Method and apparatus for manufacturing metal laminated structures

By using nitrogen gas with a small molecular weight as the outer protective gas and argon gas as the central protective gas in the metal lamination forming technology, laminar gas flow is formed, which solves the problem of limited oxidation suppression range of protective gas in the existing technology, and realizes effective oxidation protection and high-precision forming of metal raw materials at high temperature.

CN123125075APending Publication Date: 2026-11-17MITSUBISHI ELECTRIC CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202480091035.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-04-23
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing metal lamination forming technology, the oxidation suppression range of protective gas is limited, which makes metal raw materials easy to oxidize at high temperatures. In particular, it is difficult to achieve high-precision and wide-range oxidation protection in easily oxidized materials such as titanium alloys.

Method used

The outer protective gas nozzle injects nitrogen gas with a smaller molecular weight, while the central protective gas nozzle injects inert argon gas to form a laminar gas flow, which expands the oxidation inhibition range. By controlling the gas flow rate and volume, effective protection is ensured around the processing point.

Benefits of technology

It effectively expands the oxidation inhibition range of the protective gas, prevents the metal raw materials from oxidizing at high temperatures, improves the quality and precision of the metal laminate structure, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123125075A_ABST
    Figure CN123125075A_ABST
Patent Text Reader

Abstract

The method for manufacturing a metal laminate structure is a method for manufacturing a metal laminate structure by depositing metal on a workpiece, comprising the following steps: supplying a laser beam (3) and a central protective gas (6) from a processing head (13); while supplying the laser beam (3) and the central protective gas (6), spraying an outer protective gas (10) from an outer protective gas nozzle (11) provided around the processing head (13), the outer protective gas containing a gas type with a molecular weight smaller than that of the central protective gas (6); and while supplying the laser beam (3) and the central protective gas (6), supplying a wire (1) to a processing point (5) from the wire supply mechanism (16) while operating the wire supply mechanism (16).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a metal laminate structure and an apparatus for manufacturing a metal laminate structure. Background Technology

[0002] Previously, as a technique for creating three-dimensional objects, it was known to use a manufacturing apparatus for metal lamination, a technique called additive manufacturing (AM). Metal lamination is a technique that involves repeatedly melting and solidifying metal raw materials to layer metal shapes onto a substrate.

[0003] When melting metal raw materials, the materials reach high temperatures. To suppress oxidation, an inert gas, known as a protective gas, is injected near the processing point. This protective gas is integrated with the processing nozzle, isolating oxygen near the processing point. If the forming process continues, the input heat exceeds the dissipation heat, causing the base metal to accumulate heat. If additive forming is performed on a heated object, the formed object reaches an even higher temperature, exceeding the oxidation temperature of the metal raw material. This temperature is not limited to the area near the processing point; the entire formed object becomes extremely hot. Under such conditions, oxidation of the formed object cannot be suppressed. As a result, for example, when using easily oxidized titanium alloys as the metal raw material, a significant reduction in ductility due to oxidation occurs, thus failing to obtain the desired properties. Therefore, to broaden the range of protective gases, a technical solution involving dual or triple protective gas nozzles has been proposed.

[0004] Patent Document 1 relates to a dual nozzle used in gas-shielded arc welding, disclosing a basic dual nozzle structure with gas nozzles arranged around the arc welding heat source. Patent Document 2 relates to a triple nozzle, disclosing a structure and flow rate for an intermediate shielding gas to prevent mixing of the inner and outer shielding gases. Patent Document 3 discloses a structure that uses both nitrogen and argon gases simultaneously to suppress defects during laser welding.

[0005] Patent Document 1: Japanese Patent Application Publication No. 2023-23971

[0006] Patent Document 2: International Publication No. 2022 / 163820

[0007] Patent Document 3: Japanese Patent Application Publication No. 2009-39749 Summary of the Invention

[0008] There are two major challenges with existing technology. The first challenge stems from the use of dual nozzles that extend the oxygen isolation range obtained through the protective gas. A wider oxygen isolation range makes the shaped object less susceptible to oxidation. Therefore, in principle, using the largest possible dual nozzle is sufficient. However, in recent years, high-precision shaping via feedback control through height and temperature measurements has become necessary in AM (Advanced Machining) shaping. This necessitates the installation of various sensors, such as height, temperature, and vision sensors, near the machining point. Therefore, there are limits to increasing the size of the dual nozzle. Furthermore, 5-axis machining is required for high-precision machining, but if the protective gas nozzle near the machining point becomes larger, interference will occur between the worktable and the protective gas nozzle when the worktable is tilted.

[0009] In the technologies disclosed in Patent Documents 1 and 2, techniques are employed to make the airflow spiral or triple-structured for the purpose of rectifying the gas flow, tending to increase the overall size of the nozzle. The technology also discloses setting the flow rate to a predetermined value or higher; however, increasing the flow rate will generate turbulence, so simply increasing the flow rate may not be effective.

[0010] Another issue arises from the differences between laser welding and AM (arm welding). Patent Document 3 employs a double nozzle to suppress porosity during laser welding, but the purpose of laser welding is to join two components, requiring fewer heating cycles than AM. The technology disclosed in Patent Document 3 aims to isolate oxygen near the processing point during processing, not to suppress oxidation during heat accumulation by setting the protective gas range over a wide area. Therefore, unlike laser welding, suppressing oxidation of the stacked metal structure after heat accumulation becomes a challenge.

[0011] The present invention was made in view of the above circumstances, and its object is to provide a method for manufacturing a metal laminate structure that can appropriately expand the range of protective gases that inhibit oxidation.

[0012] To address the aforementioned issues and achieve the objectives, the present invention relates to a method for manufacturing a metal laminate structure by depositing metal onto a workpiece. This method is characterized by comprising the following steps: supplying a heat source and a central protective gas from a processing head; while supplying the heat source and central protective gas, ejecting an outer protective gas from an outer protective gas nozzle disposed around the processing head, the outer protective gas containing gas types with a molecular weight smaller than that of the central protective gas; and while supplying the heat source and central protective gas, supplying metal raw materials to the processing point from the raw material supply mechanism while simultaneously operating the raw material supply mechanism.

[0013] The effects of the invention

[0014] The method for manufacturing the metal laminate structure according to the present invention has the following effect: it can appropriately expand the range of protective gases that inhibit oxidation. Attached Figure Description

[0015] Figure 1 This is a partial cross-sectional view of the manufacturing apparatus for the metal laminate shape according to the embodiment.

[0016] Figure 2 This is an overall cross-sectional view of the manufacturing apparatus for the metal laminate shape involved in the embodiment.

[0017] Figure 3 This is a block diagram showing the hardware structure of the control device in the manufacturing apparatus for the metal laminate shape involved in the embodiment.

