Copper-nickel alloy spherical cores with tin plating (BGA) and their preparation methods
By combining a copper-nickel alloy core with a tin plating layer, the problems of electromigration, thermal fatigue, and dimensional consistency of the tin balls are solved, improving the reliability of the solder joint and the integrity of signal transmission, making it suitable for high-density electronic packaging.
Patent Information
- Application Number
- CN202611224133.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-13
- Publication Date
- 2026-11-17
AI Technical Summary
Existing solder balls are prone to electromigration, have short thermal fatigue life, and exhibit poor whisker growth and dimensional consistency under high current density, making it difficult to meet the requirements of high-density, high-reliability electronic packaging.
The design employs a copper-nickel alloy sphere core combined with a tin plating layer. The sphere core is prepared by ultrasonic atomization, and the tin plating layer is deposited by chemical plating or electroplating. The sphere core is then reflowed and remelted in a reducing atmosphere to form a metallurgical bond. The sphericity and diameter tolerance of the tin sphere are controlled to form an intermetallic compound layer to enhance the bonding strength.
It significantly improves the thermal fatigue life of solder joints, inhibits electromigration and tin whisker growth, ensures the size consistency of solder balls, and enhances the mechanical connection reliability and signal transmission integrity of solder joints.
Smart Images

Figure CN123124846A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of electronic packaging technology, and in particular to copper-nickel alloy ball core tin-plated BGA tin balls and their preparation methods. Background Technology
[0002] With the rapid development of microelectronics technology, products continue to move towards miniaturization, high density, and high performance, making ball grid array (BGA) packaging the mainstream packaging solution for integrated circuits due to its high I / O density and excellent electrical performance.
[0003] In BGA packaging, solder balls play a crucial role in providing electrical interconnection and mechanical support between the chip and the substrate. Their quality directly determines the electrical performance stability, mechanical connection reliability, and long-term lifespan of the entire packaged device. Therefore, innovation in solder ball materials is one of the core elements driving the development of advanced packaging technologies.
[0004] However, the limitations of traditional pure tin balls or conventional tin alloy balls, which are widely used at present, are becoming increasingly apparent in increasingly harsh application environments. These limitations are mainly reflected in the following aspects: 1. Electromigration problem: Under high current density, tin atoms are prone to electromigration, which can lead to short circuits or open circuits in the circuit.
[0005] 2. Short thermal fatigue life: Under temperature cyclic loading, the weld joint is prone to cracking due to the mismatch of thermal expansion coefficients.
[0006] 3. Whisker growth: Pure tin plating is prone to spontaneous tin whisker growth under stress and time, which can cause short circuit risks.
[0007] 4. Poor dimensional consistency: Traditional manufacturing processes make it difficult to guarantee extremely high sphericity and diameter consistency of solder balls.
[0008] Therefore, there is an urgent need for a new BGA solder ball design and fabrication scheme that can synergistically improve the solder joint's resistance to electromigration and thermal fatigue, effectively suppress solder whisker growth, and at the same time have extremely high dimensional consistency and sphericity to meet the needs of high-density, high-reliability electronic packaging. Summary of the Invention
[0009] The technical problem to be solved by the present invention is to provide copper-nickel alloy ball core tin-plated BGA tin balls and their preparation method, which solves the technical problems of existing tin balls being prone to electromigration, thermal fatigue, whisker growth and poor dimensional uniformity.
[0010] To achieve the above objectives, the present invention provides the following technical solution: Copper-nickel alloy ball core tin-plated BGA solder balls, including: The core is made of a copper-nickel alloy, in which nickel accounts for 5%-15% by mass, with the balance being copper and unavoidable impurities; A tin plating layer is applied to the outer surface of the sphere core, forming a metallurgically bonded intermetallic compound layer with the sphere core. The overall sphericity of the solder balls is greater than 99.5%, and the diameter tolerance is within ±10μm. Furthermore, the oxygen content of the copper-nickel alloy sphere is less than 50 ppm.
[0011] Furthermore, the intermetallic compound layer includes and And its thickness is 1μm to 3μm.
