Polyolefin plasmid

By synthesizing ethylene and 1-octene copolymers in a solution process using metallocene catalysts, the performance balance problem of existing plasmon materials in terms of sealing and flexibility has been solved, and a high-efficiency sealing material suitable for packaging and automotive parts has been prepared.

CN123125249APending Publication Date: 2026-11-17BASELL POLIOLEFINE ITALIA SRL
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202580029225.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-05-02
Filing Date
2025-04-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing plasmon materials struggle to provide a balance of specific properties for many end-use applications, particularly in terms of sealing, flexibility, and processability, failing to meet the specific needs of fields such as packaging and automotive parts.

Method used

Ethylene and 1-octene copolymers were synthesized in solution using metallocene catalysts. By controlling polymerization conditions and catalyst composition, polyolefin plastics with density, melt index, and reactivity ratio within a specific range were prepared, combined with appropriate long-chain branching index and melt index ratio.

Benefits of technology

The prepared polyolefin plastide forms a strong seal at low temperatures, providing excellent seal integrity and versatility over a wide temperature range, suitable for a variety of packaging and automotive parts, improving seal strength and processing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123125249A_ABST
    Figure CN123125249A_ABST
Patent Text Reader

Abstract

A vinyl plastomer is produced in a solution process using a metallocene catalyst. This polyolefin plastomer comprises units derived from ethylene and 1-octene and has a viscosity of 0.890 g / cm³. 3 Up to 0.910 g / cm 3 The density within the range, the melt index (2.16 kg, 190 °C) within the range of 0.10 g / 10 min to 3.00 g / 10 min (I2), and the density of the components within the range of 0.820 to 1.08. 13 The product of the reactivity ratios obtained from the C NMR triplet distribution is r1×r2.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Previous related applications This application is filed pursuant to the Patent Cooperation Treaty and claims priority to U.S. Provisional Application No. 63 / 641,783, filed May 2, 2024, which is incorporated herein by reference in its entirety.

[0002] Invention Field This invention relates to polyolefin plastics, and more particularly to a copolymer of ethylene and 1-octene produced in a solution process using a metallocene catalyst. Background of the Invention In the development of advanced polymer materials, the unique properties of plastomers have attracted considerable interest, particularly in packaging, automotive parts, building materials, medical devices, sporting goods, household goods, and wire and cable insulation. These materials cleverly combine the advantageous properties of plastics and elastomers, offering an unparalleled balance in processability, flexibility, and toughness. Specifically, plastomers excel in their heat-sealing properties, providing a superior alternative to conventional plastics and elastomers.

[0004] Their ability to form strong and reliable seals at relatively low temperatures is particularly noteworthy, thanks to their enhanced deformability under heat and pressure, ensuring an optimal interface between sealing surfaces. This property not only promises to enhance seal integrity and strength but also broadens the sealing temperature range, providing a level of versatility and efficiency not easily achieved with conventional plastics.

[0005] Although plastids have been developed that demonstrate practicality in many end uses, there is still a need for plastid materials with a unique balance of properties that can be tailored to specific end uses. Summary of the Invention

[0006] This invention provides a polyolefin plastide comprising units derived from ethylene and 1-octene. The polyolefin plastide has a content of 0.890 g / cm³. 3 Up to 0.910 g / cm 3 The density within the range, the melt index (2.16 kg, 190 °C) within the range of 0.10 g / 10 min to 3.00 g / 10 min (I2), and the density of the components within the range of 0.820 to 1.08. 13 The product of the reactivity ratios obtained from the C NMR ternary distribution is r1×r2, where r1 is the reactivity ratio of ethylene to 1-octene, and r2 is the reactivity ratio of 1-octene to ethylene.

[0007] In some embodiments, the polyolefin plastome has a long chain branching index (LCBI) in the range of 0.04 to 0.38, a long chain branching content in the range of 0.005 LCB / 1000C to 0.025 LCB / 1000C, or a combination thereof.