[0018] Figure 4 This is a diagram showing the processing circuit when the function of the control device in the manufacturing apparatus for the metal laminate shape involved in the embodiment is implemented by the processing circuit.

[0019] Figure 5 Figure 1 shows the oxidation and nitriding temperatures estimated based on the TG (Thermogravimetry)-DTA (Differential Thermal Analysis) measurements of pure titanium.

[0020] Figure 6 The second figure shows the oxidation and nitriding temperatures estimated based on TG-DTA measurements of pure titanium.

[0021] Figure 7 Figure 1 is a schematic cross-section of the outer protective gas nozzle involved in Embodiment 1.

[0022] Figure 8 Figure 2 is a schematic cross-section of the outer protective gas nozzle involved in Embodiment 1.

[0023] Figure 9 Figure 3 is a schematic cross-section of the outer protective gas nozzle involved in Embodiment 1.

[0024] Figure 10 Figure 4 is a schematic cross-section of the outer protective gas nozzle involved in Embodiment 1.

[0025] Figure 11 This is a schematic diagram showing the plan of the outer protective gas nozzle involved in Embodiment 1.

[0026] Figure 12 This is a graph showing the conditions and oxygen content measurement results involved in Example 1.

[0027] Figure 13 This is a diagram illustrating the settings involved in Embodiment 1.

[0028] Figure 14 This is a diagram illustrating the conditions and results involved in Example 2.

[0029] Figure 15 This is a schematic cross-sectional view of the connection between the outer protective gas nozzle and the outer protective gas piping involved in Embodiment 3.

[0030] Figure 16 This is a diagram illustrating the conditions and results involved in Example 3.

[0031] Figure 17 This is a schematic diagram showing the cross-section and plan view of the outer protective gas nozzle involved in Embodiment 4.

[0032] Figure 18 This is a diagram illustrating the conditions and results involved in Example 4.

[0033] Figure 19 The graph shows whether the performance is qualified or not based on the oxygen and nitrogen content of each condition involved in Example 5. Detailed Implementation

[0034] The manufacturing method and apparatus for the metal laminate structure according to the embodiments will now be described in detail based on the accompanying drawings.

[0035] Implementation

[0036] The embodiments relate to a method for manufacturing a metal laminated shape and an apparatus 100 for manufacturing a metal laminated shape. First, the apparatus 100 for manufacturing a metal laminated shape used in the method for manufacturing a metal laminated shape will be described.

[0037] The structure of the manufacturing apparatus 100 for the metal laminate shape according to the embodiment will be described. Figure 1 This is a partial cross-sectional view of the manufacturing apparatus 100 for the metal laminate shape according to the embodiment. Figure 1 A partial cross-section of the manufacturing apparatus 100 for creating stacked metal structures is schematically shown. Figure 1 It contains the letters "X", "Y", and "Z". "X" refers to the X-axis, a horizontal axis; "Y" refers to the Y-axis, a horizontal axis orthogonal to the X-axis; and "Z" refers to the Z-axis, which represents the vertical direction. Figure 2 This is an overall cross-sectional view of the manufacturing apparatus 100 for the metal laminate shape according to the embodiment. Figure 2 A schematic cross-section of the manufacturing apparatus 100 for creating stacked metal structures is shown. Figure 2 Zhongyu Figure 1 Similarly, it includes characters such as "X", "Y" and "Z". Hereinafter, "manufacturing apparatus 100 for metal laminated shapes" is sometimes referred to as "manufacturing apparatus 100".

[0038] like Figure 1 As shown, the manufacturing apparatus 100 includes: a wire nozzle 2 that supplies wire 1 as a metal raw material; a beam nozzle 4 that emits a laser beam 3 as a heat source to heat the wire 1; and a central protective gas nozzle 7 that sprays a central protective gas 6 toward the processing point 5. The manufacturing apparatus 100 also includes: an outer protective gas nozzle 11 that sprays an outer protective gas 10 from around the central protective gas nozzle 7 onto the base material 8 and the shaping object 9; and a worktable 12 that holds the base material 8 and the shaping object 9. The shaping object 9 is a stack of weld beads formed by melting the wire 1 with the laser beam 3 emitted from the beam nozzle 4, and is a structural whole formed on the base material 8.

[0039] In this embodiment, the beam nozzle 4 and the central protective gas nozzle 7 are integrated. Alternatively, the beam nozzle 4 and the central protective gas nozzle 7 can be separate units, provided that the central protective gas nozzle 7 can supply the central protective gas 6 to the processing point 5. The wire nozzle 2 is the raw material supply unit, the beam nozzle 4 is the heating unit, and the central protective gas nozzle 7 and the outer protective gas nozzle 11 are protective gas injection units.

[0040] (Definition of processing point 5)

[0041] Processing point 5 is the position where the wire 1 is heated when the laser beam 3 is emitted from the beam nozzle 4 onto the shaping object 9 or the substrate material 8. The molten wire 1 is deposited on the shaping object 9 after the laser beam 3 is emitted from the beam nozzle 4 and shaped into the desired shape. Therefore, processing point 5 is also the shaping position of the shaping object 9.

[0042] (Overall structure of processing head 13)

[0043] like Figure 1 As shown, the manufacturing apparatus 100 includes a processing head 13. In this embodiment, a beam nozzle 4, a central protective gas nozzle 7, and an outer protective gas nozzle 11 are fixed to the processing head 13. The processing head 13 moves relative to the worktable 12 on which the object 9 is placed. That is, the processing head 13 moves relative to the worktable 12, thereby allowing the beam nozzle 4, the central protective gas nozzle 7, and the outer protective gas nozzle 11 to move relative to the worktable 12.

[0044] (Instructions for wire nozzle 2)

[0045] The wire nozzle 2, acting as the raw material supply unit, supplies wire 1, which is a metal raw material. The wire nozzle 2 guides the wire 1 toward the processing point 5, the location reached by the laser beam 3 emitted from the beam nozzle 4. The area fully encompassed by the region where the wire 1 is melted and expanded by the laser beam 3 is defined as the processing area. The processing point 5 is contained within the processing area. Figure 1 As shown, the wire nozzle 2 is positioned differently from the beam nozzle 4, causing the wire 1 to travel in a direction inclined relative to the direction in which the laser beam 3 is emitted from the beam nozzle 4. Depending on the shape of the object 9, one or both of the relative positions and orientations of the wire nozzle 2 and the beam nozzle 4 can be changed.