[0012] Furthermore, the tin plating layer is a pure tin layer or a tin alloy layer, and its thickness tolerance is controlled within ±2μm.
[0013] A method for preparing a copper-nickel alloy ball core with tin plating (BGA) as described in any of the above claims, comprising the following steps: S1. Preparation of copper-nickel alloy spherical cores: The copper-nickel alloy is melted and spherical cores are prepared under inert gas protection by ultrasonic atomization or rotating electrode method, and then sieved. S2. Core cleaning and activation: The sieved cores are subjected to alkaline degreasing, acid washing and activation treatment in sequence; S3, Tin plating: A tin plating layer is deposited on the surface of the activated sphere using chemical plating or electroplating processes; S4. Reflow Remelting: In a reducing protective atmosphere, the tin-plated ball core is heated to a temperature above the melting point of tin, so that the tin plating layer melts and is reshaped using surface tension to form a composite tin ball that is metallurgically bonded to the ball core. S5. Clean, dry and optically screen the reflowed and remelted solder balls.
[0014] Furthermore, in step S1, the inert gas is nitrogen or argon; the sieving is to obtain spherical nuclei with a particle size range of φ0.1mm to φ0.76mm.
[0015] Furthermore, in step S2, the activation treatment involves sensitizing and activating the surface of the sphere core using a palladium chloride-based activating solution.
[0016] Furthermore, step S3 is chemical tin plating, and the plating solution includes: Main salt: tin methane sulfonate 20-50 g / L; Reducing agent: Sodium hypophosphite 30-80 g / L; Complexing agent: Methanesulfonic acid 50-100 mL / L; The plating temperature is 60-75℃, and the ball nuclei are continuously tumbled in the plating solution by mechanical stirring, drums, or airflow.
[0017] Furthermore, in step S4, the reducing protective atmosphere is a formic acid atmosphere or a mixture of nitrogen and hydrogen; the peak heating temperature is 250°C to 280°C, and the reflux time is 1 to 3 minutes.
[0018] Furthermore, the optical screening in step S5 is a 100% fully automated inspection, and the inspection items include diameter, sphericity and surface defects. The screened solder balls have a sphericity greater than 99.5%, a diameter tolerance within ±10μm and no oxidation, pits or satellite balls on the surface.
[0019] In summary, this application includes at least the following beneficial technical effects of copper-nickel alloy ball core tin-plated BGA tin balls, their preparation methods, and the advantages of these methods: By using a copper-nickel alloy as the core, it exhibits higher strength and hardness compared to traditional tin-based materials. During reflow soldering, the intermetallic compound layer formed between the core and the outer tin plating layer constitutes a strong metallurgical bond with the core. This effectively disperses and absorbs stress caused by the mismatch in thermal expansion coefficients between the chip, solder joint, and substrate during temperature cycling, thereby significantly inhibiting crack initiation and propagation, greatly improving the thermal fatigue life of the solder joint, and enhancing the long-term reliability of the packaged device in harsh thermal environments. The outer tin plating layer undergoes reflow remelting, releasing internal stress and reducing the driving force for tin whisker growth. Secondly, the copper-nickel alloy spheres are denser and more stable, acting as a diffusion barrier layer to slow down the mutual diffusion rate between tin and copper atoms. This suppresses the electromigration of tin atoms under current, reducing short circuits or open circuits caused by atomic migration, and further lowering the risk of tin whisker growth. By setting the overall sphericity of the solder balls to greater than 99.5% and controlling the diameter tolerance within ±10μm, the solder balls can be precisely aligned during ball placement and reflow, resulting in uniform solder joint height and solder contour. This reduces defects such as bridging and cold solder joints caused by solder ball size differences, thereby improving the integrity of signal transmission. Attached Figure Description
[0020] Figure 1 This is the main solder ball preparation process provided in this application. Detailed Implementation
[0021] To facilitate a clear understanding of the technical means, creative features, objectives, and effects of this invention, the invention will be further described below in conjunction with specific embodiments.
[0022] The following is in conjunction with the appendix Figure 1 This application will be described in further detail.
