Release film

By setting a resin layer with a specific energy storage modulus and a multilayer structure on the copolyester film, the problem of insufficient strength of polyester film during high-temperature molding is solved, and the demolding effect without damaging the semiconductor package is achieved in the compression molding method, providing an alternative to fluoropolymer film.

CN123125091APending Publication Date: 2026-11-17MITSUBISHI CHEM CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202580014740.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-03-22
Filing Date
2025-02-07
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing polyester films suffer from reduced strength during high-temperature molding and processing, making them difficult to replace fluoropolymer films as release materials for semiconductor packaging, especially as they can easily damage semiconductor packages during compression molding.

Method used

A copolyester film is used, and a resin layer A is provided on at least one side to ensure that the storage modulus at 80°C is below 1000 MPa, the storage modulus at 180°C is above 30 MPa, and the ratio of the storage modulus at 80°C to 180°C is below 13. A specific proportion of dicarboxylic acid components with 4 to 10 carbon atoms and other alcohol components are introduced into the copolyester to form a multilayer structure to improve flexibility and strength.

Benefits of technology

It enables demolding without damaging the semiconductor package during high-temperature molding, can serve as a substitute for fluoropolymer films, and possesses good flexibility and strength, making it suitable for semiconductor compression molding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123125091A_ABST
    Figure CN123125091A_ABST
Patent Text Reader

Abstract

A release film having a resin layer A on at least one side of a copolyester film containing a copolyester, wherein the release film has a storage modulus of 1000 MPa or less at 80°C, a storage modulus of 30 MPa or more at 180°C, and a ratio of the storage modulus at 80°C to the storage modulus at 180°C of 13 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a release film. Background Technology

[0002] As a polyester film, the representative polyethylene terephthalate (PET) film, especially biaxially stretched PET film, is used in various fields such as industrial materials, optical materials, electronic component materials, and battery packaging materials due to its excellent transparency, mechanical strength, heat resistance, and flexibility.

[0003] However, semiconductor chips are usually sealed with resin to isolate and protect them from external gases, and are mounted on a substrate in a molded state known as a package.

[0004] On the other hand, due to the requirements of miniaturization and multi-pin packaging, in the fields of BGA and WL-CSP, the molding method is changing from the previous transfer molding method to compression molding method based on the goal of large size and high efficiency of single injection.

[0005] Previously, fluoropolymer films (e.g., ETFE (ethylene-tetrafluoroethylene copolymer) films) were commonly used as release films, but due to concerns about recent restrictions on organofluorine compounds (PFAS; polyfluoroalkyl substances), research is underway on alternative films.

[0006] Existing technical documents

[0007] Patent documents

[0008] Patent Document 1: Japanese Patent No. 6414345

[0009] Patent Document 2: Japanese Patent No. 7170975

[0010] Patent Document 3: Japanese Patent No. 7287273 Summary of the Invention

[0011] The problem that the invention aims to solve

[0012] As mentioned above, polyester films possess various properties and are promising alternatives to fluoropolymer films.

[0013] However, conventional molding polyester films, for example, used for preheating to adapt to molding processing temperatures, do not elongate significantly in the temperature range of around 80°C, which is near the Tg (glass transition temperature) of polyester films. On the other hand, in the actual molding processing temperature range, i.e., the high-temperature range exceeding 160°C, fluoropolymer films maintain their strength to a certain extent, while the strength of general molding polyester films decreases significantly. The film properties are completely different, making it difficult to use them as a substitute for fluoropolymer films.

[0014] Therefore, the objective of this invention is to provide a release film for semiconductor compression molding, which, for example, when a semiconductor package is resin molded by compression molding, allows for easy release of the sealing material from the mold without damaging the semiconductor package, and can be used as a substitute for fluoropolymer films.

[0015] Solution for solving the problem

[0016] The main points of this invention are as follows.

[0017] [1] A release film having a resin layer A on at least one side of a copolyester film containing a copolyester, wherein the release film has a storage modulus of 1000 MPa or less at 80°C, a storage modulus of 30 MPa or more at 180°C, and a ratio of the storage modulus of 80°C to the storage modulus of 180°C of 13 or less.

[0018] [2] According to the release film described in [1] above, wherein the copolyester comprises a copolyester (z1) containing terephthalic acid (X1) and a dicarboxylic acid component (X2) with 4 to 10 carbon atoms and an alcohol component (Y2) other than ethylene glycol (Y1), wherein the dicarboxylic acid component (X2) with 4 to 10 carbon atoms accounts for 1 to 30 mol% of the dicarboxylic acid component in all the polyester (Z) contained in the copolyester film, and the other alcohol component (Y2) accounts for 15 to 60 mol% of the alcohol component.

[0019] [3] According to the release film described in [2] above, the dicarboxylic acid component (X2) with 4 to 10 carbon atoms includes aliphatic dicarboxylic acids.

[0020] [4] According to the release film described in [3] above, wherein the aliphatic dicarboxylic acid includes adipic acid.

[0021] [5] The release film according to any one of [2] to [4] above, wherein the other alcohol component (Y2) comprises 1,4-butanediol.

[0022] [6] The release film according to any one of [2] to [5] above, wherein the other alcohol component (Y2) comprises 1,4-butanediol and 1,6-hexanediol.

[0023] [7] The release film according to any one of [1] to [6] above, wherein the release film is a copolyester film having a copolyester layer (A1) containing a copolyester (a1) as the copolyester.

[0024] [8] According to the release film described in [7] above, the copolyester layer (A1) further comprises polyester (a2), wherein the polyester (a2) is a polyester other than the copolyester (a1), and contains terephthalic acid as a dicarboxylic acid component and ethylene glycol as an alcohol component.

[0025] [9] The release film according to any one of [7] to [8] above, wherein a polyester layer (B1) and a polyester layer (B2) are respectively provided on the front and back sides of the copolyester layer (A1).

[0026]

[10] According to the release film described above [9], the temperature difference between at least any one of the copolyester layer (A1), polyester layer (B1), and polyester layer (B2), as determined by the softening temperature of nano TA, is 5°C or more.

[0027]

[11] The release film according to any one of [1] to

[10] above, wherein the resin layer A comprises a silicone resin.

[0028]

[12] The release film according to any one of [1] to

[10] above, wherein the resin layer A comprises a non-silicone resin.

[0029]

[13] The release film according to any one of [1] to

[12] above is used in semiconductor manufacturing.

[0030]

[14] The release film described in

[13] above is used for compression molding.

[0031] Invention Effects

[0032] According to the present invention, for example, a release film for semiconductor compression molding can be provided, which, when a semiconductor package is resin molded by compression molding, can easily release the sealing material from the mold without damaging the semiconductor package, and can be used as a substitute for fluoropolymer film. Attached Figure Description

[0033] Figure 1 The data curves are shown for Example 1-1, 1-2, Comparative Example 1, 2 and Reference Example (fluoropolymer membrane), obtained by plotting the change in storage modulus relative to temperature change in the TD direction. Detailed Implementation

[0034] Next, an example of an embodiment of the present invention will be described. However, the present invention is not limited to the embodiments described below.

[0035] [Mold release film]

[0036] The release film of the present invention is characterized in that at least one side of the copolyester film containing copolyester has a resin layer A, the storage modulus of the release film at 80°C is 1000 MPa or less, the storage modulus at 180°C is 30 MPa or more, and the ratio of the storage modulus at 80°C to the storage modulus at 180°C is 13 or less.

[0037] <Copolyester film>

[0038] The release film constituting one embodiment of the present invention comprises a copolyester film (hereinafter referred to as "this copolyester film") containing a copolyester. This copolyester film is, for example, a single-layer or laminated film having a copolyester layer (A1) containing a copolyester (a1) as the copolyester.

[0039] The copolyester film is preferably a stretched film formed by stretching along a uniaxial or biaxial direction. It can be a uniaxial stretched film or a biaxial stretched film. Among them, from the perspective of balancing mechanical properties and excellent planarity, a biaxial stretched film is preferred.

[0040] If this copolyester film is a stretched film, it is easy to make the storage modulus of the release film at 80°C below 1000MPa, or the storage modulus at 180°C above 30MPa.

[0041] <Copolyester layer (A1)>

[0042] The copolyester layer (A1) is a layer containing copolyester (a1). Preferably, the copolyester layer (A1) also contains polyester (a2) in addition to copolyester (a1). Furthermore, the copolyester layer (A1) may also contain resin (a3) ​​in addition to these copolyesters (a1) and polyesters (a2).

[0043] (Copolyester (a1))

[0044] Copolyester (a1) is a copolymer of terephthalic acid (X1), a dicarboxylic acid component with 4 to 10 carbon atoms (X2), and an alcohol component (Y2) other than ethylene glycol (Y1). It should be noted that such a copolymer polyester is sometimes also referred to as copolyester (z1) in this specification, and the following description of copolyester (a1) is also a description of copolyester (z1). Copolyester (a1) can be crystalline or amorphous. It should be noted that the dicarboxylic acid component with 4 to 10 carbon atoms (X2) refers to dicarboxylic acids with 4 to 10 carbon atoms other than terephthalic acid (X1).

[0045] Copolyester (a1) (copolyester (z1)) is a condensation polymer of a dicarboxylic acid containing terephthalic acid (X1) and a dicarboxylic acid component with 4 to 10 carbon atoms (X2), and an alcohol component (Y2) containing an alcohol component other than ethylene glycol (Y1). The alcohol component is usually a diol component.

[0046] Examples of dicarboxylic acid components (X2) with 4 to 10 carbon atoms include aromatic dicarboxylic acids, alicyclic dicarboxylic acids, aliphatic dicarboxylic acids, and polyfunctional acids. Among these, aliphatic dicarboxylic acids are preferred from the viewpoint of providing good storage modulus at room temperature, improving flexibility, and elongation. Aliphatic dicarboxylic acids can be used alone as the dicarboxylic acid component (X2) with 4 to 10 carbon atoms, or they can be used in combination with other dicarboxylic acid components with 4 to 10 carbon atoms.

[0047] Examples of aliphatic dicarboxylic acids with 4 to 10 carbon atoms include succinic acid, glutaric acid, adipic acid, pimelic acid, octanoic acid, azelaic acid, sebacic acid, and other saturated aliphatic dicarboxylic acids. Among these, adipic acid and sebacic acid are preferred from the viewpoint of ease of reaction during polymerization, and adipic acid is even more preferred.

[0048] The proportion of the dicarboxylic acid component (X2) with 4 to 10 carbon atoms in the dicarboxylic acid component constituting the copolyester (a1) (copolyester (z1)) is not limited as long as the proportion of (X2) relative to the total polyester (Z) described later is within a specified range, for example, 1 to 30 mol%, preferably 1 to 25 mol%, more preferably 1 to 20 mol%, and particularly 4 to 15 mol%.

[0049] In addition, the proportion of terephthalic acid (X1) in the dicarboxylic acid component constituting copolyester (a1) (copolyester (z1)) is, for example, 65 to 95 mol, preferably 75 to 92 mol, and more preferably 80 to 90 mol.

[0050] Furthermore, in the copolyester (a1) (copolyester (z1)), the dicarboxylic acid component can be composed of terephthalic acid (X1) and a dicarboxylic acid component with 4 to 10 carbon atoms (X2). Without prejudice to the spirit of the invention, other dicarboxylic acid components (other dicarboxylic acid components (X3)) besides terephthalic acid (X1) and the dicarboxylic acid component with 4 to 10 carbon atoms (X2) can also be included as copolymer components. Examples of such dicarboxylic acid components include: dodecanoic acid, arachidic acid, dimer acids, and their derivatives.

[0051] The proportion of other dicarboxylic acid components (X3) in the dicarboxylic acid components constituting the copolyester (a1) is, for example, 10 mol% or less, preferably 5 mol% or less, more preferably 3 mol% or less, and most preferably 0 mol%.

[0052] Other alcohol components (Y2) include: aliphatic diols such as 1,4-butanediol, 1,4-hexanediol, 1,6-hexanediol, diethylene glycol, trimethylenediol, pentamethylenediol, octamethylenediol, decamethylenediol, neopentyl glycol, 2-ethyl-2-butyl-1,3-propanediol, etc.; alicyclic diols such as 1,2-cyclohexanediol, 1,1-cyclohexanediethanol, 1,4-cyclohexanediethanol, etc. 2,5-norbornanediethanol, etc.; aromatic diols, such as benzenediethanol, 4,4'-dihydroxybiphenyl, 2,2-bis(4'-hydroxyphenyl)propane, 2,2-bis(4'-β-hydroxyethoxyphenyl)propane, bis(4-hydroxyphenyl)sulfone, bis(4-β-hydroxyethoxyphenyl)sulfonic acid, etc.; ethylene oxide adducts or propylene oxide adducts of 2,2-bis(4'-hydroxyphenyl)propane, dimers, etc. They may contain one or more of these compounds.

[0053] Of the above, aliphatic diols are preferred from the viewpoint of softness and crystallinity. Aliphatic diols are preferably aliphatic diols with 4 to 8 carbon atoms, and more preferably aliphatic diols with 4 to 6 carbon atoms.