[0046] like Figure 2 As shown, the supply of wire 1 is controlled by a wire supply mechanism 16, which includes a spool 14, a rotary motor 15, and a wire nozzle 2. The wire supply mechanism 16 is a raw material supply mechanism. The spool 14 is a source of metal raw material on which wire 1 is wound. The spool 14 is mounted on a rotary motor 15, which is a servo motor. The spool 14 rotates with the drive of the rotary motor 15, thereby drawing wire 1 from the spool 14. The wire 1 drawn from the spool 14 passes through the wire nozzle 2 and is supplied to the processing point 5. If the rotary motor 15 is rotated in the opposite direction to the direction in which wire 1 is drawn from the spool 14, the wire 1 supplied to the processing point 5 can be pulled out. In this case, the rotary motor 15 rotates in the opposite direction and winds up the drawn wire 1, storing it in the spool 14. The method of supplying wire 1 can also be other than the method described above.

[0047] Wire 1 is a metallic raw material used to manufacture metal laminated structures. For example, the material of wire 1 can be a Ni-based alloy, Fe-based alloy, Al-based alloy, or Ti-based alloy, or other metals. Wire 1 can also be replaced with powdered material.

[0048] (Explanation of beam nozzle 4)

[0049] The beam nozzle 4, serving as the heating element, emits a laser beam 3, which acts as a heat source, toward the shaping position of the object 9. The laser beam 3 heats the wire 1 supplied from the wire nozzle 2, causing the wire 1 to melt. As described above, the shaping position of the object 9 is the processing point 5. A heating mechanism 19 for emitting the laser beam 3 is constructed using a laser oscillator 17, an optical cable 18, and the beam nozzle 4. Figure 2 As shown, the beam nozzle 4 is connected to the laser oscillator 17, which generates the laser beam 3, via an optical cable 18. The laser beam 3 is emitted from the laser oscillator 17, through the optical cable 18, and out of the beam nozzle 4. The heat source is not limited to the laser beam 3. An electric arc can also be used as a heat source, for example.

[0050] (Instructions for using protective gas nozzles)

[0051] The central protective gas nozzle 7 and the outer protective gas nozzle 11 are protective gas injection parts that inject gas toward the mold 9 or its surroundings to suppress oxidation of the mold 9. The central protective gas nozzle 7 injects central protective gas 6 toward the processing point 5 in the same direction as the laser beam 3 emitted from the beam nozzle 4.

[0052] The central protective gas injection mechanism 20 includes a central protective gas supply device 22, a central protective gas piping 23, and a central protective gas nozzle 7. The external protective gas injection mechanism 21 includes an external protective gas supply device 24, an external protective gas piping 25, and an external protective gas nozzle 11.

[0053] Central protective gas 6 is supplied from central protective gas supply device 22 to processing point 5 via central protective gas piping 23 and central protective gas nozzle 7. Processing point 5 is a laser welding section, so the temperature of processing point 5 is very high. If cheaper nitrogen is used as central protective gas 6, nitriding will occur depending on the type of material. Therefore, argon is used as the central protective gas.

[0054] The outer protective gas 10 is supplied from the outer protective gas supply device 24 through the outer protective gas piping 25 and the outer protective gas nozzle 11 to the area surrounding the base material 8 and the molded object 9. The outer protective gas 10 can be argon or nitrogen. If nitrogen is used, a wider protection range can be obtained compared to using argon.

[0055] The outer protective gas nozzle 11 is an annular nozzle arranged around the central protective gas nozzle 7. Inside the outer protective gas nozzle 11 is a mechanism for dispersing the outer protective gas 10 supplied from the outer protective gas supply device 24 and the outer protective gas piping 25. The outer protective gas nozzle 11 disperses the outer protective gas 10, spraying it as a laminar flow around the base material 8 and the molding 9.

[0056] (Instructions for workbench 12)

[0057] A machining head 13, equipped with a beam nozzle 4, a central protective gas nozzle 7, and an outer protective gas nozzle 11, moves relative to a worktable 12. The machining head 13 is moved by a machining head drive device 26. The worktable 12 rotates or moves via a rotating device 27. The machining head 13, the machining head drive device 26, the worktable 12, and the rotating device 27 together form a moving mechanism 28 that enables relative movement between the machining head 13 and the worktable 12. The moving mechanism 28 has five machining axes. The above structure is one example of the structure of the moving mechanism 28, and the structure of the moving mechanism 28 is not limited to the above structure.

[0058] like Figure 2 As shown, the worktable 12 is connected to the rotating device 27 located above the rotating device 27. A base material 8 is placed on the worktable 12, and deposits are accumulated on the base material 8. By rotating or moving the worktable 12 via the rotating device 27, the posture or position of the shaped object 9 can be changed. That is, by moving the worktable 12, the shaped object 9 can be moved relative to the processing head 13. Since the manufacturing apparatus 100 has the rotating device 27, it is also possible to form shaped objects 9 with complex shapes.

[0059] (Control mechanism of control device 29)

[0060] like Figure 2 As shown, the manufacturing apparatus 100 also includes a control device 29, which controls the operation of the manufacturing apparatus 100 according to an NC (Numerical Control) program. The control device 29 controls the wire supply mechanism 16, the heating mechanism 19, the central protective gas injection mechanism 20, the outer protective gas injection mechanism 21, and the moving mechanism 28. The control device 29 may be, for example, a numerical control (NC) device. The control device 29 outputs various commands, thereby controlling the operation of the manufacturing apparatus 100.

[0061] Regarding the control of the wire supply mechanism 16, the control device 29 outputs a command corresponding to the supply quantity of metal raw materials to the rotary motor 15, thereby controlling the drive of the rotary motor 15. The control device 29 controls the drive of the rotary motor 15, thereby adjusting the speed at which wire 1 is supplied from the spool 14 towards the processing point 5. Regarding the control of the heating mechanism 19, the control device 29 outputs a command corresponding to the output conditions of the laser beam 3 to the laser oscillator 17, thereby controlling the laser oscillation in the laser oscillator 17, and emitting the laser beam 3 from the beam nozzle 4.

[0062] Regarding the control of the protective gas injection mechanism, the control device 29 outputs a command corresponding to the supply amount of the central protective gas 6 to the central protective gas supply device 22, and outputs a command corresponding to the supply amount of the outer protective gas 10 to the outer protective gas supply device 24, thereby controlling the supply amounts of the central protective gas 6 and the outer protective gas 10. Regarding the control of the processing head 13 constituting the moving mechanism 28, the control device 29 outputs a movement command to the processing head drive device 26, thereby controlling the drive of the processing head drive device 26 to move the processing head 13.