[0008] In some embodiments, the polyolefin plastome has a melt index (21.6 kg, 190°C) in the range of 5.0 g / 10 min to 45.0 g / 10 min, measured according to ISO 1133-1 2012-03 at 190°C and a load of 21.6 kg (I 21 Melt flow index (MFR) in the range of 0.50 g / 10 min to 3.50 g / 10 min, measured at 230 °C and with a load of 2.16 kg, according to ISO 1133-1 2012-03; and melt flow index (MFR) in the range of 3.0 g / 10 min to 15.0 g / 10 min, measured at 10.0 kg and with a load of 10 kg, according to ISO 1133-1 2012-03, measured at 190 °C and with a load of 10.0 kg, according to ISO 1133-1 2012-03, measured at 190 °C and with a load of 10.0 kg, according to ISO 1133-1 2012-03, measured at 190 °C and with a load of 10.0 kg, measured at 190 °C, according to ISO 1133-1 2012-03, measured at 230 °C and with a load of 2.16 kg ...0 kg, measured at 230 °C and with a load of 2.0 kg, measured at 230 °C and with a load of 2.0 kg, measured at 23 10 (or combinations thereof). In some embodiments, the polyolefin plasticite is further characterized by I 21 The ratio of I / I2 is ≤28.0, and within the range of 17.0 to 28.0, I 10 The ratio of I / I2 is in the range of 3.0 to 10.0, or a combination thereof.

[0009] In some embodiments, the polyolefin plastic body has a 1-octene content (C8) ranging from 10.0 wt.% to 26.0 wt.% relative to the weight of the polyolefin plastic body. cont .

[0010] The foregoing has provided a fairly broad overview of the features and technical advantages of the invention in order to better understand the detailed description of the invention below. Further features and advantages of the invention, which form the subject matter of the claims, will be described below. Those skilled in the art will understand that the disclosed concepts and specific embodiments can be readily used as the basis for modifying or designing other catalyst compositions and / or processes to achieve the same objectives of the invention. Those skilled in the art will also recognize that such equivalent constructions do not depart from the spirit and scope of the invention as set forth in the appended claims. The novel features considered characteristic of the invention (whether relating to its compositions or methods) and further objects and advantages will be better understood from the following description. Attached Figure Description

[0011] The claimed subject matter can be understood by referring to the following description and the accompanying drawings, in which the same reference numerals identify the same elements, and wherein: Figure 1 A superimposed graph showing the change of short-chain branching with molecular weight is shown, which compares the polyolefin plastomer of the present invention with a comparative polymer. Figure 2 A superimposed graph showing the complex viscosity as a function of frequency is displayed, which compares the polyolefin plastide of the present invention with a comparative polymer. Figure 3 A superimposed plot of dw / dt versus elution temperature is shown, comparing the polyolefin plastomer of the present invention with a comparative polymer; or Figure 4 A superimposed graph showing the variation of tan δ with complex modulus is displayed, which compares the polyolefin plastomer of the present invention with a comparative polymer.

[0012] While the disclosed processes and compositions are readily modified and substituted, the accompanying drawings illustrate specific embodiments described in detail herein by way of example. However, it should be understood that the description of specific embodiments herein is not intended to limit the invention to the particular forms disclosed; rather, the invention is intended to cover all modifications, equivalents, and alternatives falling within the spirit and scope of the invention as defined in the appended claims. Detailed Implementation

[0013] The following exemplary embodiments of the claimed subject matter will now be disclosed. For clarity, some features of certain practical implementations may not be described in this specification. It should be understood that in the development of any such practical implementation, numerous decisions must be made regarding the implementation to achieve the developer's specific goals, such as complying with system and business-related constraints, which will vary from implementation to implementation. Furthermore, it should be understood that such development efforts, even if complex and time-consuming, are routine tasks for those skilled in the art who will benefit from this invention.

[0014] The words and phrases used herein should be understood and interpreted in accordance with the understanding of those skilled in the art. Any particular definition of a term or phrase, that is, a definition different from the usual and customary meaning understood by those skilled in the art, is not intended to be implied by the consistent use of the terms or phrases herein. Such particular or clear definitions, which are intended to have a particular meaning, that is, a meaning different from the broadest meaning understood by those skilled in the art, will be clearly stated in the specification in a manner that provides for the particular or clear definition of the term or phrase.