[0054] More specifically, the aliphatic diol is preferably selected from at least one of diethylene glycol, 1,4-butanediol, 1,4-hexanediol, and 1,6-hexanediol. Furthermore, it is more preferable that the alcohol component includes at least 1,4-butanediol, and even more preferably, the alcohol component in the copolyester (a1) includes both 1,4-butanediol and 1,6-hexanediol.

[0055] Additionally, the copolyester (a1) (copolyester (z1)) may also contain ethylene glycol (Y1) as an alcohol component (copolymer component). It should be noted that any of the polyesters (A) constituting the copolyester layer (A1) preferably contains ethylene glycol (Y1) as an alcohol component (copolymer component). Therefore, in cases where the copolyester (a1) does not contain ethylene glycol (Y1) as an alcohol component (copolymer component), for example, polyester (a2) preferably contains ethylene glycol (Y1) as an alcohol component.

[0056] Copolyester (a1) (copolyester (z1)) can be used alone or in combination with two or more.

[0057] Regarding the proportion of other alcohol components (Y2) in the alcohol components constituting copolyester (a1) (copolyester (z1)), there is no limitation as long as the proportion of (Y2) relative to the total polyester (A) described later is within a specified range, for example, 50 to 100 mol%, preferably 70 to 100 mol%, more preferably 90 to 100 mol%.

[0058] In addition, the copolyester film (a1) contains a certain amount of polyester with one or both of the following as structural units: terephthalic acid, dicarboxylic acid with 4 to 10 carbon atoms, 1,4-butanediol and 1,6-hexanediol. This makes the copolyester layer (A1) soft, with excellent elongation at low temperatures, and also has both strength and heat resistance.

[0059] (Inherent viscosity (IV) of copolyester (a1))

[0060] The intrinsic viscosity (IV) of the copolyester (a1) (copolyester (z1)) (or a polyester mixture when two or more copolyesters are used) is preferably 0.40 dL / g to 1.20 dL / g, more preferably 0.45 dL / g or more, even more preferably 0.48 dL / g or more, and even more preferably 1.15 dL / g or less, even more preferably 1.10 dL / g or less.

[0061] If the intrinsic viscosity of the copolyester (a1) is within the above range, a polyester with excellent molding and processability can be produced without compromising productivity.

[0062] It should be noted that the intrinsic viscosity (IV) of polyester is the value obtained by accurately weighing 1g of polyester after removing incompatible components, dissolving 1g of polyester in 100ml of a phenol / tetrachloroethane mixture of 50 / 50 (by weight), and measuring the result at 30°C.

[0063] Regarding the content of the copolyester (a1), it is sufficient that it constitutes a certain proportion or more of the resin components forming the copolyester layer (A1), so that the proportions of each component in all polyester (Z) or polyester (A) described later are within a specified range. In the copolyester layer (A1), the copolyester (a1) constitutes, for example, 30% by mass or more, preferably 35% by mass or more, and more preferably 50% by mass or more; for example, it may also constitute 80% by mass or more. Furthermore, the copolyester (a1) only needs to constitute 100% by mass or less of the resin components forming the copolyester layer (A1); for example, it may constitute 70% by mass or less, or 60% by mass or less.

[0064] (Polyester (a2))

[0065] In the copolyester layer (A1), the resin may be only copolyester (a1), but preferably it also includes polyester (a2) in addition to copolyester (a1).

[0066] Here, polyester (a2) refers to polyester other than copolyester (a1), and is a homopolymer or copolyester containing terephthalic acid (X1) as a dicarboxylic acid component and ethylene glycol (Y1) as an alcohol component. It should be noted that polyester containing terephthalic acid (X1) as a dicarboxylic acid component and ethylene glycol (Y1) as an alcohol component is sometimes referred to as polyester (z2) as described below.

[0067] When polyester (a2) (polyester (z2)) is a homopolymer polyester, the homopolymer polyester is polyethylene terephthalate with terephthalic acid (X1) as the dicarboxylic acid component and ethylene glycol (Y1) as the alcohol component. Homopolymer polyester is preferred as polyester (a2). However, when described as a homopolymer polyester, the alcohol component may inevitably contain diethylene glycol. Specifically, in polyethylene terephthalate (homogeneous polyester), the proportion of diethylene glycol in the alcohol component may, for example, be 5 mol% or less, or 3 mol% or less. The same applies to polyester (B) described later.

[0068] It should be noted that diethylene glycol is obtained by modifying a portion of ethylene glycol into diethylene glycol and introducing it into the polyester backbone when ethylene glycol is used as one of the raw materials to manufacture (polymerization) polyester.

[0069] When polyester (a2) (polyester (z2)) is a copolyester, dicarboxylic acid components other than terephthalic acid (X1) can be listed as: aromatic dicarboxylic acids, alicyclic dicarboxylic acids, aliphatic dicarboxylic acids, polyfunctional acids, etc. As these dicarboxylic acid components, dicarboxylic acid components that are the same as those listed in copolyester (a1) can be listed.

[0070] When polyester (a2) (polyester (z2)) is a copolyester, the proportion of dicarboxylic acid components other than terephthalic acid in the dicarboxylic acid components is preferably 1 to 30 mol%, more preferably 3 mol% or more, further preferably 5 mol% or more, and even more preferably 20 mol% or less, and even more preferably 10 mol% or less.

[0071] When the polyester (a2) (polyester (z2)) is a copolyester, the alcohol component (Y2) other than ethylene glycol (Y1) can be appropriately selected from the compounds listed in the copolyester (a1), preferably including: 1,4-butanediol, 1,6-hexanediol, 1,4-hexanediol, diethylene glycol, trimethylene glycol, neopentyl glycol, 1,4-cyclohexanediol, etc.

[0072] When the polyester (a2) (polyester (z2)) is a copolyester, the proportion of alcohol components (Y2) other than ethylene glycol in the alcohol component of the copolymer polyester is preferably 1 mol% or more and less than 100 mol%, more preferably 3 mol% or more, more preferably 5 mol% or more, and even more preferably 90 mol% or less, more preferably 50 mol% or less, more preferably 30 mol% or less, and particularly preferably 10 mol% or less.

[0073] The intrinsic viscosity (IV) of the polyester (a2) (polyester (z2) (a polyester mixture when two or more polyesters (a2) are used) is preferably 0.40 dL / g to 1.20 dL / g, more preferably 0.45 dL / g or more, even more preferably 0.48 dL / g or more, and even more preferably 1.15 dL / g or less, even more preferably 1.10 dL / g or less.

[0074] If the intrinsic viscosity of the copolyester (a2) is within the above range, a polyester with excellent molding and processability can be produced without deteriorating productivity.

[0075] Polyester (a2) (polyester (z2)) can be used alone or in combination with two or more.

[0076] Regarding the content of polyester (a2), as long as the proportion of each component in polyester (A) is within the range described below, the content of polyester (a2) in the resin component constituting the copolyester layer (A1) is, for example, 70% by mass or less, preferably 65% ​​by mass or less, more preferably 50% by mass or less, and preferably 30% by mass or more, more preferably 40% by mass or more.

[0077] (Resin (a3))

[0078] The copolyester layer (A1) may also be a layer containing a resin (a3) ​​other than the copolyester (a1) and the polyester (a2). As for the resin (a3), any resin that is compatible with the copolyester (a1) may be used, and if the resin is a polyester (a2), it may also be compatible with the polyester (a2).

[0079] The copolyester layer (A1) is a layer that forms an island structure by copolyester (a1) or copolyester (a1) and polyester (a2) with resin (a3). By selecting polyesters such as polyolefin, polystyrene, acrylic resin, urethane resin, polybutylene terephthalate (PBT) as resin (a3), it is possible to impart shielding and heat resistance.

[0080] In the copolyester layer (A1), the mass ratio of the total amount of copolyester (a1) and polyester (a2) to the mass ratio of resin (a3) ​​((a1+a2):a3) is preferably 98:2 to 50:50, more preferably 95:5 to 60:40, and more preferably 90:10 to 65:35.

[0081] Furthermore, the resin (a3) ​​is preferably a resin compatible with the copolyester (a1) or a combination of copolyester (a1) and polyester (a2), and the resin has a melting point of 270°C or less and a glass transition temperature of 30–120°C. By selecting such a resin (a3), the glass transition temperature of the copolyester layer (A1) can be increased, thereby improving heat resistance. Polybutylene terephthalate (PBT) is an example of such a resin, but it is not limited to PBT.

[0082] Resin (a3) ​​can be used alone or in combination with two or more.

[0083] (The proportions of each component in the copolyester layer (A1))

[0084] In this invention, the proportion of the dicarboxylic acid component (X2) with 4 to 10 carbon atoms in the total dicarboxylic acid component of the total polyester (A) contained in the copolyester layer (A1) is preferably 1 to 30 mol%. It should be noted that "total polyester (A)" here refers to all the polyester contained in the copolyester layer (A1). Therefore, the above proportion refers to the proportion based on the dicarboxylic acid component constituting the total polyester (A), and similar terms will be used with the same meaning below.

[0085] Here, if the proportion of dicarboxylic acid component (X2) with 4 to 10 carbon atoms is 1 mol% or more, the effect of using dicarboxylic acid component (X2) with 4 to 10 carbon atoms can be fully obtained, ensuring softness and elongation at low temperatures. In addition, if it is 30 mol% or less, the heat shrinkage rate becomes higher, ensuring heat resistance.

[0086] From the viewpoint of achieving good softness and elongation at low temperatures and ensuring heat resistance, the proportion of the dicarboxylic acid component (X2) with 4 to 10 carbon atoms is more preferably 2 mol% or more, further preferably 3 mol% or more, particularly 4 mol% or more, and even more preferably 25 mol% or less, further preferably 20 mol% or less, and particularly preferably 15 mol% or less.

[0087] As described above, adicarboxylic acid (X2) with 4 to 10 carbon atoms is preferably used. When using adicarboxylic acid, adicarboxylic acid (X2) with 4 to 10 carbon atoms can be used alone or in combination with dicarboxylic acids with 4 to 10 carbon atoms other than adicarboxylic acid.

[0088] The proportion of adipic acid in the dicarboxylic acid component of all polyester (A) is, for example, 1 to 30 mol%, preferably 2 mol% or more, more preferably 3 mol% or more, particularly 4 mol% or more, and preferably 25 mol% or less, more preferably 20 mol% or less, and even more preferably 15 mol% or less.

[0089] Furthermore, from the viewpoint of maintaining various properties such as heat resistance, the proportion of terephthalic acid (X1) in the dicarboxylic acid component of all polyester (A) is, for example, 65 to 98 mol%, preferably 97 mol% or less, more preferably 96 mol% or less, and preferably 75 mol% or more, more preferably 80 mol% or more, and particularly preferably 85 mol% or more.

[0090] Furthermore, the proportion of other dicarboxylic acids (X3) in the dicarboxylic acid component of the entire polyester (A) is, for example, 10 mol% or less, preferably 5 mol% or less, more preferably 3 mol% or less, and most preferably 0 mol%. That is, the dicarboxylic acid component of the polyester (A) preferably does not contain other dicarboxylic acids (X3).

[0091] It should be noted that the dicarboxylic acid content of the polyester (A) contained in the copolyester layer (A1) can be determined by measurement. 1 Quantitative analysis is performed using ¹H-NMR spectroscopy. The same applies to the dicarboxylic acid content of the polyester contained in the polyester layers (B1), (B2), and copolyester films described later.

[0092] In this invention, the proportion of other alcohol components (Y2) in the total alcohol components of the polyester (A) contained in the copolyester layer (A1) is preferably 15 to 60 mol%. If it is 15 mol% or more, it is easy to ensure softness, elongation, etc. at low temperatures. In addition, if it is 60 mol% or less, it is easy to ensure heat resistance by preventing the heat shrinkage rate from becoming high. From the viewpoint of ensuring good softness and elongation at low temperatures and ensuring heat resistance, the proportion of other alcohol components (Y2) is more preferably 20 mol% or more, further preferably 25 mol% or more, even more preferably 30 mol% or more, and even more preferably 55 mol% or less.

[0093] From the viewpoint of ensuring softness and high elongation at low temperatures, the other alcohol components (Y2) preferably contain at least 1,4-butanediol, and more preferably both 1,4-butanediol and 1,6-hexanediol.

[0094] The proportion of 1,4-butanediol and 1,6-hexanediol in the alcohol content of all polyester (A) is preferably 15 to 60 mol%, more preferably 20 mol% or more, even more preferably 25 mol% or more, even more preferably 30 mol% or more, and even more preferably 55 mol% or less.

[0095] It should be noted that the so-called proportion of 1,4-butanediol and 1,4-hexanediol, for example, when only 1,4-butanediol is used, it refers to the proportion of 1,4-butanediol; when both 1,4-butanediol and 1,6-hexanediol are used, it refers to their combined proportion.

[0096] In the case of containing 1,4-butanediol and 1,6-hexanediol, the molar ratio of 1,6-hexanediol to 1,4-butanediol is, for example, 0.5 or more, preferably 0.7 or more, more preferably 0.8 or more, even more preferably 0.9 or more, or for example, 2.5 or less, preferably 2.0 or less, more preferably 1.6 or less, even more preferably 1.4 or less.