[0063] Regarding the control of the worktable 12 constituting the moving mechanism 28, the control device 29 outputs a rotation command to the rotating device 27, thereby controlling the drive of the rotating device 27 to cause the worktable 12 to move or rotate. In order to shape the desired object 9, the control device 29 controls the moving mechanism 28, thereby causing the processing head 13 and the worktable 12 to move relative to each other. As described above, the control device 29 controls the wire supply mechanism 16, the heating mechanism 19, the central protective gas injection mechanism 20, the outer protective gas injection mechanism 21, and the moving mechanism 28, thereby enabling the manufacturing apparatus 100 to manufacture the desired object 9.

[0064] (Regarding the hardware of control device 29)

[0065] The hardware structure of the control device 29 will be described. Figure 2 The control performed by the control device 29 shown is achieved by executing a control program by hardware, which is a program for controlling the manufacturing device 100.

[0066] Figure 3 This is a block diagram illustrating the hardware structure of the control device 29 included in the manufacturing apparatus 100 for the metal laminated structure according to the embodiment. The control device 29 includes: a CPU (Central Processing Unit) 30, which performs various processes; RAM (Random Access Memory) 31, which contains a data storage area; ROM (Read Only Memory) 32 as non-volatile memory; an external storage device 33; and an input / output interface 34, which is used to input information to and output information from the control device 29. Figure 3 Each structural element shown is connected to all other structural elements via bus 35.

[0067] The CPU 30 executes the programs stored in the ROM 32 and the external storage device 33. The overall control of the manufacturing apparatus 100 by the control device 29 is achieved by the CPU 30 executing the aforementioned programs.

[0068] External storage device 33 is either an HDD (Hard Disk Drive) or an SSD (Solid State Drive). External storage device 33 stores control programs and various data. ROM 32 stores the control program, such as a boot loader like BIOS (Basic Input / Output System) or UEFI (Unified Extensible Firmware Interface); that is, it stores the software or program that controls the hardware. The control program can also be stored in ROM 32.

[0069] The program stored in ROM 32 and external storage device 33 is loaded into RAM 31. CPU 30 expands the control program into RAM 31 and executes the control program, thereby performing various processes. Input / output interface 34 is an interface that connects control device 29 to devices outside control device 29. Processing programs are input to input / output interface 34. Input / output interface 34 outputs various instructions. Control device 29 may also have input devices such as keyboard and pointing devices and output devices such as displays.

[0070] The control program can also be stored on a computer-readable storage medium. The control device 29 can also store the control program stored in the storage medium to an external storage device 33. The storage medium can be a floppy disk (i.e., a portable storage medium) or a semiconductor memory (i.e., flash memory). The control program can also be installed from a computer or server device external to the control device 29 via a communication network. As described above, the functions of the control device 29 are implemented through a computer or controller.

[0071] The function of the control device 29 can also be realized by a dedicated hardware, namely a processing circuit, used to control the manufacturing device 100. Figure 4 This is a diagram showing the processing circuit 99 when the function of the control device 29 in the manufacturing apparatus 100 of the metal laminate shape according to the embodiment is implemented by the processing circuit 99. Figure 4 The processing circuit 99 is shown in the block diagram. That is, the functions of the control device 29 can also be implemented by the processing circuit 99. The processing circuit 99 can be a single circuit, a composite circuit, a programmable processor, a parallel-programmable processor, an ASIC (Application Specific Integrated Circuit), an FPGA (Field-Programmable Gate Array), or a combination thereof. Regarding the various functions of the control device 29, some can be implemented using dedicated hardware, while the remainder can be implemented using software or firmware.

[0072] (Instructions for manufacturing and use)

[0073] Next, the operation of the manufacturing apparatus 100 according to the embodiment and the manufacturing method of the metal laminate shape using the manufacturing apparatus 100 will be described.

[0074] A laser beam 3 is emitted from a beam nozzle 4 that moves relative to a worktable 12 on which the substrate material 8 and the shaping object 9 are placed. The laser beam 3 heats the wire 1 supplied by the wire nozzle 2, thereby attaching the shaping object 9 onto the substrate material 8. The manufacturing apparatus 100 then stacks the shaping object 9 on the attached shaping object 9 through the same process as described above, thereby producing the desired metal laminated shaping object.

[0075] The manufacturing conditions for the metal laminated shape are determined by the laser output conditions selected based on the material of the wire 1, the supply amount of the wire 1, the axial movement speed of the beam nozzle 4 fixed to the processing head 13, the type and flow rate of the central protective gas 6, and the type and flow rate of the outer protective gas 10.

[0076] (Explanation of Central Protective Gas 6)

[0077] A central protective gas 6 is injected toward processing point 5. The purpose of the central protective gas 6 is to prevent the entrapment of oxygen and nitrogen from the air into processing point 5, thus preventing oxidation or other changes in the wire 1. Oxidation or other changes include oxidation and nitriding, or both. Sometimes the wire 1 is replaced with powdered metal material. Due to the heat source of the irradiated laser beam 3, the temperature of processing point 5 becomes a high temperature above the melting point of the metal material. Therefore, it is required that no changes in state such as oxidation or nitriding occur at the high temperature of the molten metal material. Argon or helium, among other inert gases, are selected as candidates for the central protective gas 6. From an economic point of view, argon is used as the central protective gas 6. Furthermore, the heat source is not limited to the laser beam 3.

[0078] (Explanation of outer protective gas 10)

[0079] The outer protective gas 10 is sprayed from the outer protective gas nozzle 11, which is located outside the central protective gas nozzle 7 that sprays the central protective gas 6, towards the area surrounding the processing point 5. The area where the oxygen is isolated by the central protective gas 6 is obtained has a width of about 5 mm to 10 mm in the planar direction. If the size of the shaped object 9 exceeds 10 mm, the oxygen isolation effect of the central protective gas 6 cannot be obtained for a portion of the shaped object 9. The purpose of the outer protective gas 10 is to prevent oxidation by preventing that portion from contacting air when it deviates from the area where the oxygen is isolated by the central protective gas 6, as a part of the shaped object 9 that has accumulated heat through continuous forming. The central protective gas 6 is sprayed onto the processing point 5 as described above to suppress the oxidation and nitriding of the molten metal, and the temperature of the area targeted by the central protective gas 6 is very high. On the other hand, the temperature of the area targeted by the outer protective gas 10 is the temperature of the heat accumulation, which is lower than the temperature of the processing point 5. As described above, this application focuses on the difference in temperature between the areas targeted by the central protective gas 6 and the outer protective gas 10.

