Alkylphosphonium-functionalized ion exchange resins

By using insoluble matrix ion exchange resins bonded with quaternary alkyl phosphonium salts, the problem of low removal efficiency of short-chain PFAS in existing technologies has been solved, achieving high-efficiency removal of short-chain PFAS and significantly improving the adsorption efficiency of some resins.

CN123125045APending Publication Date: 2026-11-173M INNOVATIVE PROPERTIES CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202580029425.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-23
Filing Date
2025-04-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies are ineffective at removing short-chain perfluorinated and polyfluorinated alkyl substances (PFAS) contaminants, especially PFAS materials with four or fewer carbon atoms, which have low removal efficiency in aqueous solutions.

Method used

An ion exchange resin comprising an insoluble matrix bonded with a quaternary alkyl phosphonium salt represented by the formula P(R1R2R3)+X-, wherein R1, R2, and R3 are acyclic hydrocarbon groups with carbon chain lengths from C4 to C18, is used to remove PFAS from water.

Benefits of technology

It improves the affinity for short-chain PFAS and significantly enhances the removal efficiency of PFAS. Some resins have improved the adsorption efficiency by more than three times compared with traditional tributylammonium functionalized resins.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123125045A_ABST
    Figure CN123125045A_ABST
Patent Text Reader

Abstract

An ion exchange resin comprising an insoluble matrix having functional groups bonded thereto, the functional groups comprising quaternary alkyl phosphonium salts represented by the following formula: -P(R1R2R3) + X ‑ Where X ‑ They are anionic counterions; and R1, R2, and R3 are independently carbon chain lengths from C4 to C6. 18 The acyclic hydrocarbon groups are also provided. Systems and methods for removing PFAS from water are also provided.
Need to check novelty before this filing date? Find Prior Art

Description

Background Technology

[0001] Domestic and industrial water use (i.e., wastewater) typically requires treatment before it can be safely returned to the environment. Wastewater treatment can involve a variety of physical, chemical, and biological processes and is a common form of pollution control.

[0002] As the demand for water continues to grow, there is a need to improve the efficiency and effectiveness of wastewater treatment methods and systems. Summary of the Invention

[0003] In one aspect, an ion exchange resin comprising an insoluble matrix having functional groups bonded thereto, the functional groups comprising quaternary alkylphosphonium salts represented by the following formula: - P(R1R2R3) + X - in X - It is an anion counterion; and R1, R2, and R3 are independently carbon chain lengths from C4 to C6. 18 Acyclic hydrocarbon groups.

[0004] On the other hand, a system for removing PFAS from water is provided, the system comprising: A container for containing an ion exchange resin, the ion exchange resin comprising an insoluble matrix having functional groups bonded thereto, the functional groups comprising quaternary alkyl phosphonium salts represented by the following formula: - P(R1R2R3) + X - in X- is an anion counterion; and R1, R2, and R3 are independently carbon chain lengths from C4 to C6. 18 Acyclic hydrocarbon groups; An inlet, used to direct water flow into the container to contact the ion exchange resin; and The outlet is used to direct the water flow out of the container.

[0005] On the other hand, a method for removing PFAS from water is provided, the method comprising: An aqueous solution containing PFAS is exposed to an ion exchange resin comprising an insoluble matrix having functional groups bonded thereto, the functional groups comprising quaternary alkyl phosphonium salts represented by the following formula: - P(R1R2R3) + X - in X- is an anion counterion; and R1, R2, and R3 are independently carbon chain lengths from C4 to C6. 18 Acyclic hydrocarbon groups.