[0097] The proportion of ethylene glycol (Y1) in the total alcohol content of the polyester (A) is 40 to 85 mol%, preferably 45 mol% or more, preferably 80 mol% or less, more preferably 75 mol% or less, and even more preferably 70 mol% or less.

[0098] It should be noted that the alcohol content of the polyester (A) contained in the copolyester layer (A1) can be determined by measurement. 1 Quantitative analysis is performed using H-NMR spectroscopy. The same applies to the polyester layers (B1), (B2), and copolyester films described later.

[0099] As a particularly preferred embodiment of the above, the copolyester (a1) is a crystalline copolyester (hereinafter sometimes referred to as "copolyester (Za)") composed of terephthalic acid and an aliphatic dicarboxylic acid having 4 to 10 carbon atoms, and one or both of 1,4-butanediol and 1,6-hexanediol, wherein the aliphatic dicarboxylic acid having 4 to 10 carbon atoms accounts for 3 to 50 mol% of the dicarboxylic acid component in the total polyester (A), and the combined proportion of 1,4-butanediol and 1,6-hexanediol in the alcohol component is 15 to 60 mol%.

[0100] Typically, for copolyesters, increasing the proportion of the copolymer component to reduce the elastic modulus results in decreased crystallinity and amorphous properties. The aforementioned copolyester (Za) has a high copolymer component ratio, achieving a low elastic modulus while maintaining crystallinity, thus allowing for heat fixation through heat treatment after stretching. As a result, the copolyester (Za) is soft, while exhibiting good elongation and strength, thereby suppressing heat shrinkage.

[0101] like Figure 1 As can be seen, conventional copolyester films (Comparative Example 1) have a high storage modulus at around 80°C, lack flexibility, and a very low storage modulus at around 180°C, making it unable to maintain strength. Under these circumstances, even those skilled in the art would need to carefully consider how to approximate the storage modulus curve of the fluoropolymer film (Reference Example). However, the inventors have discovered that by using the aforementioned polyester (A) or the polyester (Z) described later, a fitting curve approximating the storage modulus of the fluoropolymer film can be plotted. Specifically, compared to the past, the storage modulus at around 80°C can be further reduced, while the storage modulus at around 180°C can be maintained at a certain high level (Example), thereby completing the present invention.

[0102] It should be noted that the copolyester film, by containing the aforementioned copolyester (a1), or copolyester (a1) and polyester (a2) (or copolyester (z1), or copolyester (z1) and polyester (z2) as described later), also exhibits good solvent resistance. Therefore, as will be explained later, when forming a resin layer using an organic solvent, the copolyester film can be prevented from being dissolved by the solvent.

[0103] (Polyester blend)

[0104] As described above, the polyester (A) contained in the copolyester layer (A1) can be a single polyester or a blend of two or more polyesters. When the polyester (A) is composed of a single polyester, i.e., when the copolyester layer (A1) contains a single polyester as the copolyester (a1), this polyester is preferably a copolyester containing dicarboxylic acid with 4 to 10 carbon atoms and terephthalic acid as the dicarboxylic acid component, and ethylene glycol and one or both of 1,4-butanediol and 1,6-hexanediol as the alcohol component.

[0105] On the other hand, when the polyester (A) contained in the copolyester layer (A1) is composed of two or more polyesters, that is, when the copolyester layer (A1) contains a polyester blend composed of two or more polyesters as polyester (A), the polyester blend preferably contains dicarboxylic acid and terephthalic acid with 4 to 10 carbon atoms as the dicarboxylic acid component, and contains ethylene glycol and one or both of 1,4-butanediol and 1,6-hexanediol as the diol component.

[0106] At this time, as a polyester blend, it is sufficient to have the above-mentioned structural units. For example, if the polyester blend is a mixed resin of a first polyester and a second polyester, each of the first polyester and the second polyester does not need to have all of the above-mentioned structural units.

[0107] In the copolyester layer (A1), polyester (A) is the main component resin. "Main component resin" refers to the resin that constitutes the copolyester layer (A) in the largest proportion.

[0108] The content of polyester (A) relative to the resin component contained in the copolyester layer (A1) is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 80% by mass or more, and there is no particular limitation as long as it is 100% by mass or less.

[0109] It should be noted that the polyester (A) content refers to the total amount of all polyester contained in the copolyester layer (A1).

[0110] The copolyester layer (A1) may also contain particles. Specific examples of particles include: inorganic particles such as silica, calcium carbonate, magnesium carbonate, barium carbonate, calcium sulfate, calcium phosphate, magnesium phosphate, kaolin, alumina, and titanium dioxide; organic particles such as acrylic resin, styrene resin, urea resin, phenolic resin, epoxy resin, and benzoguanamine resin; and so on. Furthermore, in the polyester manufacturing process, precipitated particles formed by precipitating and micro-dispersing a portion of a metal compound such as a catalyst may also be used.

[0111] One type of granule can be used alone, or two or more types can be used together.

[0112] There are no particular restrictions on the shape of the granules used; any shape, such as spherical, blocky, rod-shaped, or flat, can be used. Furthermore, there are no particular restrictions on their hardness, specific gravity, or color. Two or more types of these granules can be used in combination as needed.

[0113] Furthermore, the average particle size of the particles used is preferably 5 μm or less, more preferably in the range of 0.1 to 4 μm. By using an average particle size within the above range, a suitable surface roughness can be imparted to the film, ensuring good sliding properties and smoothness.

[0114] It should be noted that more than 10 particles in the copolyester layer (A1) can be selected arbitrarily using a scanning electron microscope (SEM) to measure the diameter of each particle, and the average particle size can be calculated from the average value. In the case of non-spherical particles, the average value of the longest and shortest diameters ((short diameter + long diameter) / 2) can be used as the diameter of each particle for measurement.

[0115] The copolyester layer (A1) can also contain two or more particles with different particle sizes.

[0116] The particle content in the copolyester layer (A1) is preferably 5% by mass or less, more preferably in the range of 0.0003% to 3% by mass, and even more preferably in the range of 0.001% to 0.2% by mass. By setting the particle content within the above range, the transparency of the substrate film is ensured, and the substrate film is easily given slip properties. In addition, by suppressing the particle content to a low level, the tensile elongation at break is easily improved.

[0117] In addition to the particles mentioned above, the copolyester layer (A1) may also contain at least one additive selected from the following as needed: crystal nucleating agent, antioxidant, anti-coloring agent, pigment, dye, ultraviolet absorber, release agent, slip agent, flame retardant, antistatic agent, etc.

[0118] (Method for manufacturing copolyester (a1))

[0119] There are no particular restrictions on the manufacturing method of copolyester (a1) (polyester (z1)), and conventional methods can be used. For example, firstly, a dicarboxylic acid component containing terephthalic acid or its ester-forming derivative, a dicarboxylic acid having 4 to 10 carbon atoms or its ester-forming derivative, and a diol component containing ethylene glycol, preferably also containing diethylene glycol, are mixed in a predetermined ratio under stirring to prepare a raw material slurry (raw material slurry preparation step). Next, the raw material slurry is heated under normal or pressurized pressure to carry out an esterification reaction to produce a polyester oligomer (hereinafter, sometimes referred to as "oligomer") (oligomer preparation step). Then, a dicarboxylic acid having 4 to 10 carbon atoms or its ester-forming derivative, and an alcohol component other than ethylene glycol and diethylene glycol, such as 1,4-butanediol and 1,6-hexanediol, are added to the obtained oligomer. Under the presence of an ester exchange catalyst or the like, the pressure is gradually reduced, and the mixture is heated to carry out a melt polycondensation reaction to obtain polyester (polyester preparation step). The resulting polyester can also be further supplied to solid-state polycondensation reaction (solid-state polycondensation process) as needed.

[0120] However, the manufacturing method of polyester (a1) is not limited to the above method. As mentioned above, dicarboxylic acids or their ester-forming derivatives with 4 to 10 carbon atoms do not need to be added to both the raw material slurry and the oligomer. They can be added only to the raw material slurry or only to the oligomer.

[0121] Similarly, alcohol components other than ethylene glycol and diethylene glycol are not limited to the method described above of adding only to oligomers; they can be added to both the raw material slurry and the oligomers, or only to the raw material slurry.

[0122] Examples of transesterification catalysts include: germanium compounds, such as antimony compounds like antimony trioxide; germanium dioxide, germanium tetroxide, etc.; titanium compounds, such as tetramethyl titanate, tetraisopropyl titanate, tetrabutyl titanate, etc., titanium alkoxides, tetraphenyl titanate, etc.; tin compounds, such as dibutyltin oxide, methylphenyltin oxide, tetraethyltin, hexaethyltin dioxide, cyclohexyltin dioxide, didodecyltin oxide, triethyltin hydroxide, triphenyltin hydroxide, triisobutyltin acetate, dibutyltin diacetate, diphenyltin dilaurate, monobutyltin trichloride, tributyltin chloride, dibutyltin chloride, dibutyltin sulfide, butyltin hydroxide, methylstannic acid, ethylstannic acid, butylstannic acid, etc.; magnesium compounds, such as magnesium acetate, magnesium hydroxide, magnesium carbonate, magnesium oxide, magnesium alkoxide, magnesium hydrogen phosphate, etc.; calcium compounds, such as calcium acetate, calcium hydroxide, calcium carbonate, calcium oxide, calcium alkoxide, calcium hydrogen phosphate, etc.; and so on.

[0123] It should be noted that these catalysts can be used alone or in combination of two or more.

[0124] In addition, when manufacturing polyester, it is preferable to use a stabilizer together with the transesterification catalyst. Examples of stabilizers include: pentavalent phosphorus compounds, such as orthophosphoric acid, polyphosphoric acid, and trimethyl phosphate, triethyl phosphate, tributyl phosphate, trioctyl phosphate, triphenyl phosphate, tricresyl phosphate, tri(triethylene glycol) phosphate, diethylphosphonoethyl acetate, methyl phosphate, ethyl phosphate, isopropyl phosphate, butyl phosphate, monobutyl phosphate, dibutyl phosphate, dioctyl phosphate, triethylene glycol phosphate, etc.; trivalent phosphorus compounds, such as phosphorous acid, hypophosphoric acid, and diethyl phosphite, tri(dodecyl) phosphite, tri(nonyldecyl) phosphite, triphenyl phosphite, etc.; and so on.

[0125] Among them, trivalent phosphorus compounds generally have stronger reducing properties than pentavalent phosphorus compounds. When metal compounds added as condensation catalysts are reduced and precipitated, they may become the cause of foreign matter. Therefore, pentavalent phosphorus compounds are preferred.

[0126] The reaction pressure in the melt polycondensation reaction is preferably 0.001 kPa to 1.33 kPa using an absolute pressure gauge. Furthermore, the reaction temperature in the melt polycondensation reaction is preferably 220°C to 280°C, more preferably 230°C or higher, and even more preferably 260°C or lower.

[0127] Solid-state polycondensation can be carried out under reduced pressure or an inert gas atmosphere, with the preferred reaction temperature being 180℃ to 220℃. The preferred reaction time for solid-state polycondensation is 5 to 100 hours.

[0128] By employing the aforementioned melt polycondensation reaction conditions and solid-phase polycondensation reaction conditions, polyesters with the desired intrinsic viscosity can be obtained.

[0129] <Multi-layered structure>

[0130] As described above, this copolyester film can also have a multilayer structure having a copolyester layer (A1) and other layers.

[0131] In the case where the copolyester film has a multilayer structure, it is preferable to have a copolyester layer (A1) and polyester layers (B1) and (B2) on both sides of the copolyester layer (A1). Each polyester layer (B1) and polyester layer (B2) contains polyester (B) as the main component resin.

[0132] Here, "main component resin" refers to the resin that constitutes the copolyester layers (B1) and (B2) in the largest proportion. This main component resin preferably accounts for more than 50% by mass, more than 70% by mass, more than 80% by mass, and, for example, less than 100% by mass in the resin components constituting the polyester layers (B1) and (B2) respectively.

[0133] When the copolyester (a1) is crystalline, the polyester (B) contained in each polyester layer (B1) and (B2) should preferably contain a polyester with a melting point higher than that of the copolyester (a1). Such a polyester should preferably comprise 50% by mass or more of the resin composition constituting each polyester layer (B1) and (B2). Furthermore, when the copolyester (a1) is amorphous, the polyester (B) should preferably contain a polyester with a melting point higher than that of the copolyester (a1). Such a polyester should preferably comprise 50% by mass or more of the resin composition constituting each polyester layer (B1) and (B2).

[0134] If the structure is a multilayer structure consisting of polyester layers (B1) and (B2) with polyester (B) as the main component resin, the raw material resin composition can be laminated into polyester layer (B1) / copolyester layer (A1) / polyester layer (B2) by co-extrusion or the like. After stretching, it is heat-fixed at a higher temperature than the case where it consists of a single layer of copolyester layer (A1). Therefore, it is possible to soften to a level that cannot be achieved with a single layer of copolyester layer (A1), or to further prevent heat shrinkage.