[0080] (Explanation of the difference between the oxidation temperature and the nitriding temperature)

[0081] The oxidation and nitriding of metallic raw materials caused by temperature differences are explained. Figure 5 Figure 1 shows the oxidation and nitriding temperatures estimated based on TG-DTA measurements of pure titanium. Figure 6 Figure 2 shows the oxidation and nitriding temperatures estimated based on TG-DTA measurements of pure titanium. When titanium powder is heated to a constant temperature in an air atmosphere, the oxidation behavior is estimated based on the mass increase due to oxidation. It is determined that oxidation is gradual up to approximately 400°C, accelerates around 500°C, and rapidly increases above 600°C. Similarly, when titanium powder is heated to a constant temperature in a nitrogen atmosphere, nitriding does not occur up to 400°C, begins gradually above 400°C, and intensifies above approximately 700°C. Since the mass increase is smaller than that of oxidation, nitriding is less sensitive than oxidation. That is, it is assumed that titanium, when heated to, for example, 600°C, will oxidize rapidly when exposed to air, but hardly nitriding occurs in a nitrogen atmosphere. Therefore, it is possible to appropriately differentiate the type of gas used for the temperature range during molding.

[0082] (The effect caused by the difference in the types of gases)

[0083] The effects of differentiating gas types are explained. The central protective gas 6 uses argon, which has a relatively high molecular weight, while the outer protective gas 10, which surrounds the central protective gas 6, uses nitrogen, which has a relatively low molecular weight. This reduces pressure loss. Regarding the outer protective gas 10, to prevent the entrainment of surrounding air, it needs to be ejected from the outer protective gas nozzle 11 in a laminar flow manner. Because a large flow rate of gas is ejected from the piping, the outer protective gas 10 flowing into the outer protective gas piping 25 becomes turbulent. Therefore, it is necessary to uniformly disperse the outer protective gas 10 within the outer protective gas nozzle 11 to achieve a laminar flow before ejection.

[0084] The outer protective gas 10 is supplied from the outer protective gas nozzle 11 via the outer protective gas supply device 24 and the outer protective gas piping 25. The diameter of the outer protective gas nozzle 11 is larger than that of a typical piping, resulting in a greater inflow velocity than outflow velocity of the outer protective gas 10. This difference in velocity leads to pressure loss. The pressure loss of the gas flowing through the circular pipe can be calculated using the Darcy-Weisbach equation, which states that pressure loss is proportional to fluid density. Therefore, nitrogen, with its smaller molecular weight and lower density, reduces pressure loss compared to argon. Consequently, if nitrogen is used instead of argon for the outer protective gas 10, the outer protective gas 10 ejected from the outer protective gas nozzle 11 can be dispersed over a wider area, providing protection over a broader range compared to the case where argon is used.

[0085] As a side effect of using nitrogen as the outer protective gas 10 instead of argon, nitrogen is cheaper and more economical than argon. As mentioned above, considering the difference between the nitriding and oxidation temperatures of the metal raw material, argon is not required for the outer protective gas 10; nitrogen, with its relatively small molecular weight and good dispersibility, can be used. That is, if nitrogen is used as the outer protective gas 10, a large-scale oxygen isolation effect that was previously unattainable can be achieved.

[0086] (Explanation of gas flow rate, etc.)

[0087] Several points should be noted regarding the use of the outer protective gas 10. The common purpose of both the central protective gas 6 and the outer protective gas 10 is to prevent the entrainment of oxygen and nitrogen from the air into the processing point 5, thus avoiding oxidation and nitriding of the metal raw material. Therefore, it is important to be able to inject the central protective gas 6 and the outer protective gas 10 into the processing point 5, the base material 8, and the shaping object 9, or their surroundings, without entraining ambient gases. Therefore, the central protective gas 6 and the outer protective gas 10 are preferably laminar flows rather than turbulent flows.

[0088] Whether a flow is laminar or turbulent is determined by the Reynolds number. Generally, it is known that turbulence occurs when the Reynolds number exceeds 2300. The Reynolds number is determined by the kinematic viscosity coefficient, characteristic length, and flow velocity. Therefore, the smaller the nozzle diameter and the higher the flow velocity, the easier it is to generate turbulence. Thus, it is necessary to control the flow velocity of the protective gas and the flow rate used to determine that velocity.

[0089] Next, we will explain the precautions when using nitrogen as the outer protective gas 10. As mentioned above, since processing point 5 is at a high temperature, nitrogen flow could cause nitriding. Therefore, it is necessary to prevent the outer protective gas 10 from flowing into processing point 5. To do this, the flow rate of the central protective gas 6 needs to be greater than the flow rate of the outer protective gas 10.

[0090] The central protective gas 6 and the outer protective gas 10 are in laminar flow, and the flow rate of the central protective gas 6 is greater than that of the outer protective gas 10, thereby obtaining the desired characteristics.

[0091] As described above, the metal laminate manufacturing apparatus 100 according to the embodiment includes: a wire supply mechanism 16 that supplies wire 1; and a processing head 13 that includes a portion of a heating mechanism 19 and a central protective gas nozzle 7 for injecting central protective gas 6. The manufacturing apparatus 100 also includes: an outer protective gas injection mechanism 21 that injects outer protective gas 10 supplied from an outer protective gas pipe 25 connected to the side of the outer protective gas nozzle 11 provided outside the central protective gas nozzle 7; and a moving mechanism 28 that moves a worktable 12 on which a shape 9 formed based on the wire 1 supplied from the wire supply mechanism 16 is placed.

[0092] The method for manufacturing a metal laminate shape by depositing metal on a workpiece according to the embodiment includes the following steps: supplying a laser beam 3 and a central protective gas 6 from a processing head 13; while supplying the laser beam 3 and the central protective gas 6, ejecting an outer protective gas 10 from an outer protective gas nozzle 11 disposed around the processing head 13, the outer protective gas 10 containing gas types with a molecular weight smaller than that of the central protective gas 6; and while supplying the laser beam 3 and the central protective gas 6, supplying wire 1 to the processing point 5 from the wire supply mechanism 16 while activating the wire supply mechanism 16. More specifically, the laser beam 3 and the central protective gas 6 are supplied to the processing point 5, and the outer protective gas 10 is supplied around the processing point 5.

[0093] The outer protective gas 10 contains gas species with molecular weights smaller than those of the central protective gas 6. Therefore, the manufacturing method of the metal laminate structure according to the embodiment can appropriately expand the range of protective gases that inhibit oxidation. Furthermore, since the outer protective gas 10 contains gas species with molecular weights smaller than those of the central protective gas 6, the range of protective gases that inhibit oxidation can be appropriately expanded without increasing the size of the central protective gas nozzle 7 and the outer protective gas nozzle 11. For example, the central protective gas 6 uses argon, and the outer protective gas 10 uses nitrogen.

[0094] The following are specific examples. In Examples 1 to 3, for the purpose of quantifying the effect of oxygen isolation, the shape was not evaluated, but the oxygen concentration was measured.