[0006] As used in this article: The term "fully saturated" refers to an organic group that contains only carbon-carbon single bonds; The term "partially saturated" refers to an organic group that contains at least one carbon-carbon double or triple bond; The term “PFAS” refers to perfluorinated and polyfluoroalkyl substances, such as, for example, perfluorooctanoic acid (“PFOA”), perfluorooctane sulfonic acid (“PFOS”), perfluoropropionic acid (“PFPA”), perfluorobutyric acid (“PFBA”), trifluoroacetic acid (“TFA”), and perfluorobutane sulfonic acid (“PFBS”). The term "substituted" refers to a hydrocarbon group in which at least one hydrogen atom is replaced by a non-hydrogen atom or a group (e.g., halogen, ethyl, phenyl). The term "unsubstituted" refers to a hydrocarbon group in which no hydrogen atom is replaced by a non-hydrogen atom or group.

[0007] The features and advantages of this disclosure will be further understood when considered in conjunction with the specific embodiments and the appended claims. Attached Figure Description

[0008] Figure 1 This is a schematic diagram of a system including the alkylphosphonium-functionalized ion exchange resin according to the present disclosure.

[0009] Figure 2 The PFPA isotherms of trialkylphosphonium and trialkylammonium functionalized PS resins are shown.

[0010] Figure 3 The TFA isotherms of trialkylphosphonium and trialkylammonium functionalized PS resins are shown.

[0011] Reference numerals used repeatedly in the specification and drawings are intended to indicate the same or similar features or elements of this disclosure. It should be understood that those skilled in the art can devise many other modifications and embodiments that fall within the scope and spirit of the principles of this disclosure. The drawings may not be drawn to scale. Detailed Implementation

[0012] Removal of perfluorinated and polyfluoroalkyl substances (“PFAS”) from water is an increasingly important aspect of wastewater treatment. One method for removing PFAS is extraction using ion exchange resins. By passing PFAS-contaminated water through a bed of appropriately functionalized ion exchange resins, target PFAS molecules can be removed from the wastewater stream. However, because each PFAS is unique and different resins have different affinities for a given molecule, there has been a need to develop novel resins to effectively remove specific PFAS from wastewater streams.

[0013] For example, PFAS materials containing four or fewer carbon atoms (e.g., sodium pentafluoropropionate, trifluoroacetic acid, heptafluorobutyric acid, trifluoromethanesulfonic acid, nonafluorobutyric acid) are generally more difficult to remove from aqueous solutions than long-chain PFAS materials. Therefore, resins with higher affinity for these short-chain compounds may be more advantageous compared to resins currently available for ion exchange wastewater treatment.

[0014] Functionalized polystyrene (“PS”) resins containing ammonium groups are known and used to remove short-chain PFAS from wastewater streams, with tributylammonium-functionalized PS being the most efficient resin for removing short-chain PFAS. The synthesis of resins such as these typically involves substitution between an amine nucleophile and a chloromethylene group attached to the polystyrene polymer backbone. While direct functionalization of polystyrene beyond C4 tertiary amines has proven impractical, at least in part due to the reduced reactivity of the amine with the chloromethylene residues of the resin, leading to a lower rate of ammonium functional group formation, it has been surprisingly determined that phosphonium-functionalized PS epoxy resins, where the phosphonium functional group consists of an acyclic alkyl chain longer than four carbons (e.g., trihexylphosphine, trioctylphosphine), can provide materials with higher PFAS affinity than tributylammonium-functionalized epoxy resins.

[0015] This disclosure provides an ion exchange resin comprising an insoluble matrix having functional groups bonded thereto, wherein the functional groups comprise quaternary alkylphosphonium salts represented by the following formula: - P(R1R2R3) + X - Where X - As an anionic counterion, R1, R2, and R3 are independently carbon chain lengths from C4 to C6. 18The acyclic hydrocarbon group. The acyclic hydrocarbon group can be straight-chain or branched. The acyclic hydrocarbon group can be fully saturated or partially saturated. The acyclic hydrocarbon group can be substituted or unsubstituted. Any hydrocarbon group may optionally contain heteroatoms (e.g., O, N, S) in the hydrocarbon chain. In some embodiments, R1, R2, and R3 are the same. In some embodiments, R1, R2, and R3 are independently acyclic hydrocarbon groups with carbon chain lengths of C6 to C8. In some embodiments, the insoluble matrix is ​​selected from the group consisting of polymers, gels, clays, diatomaceous earth, and combinations thereof. In some preferred embodiments, the polymer comprises polystyrene. In some embodiments, the anionic counterion is selected from the group consisting of halide ions (e.g., chloride ions, bromide ions, iodide ions), inorganic ionic oxides (e.g., sulfate ions, nitrate ions), organic anions (e.g., acetate ions), and combinations thereof.