[0135] Specifically, the energy storage modulus of the release film at 80°C can be 1000 MPa or less, preferably 800 MPa or less, and more preferably 100 MPa or more and 400 MPa or less.

[0136] In the above multilayer structure, the thickness of each layer of polyester layer (B1) and (B2) is preferably 1 to 20% of the thickness of copolyester layer (A1).

[0137] If the thickness of each layer of polyester layer (B1) and (B2) is more than 1% of the thickness of copolyester layer (A1), film can be made without significantly impairing productivity; if it is less than 20%, the required softness can be fully ensured.

[0138] Based on the above viewpoint, the thickness of each layer of polyester layer (B1) and (B2) is more preferably 3% or more and 15% or less of the thickness of copolyester layer (A1), and more preferably 5% or more and 12% or less.

[0139] It should be noted that the thickness of each layer of polyester layer (B1) and (B2) existing on both sides of the copolyester layer (A1) can be different or the same on both sides.

[0140] However, in a multilayer structure, the number of polyester layers is not limited to three; it can be two or more layers.

[0141] One or both of the polyester layers (B1) and (B2) may contain particles. Specific examples, shapes, average particle sizes, contents, and other details of the particles are as described in the description of polyester layer (A). The contents are referred to as the content of particles in each of the polyester layers (B1) and (B2).

[0142] In addition, one or both of the polyester layers (B1) and (B2) may contain at least one additive besides the aforementioned particles. Details of the additives are as described above.

[0143] It should be noted that in the case of a multilayer structure, one or both of the polyester layers (B1) and (B2) contain particles, while the polyester layer (A) may not contain particles.

[0144] When the copolyester (a1) is crystalline, the polyester (B) preferably contains a polyester having a melting point 10 to 100°C higher than that of the copolyester (a1), more preferably 20°C or more, even more preferably 40°C or more, and even more preferably 90°C or less, even more preferably 70°C or less. Such a polyester preferably constitutes 50% by mass or more of the resin components constituting the polyester layers (B1) and (B2) respectively.

[0145] On the other hand, when the copolyester (a1) is amorphous, the polyester (B) preferably contains a polyester having a glass transition temperature that is 120 to 260°C higher than that of the copolyester (a1), more preferably 140°C or more higher, even more preferably 160°C or more higher, and even more preferably 230°C or less higher, with the latter being more preferably 200°C or less higher. Such a polyester preferably constitutes 50% by mass or more of the resin components that respectively constitute the polyester layers (B1) and (B2).

[0146] It should be noted that the polyester (B) that is the main component of the polyester layers (B1) and (B2) existing on both sides of the copolyester layer (A1) can preferably be different or the same on both sides, but the melting points of the polyester (B) on both sides should not be significantly different.

[0147] As polyester (B), for example, homopolymer polyesters or copolymer polyesters (also referred to as "polyester (Z2)") containing terephthalic acid as a dicarboxylic acid component and ethylene glycol as an alcohol component can be suitably used. However, the polyester in polyester (B) is not limited to this. It should be noted that homopolymer polyester is polyethylene terephthalate.

[0148] When polyester (B) is a copolyester, dicarboxylic acid components other than terephthalic acid can be listed as: aromatic dicarboxylic acids, alicyclic dicarboxylic acids, aliphatic dicarboxylic acids, polyfunctional acids, etc. Dicarboxylic acid components that are the same as those listed in the copolyester (a1) can be cited as these dicarboxylic acid components.

[0149] When polyester (B) is a copolyester, the proportion of dicarboxylic acid components other than terephthalic acid in the dicarboxylic acid components is preferably 1 to 30 mol%, more preferably 5 mol% or more, more preferably 10 mol% or more, and even more preferably 25 mol% or less, and even more preferably 20 mol% or less.

[0150] When polyester (B) is a copolyester, alcohol components other than ethylene glycol can be listed as: 1,4-butanediol, 1,6-hexanediol, ethylene glycol, diethylene glycol, trimethylene glycol, neopentyl glycol, 1,4-cyclohexanediol, bisphenol and their derivatives, etc.

[0151] In polyester (B), the proportion of alcohol components other than ethylene glycol in the total alcohol content is preferably 1 mol% or more and less than 100 mol%, more preferably 5 mol% or more, even more preferably 10 mol% or more, and even more preferably 95 mol% or less, and even more preferably 90 mol% or less.

[0152] The polyester in polyester (B) preferably includes polyester (z2) as described above, as detailed in the description of polyester (a2) above.

[0153] Furthermore, as the copolyester in polyester (B), a copolyester containing terephthalic acid as a dicarboxylic acid component and an alcohol component other than ethylene glycol (Y1) (Y2) as an alcohol component can also be suitably used. Among these, as for the copolymer polyester of polyester (B), a copolymer of terephthalic acid (X1) and a dicarboxylic acid component with 4 to 10 carbon atoms (X2) with an alcohol component other than ethylene glycol (Y1) (Y2) is preferred, namely copolyester (z1). The details of such copolyester (z1) are as described in the copolyester (a1) above, and therefore its detailed description is omitted.

[0154] (The proportions of each component in polyester layers (B1) and (B2))

[0155] The content of each polyester in the polyester (B) contained in the polyester layers (B1) and (B2) can be appropriately adjusted so that the proportion of each component in all the polyester (Z) contained in the copolyester film is within the range described later.

[0156] However, the proportion of the copolymer component of polyester (B) contained in each of the polyester layers (B1) and (B2), on a mol% basis, is preferably lower than the proportion of the copolymer component in the polyester layer (A), and more preferably lower than this proportion. By reducing the proportion of the copolymer component in each of the polyester layers (B1) and (B2), it is easy to ensure softness, high elongation, and good heat resistance.

[0157] Hereinafter, specifically, a more detailed description will be given of the use of the aforementioned copolyester (z1), polyester (z2), or both of them as the polyester (B) contained in each of the polyester layers (B1) and (B2). It should be noted that the copolyester (z1) in each of the polyester layers (B1) and (B2) is particularly preferably the aforementioned copolyester (Za). Furthermore, the polyester (z2) is preferably polyethylene terephthalate.

[0158] Furthermore, the proportion of the dicarboxylic acid component (X2) with 4 to 10 carbon atoms in the total dicarboxylic acid component of polyester (B) contained in each of the polyester layers (B1) and (B2), on a mol% basis, is preferably lower than the proportion of the dicarboxylic acid component (X2) with 4 to 10 carbon atoms in the total dicarboxylic acid component of polyester (A) contained in the polyester layer (A). It should be noted that when the proportion is lower than this, the difference in proportion is, for example, 1 to 30 mol%, preferably 2 to 20 mol%, and more preferably 3 to 10 mol%.

[0159] It should be noted that the term "total polyester (B)" here refers to all the polyester contained in each of the polyester layers (B1) and (B2). Therefore, the proportion of the total polyester (B) mentioned above refers to the proportion based on the dicarboxylic acid content of the polyester (B) constituting the polyester layer (B1) or the polyester (B) in (B1). Hereafter, similar terms will be used with the same meaning.

[0160] Furthermore, as the dicarboxylic acid component (X2) with 4 to 10 carbon atoms, adipic acid is preferably used as described above. When using adipic acid, the proportion of adipic acid in the total dicarboxylic acid component of the polyester (B) contained in each of the polyester layers (B1) and (B2), in mol%, is preferably less than the proportion of adipic acid in the total dicarboxylic acid component of the polyester (A) contained in the polyester layer (A), and more preferably less than this proportion. It should be noted that when the proportion is less than this, the difference in proportion is, for example, 1 to 30 mol%, preferably 2 to 20 mol%, and more preferably 3 to 10 mol%.

[0161] On the other hand, the proportion of terephthalic acid (X1) in the dicarboxylic acid component of all polyester (B) contained in each of the polyester layers (B1) and (B2), based on mol%, is preferably higher than the proportion of terephthalic acid (X1) in the dicarboxylic acid component of all polyester (A) contained in the polyester layer (A).

[0162] The proportion of other alcohol components (Y2) in the total alcohol content of all polyester (B) contained in each of the polyester layers (B1) and (B2), in mol%, is preferably less than the proportion of other alcohol components (Y2) in the total alcohol content of all polyester (A) contained in the polyester layer (A), more preferably less than this proportion. When the proportion is less than this, the difference is, for example, 1 to 50 mol%, preferably 5 to 40 mol%, and even more preferably 10 to 35 mol%.

[0163] Furthermore, as other alcohol components (Y2), 1,4-butanediol, 1,6-hexanediol, or both are preferably used. The proportion of 1,4-butanediol and 1,6-hexanediol in the total alcohol content of all polyester (B) contained in each polyester layer (B1) and (B2), in mol%, is preferably less than or equal to the proportion of 1,4-butanediol and 1,6-hexanediol in the total alcohol content of all polyester (A) contained in the polyester layer (A). It should be noted that when the proportion is less than or equal to this, the difference in proportion is, for example, 1 to 50 mol%, preferably 5 to 40 mol%, and more preferably 10 to 35 mol%.

[0164] On the other hand, the proportion of ethylene glycol (Y1) in the total alcohol content of all polyester (B) contained in each of the polyester layers (B1) and (B2), based on mol%, is preferably higher than the proportion of ethylene glycol (Y1) in the total alcohol content of all polyester (A) contained in the polyester layer (A).

[0165] (The proportions of each component in the overall membrane)

[0166] The polyester used in the copolyester film preferably comprises copolyester (z1), and particularly preferably copolyester (Za). Details of the copolyester (z1) and copolyester (Za) are as described in the copolyester layer (A1).

[0167] Furthermore, the proportion of the dicarboxylic acid component (X2) with 4 to 10 carbon atoms in the total dicarboxylic acid component (Z) contained in the copolyester film is preferably 1 to 30 mol%. It should be noted that "total polyester (Z)" here refers to all the polyester contained in the copolyester film. Therefore, the above proportion refers to the proportion based on the dicarboxylic acid component constituting all the polyester (Z) contained in the copolyester film; similar terms will be used with the same meaning below.

[0168] Here, if the proportion of dicarboxylic acid component (X2) with 4 to 10 carbon atoms is 1 mol% or more, the effect of using dicarboxylic acid component (X2) with 4 to 10 carbon atoms can be fully obtained, easily reducing the storage modulus and ensuring flexibility and high elongation at low temperatures. In addition, if it is 30 mol% or less, the heat shrinkage rate becomes higher, but heat resistance is easily ensured.

[0169] The proportion of the dicarboxylic acid component (X2) with 4 to 10 carbon atoms in the polyester (Z) is more preferably 2 mol% or more, more preferably 3 mol% or more, particularly 4 mol% or more, and more preferably 20 mol% or less, more preferably 15 mol% or less, and particularly preferably 10 mol% or less.

[0170] In addition, the proportion of adipic acid in the dicarboxylic acid component of all polyester (Z) is, for example, 1 to 30 mol%, preferably 2 mol% or more, more preferably 3 mol% or more, particularly 4 mol% or more, and preferably 20 mol% or less, more preferably 15 mol% or less, and even more preferably 10 mol% or less.

[0171] Furthermore, from the viewpoint of maintaining various properties such as heat resistance, the proportion of terephthalic acid (X1) in the dicarboxylic acid component of all polyester (Z) is, for example, 65 to 98 mol%, preferably 97 mol% or less, more preferably 96 mol% or less, and preferably 75 mol% or more, more preferably 80 mol% or more, and particularly 85 mol% or more.

[0172] Furthermore, the proportion of other dicarboxylic acids (X3) in the dicarboxylic acid content of the entire polyester (Z) is, for example, 10 mol% or less, preferably 5 mol% or less, more preferably 3 mol% or less, and most preferably 0 mol%. That is, the dicarboxylic acid content in the polyester (A) preferably does not contain other dicarboxylic acids (X3).

[0173] Furthermore, the proportion of other alcohol components (Y2) in the total alcohol components of the polyester (Z) contained in the copolyester film is, for example, 10 to 60 mol, preferably 15 mol or more, more preferably 20 mol% or more, further preferably 23 mol% or more, even more preferably 25 mol% or more, and preferably 60 mol or less, more preferably 55 mol% or less, even more preferably 45 mol% or less, and even more preferably 35 mol% or less. If the proportion of alcohol components (Y2) in the polyester (Z) is a certain level or higher, it is easy to reduce the storage modulus and ensure softness and high elongation at low temperatures. In addition, if the proportion of alcohol components (Y2) is a certain level or lower, it is easy to prevent the heat shrinkage rate from becoming high and to ensure heat resistance.

[0174] In addition, the proportion of 1,4-butanediol and 1,6-hexanediol in the alcohol content of polyester (Z) is, for example, 10 to 60 mol, preferably 15 mol or more, more preferably 20 mol% or more, even more preferably 22 mol% or more, even more preferably 24 mol% or more, and preferably 60 mol or less, more preferably 55 mol% or less, even more preferably 44 mol% or less, and even more preferably 34 mol% or less.

[0175] Furthermore, when the polyester (Z) contains 1,4-butanediol and 1,6-hexanediol, the molar ratio of 1,6-hexanediol to 1,4-butanediol in the polyester (Z) is, for example, 0.5 or more, preferably 0.7 or more, more preferably 0.8 or more, even more preferably 0.9 or more, or for example, 2.5 or less, preferably 2.0 or less, more preferably 1.6 or less, even more preferably 1.4 or less.