[0095] (Example 1) (Differences between argon and nitrogen)

[0096] In Example 1, the difference between using argon and using nitrogen as the outer protective gas 10 is explained based on the measurement of oxygen concentration.

[0097] Figure 7 Figure 1 is a schematic cross-section of the outer protective gas nozzle 11 according to Embodiment 1. The outer protective gas pipe 25 is provided on the opposite side of the outlet of the outer protective gas 10. A structure is formed inside the outer protective gas nozzle 11 to disperse and uniformly spray the gas. The diameter of the outlet of the central protective gas nozzle 7 is set to 10 mm, the outer diameter of the outlet of the outer protective gas nozzle 11 is set to 70 mm, the inner diameter of the outlet of the outer protective gas nozzle 11 is set to 15 mm, and the shape of the outlet of the outer protective gas nozzle 11 is set to annular. The central protective gas nozzle 7 and the outer protective gas nozzle 11 are combined by placing the central protective gas nozzle 7 at the hole inside the outer protective gas nozzle 11.

[0098] To ensure uniform and dispersed gas ejection, a dot matrix structure and a partition structure are provided inside the outer protective gas nozzle 11. The dot matrix structure can be fabricated using a 3D printing device, with fine grid dimensions set according to CAD (Computer-Aided Design) data. The partition structure is designed to rectify the flow of the outer protective gas 10, which flows from the inlet through the outer protective gas piping 25, after being dispersed by the dot matrix structure. For example, a partition structure is provided at the nozzle outlet, which divides the space into rings at 5mm intervals in the radial direction. The dot matrix structure is one example; alternatively, the interior of the outer protective gas nozzle 11 can be filled with a component consisting of wool, which serves as a gas dispersion mechanism. Regarding the partition structure, partition plates can be provided, or it can be integrally formed with the outer protective gas nozzle 11. Figure 11 This is a schematic diagram showing the planar shape of the outer protective gas nozzle 11 according to Embodiment 1. Figure 11 As shown, a plurality of partition structures 36 are provided inside the outer protective gas nozzle 11 involved in Embodiment 1. Each of the plurality of partition structures 36 is cylindrical in shape. A single partition structure 36 may also be provided inside the outer protective gas nozzle 11.

[0099] The outlet of the outer protective gas nozzle 11 is set to form a 45° cone angle relative to the outlet of the central protective gas 6. This is to suppress interference between the outer protective gas 10 and the worktable 12 when the worktable 12 is tilted during 5-axis machining. The aforementioned 45° cone angle is not mandatory for the outlet of the outer protective gas nozzle 11. Figures 8 to 10 As shown, the outlet of the central protective gas nozzle 7 and the outlet of the outer protective gas nozzle 11 can be aligned, the distance between the outlet and the substrate material can be constant, or a portion of the wire 1 supplied from the wire nozzle 2 can be wrapped inside the outer protective gas nozzle 11. Figure 8 Figure 2 is a schematic cross-section of the outer protective gas nozzle 11 involved in Embodiment 1. Figure 9 Figure 3 is a schematic cross-section of the outer protective gas nozzle 11 involved in Embodiment 1. Figure 10 Figure 4 is a schematic cross-section of the outer protective gas nozzle 11 involved in Embodiment 1.

[0100] In Example 1, for the purpose of comparing argon and nitrogen, as an example of gas flow rate, etc., by... Figure 12 The oxygen content was measured under conditions A to C as shown on the left. Figure 12 This is a graph showing the conditions and oxygen content measurement results involved in Example 1. Figure 13 This diagram illustrates the setup involved in Example 1. An oxygen concentration meter 37 is disposed on the substrate material 8. Argon is used as the central protective gas 6, and the central protective gas 6 flows at 10 L / min. Comparisons were made under three conditions: condition A (without using the outer protective gas 10), condition B (using nitrogen as the outer protective gas 10), and condition C (using argon as the outer protective gas 10). Figure 12 The flow rate is recorded as a reference. While the exact flow rate is difficult to determine, the reference flow rate at the nozzle can be easily calculated by dividing the flow rate by the cross-sectional area. With processing point 5 set to 0mm, an oxygen concentration meter 37 is installed at a distance from processing point 5 along the shaping direction. The oxygen concentration is measured under conditions A through C.

[0101] Figure 12The results of oxygen concentration measurements under various conditions are shown. It was determined that the oxygen concentration was high under condition A, without the use of the outer protective gas 10. This is because the central protective gas 6 alone cannot adequately isolate the air. Next, conditions B and C, using the outer protective gas 10, are compared. Under condition B, the oxygen concentration at the 8mm position is 300ppm, and under condition C, the oxygen concentration at the 16mm position is also 300ppm. As described above, it is evident that using nitrogen as the outer protective gas 10 doubles the protective performance under the same flow rate conditions. Even when protection is provided through the same nozzle under the same conditions, the protection range expands due to the difference in gas type.

[0102] (Example 2) (Study on flow conditions)

[0103] The flow conditions are described in Example 2. In Example 2, to determine whether there is an oxygen barrier effect, the results of using argon in Example 1 were used as a reference. Based on the fact that the flow rate can be below 1000 ppm at the 12 mm position, it is determined that oxygen barrier performance is achieved. Figure 14 This is a diagram illustrating the conditions and results involved in Example 2.

[0104] (Conditions D~G)

[0105] To confirm the protective performance when the flow rate of the central protective gas 6 is set to the lower limit, the flow rate of the central protective gas 6 was set to a small amount of 5 L / min, and the flow rate of the outer protective gas 10 was adjusted. It was determined that under condition D, a flow rate of 30 L / min for the outer protective gas 10 was insufficient to achieve adequate protective performance. This indicates that the flow rate per unit area is low relative to the spray area of ​​the outer protective gas nozzle 11, and 30 L / min is not sufficient to ensure appropriate protective performance. It was determined that appropriate protective performance was achieved under conditions E and F, but a tendency for high oxygen concentration was observed under condition G with a flow rate of 150 L / min.

[0106] The gas was visualized using schlieren, confirming that the outer protective gas 10 ejected from the outer protective gas nozzle 11 was ejected as turbulent flow. This is believed to be because the flow rate became excessive, resulting in an extremely high velocity of the outer protective gas 10 flowing from the outer protective gas piping 25 to the outer protective gas nozzle 11. Inside the outer protective gas nozzle 11, the outer protective gas 10 was not properly dispersed and was ejected. Based on this result, it can be concluded that increasing the flow rate of the outer protective gas 10 to ensure adequate protective performance may induce turbulence.

[0107] (Conditions H~I)

[0108] With the aim of controlling the oxygen isolation effect by changing the flow rate of the central protective gas 6, the flow rate of the central protective gas 6 was set to 10 L / min, and the flow rate of the outer protective gas 10 was adjusted. It was confirmed that under condition I, turbulence was generated in the same way as under condition G.