[0016] One or more ion exchange resins may be used in embodiments of this disclosure. Such ion exchange resins typically comprise an insoluble matrix, substrate, or support structure. In some embodiments, the support structure is in the form of small spherical beads with an average diameter ranging from about 1 mm to about 2 mm. In some embodiments, the support structure is a polymer substrate, wherein the surface of the polymer substrate includes sites for capturing and releasing ions. In some embodiments, the ion exchange resins used in this invention may be based on one or more polymer materials that may or may not be crosslinked. In some embodiments, the substrate is based on styrene that has been crosslinked with a crosslinking agent such as divinylbenzene. The crosslinked polymer substrate may also be porous, and the crosslinked substrate will tend to be rigid and non-stretchable. Uncrosslinked polymer substrates may be softer and more stretchable than crosslinked substrates and may have a gel-like consistency, depending on the materials used.

[0017] In some embodiments, the ion exchange resin may comprise a matrix material in the form of non-spherical particles. In other embodiments, the matrix may comprise a more amorphous or gel-like material, such as silica gel, diatomaceous earth, clay, etc.

[0018] In other embodiments, the ion exchange resin of this disclosure is a "bifunctional" resin comprising two or more distinct quaternary alkylphosphonium groups. For example, a mono-ion exchange resin may comprise a quaternary ammonium group + P(C6H) 13 )3 and +P(C8H 17 3.

[0019] Ion exchange resins suitable for embodiments of this disclosure can be prepared by chemical modification of resins known to those skilled in the art. In one embodiment, a suitable ion exchange resin is prepared by reacting chloromethylated styrene beads (or other resins containing electrophilic groups) with tertiary phosphine (such as, for example, trihexylphosphine or trioctylphosphine) in a polar aprotic solvent (such as 1,4-dioxane). The reaction of tertiary phosphine and chloromethylated styrene beads is represented by Scheme 1, wherein R1, R2, and R3 are as previously described.

[0020] Option 1:

[0021] Those skilled in the art will understand that the resins within the scope of this disclosure may contain matrix materials other than styrene. Suitable matrix materials include, but are not limited to, polymers, gels, clays, diatomaceous earth, and combinations of two or more of the foregoing. In some embodiments, a suitable polymer matrix is ​​polystyrene. In some embodiments, a suitable gel matrix is ​​silica gel.

[0022] Now refer to the attached diagram, Figure 1 An ion exchange system 10 for removing PFAS from water according to the present disclosure is schematically shown. System 10 includes a flow-through container 12 that can be provided in any of a variety of configurations. In the illustrated embodiment, container 12 is a cylindrical column having an ion exchange bed 14 composed of ion exchange resin contained within container 12. The ion exchange resin within bed 14 is one described herein. An inlet 16 at a first end of container 12 allows untreated water to be introduced into container 12. Water is pumped into container 12 through inlet 16 and passes through ion exchange bed 14. PFAS and other contaminants are removed from the water stream by an ion exchange mechanism provided by the resin in ion exchange bed 14. The treated water is then directed out of container 12 through an outlet valve 18 at the end of container opposite inlet 16.

[0023] In all embodiments, untreated water containing PFAS is exposed to an ion exchange resin for a sufficient time to allow the PFAS in the untreated water to be adsorbed onto the resin during the ion exchange process, which replaces the PFAS with another anion, such as chloride ions. The untreated water can be exposed to the resin in any manner. Figure 1In the method of the ion exchange system 10, an ion exchange bed is provided within a container including an inlet valve and an outlet valve. Untreated water is directed into the container through the inlet valve and passes through the ion exchange bed, where PFAS are removed. The water thus treated contains reduced levels of PFAS and exits the container through the outlet valve. The stream can be directed from the outlet valve to another treatment station for further PFAS reduction, or for removal or treatment to remove or neutralize other impurities.

