structure during epoxy curing, which can improve the interfacial toughness without reducing or even increasing the glass transition temperature of the material.
[0061] In Examples 7-10, the viscosity and viscosity ratio of the surface adhesive and the core adhesive were adjusted to verify the effect of the viscosity ratio on gradient formation. When the viscosity of the surface adhesive was significantly lower than that of the core adhesive, the low-viscosity adhesive could preferentially accumulate on the surface of the fiberglass cloth under capillary action during the secondary impregnation process, forming a clear compositional gradient. When the viscosities of the two were similar, the gradient structure became blurred or even disappeared, and the interfacial performance deteriorated. When the viscosity of the surface adhesive was too low, excessive penetration of the adhesive led to an excessively wide transition layer and an unclear gradient structure. When the viscosity of the core adhesive was too high, poor wetting during the first impregnation and excessive semi-curing after hot air purging resulted in an overly dense barrier layer, affecting subsequent interfacial diffusion. The results of these examples demonstrate that controlling the viscosity ratio of the surface adhesive to the core adhesive within an appropriate range is a key technical means to form a stable gradient structure.
[0062] Example 11 reduced the content of inorganic fillers in the core layer adhesive. The reduction in filler content led to a decrease in core layer rigidity, an increase in the coefficient of thermal expansion, and a decrease in solderability. This shows that a high filler content in the core layer is also a key factor in achieving low thermal expansion and high heat resistance.
[0063] Comparative Example 1 uses a homogeneous structure instead of a gradient structure. The surface and core layers are homogeneous, which cannot simultaneously meet the performance requirements of high adhesion of the surface layer and low expansion of the core layer. As a result, the performance of Comparative Example 1 is also degraded across the board.
[0064] Comparative Example 2 uses ordinary aminosilane instead of imidazoline-containing silane coupling agent. Ordinary aminosilane coupling agent can only bind to copper foil through hydrogen bonding or physical adsorption, and cannot form stable coordination bonds. Therefore, the interfacial bonding strength is significantly reduced, and the resistance to damp heat aging is also reduced accordingly. This can prove the mechanism of action of imidazoline-containing silane coupling agent in forming chemical bonds to achieve interfacial enhancement.
[0065] Comparative Example 3 made the viscosity of the surface layer adhesive and the core layer adhesive similar. During the secondary impregnation process, the surface enrichment effect of the low viscosity adhesive was weakened, the gradient structure was difficult to form, and the product performance was close to that of homogeneous products (i.e., Comparative Example 1).
[0066] Comparative Example 4 eliminated the hot air purging step after the first impregnation. The core layer adhesive that was not purged by hot air was still in a liquid state. During the second impregnation, the surface adhesive could easily penetrate into the core layer, resulting in a blurred gradient structure, an excessively wide transition zone, and a decrease in interface performance.
[0067] In summary, this invention constructs a gradient structure between the surface layer and the core layer, uses an imidazoline-containing silane coupling agent to achieve interfacial chemical bonding, and optimizes the viscosity ratio of the surface layer adhesive and the core layer adhesive, as well as the hot air purging process. The resulting FR-4 copper clad laminate possesses high peel strength, low coefficient of thermal expansion, excellent resistance to dip soldering, and good resistance to damp heat aging.
[0068] Of course, the above description is only a specific embodiment of this application and is not intended to limit the scope of the invention. All equivalent changes or modifications made in accordance with the features and principles described in the claims of this invention should be included in the scope of the claims of this invention.