[0023] This application discloses copper-nickel alloy spherical core tin-plated BGA tin balls and their preparation method. Example 1
[0024] Preparation of Cu-10%Ni alloy spherical cores with tin plating (BGA) tin balls with a diameter of 0.1 mm. Step 1: Preparation of copper-nickel alloy spherical cores Smelting: High-purity electrolytic copper (purity ≥99.99%) and high-purity nickel plate (purity ≥99.99%) are mixed in a mass ratio of 90:10 and smelted in a vacuum induction melting furnace to form Cu-10%Ni alloy ingots with uniform composition.
[0025] Pellet Formation: Alloy spherical cores are prepared using ultrasonic atomization. The alloy ingot is remelted under an inert gas (preferably argon) atmosphere at a controlled temperature of 150°C. The molten metal flows through an ultrasonic vibrating head (frequency 2.0 MHz), breaking it into tiny droplets. These droplets fall freely into a vertical atomization tower filled with argon gas, cool, and solidify into spherical particles.
[0026] Screening: The collected spherical particles are graded and screened using an electromagnetic screening machine, and the spherical nuclei with a particle size distribution between 0.09 mm and 0.11 mm are selected as raw materials for subsequent processing.
[0027] Step 2: Core Cleaning and Activation Alkaline degreasing: The sieved copper-nickel alloy spheres are placed in an alkaline degreasing solution at 50°C. The alkaline degreasing solution contains sodium hydroxide, sodium carbonate, trisodium phosphate and surfactants. The mixture is then ultrasonically cleaned for 5 minutes.
[0028] Overflow rinsing: Use a large volume of flowing deionized water for overflow rinsing until the rinsing solution is neutral.
[0029] Acid washing and activation: Immerse in a 5% (v / v) dilute sulfuric acid solution at room temperature for 2 minutes to remove the extremely thin oxide film on the surface. Subsequently, activate the surface with a palladium chloride-based activating solution (PdCl2 concentration 50 mg / L) for 3 minutes to allow the spherical cores to adsorb catalytically active palladium cores.
[0030] Secondary overflow cleaning: Rinse thoroughly again with deionized water to ensure no acid residue and free palladium ions remain.
[0031] Step 3: Chemical Tin Plating Plating solution preparation: Prepare a chemical tin plating solution, the composition of which is as follows: Tin methane sulfonate: 20 g / L Sodium hypophosphite: 30g / L Methanesulfonic acid: 50 mL / L Stabilizer (to prevent oxidation of tin ions and self-decomposition of the plating bath): 1.5 mL / L Adjust the pH to 4.5 using NaOH solution.
[0032] Coating process: The cleaned and activated ball nuclei are placed into a coating drum lined with polypropylene and immersed in a plating solution heated to 60°C. The drum rotates slowly at 15 rpm to ensure full and uniform contact between the ball nuclei and between the ball nuclei and the solution. The coating process lasts for 40 minutes.
[0033] Post-treatment: After the plating is completed, the spherical core is removed and quickly rinsed with deionized water to remove residual plating solution.
[0034] Step 4: Reflow and Remelting Reflux equipment: A mesh belt reflux furnace is used, and a reducing protective atmosphere is introduced.
[0035] Reflow Process: Tin-plated spheres are evenly distributed on a silicon nitride ceramic mesh belt and then introduced into a reflow oven. Formic acid vapor (formic acid concentration approximately 10% v / v) carried by nitrogen is introduced into the oven. The peak temperature of the reflow zone is set to 250°C, and the reflow time is approximately 1 minute. During this process, the tin plating completely melts, forming spheres under surface tension, and reacts with the internal copper-nickel alloy spheres to form a metallurgically bonded interface layer.
[0036] Cooling: In the cooling zone at the furnace outlet, the furnace is cooled to room temperature under nitrogen protection.
[0037] Step 5: Cleaning and Drying The cooled composite tin balls were placed in a neutral cleaning agent (5% ammonium citrate solution) and ultrasonically cleaned at a frequency of 40 kHz for 5 minutes to remove any trace oxides or contaminants that may have adhered to the surface. They were then rinsed thoroughly with deionized water and finally dried in a centrifuge at 60°C for 20 minutes.