[0176] The proportion of ethylene glycol (Y1) in the total alcohol content of the polyester (Z) is, for example, 40 to 85 mol%, preferably 40 mol% or more, more preferably 45 mol% or more, even more preferably 55 mol% or more, and even more preferably 60 mol% or more. It is also preferably 82 mol% or less, more preferably 80 mol% or less, even more preferably 77 mol% or less, and even more preferably 75 mol% or less.

[0177] <Thickness of this copolyester film>

[0178] There is no particular limitation on the thickness of this copolyester film; an appropriate thickness can be selected according to the application.

[0179] From the viewpoint of further maximizing the characteristics of this copolyester film, the total thickness of the film is preferably greater than 5 μm.

[0180] It is generally believed that the stiffness of a membrane is proportional to the cube of its thickness. However, this copolyester membrane, even with a thickness exceeding 5 μm, exhibits weak stiffness and flexibility, allowing for further enjoyment of the benefits of this invention.

[0181] Based on the above viewpoints, the total thickness of the copolyester film is preferably greater than 5 μm, more preferably greater than 12 μm, and even more preferably greater than 30 μm.

[0182] In addition, the total thickness of this copolyester film is not particularly limited, for example, it is 200 μm or less, preferably 150 μm or less, and more preferably 100 μm or less.

[0183] <Method for manufacturing this copolyester film>

[0184] As an example of the manufacturing method of this copolyester film, the manufacturing method when the copolyester film is a biaxially stretched film will be described. However, the manufacturing method described here is not the only one.

[0185] First, using a known method, raw materials, such as polyester flakes, are fed into a melt extrusion apparatus, heated to above the melting point of each polymer, and the molten polymer is extruded from the die and cooled and solidified on a rotating cooling drum to a temperature below the glass transition temperature of the polymer, thus obtaining an unoriented sheet that is essentially in an amorphous state.

[0186] Next, the unoriented sheet is stretched in one direction using a stretching machine, either a roller or a tenter frame. The stretching temperature is typically 25–120°C, preferably 35–100°C, and the stretching ratio is typically 2.5–7 times, preferably 2.8–6 times.

[0187] Next, stretching is performed in a direction orthogonal to the stretching direction of the first stage. At this time, the stretching temperature is usually 50 to 140°C, and the stretching ratio is usually 3.0 to 7 times, preferably 3.5 to 6 times.

[0188] It should be noted that, in the above stretching process, a method of stretching in one direction in two or more stages can also be adopted.

[0189] After stretching, the film undergoes heat-fixing treatment at a temperature of 130–270°C under tension or with a relaxation of up to 30%, thereby obtaining this copolyester film as a biaxially oriented film. This heat-fixing treatment improves the flexibility and heat resistance of the copolyester film.

[0190] Regarding the heat-setting treatment (also referred to as "heat treatment"), in the case of a single layer of copolyester (A1), it is preferable to perform the treatment at a temperature 5 to 70°C lower than the melting point of the polyester used to form the copolyester layer (A1). In the case of a multilayer structure, it is also preferable to perform the treatment at a temperature 5 to 70°C lower than the melting point of the polyester used to form the copolyester layer (A1), and more preferably at a temperature 5 to 70°C lower than the melting point of the polyester used to form the polyester layer (B).

[0191] When this copolyester film has a laminated structure of polyester layer (A1) and polyester layers (B1) and (B2), the polyester layers (A1) and (B1) and (B2) are co-extruded to form an integral film, which can then be stretched and heat-fixed as described above. It should be noted that this copolyester film can also be manufactured by co-extrusion in laminated structures other than those described above, such as layers (A1), (B1), and (B2).

[0192] Properties of release film

[0193] (Storage modulus at 80℃)

[0194] The release film of the present invention requires a storage modulus of 1000 MPa or less at 80°C. By having a storage modulus of 1000 MPa or less at 80°C, good flexibility and surface conformability can be ensured, for example, when installed in a mold, it can fully conform to the shape of the mold.

[0195] Based on the above viewpoint, the storage modulus of the release film at 80°C is more preferably 1000 MPa or less, more preferably 800 MPa or less, and particularly preferably 400 MPa or less.

[0196] On the other hand, from the viewpoint of operability in each process, the energy storage modulus at 80°C is preferably 100 MPa or more, and more preferably 200 MPa or more.

[0197] It should be noted that the energy storage modulus at 80°C and 180°C (described later) are values ​​obtained by the measurement method described in the examples described later.

[0198] In the release film, to achieve the storage modulus within the aforementioned range at 80°C, this can be achieved by adjusting the type and content of the copolymer component in the copolyester film. From this perspective, the copolymer component in the copolyester film preferably includes, for example, an aliphatic dicarboxylic acid with 4 to 10 carbon atoms, and one or both of 1,4-butanediol and 1,6-hexanediol. The proportions of these components in the dicarboxylic acid and alcohol components of the polyester (Z) are preferably 1 to 30 mol% and 15 to 60 mol%, as described above. More preferably, the aliphatic dicarboxylic acid with 4 to 10 carbon atoms is adipic acid.

[0199] The other alcohol components (Y2) are preferably 1,4-butanediol and 1,6-hexanediol, and in this case, the total amount (mol%) of the other alcohol components (Y2) is preferably 15 to 60 mol.

[0200] In addition, by stacking polyester layers (B1) and (B2) containing polyester (B) as the main component resin on both sides of the copolyester layer (A1) to form a multilayer structure, it is also easy to adjust the energy storage modulus at 80°C to the above range.

[0201] Furthermore, the energy storage modulus at 80°C can also be adjusted by the stretching conditions during the manufacture of this copolyester film and the subsequent heat-fixing conditions.

[0202] (Storage modulus at 180℃)

[0203] The energy storage modulus of the release film of the present invention at 180°C is 30 MPa or more, preferably 40 MPa or more, and more preferably 50 MPa or more, especially 60 MPa or more.

[0204] With a storage modulus of 30 MPa or more, especially 40 MPa or more, near the processing temperature (180°C), the heat resistance becomes excellent. Furthermore, the improved heat resistance also makes it easier to suppress thermal shrinkage.

[0205] In addition, the energy storage modulus at 180°C is not particularly limited, but from the viewpoint of flexibility, it is, for example, 400 MPa or less, preferably 200 MPa or less, and even more preferably 150 MPa or less.

[0206] (Storage modulus at 80℃ / Storage modulus at 180℃)

[0207] The ratio of the storage modulus at 80°C to the storage modulus at 180°C (storage modulus at 80°C / storage modulus at 180°C) of the release film of the present invention is 13 or less. If the above-mentioned storage modulus ratio is higher than 13, it is difficult to increase the storage modulus at around 180°C while reducing the storage modulus at around 80°C, making it difficult to use as a substitute for fluoropolymer films. The above-mentioned storage modulus ratio is preferably 12 or less, more preferably 10 or less. In addition, the lower the above-mentioned storage modulus ratio, the better; it is acceptable as long as it is 1 or more, and in practical applications, it can be 2 or more, or even 3 or more.

[0208] (Softening temperature determined by nano TA)

[0209] For the release film, when the copolyester film has a multilayer structure, the temperature difference between at least one of the copolyester layer (A1) and polyester layers (B1) and (B2), as determined by the softening temperature measurement using nano TA, is preferably 5°C or more. Specifically, the temperature difference between the copolyester layer (A1) and the polyester layers (B1) and (B2) is preferably 5°C or more. By ensuring that the difference in softening temperature between layer (A) and layers (B1), (B2), or both, is constant or greater, the amount of copolymer components between layers (A) and layers (B1), (B2), or both, can easily vary, thus improving various properties.

[0210] Furthermore, the softening temperature of at least one, preferably both, of the polyester layers (B1) and (B2) is preferably higher than that of the copolyester layer (A1). By having one or both of the polyester layers (B1) and (B2) have a higher softening temperature than the copolyester layer (A1) and by having a predetermined temperature difference, the copolymer content in the copolyester layer (A1) increases, while the copolymer content in the polyester layers (B1) and (B2) decreases, ensuring softness and high elongation, and also easily improving heat resistance.

[0211] The aforementioned temperature difference is more preferably 10°C or more, further preferably 15°C or more, and even more preferably 40°C or more. Furthermore, from the viewpoint of easily adjusting various physical properties, the aforementioned temperature difference is preferably 100°C or less, more preferably 90°C or less, further preferably 80°C or less, and even more preferably 70°C or less.

[0212] Furthermore, from the viewpoint of heat resistance, the softening temperature of the copolyester layer (A1) obtained by nano TA measurement is preferably 160°C or higher, more preferably 170°C or higher, and even more preferably 180°C or higher. In addition, from the viewpoint of softness, elongation, etc., it is preferably 230°C or lower, more preferably 220°C or lower, and even more preferably 215°C or lower.

[0213] Furthermore, from the viewpoint of heat resistance, the softening temperature of each of the polyester layer (B1) and polyester layer (B2) obtained by nano TA measurement is preferably 180°C or higher, more preferably 200°C or higher, and even more preferably 210°C or higher. In addition, from the viewpoint of softness, elongation, etc., the softening temperature is preferably 265°C or lower, more preferably 260°C or lower, and even more preferably 255°C or lower.

[0214] <Details about the release film>

[0215] The release film of one embodiment of the present invention has the above-described copolyester film and a resin layer A disposed on at least one side of the copolyester film.

[0216] The resin layer can also be stretched together with the copolyester film while it is laminated on top of the aforementioned copolyester film. As a result, the thickness of resin layer A becomes thinner, forming a functional sheet.

[0217] This copolyester film is soft and has a higher elongation at room temperature, making it easy to stretch and suitable for forming functional sheets by stretching. Furthermore, due to its good heat resistance, heat shrinkage is minimal even when the laminated film is heat-treated.

[0218] In the release film of the present invention, the resin layer A has the function of serving as a release layer.

[0219] <<Resin Layer A>>

[0220] Resin layer A is preferably a layer cured from a release layer composition (sometimes referred to as "this release layer composition") mainly composed of a silicone-based resin and preferably a curable silicone resin (sometimes referred to as "this curable silicone resin"), and is disposed on at least one side of the aforementioned copolyester film. Resin layer A can also be described as a release layer containing a cured product of the release layer composition.

[0221] Alternatively, resin layer A may also contain non-silicone resins. Examples of non-silicone resins include: alkyd resins, olefin resins, acrylic resins, compounds containing long-chain alkyl groups, rubber resins, waxes, and other non-silicone resins.

[0222] Resin layer A can be composed solely of non-silicone resin, or it can be combined with other components such as adhesive resin and crosslinking agent. By using non-silicone resin for resin layer A, the release layer can also be set as a non-silicone release layer.

[0223] When resin layer A contains a non-silicone resin, the content of the non-silicone resin in this resin layer composition, relative to the total mass of the non-volatile components in resin composition A, is preferably 5 to 90% by mass, more preferably 10 to 70% by mass, and even more preferably 10 to 50% by mass. By setting the content of the non-silicone resin within the above range, the demolding properties of resin layer A from the mold become good.

[0224] (wax)

[0225] Examples of waxes include natural waxes, synthetic waxes, and modified waxes.

[0226] As natural waxes, they include plant-based waxes, animal-based waxes, mineral-based waxes, and petroleum waxes.

[0227] Examples of plant-based waxes include: candelilla wax, carnauba wax, rice bran wax, wood wax, and jojoba oil.

[0228] Examples of animal-derived waxes include beeswax, lanolin, and whale wax.

[0229] Examples of mineral-based waxes include: lignite wax, ceresin wax, and pure ceresin wax.

[0230] Examples of petroleum waxes include paraffin wax, microcrystalline wax, and petrolatum.

[0231] Examples of synthetic waxes include: synthetic hydrocarbons, hydrogenated waxes, fatty acids, acid amides, amines, imides, ester waxes, and ketones. Other examples include: Fischer-Tropsch wax (also known as Sasol wax), polyethylene wax, etc. In addition, examples of low molecular weight polymers (specifically, polymers with a number average molecular weight of 500 to 20,000) include: polypropylene, ethylene-acrylic acid copolymers, polyethylene glycol, polypropylene glycol, and block or graft copolymers of polyethylene glycol and polypropylene glycol, etc.

[0232] Examples of modified waxes include, for example, lignite wax derivatives, paraffin wax derivatives, and microcrystalline wax derivatives. Here, "derivative" refers to a compound obtained through any of the following treatments: purification, oxidation, esterification, saponification, or a combination thereof. Examples of hydrogenated waxes include hydrogenated castor oil and hydrogenated castor oil derivatives.

[0233] From the viewpoint of excellent demolding performance, synthetic waxes are preferred, with polyethylene wax being more preferred, and oxidized polyethylene wax being even more preferred.

[0234] From the viewpoint of the surface-forming properties and operability resulting from phase separation, the number-average molecular weight of the synthetic wax is preferably 500 to 30,000, more preferably 1,000 to 15,000, and even more preferably in the range of 2,000 to 8,000.