[0015] For example, the following discussion contains a non-exhaustive list of definitions for several specific terms used in this invention (other terms may be defined or clarified in the manner defined elsewhere herein). These definitions are intended to clarify the meaning of the terms used herein. It is believed that terms are used in a manner consistent with their usual meaning, but definitions are specified herein for clarity.

[0016] definition As used herein, "polymer" refers to a class of polymers derived from two (or more) different monomers chemically bonded together in a repeating sequence. The properties and structure of copolymers can vary widely and are determined by the specific monomers used, their ratios, and the arrangement of the monomer units along the polymer chain.

[0017] As used herein, the term "polyolefin plastomer" refers to a copolymer that comprises mostly ethylene-derived units with the remainder comprising 1-octene-derived units.

[0018] As used herein, when used in conjunction with the term “comprising” in the claims or description, “a” or “an” means one or more, unless the context otherwise requires.

[0019] As used in this article, “about” means the stated value plus or minus the measurement error limit, or, if the measurement method is not specified, plus or minus 10%.

[0020] As used herein, “comprising,” “having,” “including,” and “containing” (and variations thereof) are open-ended connecting verbs and allow for the addition of other elements when used in claims.

[0021] As used herein, “consistent with…” does not include additional material elements, but may include non-material elements that do not substantially alter the nature of the invention.

[0022] As used in this article, “composed of” is a closed phrase and does not include any additional elements.

[0023] The exemplary embodiments disclosed herein may be practiced in the absence of any elements not specifically disclosed herein and / or any optional elements disclosed herein. Although compositions and methods are described with the terms “comprising,” “containing,” or “including” various components or steps, compositions and methods may also be “consistently composed of various components and steps” or “comprise various components and steps.”

[0024] Production of polyolefin plastides The ethylene copolymer of the present invention can be obtained by polymerizing monomers in the presence of a metallocene catalyst system, which can be obtained by contacting the following substances: -Stereorigid metallocene compounds; -Aluminoxanes or compounds capable of forming alkyl metallocene cations; and optionally, - Organoaluminum compounds.

[0025] In some implementations, the stereolithic metallocene compound belongs to the following formula (I): in: M is an atom selected from transition metals belonging to Group 4; preferably, M is zirconium; X may be the same as or different from each other, and is a hydrogen atom, a halogen atom, R, OR, OR'O, OSO2CF3, OCOR, SR, NR2, or PR2 group, wherein R is a straight-chain or branched, saturated or unsaturated C1-C group. 20 Alkyl, C3-C 20 cycloalkyl, C6-C 20 Aryl, C7-C 20 Alkyl or C7-C 20 An aralkyl radical, optionally containing a heteroatom belonging to Groups 13-17 of the periodic table; and R' is C1-C. 20 Alkylene, C6-C 20 Aspartic, C7-C 20 alkylene aryl or C7-C 20 Aromatic alkyl radical; preferably, X is a hydrogen atom, a halogen atom, an OR'O or an R group; more preferably, X is a chlorine or methyl radical; R 1 R 2 R 5 R 6 R 7 R 8 and R 9 They may be the same or different, and are either hydrogen atoms, or straight-chain or branched, saturated or unsaturated C1-C atoms. 20 Alkyl, C3-C 20 cycloalkyl, C6-C 20 Aryl, C7-C 20 Alkyl or C7-C 20 Aryl alkyl radical, optionally containing heteroatoms belonging to groups 13-17 of the periodic table; or R 5 and R 6 , and / or R 8 and R 9 Saturated or unsaturated 5- or 6-membered rings can be optionally formed, and the rings may have C1-C2 elements.20 Alkyl radicals are used as substituents; the condition is R. 6 Or R 7 At least one of them is a straight-chain or branched, saturated or unsaturated C1-C 20 Alkyl radical, optionally containing heteroatoms belonging to groups 13-17 of the periodic table; in some embodiments, C1-C2. 10 Alkyl radicals; R 3 and R 4 They may be the same or different, straight or branched, saturated or unsaturated C1-C 20 An alkyl radical, optionally containing a heteroatom belonging to Groups 13-17 of the periodic table; in some embodiments, R 3 and R 4 Whether they are the same or different is C1-C 10 Alkyl radical; in other embodiments, R 3 It is a methyl or ethyl radical; and R 4 It is a methyl, ethyl, or isopropyl free radical.