[0038] Step Six: Optical Screening and Detection A high-precision, fully automated optical sorting machine is used to perform 100% inspection on the dried solder balls.
[0039] Diameter inspection: Using a laser measurement system with a resolution of ±1μm, solder balls with diameters strictly within the range of 0.1mm±0.008mm are screened out.
[0040] Sphericity detection: Two-dimensional projection is captured by a high-speed camera, its roundness is calculated, and solder balls with a sphericity greater than 99.5% are selected.
[0041] Surface defect detection: Using multi-angle light sources and image recognition algorithms, defective products with oxidation, pits, scratches or "satellite balls" on the surface are detected and rejected.
[0042] Step 7: Packaging In a constant temperature and humidity cleanroom (temperature 23±1℃, humidity <5% RH), qualified solder balls are loaded into anti-static plastic tapes. Once each tape is full, it is immediately placed into an aluminum foil packaging bag, vacuumed, filled with high-purity nitrogen, and then sealed.
[0043] Example 2 Preparation of Cu-10%Ni alloy spherical cores with tin plating (BGA) tin balls with a diameter of 0.3 mm. Step 1: Preparation of copper-nickel alloy spherical cores Smelting: High-purity electrolytic copper (purity ≥99.99%) and high-purity nickel plate (purity ≥99.99%) are mixed in a mass ratio of 90:10 and smelted in a vacuum induction melting furnace to form Cu-10%Ni alloy ingots with uniform composition.
[0044] Pellet Formation: Alloy spherical cores are prepared using ultrasonic atomization. The alloy ingot is remelted under an inert gas (preferably argon) atmosphere at a controlled temperature of 150°C. The molten metal flows through an ultrasonic vibrating head (frequency 2.0 MHz), breaking it into tiny droplets. These droplets fall freely into a vertical atomization tower filled with argon gas, cool, and solidify into spherical particles.
[0045] Screening: The collected spherical particles are graded and screened using an electromagnetic screening machine, and the spherical nuclei with a particle size distribution between 0.29 mm and 0.31 mm are selected as raw materials for subsequent processing.
[0046] Step 2: Core Cleaning and Activation Alkaline degreasing: The sieved copper-nickel alloy spheres are placed in an alkaline degreasing solution at 60°C. The alkaline degreasing solution contains sodium hydroxide, sodium carbonate, trisodium phosphate and surfactants. The mixture is then ultrasonically cleaned for 8 minutes.
[0047] Overflow rinsing: Use a large volume of flowing deionized water for overflow rinsing until the rinsing solution is neutral.
[0048] Acid washing and activation: Immerse in 8% (v / v) dilute sulfuric acid solution at room temperature for 5 minutes to remove the extremely thin oxide film on the surface. Subsequently, activate with palladium chloride-based activating solution (PdCl2 concentration 50 mg / L) for 3 minutes to allow catalytically active palladium nuclei to be adsorbed on the surface of the spheres.
[0049] Secondary overflow cleaning: Rinse thoroughly again with deionized water to ensure no acid residue and free palladium ions remain.
[0050] Step 3: Chemical Tin Plating Plating solution preparation: Prepare a chemical tin plating solution, the composition of which is as follows: Tin methane sulfonate: 35 g / L Sodium hypophosphite: 50g / L Methanesulfonic acid: 80 mL / L Stabilizer (to prevent oxidation of tin ions and self-decomposition of the plating bath): 1.5 mL / L Adjust the pH to 4.5 using NaOH solution.
[0051] Coating process: The cleaned and activated spheres are placed into a coating drum lined with polypropylene and immersed in a plating solution heated to 70°C. The drum rotates slowly at 15 rpm to ensure full and uniform contact between the spheres and between the spheres and the solution. The coating process lasts for 40 minutes.
[0052] Post-treatment: After the plating is completed, the spherical core is removed and quickly rinsed with deionized water to remove residual plating solution.