[0235] Furthermore, when forming resin layer A, if heating is taken into account for crosslinking, the melting point or softening point of the wax is preferably 80°C or higher, more preferably 110°C or higher. On the other hand, from the viewpoint of controlling phase separation performance after heat treatment, the melting point or softening point of the wax is preferably 200°C or lower, more preferably 170°C or lower, and even more preferably 150°C or lower.

[0236] (Compounds containing long-chain alkyl groups)

[0237] The term "compound containing long-chain alkyl" refers to a compound having a straight-chain or branched alkyl group having 6 or more carbon atoms, preferably 8 or more, and more preferably 12 or more.

[0238] Examples of alkyl groups include hexyl, octyl, decyl, lauryl, octadecyl, and behenyl. Examples of compounds containing alkyl groups include various polymers containing long-chain alkyl groups, amines containing long-chain alkyl groups, ethers containing long-chain alkyl groups, and quaternary ammonium salts containing long-chain alkyl groups. Considering heat resistance, polymers are preferred, and from the viewpoint of effectively obtaining moderate phase separation and resulting surface roughness with a low content, polymers having long-chain alkyl groups in their side chains are more preferred.

[0239] Polymer compounds with long-chain alkyl side chains can be obtained by reacting a polymer with a reactive group with a compound having an alkyl group capable of reacting with that reactive group. Examples of such reactive groups include hydroxyl, amino, carboxyl, and acid anhydride groups. Examples of compounds containing these reactive groups include polyvinyl alcohol, polyethyleneimine, polyethyleneamine, polyester resins containing reactive groups, and poly(meth)acrylic acid resins containing reactive groups. Among these, polyvinyl alcohol is preferred considering ease of handling.

[0240] Examples of compounds containing alkyl groups capable of reacting with the aforementioned reactive groups include: isocyanates containing long-chain alkyl groups such as hexyl isocyanate, octyl isocyanate, decyl isocyanate, lauryl isocyanate, octadecyl isocyanate, and behenyl isocyanate; acyl chlorides containing long-chain alkyl groups such as hexanoyl chloride, octanoyl chloride, decanoyl chloride, lauroyl chloride, octadecanoyl chloride, and behenyl chloride; amines containing long-chain alkyl groups; and alcohols containing long-chain alkyl groups. Among these, isocyanates containing long-chain alkyl groups are preferred for ease of handling, and octadecyl isocyanate is particularly preferred.

[0241] In addition, polymers with long-chain alkyl side chains can also be obtained by polymerizing long-chain alkyl methacrylates or by copolymerizing long-chain alkyl methacrylates with other vinyl-containing monomers. Examples of long-chain alkyl methacrylates include: hexyl methacrylate, octyl methacrylate, decyl methacrylate, lauryl methacrylate, octadecyl methacrylate, and behenyl methacrylate.

[0242] (Adhesive resin)

[0243] To improve the coatability of the polyester film, an adhesive resin may also be used. The adhesive resin is preferably a polymer with a number-average molecular weight (Mn) of 1000 or higher, as determined by gel permeation chromatography (GPC) according to the "Flowchart for Safety Evaluation of Polymer Compounds" (November 1985, sponsored by the Chemical Substances Review Board), and possesses film-forming properties. There are no particular limitations on the adhesive resin used; conventionally known adhesive resins can be used. Examples include (meth)acrylic resin, polyvinyl alcohol, polyester resin, and polyurethane resin. From the viewpoint of high hydrophilicity and film formation, the (B) adhesive resin is preferably selected from at least one of (meth)acrylic resin and polyvinyl alcohol, more preferably (meth)acrylic resin. It should be noted that the (B) adhesive resin can be used alone or in combination with two or more.

[0244] (Cross-linking agent)

[0245] To impart durability to resin layer A, a crosslinking agent may also be used. There are no particular limitations on the crosslinking agent; conventionally known crosslinking agents can be used. Examples include melamine compounds, oxazoline compounds, epoxy compounds, carbodiimide compounds, isocyanate compounds, and silane coupling compounds. From the viewpoint of imparting durability to resin layer A, it is preferable to include at least one selected from melamine compounds and oxazoline compounds.

[0246] <Mold Release Layer Composition>

[0247] The release layer composition is preferably a composition with a curable silicone resin as the main component resin. Here, "main component resin" refers to the resin with the largest mass proportion in the resin constituting the release layer composition, which is envisioned to account for 50% or more, 75% or more, 90% or more, or 100% of the resin constituting the release layer composition.

[0248] (Cureable silicone resin)

[0249] In this invention, "curing silicone resin" refers to a silicone resin that has the property of being able to cure.

[0250] The curing method for curable silicone resins is arbitrary. For example, it can be a substance that cures through a condensation reaction by reacting with moisture in the air, a substance that cures through a heat-based addition reaction, or a substance that cures through photo-addition polymerization or free radical polymerization.

[0251] From the perspective of having no byproducts of the curing reaction and stable physical properties of the cured film, thermosetting silicone resins that are cured by heating-based addition reactions are preferred.

[0252] When the curable silicone resin is thermosetting, it is characterized in that, in the structure, vinyl (Vi) or hexenyl or other alkenyl groups are introduced into the side chains and / or ends of the main chain composed of siloxane bonds.

[0253] Curing silicone resins can be any polymer whose main chain is composed of siloxane bonds formed by silicon and oxygen.

[0254] Examples of cured silicone resins include resins in which various substituents are introduced into the side chains or ends of the main chain composed of siloxane bonds. Examples of such substituents include any one or more combinations of methyl, phenyl, polyether, epoxy, amine, carboxyl, and aralkyl groups.

[0255] In addition, as an example of a cured silicone resin, another example is a silicone resin in which Si-H groups and vinyl groups are introduced into the side chains and / or ends of the straight-chain main chain composed of siloxane bonds.

[0256] When the cured silicone resin contains Si-H groups, the content of Si-H groups relative to the total amount of siloxane components is preferably 0.8 to 2.2 mol%, more preferably 1.2 mol% or more, particularly preferably 1.4 mol% or more, and even more preferably 2.1 mol% or less, preferably 2.0 mol% or less.

[0257] Furthermore, when the cured silicone resin with introduced alkenyl groups does not inherently possess Si-H groups, but rather Si-H groups are added as a crosslinking agent, the content of Si-H groups, relative to the total siloxane content in the cured silicone resin, preferably includes 0.8 to 2.2 mol% Si-H groups, more preferably 1.2 mol% or more, particularly preferably 1.4 mol% or more, and even more preferably 2.1 mol% or less, preferably 2.0 mol% or less. It should be noted that, as a crosslinking agent, a silicone crosslinking agent described later is preferred.

[0258] Regarding the vinyl content in the cured silicone resin, it is preferable to contain 0.4 to 1.5 mol% vinyl content relative to the total siloxane content, more preferably 0.5 mol% or more, even more preferably 0.6 mol% or more, and even more preferably 1.3 mol% or less.

[0259] Cured silicone resins can also be a combination of two or more cured silicone resins. In this case, regarding the content ratio of each functional group mentioned above, it is preferable that the vinyl content and Si-H group content in the total amount of the two or more cured silicone resins are within the ranges described above.

[0260] When using two or more curable silicone resins, for example, a curable silicone resin (main agent) having vinyl or other alkenyl groups can be used in combination with a silicone resin having Si-H groups (also known as a silicone crosslinking agent). By mixing the main agent and the silicone crosslinking agent and heating it to allow an addition reaction, the release layer composition can be properly cured.

[0261] The vinyl content in the cured silicone resin constituting the main agent is preferably 0.4 to 2.5 mol%, more preferably 0.5 mol% or more, even more preferably 0.6 mol% or more, and even more preferably 2.0 mol% or less, and even more preferably 1.5 mol% or less.

[0262] Another example of a silicone crosslinking agent is a silicone resin in which Si-H groups and vinyl groups are introduced into the side chains and / or ends of a straight-chain main chain composed of siloxane bonds. The silicone crosslinking agent is preferably part of a cured silicone resin.

[0263] The number average molecular weight (Mn) of the cured silicone resin is preferably above 9000 and below 350000.

[0264] If the number average molecular weight (Mn) of the cured silicone resin is above the lower limit mentioned above, the amount of low molecular weight silicone resin dissolving or migrating into the adhesive layer can be reduced when the release film is laminated. Furthermore, a light peeling effect is easily obtained by applying a thicker release layer. On the other hand, if the number average molecular weight (Mn) of the cured silicone resin is below the upper limit mentioned above, the viscosity is prevented from increasing, thus reducing the fluidity of the release layer composition. Therefore, when applying the release layer composition, streaky coating unevenness can be prevented, and the surface of the release layer is easily smoothed.

[0265] Based on the above viewpoint, the number average molecular weight (Mn) of the cured silicone resin is more preferably 10,000 or more, further preferably 20,000 or more, and particularly preferably 30,000 or more. On the other hand, it is more preferably 50,000 or less, and further preferably 40,000 or less.

[0266] From the same viewpoint as the number-average molecular weight, the mass-average molecular weight (Mw) of the cured silicone resin is preferably 10,000 to 500,000, more preferably 20,000 or more, even more preferably 50,000 or more, particularly preferably 80,000 or more, and even more preferably 250,000 or less, even more preferably 100,000 or less.

[0267] The ratio (Mw / Mn) of the weight-average molecular weight (Mw) to the number-average molecular weight (Mn) of the cured silicone resin is preferably 1.7 to 2.7, more preferably 1.9 or more, and even more preferably 2.5 or less. By satisfying this range, it is expected that the crosslinking reaction can proceed efficiently.

[0268] It should be noted that the number-average molecular weight (Mn) and mass-average molecular weight (Mw) are values ​​obtained by gel permeation chromatography (GPC) based on polystyrene. The specific determination method is as follows: using a GPC apparatus, the chromatogram is measured, and the number-average molecular weight (Mn) and mass-average molecular weight (Mw) are determined based on a standard curve using standard polystyrene. Specifically, 4 mg of the sample is dissolved in 4 mL of THF to prepare the assay solution, and 100 μL of the assay solution is injected into the GPC apparatus for analysis. Tetrahydrofuran (THF) is used as the eluent. For analysis, Tosoh Corporation's "Ecosec 8320" is used, and the guard column is Tosoh Corporation's "TSKgel guardcolumn HXL-L". The column is a four-piece column (Tosoh Corporation's "TSKgel GMHXL"). Furthermore, the analysis is performed at an oven temperature of 40°C and a THF flow rate of 1.0 mL / min, using RI for detection.

[0269] Curing silicone resins can also be composed of a combination of two or more curing silicone resins. In this case, it is preferable that the average molecular weight of the two or more curing silicone resins is within the aforementioned range. It should be noted that the "average" referred to here is a weighted average obtained by weighting according to the mass of each resin.

[0270] In addition, when using a main agent and a silicone crosslinking agent, the number-average molecular weight, mass-average molecular weight, and Mw / Mn of the main agent should preferably be within the above ranges.

[0271] The preferred curable silicone resin has a viscosity of 1–400 mcps at 25°C when diluted with n-heptane solvent to 15% by mass.

[0272] If the viscosity of this curable silicone resin is 1 mcps or more, shrinkage can be suppressed by the appropriate viscosity of the coating liquid, and a good coating appearance can be obtained. Therefore, it is preferable that if it is 400 mcps or less, the fluidity of the release layer composition can be maintained, and when coating the release layer composition, the formation of striped coating unevenness can be suppressed, thereby making the surface of the release layer smooth.

[0273] Based on the above viewpoint, the viscosity of the cured silicone resin is further preferably 1.0 mcps or more, and more preferably 10 mcps or more. On the other hand, it is more preferably 300 mcps or less, and more preferably 200 mcps or less.

[0274] Viscosity was measured by diluting the cured silicone resin to 15% by mass with n-heptane solvent and then measuring the viscosity of the solution at 25°C using an E-type viscometer (Toki Sangyo Co., Ltd. "TVE-22L").

[0275] The curing silicone resin can be either solvent-free curing silicone or solvent-based curing silicone. Alternatively, a combination of both can be used.

[0276] Here, "solvent-free curable silicone" refers to a silicone with a viscosity that can be coated even without being diluted in a solvent. It is composed of short polysiloxane chains and is a silicone resin with a low molecular weight.

[0277] On the other hand, "solvent-cured silicone" refers to silicone resins with such high viscosity that they cannot be coated without being diluted in a solvent. Compared to solvent-free cured silicone, it is a silicone with a higher molecular weight.

[0278] As described above, the curing silicone resin preferably has a moderate number-average molecular weight (Mn) and moderate viscosity. Furthermore, from the viewpoint that it provides good adhesion to the substrate film, eliminates uneven coating, provides a good coating appearance, and facilitates adjustment of the release layer film thickness, solvent-based curing silicone is preferred.

[0279] In the release layer composition, when the amount of vinyl groups is above a certain level relative to the total amount of siloxane components, the release layer is sufficiently cured. On the other hand, the amount of alkenyl groups, i.e., vinyl groups, does not become excessive, thereby preventing the peel force from becoming heavy after exposure to air. Therefore, the release layer composition preferably contains 0.4 to 1.0 mol% vinyl groups relative to the total amount of siloxane components. Particularly preferred is that it contains 0.5 mol% or more, and particularly preferred is 0.6 mol% or more and 0.9 mol% or less vinyl groups.