[0109] (Conditions J to M)

[0110] The behavior of the central protective gas 6 was confirmed when its flow rate was increased to 20 L / min. At flow rates above 20 L / min, the central protective gas 6 became turbulent; therefore, 20 L / min is the upper limit for the flow rate of the central protective gas 6. It was determined that under condition J, insufficient protective performance was not achieved due to insufficient flow rate of the outer protective gas 10. At a flow rate of 50 L / min, an oxygen concentration less than or equal to the desired concentration was confirmed. Under condition M, the flow rate of the outer protective gas 10 was 150 L / min, thus generating turbulence similar to that under conditions G and J.

[0111] Based on the above verification results, it can be seen that in order for the outer protective gas 10 to perform fully, a flow rate of nitrogen greater than or equal to 50 L / min and less than 150 L / min is required.

[0112] (Example 3) (Improved dispersion of outer protective gas nozzle 11)

[0113] Under conditions G, I, and M of Example 2, the outer protective gas 10 from the outer protective gas nozzle 11 becomes turbulent at a flow rate of 150 L / min, failing to achieve the desired results. Therefore, in order to improve the dispersion of the outer protective gas 10, the installation method of the outer protective gas piping 25 supplying the outer protective gas 10 to the outer protective gas nozzle 11 was changed.

[0114] Figure 15 This is a schematic cross-sectional view showing the connection between the outer protective gas nozzle 11 and the outer protective gas piping 25 according to Embodiment 3. The outer protective gas piping 25 is provided in a direction orthogonal to the outlet of the outer protective gas 10, and a structure is formed inside the outer protective gas nozzle 11 to disperse and uniformly spray the outer protective gas 10. Connecting the outer protective gas piping 25 to the outlet of the outer protective gas 10 in the vertical direction serves to prevent the outer protective gas 10 from being sprayed out of the outer protective gas nozzle 11 without being dispersed.

[0115] Figure 16 This is a diagram illustrating the conditions and results involved in Example 3.

[0116] (Condition N~S)

[0117] Under condition N, the outer protective gas 10 was injected at a flow rate of 150 L / min. Turbulence occurred under condition G, but under condition N, the outer protective gas 10 was injected from the side, thereby dispersing it within the outer protective gas nozzle 11 and achieving laminar flow. This resulted in the desired oxygen isolation effect. Under conditions O to Q, the flow rate of the outer protective gas 10 was set to 180, 200, and 250 L / min. As a result, the oxygen concentration fluctuated more under conditions P and Q. This is believed to be because the flow rate of the central protective gas 6 was relatively lower, while the flow rate of the outer protective gas 10 was relatively higher, leading to mixing between the two gases. If this occurs, it is considered possible that the nitrogen used in the outer protective gas 10 could flow into processing point 5 and cause nitriding.

[0118] Under conditions R and S, the flow rate of the outer protective gas 10 was set to 250 L / min, and the flow rate of the central protective gas 6 was set to 10 and 20 L / min. Under these conditions, the oxygen concentration did not fluctuate, and the desired oxygen isolation effect was achieved. That is, if the flow rates of the central protective gas 6 and the outer protective gas 10 are adjusted so that they do not mix, an oxygen isolation effect can be obtained.

[0119] (Example 4) (Preventing the mixing of central protective gas 6 and outer protective gas 10)

[0120] Under conditions P and Q in Example 3, the flow rate of the central protective gas 6 is relatively low, while the flow rate of the outer protective gas 10 is relatively high. Therefore, mixing of the central protective gas 6 and the outer protective gas 10 becomes a problem. A method for preventing gas mixing will be described in Example 4.

[0121] Figure 17 This is a schematic diagram showing the cross-section and plan view of the outer protective gas nozzle 11 involved in Embodiment 4. Figure 17 The upper side shows a cross-section of the outer protective gas nozzle 11. Figure 17The lower side shows the plane of the outer protective gas nozzle 11. In Embodiment 4, a sealing structure 38 is used, which blocks a portion of the outlet of the outer protective gas nozzle 11 near the central protective gas nozzle 7. For example, for an annular outer protective gas nozzle 11 with an outer diameter of 70 mm and an inner diameter of 15 mm, a sealing structure 38 capable of blocking an inner diameter of 25 mm is used. The sealing structure 38 is an annular structural element with an outer diameter of 25 mm and an inner diameter of 15 mm. The sealing structure 38 covers a portion of the outlet of the outer protective gas nozzle 11. Therefore, nitrogen gas will not flow out from the 25 mm diameter area, thus preventing interference between the outer protective gas 10 and the central protective gas 6. The ratio between the inner and outer diameters described above is not limited to the example above; maintaining a sufficient distance between the outer protective gas 10 and the central protective gas 6 is important. Figure 18 This is a diagram illustrating the conditions and results involved in Example 4.

[0122] (Conditions T~U)

[0123] Under the condition P of mixing the central protective gas 6 and the outer protective gas 10 in Example 3, the outer protective gas nozzle 11 of Example 4 was re-evaluated. As a result, the desired oxygen isolation effect was obtained under condition T with a gas flow rate of 200 L / min. On the other hand, under condition U with a gas flow rate of 250 L / min, mixing of the two gases was still observed, and therefore the desired oxygen isolation effect could not be obtained.

[0124] Therefore, it can be seen that by providing a sealing structure 38 on a part of the outer protective gas nozzle 11, the likelihood of use is increased.

[0125] (Summarize)

[0126] Therefore, in Examples 1 and 2, which did not take into account the dispersion of the outer protective gas nozzle 11, it was determined that the oxygen isolation effect could not be sufficiently obtained at a flow rate of less than 50 L / min, and turbulence would occur at a flow rate of 150 L / min.

[0127] By improving the dispersion of the outer protective gas nozzle 11, the flow rate of the outer protective gas 10 can be increased to 250 L / min. However, due to the velocity difference, the central protective gas 6 and the outer protective gas 10 may mix, so it is necessary to consider the velocity ratio taking into account both the flow rate ratio and the spray area. It was determined that providing a blocking structure 38 on a portion of the outer protective gas nozzle 11 is effective in improving the likelihood.

[0128] Based on the results of conditions K and T, the ranges of flow ratio and velocity ratio that achieve oxygen isolation effect in the embodiments are as follows: Specifically, the flow ratio needs to be in the range of 2.5 to 40, and the velocity ratio needs to be in the range of 0.05 to 0.83. That is, preferably, the flow rate of the outer protective gas 10 is greater than or equal to 2.5 times and less than or equal to 40 times the flow rate of the central protective gas 6, and the velocity of the outer protective gas 10 is greater than or equal to 0.05 times and less than or equal to 0.83 times the velocity of the central protective gas 6.