[0024] In other embodiments, a certain amount of untreated water may be placed in a container together with a sufficient amount of ion exchange resin. The amount of resin in the container is typically selected to provide sufficient ion exchange capacity to adsorb the intended PFAS load. The container may be shaken or stirred or agitated in some way to ensure that the PFAS are fully adsorbed onto the resin and the ion exchange process is completed. The water and resin can then be separated (e.g., by centrifugation, filtration, and / or decantation) to produce a certain volume of treated water.

[0025] The purposes and advantages of this disclosure are further illustrated by the following non-limiting examples, but the specific materials and quantities cited in these examples, as well as other conditions and details, should not be considered as an excessive limitation of this disclosure.

[0026] Example

[0027] Unless otherwise specified, all parts, percentages, proportions, etc., used in the examples and other parts of the specification are by weight, and all reagents used in the examples are available from or can be purchased from general chemical suppliers, or can be synthesized by conventional methods. The following abbreviations are used in this section: mL = milliliters, min = minutes, h = hours, g = grams, mol = moles, mmol = millimoles, ℃ = degrees Celsius.

[0028]

[0029] Preparation Example 1 (PE-1). Preparation of Tributylphosphonium Functionalized Polystyrene Resin .

[0030] The resin (1.0 g) was placed in a 25 mL thick-walled flask with tributylphosphine (1.0 g, 4.9 mmol) and 1,4-dioxane (5 mL, 58.57 mmol) and heated to 90 °C for 48 hours. The reaction mixture was cooled to room temperature, filtered, washed with approximately 100 mL of H₂O, followed by washing with 100 mL of MeOH, and then dried in an oven at 90 °C for two days. The material was characterized by IR spectroscopy.

[0031] Preparation Example 2 (PE-2). Preparation of Trihexylphosphonium-functionalized polystyrene resin .

[0032] The resin (1.0 g) was placed in a 25 mL thick-walled flask with trihexylphosphine (1.30 g, 4.5 mmol) and 1,4-dioxane (5 mL, 58.57 mmol) and heated to 90 °C for 48 hours. The reaction mixture was cooled to room temperature, filtered, washed with approximately 100 mL of H₂O, followed by washing with 100 mL of MeOH, and then dried in an oven at 90 °C for two days. The material was characterized by IR spectroscopy.

[0033] Preparation Example 3 (PE-3). Preparation of Trioctylphosphonium Functionalized Polystyrene Resin .

[0034] The resin (1.0 g) was placed in a 25 mL thick-walled flask with trioctylphosphine (1.70 g, 4.5 mmol) and 1,4-dioxane (5 mL, 58.57 mmol) and heated to 90 °C for 48 hours. The reaction mixture was cooled to room temperature, filtered, washed with approximately 100 mL of H₂O, followed by washing with 100 mL of MeOH, and then dried in an oven at 90 °C for 2 days. The material was characterized by IR spectroscopy.

[0035] Preparation Example 4 (PE-4). Preparation of Tricyclohexylphosphonium-functionalized polystyrene resin .

[0036] The resin (1.0 g) was placed in a 25 mL thick-walled flask with tricyclohexylphosphine (1.25 g, 4.5 mmol) and 1,4-dioxane (5 mL, 58.57 mmol) and heated to 90 °C for 48 hours. The reaction mixture was cooled to room temperature, filtered, washed with approximately 100 mL of H₂O, followed by washing with 100 mL of MeOH, and then dried in an oven at 90 °C for 2 days. The material was characterized by IR spectroscopy.

[0037] Preparation Example 5 (PE-5). Preparation of Triphenylphosphonium-Functionalized Polystyrene Resin .