[0280] In the release layer composition, when the amount of Si-H groups is above a certain level relative to the total amount of siloxane components, the release layer is fully cured. On the other hand, the amount of Si-H groups does not become excessive. This prevents the residual Si-H groups after curing from reacting with the adhesive layer and inhibits the re-peeling of the release film. Therefore, the release layer composition preferably contains 0.8 to 2.2 mol% of Si-H groups relative to the total amount of siloxane components, more preferably 1.2 mol% or more, particularly preferably 1.4 mol% or more, and even more preferably 2.1 mol% or less, particularly preferably 2.0 mol% or less of Si-H groups.

[0281] The release layer composition may also contain other components besides the curable silicone resin, and may contain, as needed, catalysts, reaction control agents, crosslinking agents, polymerization initiators, diluents, light release agents, release control agents, and other additives.

[0282] The content of all siloxane components in the release layer composition can be, for example, determined by... 1 H-NMR is determined by the integral ratio of the dimethylsiloxane unit in the main chain to the units other than those in the main chain. Additionally, the content of vinyl and Si-H groups represents the proportion relative to the total amount of functional groups bonded to the siloxane chain, and can be determined by measuring... 1 We use H-NMR for evaluation. However, we are not limited to this method.

[0283] The release layer, or release layer composition, is substantially free of particles. By being substantially free of particles, the release layer stabilizes peeling properties and reduces migration. It should be noted that "substantially free" means that the release layer (release layer composition) may contain particles, for example, unavoidably mixed particles, as long as they are in a very small amount that does not hinder the effects of the present invention. Specifically, the particle content in the release layer, based on non-volatile components, is, for example, less than 0.05% by mass, preferably less than 0.01% by mass, more preferably less than 0.0001% by mass. It should be noted that the range of particle content in this release layer composition based on non-volatile components is also the same as the aforementioned particle content range.

[0284] (Light stripping agent)

[0285] In addition to the aforementioned cured silicone resin, the release layer composition may also contain a mild release agent. As a mild release agent, a silicone oil having a dimethylsiloxane backbone (DM) as shown in formula (I) and a methylphenylsiloxane backbone (MP) as shown in formula (II) is preferred.

[0286] [Chemical Formula 1]

[0287]

[0288] [Chemical Formula 2]

[0289]

[0290] By using a light release agent with a dimethylsiloxane backbone (DM) and a methylphenylsiloxane backbone (MP), for example, when the object being bonded is an adhesive layer, it can penetrate into the interior of the adhesive layer even if it migrates into the adhesive layer, thus mitigating the reduction in adhesive strength.

[0291] The ratio (DM:MP) of the dimethylsiloxane skeleton (DM) shown in formula (I) and the methylphenylsiloxane skeleton (MP) shown in formula (II) is preferably in the range of 98:2 to 70:30, more preferably in the range of 95:5 to 80:20, and particularly preferably in the range of 92:8 to 85:15, in terms of molar ratio.

[0292] By setting DM:PM within the above range, the peelability of this release film can be ensured.

[0293] Furthermore, the mass-average molecular weight of the light stripping agent is preferably less than 10,000. A mass-average molecular weight of less than 10,000 is advantageous in terms of migration and light stripping properties.

[0294] The content of the light release agent in the release layer composition is preferably 0.1 to 10 parts by weight relative to 100 parts by weight of the cured silicone resin, more preferably 0.5 to 8 parts by weight, and even more preferably 0.8 to 5 parts by weight.

[0295] When the content of the light-release agent is above the lower limit mentioned above, light-release can be achieved; when it is below the upper limit mentioned above, the adhesion to the substrate becomes good.

[0296] On the other hand, if it is desired to re-peel the release layer, a peel control agent (MQ resin (B)) can also be used.

[0297] MQ resin (B) is a resin containing M units [R3SiO] 1 / 2 (where R is a monovalent hydrocarbon group) The siloxane unit and Q unit [SiO] shown in the formula are siloxane units and Q units. 4 / 2 The silicone resin with siloxane units shown in the figure. MQ resin can be used alone or in combination of two or more, and can also contain D units [R2SiO]. 2 / 2 (In the formula, R is a hydrocarbon with a valence of 1)], T unit [RSiO 3 / 2 (where R is a monovalent hydrocarbon). Furthermore, as a functional group contained in the molecule, it is preferable not to include either an alkenyl group or a Si-H group. When either an alkenyl group or a Si-H group is included in the MQ resin, the amount of unreacted components (Si-H groups or alkenyl groups) remaining in the release layer tends to increase, easily leading to re-peeling.

[0298] The ratio of M units to Q units in MQ resin (B), expressed as M unit:Q unit (molar ratio), is preferably 0.1:1.0 to 1.0:1.0, more preferably 0.7:1.0 to 1.0:1.0. When the M unit (molar ratio) is less than 0.1, the crosslinking density decreases, and sometimes the peel strength cannot be sufficiently increased. On the other hand, when the Q unit (molar ratio) is greater than 1.0, the coating film becomes too hard and sometimes brittle.

[0299] Examples of commercially available MQ resins (B) include, for instance, those manufactured by Shin-Etsu Chemical Co., Ltd. such as KS-3800 and X-92-183, and those manufactured by Toray Industries, Inc. such as SD7292, BY24-843, and BY24-4980.

[0300] The mass ratio ((B) / (A)) of the cured silicone resin (A) to the MQ resin (B) is preferably in the range of 0.01 to 1.5, and more preferably 0.05 to 1.0. When (B) / (A) is 0.01 or higher, the peel force can be sufficiently increased. On the other hand, when (B) / (A) is 1.5 or lower, poor appearance of the release layer due to the poor film-forming properties of the MQ resin will not occur.

[0301] <Other Ingredients>

[0302] In addition to the curable silicone resin, the release layer composition may contain, as needed, a curing catalyst, a diluent solvent, a reaction control agent, a crosslinking agent other than the aforementioned silicone crosslinking agent, a polymerization initiator, a bonding enhancer, and other additives.

[0303] For example, as a release layer composition, one could include: a composition containing a curable silicone resin (main agent) having alkenyl groups such as vinyl groups, a silicone crosslinking agent having hydrogenated silyl (Si-H) groups on the side chains and / or ends of the main chain formed by siloxane bonds, a catalyst containing platinum (Pt) (platinum-based catalyst), and a solvent.

[0304] (catalyst)

[0305] As described above, this release layer composition may contain a curing catalyst as needed, namely a catalyst for promoting the hydrosilylation addition reaction of the alkenyl group bonded to silicon atoms of the cured silicone resin with the hydrosilane (SiH) group of the silicone crosslinking agent.

[0306] Examples of platinum group metal catalysts that can be used as solidification catalysts include: platinum black, platinum chloride, chloroplatinic acid, reactants of chloroplatinic acid with monohydric alcohols, complexes of chloroplatinic acid with olefins, platinum diacetate, palladium catalysts, and rhodium catalysts. However, they are not limited to these examples.

[0307] The content of the curing catalyst in this release layer composition, relative to the curable silicone resin, is preferably 0.5 to 500 ppm by mass in metal equivalent, more preferably 5 ppm by mass or more, even more preferably 10 ppm by mass or more, and even more preferably 300 ppm by mass or less, and even more preferably 200 ppm by mass or less.

[0308] (Diluting solvent)

[0309] As described above, this release layer composition may contain a diluent as needed. Examples of diluents include: aromatic hydrocarbons such as toluene, aliphatic hydrocarbons such as hexane, heptane, and isooctane, esters such as ethyl acetate and butyl acetate, ketones such as methyl ethyl ketone (MEK) and isobutyl methyl ketone, alcohols such as ethanol and 2-propanol, and ethers such as diisopropyl ether and dibutyl ether. Considering solubility, coatability, boiling point, etc., these are preferably used alone or in combination. The diluent is a volatile component that evaporates during drying after coating.

[0310] (Reaction control agent)

[0311] As described above, this release layer composition may contain a reaction control agent as needed. Examples of reaction control agents include ethynyl alcohol. One reaction control agent may be used, or two or more may be used in combination as needed. The content of the reaction control agent, relative to 100 parts by weight of the total amount of the release layer composition (based on non-volatile components), is preferably 0.001 to 5.0 parts by weight, more preferably 0.01 parts by weight or more, further preferably 0.05 parts by weight or more, and even more preferably 1.0 parts by weight or less, and even more preferably 0.5 parts by weight or less.

[0312] <Thickness of resin layer A>

[0313] To achieve the specified peel force, the thickness of resin layer A is preferably in the range of 0.05 to 1.5 μm. If the thickness of the release layer is less than 0.05 μm, as described later, it can be difficult to control the peel force of resin layer A. Furthermore, if it is thicker than 1.5 μm, the migration of the release agent components towards the adhered material (e.g., adhesive tape) increases, or adhesion cannot be adequately prevented. From the viewpoint of preventing adhesion and suppressing increased migration, the thickness of resin layer A is preferably 0.1 to 1.3 μm, and more preferably in the range of 0.1 to 1.0 μm.

[0314] Resin layer A can be formed, for example, by coating the release layer composition onto at least one side of a copolyester film and then drying and curing it appropriately. The coating of the release layer composition can be performed online on the forming line during the forming of the copolyester film, or offline after the film is formed.

[0315] <<Other Layers>>

[0316] This release film may have "other layers" between the substrate film and the resin layer A.

[0317] Examples of "other layers" include, for instance, antistatic layers, oligomer sealing layers, and other layers with various functions. Furthermore, the layer disposed between this copolyester film and this resin layer A is preferably a cured resin layer.

[0318] <Uses of release film>

[0319] As mentioned above, the release film has excellent flexibility at room temperature. It is not only soft but also has a high elongation rate, and it can also provide sufficient heat resistance for practical use.

[0320] With the above properties, the release film is suitable for various stretching processing applications, especially for stretch forming processing to obtain various molded products.

[0321] The release film of the present invention exhibits excellent flexibility in low-temperature regions, being not only soft but also possessing high elongation, while simultaneously exhibiting a moderate storage modulus in high-temperature regions, which are the opposite characteristics, thus providing practically sufficient heat resistance. Therefore, it is useful for semiconductor manufacturing applications, particularly as a release film for semiconductor compression molding.

[0322] <Explanation of statements, etc.>

[0323] In this invention, even when referred to as a "membrane", it also includes a "sheet", and even when referred to as a "sheet", it also includes a "membrane".

[0324] In addition, when referred to as "panel" as such as image display panel or protective panel, it includes the plate body, sheet and film.

[0325] In this invention, when referred to as "X to Y" (where X and Y are arbitrary numbers), unless otherwise specified, it also includes the meaning of "X or more and Y or less", and includes the meaning of "preferably greater than X" or "preferably less than Y".

[0326] Furthermore, when it is recorded as "X or above" (where X is any number), unless otherwise specified, it includes the meaning of "preferably greater than X". When it is recorded as "Y or below" (where Y is any number), unless otherwise specified, it also includes the meaning of "preferably less than Y".

[0327] Example

[0328] Next, the present invention will be described in further detail through embodiments. However, the present invention is not limited to the embodiments described below.

[0329] <Evaluation Methods>

[0330] The following methods are used to measure and evaluate various physical properties.

[0331] (1) Film thickness

[0332] After the membrane fragments were fixed with epoxy resin, they were cut using a slicing machine, and the cross-section of the membrane was observed using a transmission electron microscope. Within this cross-section, due to differences in light and shadow, two interfaces almost parallel to the membrane surface were observed. The distances from these two interfaces to the membrane surface were measured from 10 photographs, and the average value was taken as the membrane thickness.

[0333] (2) Tensile storage modulus E'

[0334] Based on JIS K 7244, using the DVA-200 dynamic viscoelasticity measuring apparatus manufactured by IT Measurement & Control Co., Ltd., measurements were taken in the length (MD) and width (TD) directions of the sample films obtained in the examples and comparative examples, at a vibration frequency of 10 Hz, a strain of 0.1%, and a heating rate of 1 °C / min, from -100 °C to 200 °C. The tensile storage modulus E' at 80 °C and 180 °C was obtained from the data, and the average value of the length (MD) and width (TD) directions was used as the storage modulus at 80 °C and 180 °C. Furthermore, the ratio of the storage modulus at 80 °C and 180 °C was calculated.

[0335] (3) Softening temperature determination

[0336] For the sample film, the softening temperature of each polyester resin layer was determined using a nano TA measuring device (Hitachi High-Tech Corporation AFM5300E). It should be noted that the surface and intermediate layers were measured under the following conditions, and the average value of N=3 was used as the softening temperature of each layer.

[0337] It should be noted that, regarding the measured values, based on the obtained measurement graphs, the tangents in each curve of the heating and cooling curves should be drawn, and the intersection points of the tangents should be determined.

[0338] Next, the point that passes through the obtained intersection and intersects perpendicularly with the measured temperature axis is taken as the softening temperature.