Claims
1. A high-temperature resistant FR-4 copper-clad laminate, comprising fiberglass cloth and a resin impregnated on the fiberglass cloth, characterized in that, The resin adhesive includes A adhesive distributed on the surface of the glass fiber cloth and B adhesive distributed inside the glass fiber cloth. The A-type adhesive comprises, by weight, 80-120 parts of bisphenol A type epoxy resin, 5-15 parts of silane coupling agent containing imidazoline, 5-20 parts of toughening agent, 2-6 parts of curing agent, 1-3 parts of accelerator, 10-30 parts of first inorganic filler, and 5-15 parts of flame retardant. The B-type adhesive comprises, by weight: 20-60 parts of naphthalene-type epoxy resin, 40-80 parts of biphenyl-type epoxy resin, 20-40 parts of linear phenolic resin, 100-200 parts of the second inorganic filler, 1-3 parts of coupling agent, 1-3 parts of dispersant, and 10-25 parts of flame retardant. The viscosity of adhesive A at 25°C is 200-600 mPa·s, and the viscosity of adhesive B at 25°C is 600-1500 mPa·s, with the viscosity of adhesive A being lower than that of adhesive B.
2. The high-temperature resistant FR-4 copper-clad laminate according to claim 1, characterized in that, The imidazoline-containing silane coupling agent is a silane coupling agent with an amino group and / or an unsaturated double bond on the imidazoline ring.
3. The high-temperature resistant FR-4 copper-clad laminate according to claim 2, characterized in that, The imidazoline-containing silane coupling agent is prepared by reacting fatty acids with diethylenetriamine through amidation, cyclization and dehydration to generate an amino-imidazoline intermediate, which is then grafted onto a silane coupling agent. The molar ratio of the fatty acid to diethylenetriamine is 1:0.8-1.5; the molar ratio of the aminoimidazoline intermediate to the silane coupling agent is 1:0.5-2.
0.
4. The high-temperature resistant FR-4 copper-clad laminate according to claim 1, characterized in that, The toughening agent is selected from at least one of carboxyl-terminated butadiene nitrile rubber or polyethersulfone.
5. The high-temperature resistant FR-4 copper-clad laminate according to claim 1, characterized in that, The first inorganic filler is selected from at least one of spherical silica, molten silica micro powder, and boron nitride.
6. The high-temperature resistant FR-4 copper-clad laminate according to claim 5, characterized in that, The first inorganic filler comprises spherical silica with a particle size of 1-2 μm.
7. The high-temperature resistant FR-4 copper-clad laminate according to claim 1, characterized in that, The second inorganic filler comprises spherical silica, fused silica micro powder, and boron nitride; wherein the weight ratio of the spherical silica to the fused silica micro powder is 2-4:1, and the total amount of the spherical silica and the fused silica micro powder is in a weight ratio of 8-20:1 to the boron nitride.
8. A method for preparing a high-temperature resistant FR-4 copper-clad laminate according to any one of claims 1-7, characterized in that, Includes the following steps: S1. Prepare the A glue and the B glue; S2. Impregnate the fiberglass cloth with the B adhesive and blow it with hot air to form a semi-cured barrier layer in the semi-gelled state, thus obtaining a first-processed fiberglass cloth. S3. Impregnate the primary treated fiberglass cloth with adhesive A, so that adhesive A is enriched on the surface of the primary treated fiberglass cloth; S4. The fiberglass cloth obtained in step S3 is baked and cured to obtain the semi-cured sheet; S5. The multilayer prepreg and copper foil are stacked together and pressed and cured to obtain the copper-clad laminate.
9. The method for preparing high-temperature resistant FR-4 copper-clad laminate according to claim 8, characterized in that, The pressing and curing process is carried out using a gradient heating and gradient pressurization process.
10. The method for preparing high-temperature resistant FR-4 copper-clad laminate according to claim 9, characterized in that, The gradient heating and gradient pressurization process includes: a first stage of heating from room temperature to 100°C at a pressure of 0.4-0.6 MPa; a second stage of holding at 100°C at a pressure of 0.7-0.9 MPa; a third stage of heating from 100°C to 150°C at a pressure of 1.3-1.7 MPa; a fourth stage of holding at 150°C at a pressure of 1.3-1.7 MPa; a fifth stage of heating from 150°C to 190°C at a pressure of 2.3-2.7 MPa; a sixth stage of holding at 190°C at a pressure of 2.8-3.2 MPa; and a seventh stage of cooling while maintaining a pressure of 2.8-3.2 MPa.