[0026] In some embodiments, the compound of formula (I) has formula (Ia): (Ia) in: M, X, R 1 R 2 R 5 R 6 R 8 and R 9 As mentioned above; R 3 It is a straight-chain or branched, saturated or unsaturated C1-C 20 An alkyl radical, optionally containing a heteroatom belonging to Groups 13-17 of the periodic table; in some embodiments, R 3 It is C1-C 10 Alkyl radical; in other embodiments, R 3 It is a methyl or ethyl free radical.

[0027] A specific example of a metallocene compound is dimethylsilyl. (2,4,7-Trimethyl-1-indenyl)-7-(2,5-Dimethyl-cyclopentadieno[1,2-b:4,3-b']-dithiophene) Zirconium dichloride; dimethylsilyldiyl{(1-(2,4,7-trimethylindyl)-7-(2,5-dimethyl-cyclopentadieno[1,2-b:4,3-b']-dithiophene)}zirconium dichloride and dimethylsilyldiyl{(1-(2,4,7-trimethylindyl)-7-(2,5-dimethyl-cyclopentadieno[1,2-b:4,3-b']-dithiophene)}dimethylzirconium.

[0028] Examples of aluminum oxanes are methylaluminoxane (MAO), tetra-(isobutyl)aluminoxane (TIBAO), tetra-(2,4,4-trimethyl-pentyl)aluminoxane (TIOAO), tetra-(2,3-dimethylbutyl)aluminoxane (TDMBAO), and tetra-(2,3,3-trimethylbutyl)aluminoxane (TTMBAO).

[0029] An example of a compound capable of forming an alkyl metallocene cation is formula D. + E - Compound, in which D + It is a Brønsted acid, which can donate a proton and react irreversibly with the metallocene substituent X of formula (I), and E - It is a compatible anion that can stabilize the active catalyst derived from the reaction of the two compounds, and is sufficiently unstable to be removed by the olefin monomer. In some embodiments, the anion E... - It contains one or more boron atoms.

[0030] Examples of organoaluminum compounds are trimethylaluminum (TMA), triisobutylaluminum (TIBA), tri(2,4,4-trimethyl-pentyl)aluminum (TIOA), tri(2,3-dimethylbutyl)aluminum (TDMBA), and tri(2,3,3-trimethylbutyl)aluminum (TTMBA).

[0031] In some implementations, the Al / metallocene molar ratio is 500 to 10,000.

[0032] Therefore, the ethylene copolymer of the present invention can be prepared under known polymerization conditions in the presence of the catalyst described above.

[0033] One method for preparing the ethylene copolymer of the present invention is solution polymerization, which includes polymerizing ethylene and 1-octene, and possibly additional comonomers, in a liquid reaction medium capable of maintaining the nascent polymer in a solution state.

[0034] The term "solution polymerization" refers to the complete dissolution of a polymer in a polymerization medium at the polymerization temperature used.

[0035] In some embodiments, the temperature range for solution polymerization is 60°C to 200°C, 80°C to 150°C, or 89°C to 140°C.

[0036] When selecting the optimal polymerization temperature, it should be considered that increasing the temperature will increase the polymer solubility, but it will also increase the catalyst decay rate.

[0037] Hydrogen can be effectively used to adjust the molecular weight of the resulting polymer. In some embodiments, the hydrogen concentration (H2 / C2 mol ppm) in the liquid phase relative to the ethylene concentration is in the range of 1 ppm to 20,000 ppm, or 1,000 ppm to 18,000 ppm.

[0038] One or more reactors can be used in series or in parallel.

[0039] The catalyst may be added only in the first reactor or in more than one reactor.

[0040] The amount of comonomer (especially 1-octene) in the liquid phase, relative to the total weight of the liquid solution (monomer and liquid reaction medium) present in the relevant polymerization reactor, can be from 0.1 wt% to 40 wt%, especially from 15 wt% to 36 wt%.