[0129] (Example 5) Verification of the effectiveness of the outer protective gas nozzle 11

[0130] A shaping experiment was conducted using the outer protective gas nozzle 11, whose oxygen isolation effect was verified based on oxygen concentration measurements in Examples 1 to 4. In the experiment, an easily oxidizable titanium alloy was used as the metal material. A 1.2 mm diameter titanium alloy (Ti-6Al-4V) wire 1 was prepared. Figure 1 and Figure 2 The manufacturing apparatus 100 shown performs shaping. The resulting object is a wall-like structure created by layering layers on top of a 50mm long weld bead until a height of 50mm is reached. Shaping is performed with an output of 1500W and an axis speed of 400mm / min. The above-described shaping conditions and shape are described as an example for verification purposes, but the conditions and shape are not limited to these.

[0131] To confirm whether nitriding did not occur in the area where the outer protective gas 10 was sprayed, the shaping was confirmed to be effective when the temperature was less than or equal to the nitriding temperature using a radiation thermometer or thermal imager.

[0132] Titanium alloys exhibit reduced ductility due to oxygen content; therefore, the JIS standard specifies a value of less than or equal to 0.2%. Thus, to verify whether titanium has oxidized, the oxygen content of the molded object was measured. Since nitrogen gas was used, nitrogen content was also measured, with a baseline of 0.05% according to the JIS standard. The purpose of the dual-protective gas nozzle is to inhibit alloy oxidation. Therefore, as a criterion for whether oxidation has been inhibited, the judgment was made based on whether the titanium alloy of the molded object met the JIS standard for titanium alloys.

[0133] Figure 19This is a graph showing whether the performance is acceptable based on the oxygen and nitrogen content of each condition described in Example 5. Here, for the purpose of verifying the effectiveness of using nitrogen, condition B, which uses argon, is used as the benchmark. Regarding condition A, since the outer protective gas nozzle 11 is not used, oxidation is extremely significant, so it is unacceptable. Regarding condition B and subsequent conditions, since the outer protective gas nozzle 11 is used, oxidation is suppressed compared to condition A. As a result, it can be confirmed that the use of nitrogen can reduce the oxygen content and achieve healthy shaping, verifying the effectiveness of using a gas with a relatively small molecular weight as the outer protective gas 10.

[0134] The structure shown in the above embodiments is an example and can be combined with other known technologies. Parts of the structure can be omitted or changed without departing from the main idea.

[0135] Explanation of the label

[0136] 1. Wire, 2. Wire nozzle, 3. Laser beam, 4. Beam nozzle, 5. Processing point, 6. Central protective gas, 7. Central protective gas nozzle, 8. Matrix material, 9. Shape, 10. External protective gas, 11. External protective gas nozzle, 12. Worktable, 13. Processing head, 14. Wire reel, 15. Rotary motor, 16. Wire supply mechanism, 17. Laser oscillator, 18. Optical cable, 19. Heating mechanism, 20. Central protective gas injection mechanism, 21. External protective gas injection mechanism, 22. Central protective gas supply device, 23. Central protective gas piping, 24. External protective gas supply device, 25. External protective gas piping, 26. Processing head drive device, 27. Rotation device, 28. Moving mechanism, 29. Control device, 30. CPU, 31. RAM, 32. ROM, 33. External storage device, 34. Input / output interface, 35. Bus, 36. Separation structure, 37. Oxygen concentration meter, 38. Sealing structure, 99 processing circuit, 100 manufacturing device for metal stacked shapes.

Claims

1. A method for manufacturing a metal laminate structure, comprising depositing metal onto a workpiece to create a metal laminate structure. The method for manufacturing this metal laminate structure is characterized by comprising the following steps: Heat source and central protective gas are supplied from the processing head; While the heat source and the central protective gas are being supplied, an outer protective gas is ejected from an outer protective gas nozzle disposed around the processing head. This outer protective gas contains gas species with a molecular weight smaller than that of the central protective gas. While the heat source and the central protective gas are being supplied, the raw material supply mechanism is activated, and metal raw materials are supplied from the raw material supply mechanism to the processing point.

2. The method for manufacturing a metal laminated structure according to claim 1, characterized in that, The central protective gas uses argon, and the outer protective gas uses nitrogen.

3. The method for manufacturing a metal laminated structure according to claim 1 or 2, characterized in that, The flow rate of the central protective gas is less than the flow rate of the outer protective gas. The flow velocity of the central protective gas, calculated by dividing the flow rate of the central protective gas by the cross-sectional area of ​​the nozzle outlet of the central protective gas, is greater than the flow velocity of the outer protective gas, calculated by dividing the flow rate of the outer protective gas by the cross-sectional area of ​​the nozzle outlet of the outer protective gas.

4. The method for manufacturing a metal laminated structure according to claim 3, characterized in that, The flow rate of the outer protective gas is greater than or equal to 2.5 times and less than or equal to 40 times the flow rate of the central protective gas. The flow rate of the outer protective gas is greater than or equal to 0.05 times and less than or equal to 0.83 times the flow rate of the central protective gas.

5. A manufacturing apparatus for a metal laminated structure, characterized in that, have: A raw material supply organization that supplies metal raw materials; The processing head has a heating mechanism and a central protective gas nozzle for injecting central protective gas; An outer protective gas injection mechanism, which injects outer protective gas supplied from an outer protective gas pipe connected to the side of the outer protective gas nozzle from an outer protective gas nozzle disposed outside the central protective gas nozzle; and A moving mechanism that moves a worktable on which a shape formed based on the metal material supplied from the raw material supply mechanism is placed.

6. An apparatus for manufacturing a metal laminated structure, characterized in that, have: A raw material supply organization that supplies metal raw materials; The processing head has a heating mechanism and a central protective gas nozzle for injecting central protective gas; An outer protective gas injection mechanism, disposed outside the central protective gas nozzle, injects outer protective gas supplied from the outer protective gas piping through an outer protective gas nozzle with a sealing structure between it and the central protective gas nozzle; and A moving mechanism that moves a worktable on which a shape formed based on the metal material supplied from the raw material supply mechanism is placed.

7. The apparatus for manufacturing a metal laminated structure according to claim 5 or 6, characterized in that, A partition structure is provided inside the outer protective gas nozzle.

Citation Information

Patent Citations

  • Laser beam machining apparatus and laser beam machining method

    JP2009039749A

  • Shield jig and gas shield arc welder

    JP2023023971A

  • Shielding gas ejecting device, and machining device

    WO2022163820A1