[0339] Measurement Conditions

[0340] Measurement mode: nano TA mode

[0341] Probe: AN2-300 thermal cantilever beam

[0342] Measurement temperature range: room temperature (23℃)

[0343] Atmosphere being measured: Atmospheric pressure

[0344] (4) Solvent resistance

[0345] After immersing the sample film in various solvents for 24 hours, visually observe its condition and make a judgment based on the following criteria.

[0346] (Judgment criteria)

[0347] A: There is no change in appearance or flatness.

[0348] B: Membrane curling.

[0349] C: Insufficient solvent resistance, resulting in membrane dissolution.

[0350] (5) Stretch followability (an alternative evaluation of die step followability)

[0351] Using the biaxial stretching device for membranes manufactured by Jingyuan, the sample membrane was stretched at a stretching ratio of 3.5 times (equivalent to an elongation of 250%).

[0352] The tensile followability of the obtained membrane is determined according to the following criteria.

[0353] (Judgment criteria)

[0354] A: Excellent tensile follow-through (elongation at break at room temperature is over 300%).

[0355] B: Good tensile follow-through (elongation at break at room temperature is over 250%).

[0356] C: Poor tensile follow-through (elongation at break at room temperature is less than 250%).

[0357] (raw material)

[0358] The following raw materials were used in the examples and comparative examples.

[0359] (1) Copolyester (a1-1)

[0360] A copolyester (a1-1) containing terephthalic acid and adipic acid (6 carbon atoms) as dicarboxylic acid components, wherein the content of terephthalic acid is 85% by mass and the content of adipic acid is 15% by mass, and containing 45% by mass of 1,4-butanediol and 55% by mass of 1,6-hexanediol as alcohol components is prepared (intrinsic viscosity (IV) 0.70 dl / g).

[0361] (2) Copolyester (a1-2)

[0362] A copolyester (a1-2) containing terephthalic acid and isophthalic acid as dicarboxylic acid components, with terephthalic acid content of 78% by mass and isophthalic acid content of 22% by mass, ethylene glycol as alcohol component of 98% by mass, and diethylene glycol of 2% by mass (intrinsic viscosity (IV) 0.70 dl / g) was prepared.

[0363] (3) Homopolymer Polyester (a2-1)

[0364] Prepare a homopolymer polyester (a2-1) with an intrinsic viscosity (IV) of 0.64 dl / g. This homopolymer polyester (a2-1) is a polyester in which the dicarboxylic acid component is composed of terephthalic acid, and the alcohol component is 98% by mass of ethylene glycol and 2% by mass of diethylene glycol.

[0365] (4) Homopolymer Polyester (a2-2)

[0366] Prepare a granular homopolymer polyester (a2-2) (granular homopolymer PET), which is a polyester with 98% by mass of ethylene glycol and 2% by mass of diethylene glycol as the alcohol component, an intrinsic viscosity (IV) of 0.62 dl / g, and contains 0.2% by mass of silica particles with an average particle size of 3 μm.

[0367] [Example 1-1]

[0368] Fragments of a polyester composition comprising 35% by mass of copolyester (a1-1), 50% by mass of homopolymer (a2-1), and 15% by mass of homopolymer (a2-2) are fed into a main twin-screw extruder with a vent set to 270°C.

[0369] Extruded from the die, the unstretched sheet is rapidly cooled and solidified on a cooling roller with the surface temperature set at 25°C using an electrostatic application method.

[0370] Next, the unstretched sheet was stretched 3.0 times along the length direction (MD) at 60°C and then fed into a tenter frame. It was then stretched 4.3 times along the width direction (TD) at 85°C and subjected to heat treatment at 230°C for 10 seconds to obtain a copolyester film (sample) with a thickness of 50 μm.

[0371] Next, a resin layer A composed of the following resin layer composition is coated to a thickness (after drying) of 0.1 μm, and after drying at 120°C for 20 seconds, a release film (sample film) with a thickness of 50 μm is obtained.

[0372] (Resin composition)

[0373] Curing silicone resin (Dow Toray LTC856): 100 parts by weight

[0374] Hardener (Dow Toray SRX-212): 1 part by weight

[0375] Solvent: Toluene: 600 parts by weight

[0376] MEK: 600 parts by weight

[0377] Hexane: 600 parts by mass

[0378] [Examples 1-2]

[0379] In Example 1, except for changing the type of resin layer A, the rest was manufactured in the same way to obtain a release film (sample film) with a thickness of 50 μm.

[0380] (Resin composition)

[0381] Curing silicone resin (Shin-Etsu Chemical Industry X-62-5039): 80 parts by weight

[0382] Curing silicone resin (Shin-Etsu Chemical Industry KS-3800): 20 parts by weight

[0383] Curing agent (Shin-Etsu Chemical Industry PL-5000): 2 parts by weight

[0384] Solvent: Toluene: 600 parts by weight

[0385] MEK: 600 parts by weight

[0386] Hexane: 600 parts by mass

[0387] [Example 2-1]

[0388] Fragments of a polyester composition comprising 35% by mass of copolyester (a1-1) and 65% by mass of homopolymer (a2-1) were fed into a main twin-screw extruder with a vent set to 270°C for use as the intermediate layer (copolyester layer (A1)). Fragments of a polyester composition comprising 35% by mass of copolyester (a1-1), 35% by mass of homopolymer (a2-1), and 30% by mass of homopolymer (a2-2) were fed into another twin-screw extruder with a vent set to 270°C for use as the top layers (polyester layers (B1) and (B2)). The polyester raw materials were co-extruded from the die and quenched on cooling rollers with a surface temperature set to 25°C using an electrostatic curing method to obtain an unstretched sheet.

[0389] Next, the obtained unstretched sheet was stretched 3.0 times along its length (MD) at 60°C, then fed into a tenter frame, and stretched 4.3 times along its width (TD) at 85°C. It was then heat-treated at 230°C for 10 seconds to obtain a 50 μm thick copolyester film (sample) with a multilayer structure of polyester layer (B1) / copolyester layer (A1) / polyester layer (B2). Next, resin layer A, formed from the resin layer composition used in Examples 1-1, was coated to a thickness (after drying) of 0.1 μm, and dried at 120°C for 20 seconds to obtain a 50 μm thick release film (sample film).

[0390] [Example 2-2]

[0391] Except for changing the resin composition used to form resin layer A to the resin composition used in Examples 1-2, the rest was carried out in the same manner as in Examples 2-1, resulting in a release film (sample film) with a thickness of 50 μm.

[0392] [Examples 2-3, Examples 2-5]

[0393] Except for changing the composition of the polyester used for the intermediate layer and the top layer as shown in Table 1, the rest was carried out in the same manner as in Example 2-1 to obtain a release film (sample film) with a thickness of 50 μm.

[0394] [Examples 2-4, Examples 2-6]

[0395] Except for changing the composition of the polyester used for the intermediate layer and the top layer as shown in Table 1, and changing the resin composition used to form resin layer A to the resin composition used in Examples 1-2, the rest was carried out in the same manner as in Examples 2-1 to obtain a release film (sample film) with a thickness of 50 μm.

[0396] [Comparative Example 1]

[0397] Fragments of a polyester composition comprising 85% by mass of copolyester (a1-2) and 15% by mass of homopolymer (a2-2) are fed into a main twin-screw extruder with a vent set at 270°C.

[0398] Extruded from the die, the unstretched sheet is rapidly cooled and solidified on a cooling roller with the surface temperature set at 25°C using an electrostatic application method.

[0399] Next, the unstretched sheet was stretched 3.4 times along the length direction (MD) at 80°C and then fed into a tenter frame. It was then stretched 3.9 times along the width direction (TD) at 105°C and subjected to heat treatment at 185°C for 10 seconds to obtain a copolyester film (sample) with a thickness of 50 μm.

[0400] [Comparative Example 2]

[0401] Fragments of a polyester composition comprising 92% by mass of homopolymer (a2-1) and 8% by mass of homopolymer (a2-2) are fed into a main twin-screw extruder with a vent set to 280°C.

[0402] Extruded from the die, the unstretched sheet is rapidly cooled and solidified on a cooling roller with the surface temperature set at 25°C using an electrostatic application method.

[0403] Next, the unstretched sheet was stretched 3.4 times along the length direction (MD) at 90°C and then fed into a tenter frame. It was then stretched 4.5 times along the width direction (TD) at 145°C and subjected to heat treatment at 222°C for 10 seconds to obtain a polyester film (sample) with a thickness of 50 μm.

[0404] [Reference Example]

[0405] As a reference example, the following membrane samples were also evaluated.

[0406] ETFE: Aflex manufactured by AGC, 50μm

[0407] [Table 1]

[0408]

[0409] *The thickness of each layer refers to the overall thickness of the copolyester film in a single-layer copolyester film, and to the thickness of the top layer, intermediate layer, and each of the top layers in the case of a multi-layer structure.

[0410] [Table 2]

[0411]

[0412] ※In Table 2, the mol% of dicarboxylic acid and alcohol components are the respective proportions of dicarboxylic acid and alcohol components relative to the total polyester (A) (or polyester (Z)) contained in the copolyester film (copolyester layer (A1)).

[0413] [Table 3]

[0414]

[0415] ※In Table 3, the mol% of dicarboxylic acid and alcohol components are relative to the proportions of dicarboxylic acid and alcohol components in the total polyester (Z) contained in the copolyester film.

[0416] Based on the above embodiments and the test results conducted by the inventors so far, it is evident that in a release film containing a copolyester film having a resin layer A on at least one side, if the storage modulus at 80°C is 1000 MPa or less, it exhibits excellent flexibility at an ambient temperature of approximately 80°C. Furthermore, it is not only flexible but also satisfies the requirement of a storage modulus of 30 MPa or more at 180°C, and the ratio of the storage modulus at 80°C to the storage modulus at 180°C is 13 or less. This allows it to maintain strength appropriately, possesses practically sufficient heat resistance, and can be used as a substitute for fluoropolymer release films.

[0417] Furthermore, in the copolyester membrane containing copolyester in this embodiment, the copolyester is a copolyester (z1) of terephthalic acid (X1), a dicarboxylic acid component with 4 to 10 carbon atoms (X2), and an alcohol component (Y2) other than ethylene glycol (Y1). The proportion of the dicarboxylic acid component (X2) with 4 to 10 carbon atoms in the total polyester (Z) contained in the copolyester membrane is 1 to 30 mol%, and the proportion of the other alcohol component (Y2) in the alcohol component is 15 to 60 mol%, thereby achieving the above-mentioned energy storage modulus.

[0418] Industrial application

[0419] The release film of the present invention is applicable to the compression molding (compression molding) of epoxy resin sealants used in semiconductor manufacturing.

Claims

1. A release film having a resin layer A on at least one side of a copolyester film containing a copolyester, wherein the release film has a storage modulus of 1000 MPa or less at 80°C, a storage modulus of 30 MPa or more at 180°C, and a ratio of the storage modulus at 80°C to the storage modulus at 180°C of 13 or less.

2. The release film according to claim 1, wherein, The copolyester comprises a copolyester (z1) of terephthalic acid (X1) and a dicarboxylic acid component with 4 to 10 carbon atoms (X2) and an alcohol component other than ethylene glycol (Y1) (Y2). The proportion of dicarboxylic acid component (X2) with 4 to 10 carbon atoms in the total dicarboxylic acid component (Z) contained in the copolyester film is 1 to 30 mol%, and the proportion of other alcohol components (Y2) in the alcohol component is 15 to 60 mol%.

3. The release film according to claim 2, wherein, The dicarboxylic acid component (X2) with 4 to 10 carbon atoms includes aliphatic dicarboxylic acids.

4. The release film according to claim 3, wherein, Aliphatic dicarboxylic acids include adipic acid.

5. The release film according to any one of claims 2 to 4, wherein, Other alcohol components (Y2) include 1,4-butanediol.

6. The release film according to any one of claims 2 to 4, wherein, Other alcohol components (Y2) include 1,4-butanediol and 1,6-hexanediol.

7. The release film according to claim 1, wherein, The release film is a copolyester film having a copolyester layer (A1) containing a copolyester (a1) as the copolyester.

8. The release film according to claim 7, wherein, The copolyester layer (A1) also includes a polyester (a2), which is a polyester other than the copolyester (a1) and contains terephthalic acid as a dicarboxylic acid component and ethylene glycol as an alcohol component.

9. The release film according to any one of claims 7 to 8, wherein, The copolyester layer (A1) has a polyester layer (B1) and a polyester layer (B2) on its front and back sides, respectively.

10. The release film according to claim 9, wherein, The temperature difference between at least one of the copolyester layer (A1), polyester layer (B1), and polyester layer (B2), as determined by the softening temperature of nano TA, is greater than 5°C.

11. The release film according to claim 1, wherein, Resin layer A contains silicone-based resin.

12. The release film according to claim 1, wherein, Resin layer A contains a non-silicone resin.

13. The release film according to any one of claims 1 to 4, 7, 8, 11 and 12, wherein, The release film is used in semiconductor manufacturing.

14. The release film according to claim 13, wherein, The release film is used for compression molding.

Citation Information

Patent Citations

  • Fabric inspecting and treating method

    JP1989014345A