[0041] In some implementations, the polymerization pressure is in the range of 20 to 45 barg. As used herein, the term "barg" refers to pressure measured by a pressure gauge at atmospheric pressure. Atmospheric pressure at which the pressure measurement is performed is 1 bar ± 0.05.

[0042] In some implementations, the amount of polymer dissolved in the reaction medium is 10 to 40% wt / vol, or 12 to 35% wt / vol. The amount of polymer dissolved in the liquid reaction medium is often a trade-off between the maximum productivity target of polymerization and the operability of the reactor, which becomes problematic when the polymer concentration is too high.

[0043] In fact, in the latter case, the viscosity of the solution does not allow for effective stirring, and heat dissipation is problematic. Variations in polymer solubility can also originate from the production of polymers with different molecular weights (higher molecular weight polymers generally have lower solubility) and different chemical compositions (variations in polymer solubility can also be observed by changing the 1-octene content).

[0044] For all these reasons, it is important to have an inert reaction medium that ensures polymer solubility over the widest possible range of operating conditions (polymer concentration, polymer molecular weight, and polymer composition).

[0045] In some embodiments, the liquid reaction medium comprises a liquid hydrocarbon with a boiling point greater than or equal to 60°C or greater than or equal to 70°C at atmospheric pressure. In some embodiments, the liquid reaction medium comprises toluene, cyclohexane, isododecane, or combinations thereof.

[0046] It has been observed that cyclohexane is a preferred reaction medium for the preparation of the ethylene copolymer of the present invention because it allows for great flexibility in process conditions while keeping the nascent polymer in solution.

[0047] The ethylene copolymers of the present invention may also contain additives commonly used in the art, such as antioxidants, light stabilizers, heat stabilizers, colorants, and fillers.

[0048] Polyolefin plasmid A polyolefin plastide produced using the above-described catalyst and solution polymerization process comprises units derived from ethylene and 1-octene. This polyolefin plastide has a viscosity of 0.890 g / cm³, measured at 23°C according to ISO 1183-1:2012. 3 Up to 0.910 g / cm 3 0.894 g / cm 3 Up to 0.910 g / cm 3 0.898 g / cm 3 Up to 0.909 g / cm 3 0.902 g / cm 3 Up to 0.908 g / cm 3 or 0.905 g / cm 3 Up to 0.907 g / cm 3 The density is within the range specified. The polyolefin plastome further has a melt index (2.16 kg, 190°C) measured according to ISO 1133-1 2012-03 at 190°C with a load of 2.16 kg, in the ranges of 0.10 g / 10 min to 3.00 g / 10 min, 0.20 g / 10 min to 2.90 g / 10 min, 0.30 g / 10 min to 2.80 g / 10 min, 0.40 g / 10 min to 2.70 g / 10 min, 0.50 g / 10 min to 2.60 g / 10 min, or 0.60 g / 10 min to 2.50 g / 10 min. Furthermore, the polyolefin plastic body further comprises a content in the range of 0.820 to 1.08, 0.825 to 1.035, 0.830 to 0.990, 0.835 to 0.945, or 0.840 to 0.900. 13The product of the reactivity ratios obtained from the C NMR ternary distribution is r1×r2, where r1 is the reactivity ratio of ethylene to 1-octene, and r2 is the reactivity ratio of 1-octene to ethylene.

[0049] In some embodiments, the polyolefin plastome further has: a) Long chain branching index (LCBI) in the range of 0.04 to 0.38, 0.05 to 0.37, 0.06 to 0.36, 0.08 to 0.35, or 0.10 to 0.22; b) Long-chain branching content in the ranges of 0.005 LCB / 1000C to 0.025 LCB / 1000C, 0.006 LCB / 1000C to 0.024 LCB / 1000C, 0.007 LCB / 1000C to 0.023 LCB / 1000C, 0.008 LCB / 1000C to 0.022 LCB / 1000C, 0.009 LCB / 1000C to 0.021 LCB / 1000C, or 0.010 LCB / 1000C to 0.020 LCB / 1000C; or c) Its combination.