[0038] The resin (1.0 g) was placed in a 25 mL thick-walled flask with triphenylphosphine (1.17 g, 4.5 mmol) and 1,4-dioxane (5 mL, 58.57 mmol) and heated to 90 °C for 48 hours. The reaction mixture was cooled to room temperature, filtered, washed with approximately 100 mL of H₂O, followed by washing with 100 mL of MeOH, and then dried in an oven at 90 °C for 2 days. The material was characterized by IR spectroscopy.

[0039] Comparative Example 1 (CE-1). Preparation of Tributylammonium Functionalized Polystyrene Resin .

[0040] The resin (1.0 g) was placed in a 25 mL thick-walled flask with tributylamine (3.8 mL, 16 mmol) and 1,4-dioxane (5 mL, 58.57 mmol) and heated to 90 °C for 48 hours. The reaction mixture was cooled to room temperature, filtered, washed with approximately 100 mL of H₂O, followed by washing with 100 mL of MeOH, and then dried in an oven at 90 °C for 2 days. The material was characterized by IR spectroscopy.

[0041] Procedure for PFPA adsorption isotherm experiment : Preparation of TFA solution : The 1000 ppm TFA solution was prepared by dissolving sodium trifluoroacetate (1.20 g) in deionized water (998.80 mL).

[0042] Concentrated synthetic groundwater solutions (120 ppm NaCl; 120 ppm Na2SO4; 40 ppm NaNO3; and 900 ppm NaHCO3) are prepared by dissolving appropriate amounts of each of the listed salts in deionized water.

[0043] 1 L of TFA solution of a given concentration (2.5 ppm; 5 ppm; 10 ppm) is prepared by combining 500 mL of synthetic groundwater solution with the required amount of 1000 ppm TFA solution, and then diluting with deionized water to a volume of 1 L. This provides the experimental stock solution used in TFA isotherm studies.

[0044] PFPA solution preparation : The 1000 ppm PFPA solution was prepared by dissolving sodium pentafluoropropionate (1.14 g) in deionized water (998.86 mL).

[0045] Concentrated synthetic groundwater solutions (120 ppm NaCl; 120 ppm Na2SO4; 40 ppm NaNO3; and 900 ppm NaHCO3) are prepared by dissolving appropriate amounts of each of the listed salts in deionized water.

[0046] 1 L of PFPA solution of a given concentration (2.5 ppm; 5 ppm; 10 ppm) is prepared by combining 500 mL of synthetic groundwater solution with the required amount of 1000 ppm PFPA solution, and then diluting with deionized water to a volume of 1 L. This provides the experimental stock solution used in PFPA isotherm studies.

[0047] Isotherm Experiment : Add approximately 50 mg of the required resin and 50 g of the required PFPA stock solution to a 2 oz polypropylene bottle. Seal the bottle and place it on a mechanical shaker for 48 hours. After removing it from the shaker, aliquot the solution into plastic containers for LC-MS analysis (≥3 mL sample) using a 0.45 μm polypropylene syringe filter. Dilute the sample 100X and 1000X with a 1:1 acetonitrile / water solution before analysis using the following equipment and settings: Instrument: Agilent 6470 TRIPLE QUAD LCMS MAID 1665 Column: IonPac AS17-C 2x 250mm (210519005) Solvent A: Water containing 50 mM ammonium bicarbonate Solvent B: Methanol Gradient: Maintain 80% B for 1 minute, then reduce to 50% B after 10 minutes. Stop time: 11 minutes Runtime after completion: 6 minutes Injection volume: 10 mL Column temperature: 40℃ Flow rate: 0.3 mL / min MS: Negative Ion Electronic Injection “Ce” is the concentration of the analyte in the solution at equilibrium, measured by LC-MS, in ppm. The “qe” value is calculated using the following formula: .

[0048] The results are shown in Tables 2 and 3 below.

[0049]

[0050] like Figure 2 As shown, the slope of the line calculated for each resin is a measure of the resin's effectiveness in adsorbing a given analyte (in this case, PFPA). The data obtained indicate that the most effective material is the trioctylphosphine-modified resin, which is almost four times more effective than the tributylammonium-modified resin.