[0053] Step 4: Reflow and Remelting Reflux equipment: A mesh belt reflux furnace is used, and a reducing protective atmosphere is introduced.
[0054] Reflow Process: Tin-plated spheres are evenly distributed on a silicon nitride ceramic mesh belt and then introduced into a reflow oven. Formic acid vapor (approximately 10% v / v) carried by nitrogen is introduced into the oven. The peak temperature of the reflow zone is set to 260°C, and the reflow time is approximately 2 minutes. During this process, the tin plating completely melts, forming spheres under surface tension, and reacts with the internal copper-nickel alloy spheres to form a metallurgically bonded interface layer.
[0055] Cooling: In the cooling zone at the furnace outlet, the furnace is cooled to room temperature under nitrogen protection.
[0056] Step 5: Cleaning and Drying The cooled composite tin balls were placed in a neutral cleaning agent (5% ammonium citrate solution) and ultrasonically cleaned at a frequency of 40 kHz for 5 minutes to remove any trace oxides or contaminants that may have adhered to the surface. They were then rinsed thoroughly with deionized water and finally dried in a centrifuge at 60°C for 20 minutes.
[0057] Step Six: Optical Screening and Detection A high-precision, fully automated optical sorting machine is used to perform 100% inspection on the dried solder balls.
[0058] Diameter inspection: Using a laser measurement system with a resolution of ±1μm, solder balls with diameters strictly within the range of 0.3mm±0.008mm are screened out.
[0059] Sphericity detection: Two-dimensional projection is captured by a high-speed camera, its roundness is calculated, and solder balls with a sphericity greater than 99.5% are selected.
[0060] Surface defect detection: Using multi-angle light sources and image recognition algorithms, defective products with oxidation, pits, scratches or "satellite balls" on the surface are detected and rejected.
[0061] Step 7: Packaging In a constant temperature and humidity cleanroom (temperature 23±1℃, humidity <5% RH), qualified solder balls are loaded into anti-static plastic tapes. Once each tape is full, it is immediately placed into an aluminum foil packaging bag, vacuumed, filled with high-purity nitrogen, and then sealed.
[0062] Example 3 Preparation of Cu-10%Ni alloy spherical cores with tin plating (BGA) tin balls with a diameter of 0.76 mm. Step 1: Preparation of copper-nickel alloy spherical cores Smelting: High-purity electrolytic copper (purity ≥99.99%) and high-purity nickel plate (purity ≥99.99%) are mixed in a mass ratio of 90:10 and smelted in a vacuum induction melting furnace to form Cu-10%Ni alloy ingots with uniform composition.
[0063] Pellet Formation: Alloy spherical cores are prepared using ultrasonic atomization. The alloy ingot is remelted under an inert gas (preferably argon) atmosphere at a controlled temperature of 150°C. The molten metal flows through an ultrasonic vibrating head (frequency 2.0 MHz), breaking it into tiny droplets. These droplets fall freely into a vertical atomization tower filled with argon gas, cool, and solidify into spherical particles.
[0064] Screening: The collected spherical particles are graded and screened using an electromagnetic screening machine, and the spherical nuclei with a particle size distribution between 0.75 mm and 0.77 mm are selected as raw materials for subsequent processing.
[0065] Step 2: Core Cleaning and Activation Alkaline degreasing: The sieved copper-nickel alloy spheres are placed in an alkaline degreasing solution at 70°C. The alkaline degreasing solution contains sodium hydroxide, sodium carbonate, trisodium phosphate and surfactants. The mixture is then ultrasonically cleaned for 10 minutes.
[0066] Overflow rinsing: Use a large volume of flowing deionized water for overflow rinsing until the rinsing solution is neutral.
[0067] Acid washing and activation: Immerse in a 10% (v / v) dilute sulfuric acid solution at room temperature for 10 minutes to remove the extremely thin oxide film on the surface. Subsequently, activate the surface with a palladium chloride-based activating solution (PdCl2 concentration 50 mg / L) for 3 minutes to allow the spherical cores to adsorb catalytically active palladium cores.
[0068] Secondary overflow cleaning: Rinse thoroughly again with deionized water to ensure no acid residue and free palladium ions remain.
[0069] Step 3: Chemical Tin Plating Plating solution preparation: Prepare a chemical tin plating solution, the composition of which is as follows: Tin methane sulfonate: 50 g / L Sodium hypophosphite: 80g / L Methanesulfonic acid: 100 mL / L Stabilizer (to prevent oxidation of tin ions and self-decomposition of the plating bath): 1.5 mL / L Adjust the pH to 4.5 using NaOH solution.
[0070] Coating process: The cleaned and activated ball nuclei are placed into a coating drum lined with polypropylene and immersed in a plating solution heated to 75°C. The drum rotates slowly at 15 rpm to ensure full and uniform contact between the ball nuclei and between the ball nuclei and the solution. The coating process lasts for 40 minutes.
[0071] Post-treatment: After the plating is completed, the spherical core is removed and quickly rinsed with deionized water to remove residual plating solution.
[0072] Step 4: Reflow and Remelting Reflux equipment: A mesh belt reflux furnace is used, and a reducing protective atmosphere is introduced.
[0073] Reflow Process: Tin-plated spheres are evenly distributed on a silicon nitride ceramic mesh belt and then introduced into a reflow oven. Formic acid vapor (approximately 10% v / v) carried by nitrogen is introduced into the oven. The peak temperature of the reflow zone is set to 280℃, and the reflow time is approximately 3 minutes. During this process, the tin plating completely melts, forming spheres under surface tension, and reacts with the internal copper-nickel alloy spheres to form a metallurgically bonded interface layer.
[0074] Cooling: In the cooling zone at the furnace outlet, the furnace is cooled to room temperature under nitrogen protection.
[0075] Step 5: Cleaning and Drying The cooled composite tin balls were placed in a neutral cleaning agent (5% ammonium citrate solution) and ultrasonically cleaned at a frequency of 40 kHz for 5 minutes to remove any trace oxides or contaminants that may have adhered to the surface. They were then rinsed thoroughly with deionized water and finally dried in a centrifuge at 60°C for 20 minutes.
[0076] Step Six: Optical Screening and Detection A high-precision, fully automated optical sorting machine is used to perform 100% inspection on the dried solder balls.
[0077] Diameter inspection: Using a laser measurement system with a resolution of ±1μm, solder balls with diameters strictly within the range of 0.3mm±0.008mm are screened out.
[0078] Sphericity detection: Two-dimensional projection is captured by a high-speed camera, its roundness is calculated, and solder balls with a sphericity greater than 99.5% are selected.
[0079] Surface defect detection: Using multi-angle light sources and image recognition algorithms, defective products with oxidation, pits, scratches or "satellite balls" on the surface are detected and rejected.
[0080] Step 7: Packaging In a constant temperature and humidity cleanroom (temperature 23±1℃, humidity <5% RH), qualified solder balls are loaded into anti-static plastic tapes. Once each tape is full, it is immediately placed into an aluminum foil packaging bag, vacuumed, filled with high-purity nitrogen, and then sealed.
[0081] Comparative Example: Traditional Tin Ball Tin balls of the same diameter were prepared using the conventional atomization method and subjected to the same optical screening.
[0082] Performance comparison test: The solder balls prepared in Examples 1, 2, and 3 of this application, along with the solder balls from the comparative example, were balled and reflow soldered on the same BGA substrate, and then reliability tests were performed. Thermal fatigue test (-55℃-125℃, 1000 cycles): The average crack propagation length of the solder ball joints in this application is reduced by about 60% compared with the comparative application.
[0083] High-temperature storage test (150℃, 1000 hours): The thickness of the intermetallic compound (IMC) layer at the solder ball interface in this application is only 1 / 3 of that in the comparative example, and the IMC layer is denser and flatter.
[0084] Whisker observation (85℃ / 85%RH, 2000 hours): No tin whisker growth was observed on the surface of the tin balls in this application, while a small number of whiskers appeared on the surface of the tin balls in the comparative example.