[0051]

[0052] like Figure 3 As shown, the slope of the line calculated for each resin is a measure of the resin's effectiveness in adsorbing a given analyte (in this case, TFA). The data obtained indicate that the most effective materials are the resins modified with trioctylphosphonium and trihexylphosphonium, which are slightly more than three times more effective than the resin modified with tributylammonium.

[0053] All references, patents, and patent applications cited in the above-mentioned patent-certified applications are incorporated herein by reference in their entirety. In the event of any inconsistency or contradiction between the incorporated references and this application, the information in the foregoing description shall prevail. The foregoing description, given to enable those skilled in the art to practice this disclosure protected by the claims, should not be construed as a limitation on the scope of this disclosure, which is defined by the claims and all their equivalents.

Claims

1. An ion exchange resin comprising an insoluble matrix having functional groups bonded thereto, the functional groups comprising quaternary alkylphosphonium salts represented by the following formula: - P(R1R2R3) + X - in X - It is an anion counterion; and R1, R2, and R3 are independently carbon chain lengths from C4 to C6. 18 Acyclic hydrocarbon groups.

2. The ion exchange resin according to claim 1, wherein R1, R2 and R3 are the same.

3. The ion exchange resin according to claim 1, wherein R1, R2 and R3 are independently acyclic hydrocarbon groups with a carbon chain length of C6 to C8.

4. The ion exchange resin according to claim 1, wherein the insoluble matrix is ​​selected from the group consisting of polymers, gels, clays, diatomaceous earth, and combinations thereof.

5. The ion exchange resin according to claim 4, wherein the polymer comprises polystyrene.

6. The ion exchange resin according to claim 1, wherein the anion counterion is selected from the group consisting of halide ions, inorganic ionic oxides, organic anions, and combinations thereof.

7. A system for removing PFAS from water, the system comprising: A container for containing an ion exchange resin, the ion exchange resin comprising an insoluble matrix having functional groups bonded thereto, the functional groups comprising quaternary alkyl phosphonium salts represented by the following formula: - P(R1R2R3) + X - in X- is an anion counterion; and R1, R2, and R3 are independently carbon chain lengths from C4 to C6. 18 Acyclic hydrocarbon groups; An inlet, the inlet being used to direct water flow into the container, thereby contacting the ion exchange resin; and An outlet, which is used to direct water flow out of the container.

8. The system according to claim 7, wherein R1, R2 and R3 are identical.

9. The system according to claim 8, wherein R1, R2 and R3 are independently acyclic hydrocarbon groups with a carbon chain length of C6 to C8.

10. The system of claim 7, wherein the insoluble matrix is ​​selected from the group consisting of polymers, gels, clays, diatomaceous earth, and combinations thereof.

11. The system of claim 10, wherein the polymer comprises polystyrene.

12. The system according to claim 1, wherein the anion is selected from the group consisting of halide ions, inorganic ionic oxides, organic anions, and combinations thereof.

13. A method for removing PFAS from water, the method comprising: An aqueous solution containing PFAS is exposed to an ion exchange resin comprising an insoluble matrix having functional groups bonded thereto, the functional groups comprising quaternary alkylphosphonium salts represented by the following formula: - P(R1R2R3) + X - in X- is an anion counterion; and R1, R2, and R3 are independently carbon chain lengths from C4 to C6. 18 Acyclic hydrocarbon groups.

14. The method of claim 13, wherein R1, R2 and R3 are the same.

15. The method according to claim 13, wherein R1, R2 and R3 are independently straight-chain hydrocarbon groups with a carbon chain length of C6 to C8.

16. The method of claim 13, wherein the insoluble matrix is ​​selected from the group consisting of polymers, gels, clays, diatomaceous earth, and combinations thereof.

17. The method of claim 16, wherein the polymer comprises polystyrene.

18. The method of claim 13, wherein the anionic counterion is selected from the group consisting of halide ions, inorganic ionic oxides, organic anions, and combinations thereof.