[0085] Test results show that the copper-nickel alloy spherical core tin-plated BGA tin ball prepared by this invention is significantly superior to traditional alloy tin balls in terms of mechanical reliability and long-term stability.
[0086] The above are all preferred embodiments of this application, and are not intended to limit the scope of protection of this application. Therefore, all equivalent changes made in accordance with the structure, shape and principle of this application should be covered within the scope of protection of this application.
Claims
1. A copper-nickel alloy ball core with tin plating (BGA) solder ball, characterized in that, include: The core is made of a copper-nickel alloy, in which nickel accounts for 5%-15% by mass, with the balance being copper and unavoidable impurities; A tin plating layer is applied to the outer surface of the sphere core, forming a metallurgically bonded intermetallic compound layer with the sphere core. The overall sphericity of the solder balls is greater than 99.5%, and the diameter tolerance is within ±10μm.
2. The copper-nickel alloy ball core with tin plating BGA tin ball according to claim 1, characterized in that, The oxygen content of the copper-nickel alloy sphere is less than 50 ppm.
3. The copper-nickel alloy ball core with tin plating BGA tin ball according to claim 1, characterized in that, The intermetallic compound layer includes and And its thickness is 1μm to 3μm.
4. The copper-nickel alloy ball core with tin plating BGA tin ball according to claim 1, characterized in that, The tin plating layer is a pure tin layer or a tin alloy layer, and its thickness tolerance is controlled within ±2μm.
5. A method for preparing copper-nickel alloy ball core tin-plated BGA tin balls as described in any one of claims 1-4, characterized in that, Includes the following steps: S1. Preparation of copper-nickel alloy spherical cores: The copper-nickel alloy is melted and spherical cores are prepared under inert gas protection by ultrasonic atomization or rotating electrode method, and then sieved. S2. Core cleaning and activation: The sieved cores are subjected to alkaline degreasing, acid washing and activation treatment in sequence; S3, Tin plating: A tin plating layer is deposited on the surface of the activated sphere using chemical plating or electroplating processes; S4. Reflow Remelting: In a reducing protective atmosphere, the tin-plated ball core is heated to a temperature above the melting point of tin, so that the tin plating layer melts and is reshaped using surface tension to form a composite tin ball that is metallurgically bonded to the ball core. S5. Clean, dry and optically screen the reflowed and remelted solder balls.
6. The method for preparing copper-nickel alloy ball core tin-plated BGA tin balls according to claim 5, characterized in that, In step S1, the inert gas is nitrogen or argon; the sieving is to obtain spherical nuclei with a particle size range of φ0.1mm to φ0.76mm.
7. The method for preparing copper-nickel alloy ball core tin-plated BGA tin balls according to claim 1, characterized in that, In step S2, the activation treatment involves sensitizing and activating the surface of the sphere core using a palladium chloride-based activating solution.
8. The method for preparing copper-nickel alloy ball core tin-plated BGA tin balls according to claim 5, characterized in that, Step S3 is chemical tin plating, and the plating solution includes: Main salt: tin methane sulfonate 20-50 g / L; Reducing agent: Sodium hypophosphite 30-80 g / L; Complexing agent: Methanesulfonic acid 50-100 mL / L; The plating temperature is 60-75℃, and the ball nuclei are continuously tumbled in the plating solution by mechanical stirring, drums, or airflow.
9. The method for preparing copper-nickel alloy ball core tin-plated BGA tin balls according to claim 5, characterized in that, In step S4, the reducing protective atmosphere is a formic acid atmosphere or a mixture of nitrogen and hydrogen; the peak heating temperature is 250°C to 280°C, and the reflux time is 1 to 3 minutes.
10. The method for preparing copper-nickel alloy ball core tin-plated BGA tin balls according to claim 5, characterized in that, The optical screening in step S5 is a 100% fully automated inspection. The inspection items include diameter, sphericity, and surface defects. Solder balls with a sphericity greater than 99.5%, a diameter tolerance within ±10μm, and no oxidation, pits, or satellite balls on the surface are selected.