[0050] In some embodiments, the polyolefin plastome further has: a) Melt index (21.6 kg, 190 °C) measured according to ISO 1133-1 2012-03 at 190 °C with a load of 21.6 kg, in the ranges of 5.0 g / 10 min to 45.0 g / 10 min, 7.0 g / 10 min to 44.3 g / 10 min, 9.0 g / 10 min to 43.5 g / 10 min, 11.0 g / 10 min to 42.8 g / 10 min, or 13.0 g / 10 min to 42.0 g / 10 min (I) 21 ); b) Melt flow index (2.16 kg, 230 °C) measured at 230 °C with a load of 2.16 kg, in the ranges of 0.50 g / 10 min to 3.50 g / 10 min, 0.68 g / 10 min to 3.45 g / 10 min, 0.85 g / 10 min to 3.40 g / 10 min, 1.03 g / 10 min to 3.35 g / 10 min, or 1.20 g / 10 min to 3.30 g / 10 min, according to ISO 1133-1 2012-03. c) Melt index (10 kg, 190 °C) measured at 190 °C and with a load of 10.0 kg, according to ISO 1133-1 2012-03, within the ranges of 3.0 g / 10 min to 15.0 g / 10 min, 2.6 g / 10 min to 18.4 g / 10 min, 3.3 g / 10 min to 16.8 g / 10 min, 3.9 g / 10 min to 15.1 g / 10 min, or 4.5 g / 10 min to 13.5 g / 10 min. 10 );or d) Its combination.

[0051] In some embodiments, the polyolefin plastome further has: a) I in the range of 17.0 to 28.0, 17.5 to 26.0, 18.0 to 24.0, 18.5 to 22.0, or 19.0 to 20.0 21 The ratio of / I2; b) I in the range of 3.0 to 10.0, 3.8 to 9.3, 4.6 to 8.6, 5.3 to 7.9, or 6.1 to 7.2 10 The ratio of / I2; or c) Its combination.

[0052] In some embodiments, the polyolefin plastic body has a 1-octene content (C8) in the range of 10.0 wt.% to 26.0 wt.%, 11.0 wt.% to 23.8 wt.%, 12.0 wt.% to 21.5 wt.%, 13.0 wt.% to 19.3 wt.%, or 14.0 wt.% to 17.0 wt.% relative to the weight of the polyolefin plastic body. cont .

[0053] In some embodiments, the polyolefin plastome has a yield strength greater than or equal to 5.0 MPa, greater than or equal to 6.0 MPa, greater than or equal to 7.0 MPa, or greater than or equal to 7.5 MPa, as measured on a compression-molded sample according to ISO 527:2019. In some embodiments, the polyolefin plastome further has a yield strength less than or equal to 10.0 MPa or less than or equal to 8.5 MPa.

[0054] In some embodiments, the polyolefin plastome has a yield elongation greater than or equal to 80% or greater than or equal to 89% as measured on a compression-molded sample according to ISO 527:2019. In some embodiments, the polyolefin plastome further has a yield elongation less than or equal to 110% or less than or equal to 101%.

[0055] In some embodiments, the polyolefin plastome has a tensile strength greater than or equal to 19 MPa or greater than or equal to 23.2 MPa, measured on a compression-molded sample according to ISO 527:2019. In some embodiments, the polyolefin plastome further has a tensile strength less than or equal to 43.0 MPa or less than or equal to 31.8 MPa.

[0056] In some embodiments, the polyolefin plastome has an elongation at break greater than or equal to 500%, greater than or equal to 522%, or greater than or equal to 590% as measured on a compression-molded sample according to ISO 527:2019. In some embodiments, the polyolefin plastome further has an elongation at break less than or equal to 800% or less than or equal to 750%.

[0057] In some embodiments, the polyolefin plastome has a stress at 100% elongation of 5.2 MPa or 7.3 MPa, as measured on a compression-molded sample according to ISO 527:2019. In some embodiments, the polyolefin plastome further has a stress at 100% elongation of 8.3 MPa or 8.1 MPa.

[0058] In some embodiments, the polyolefin plastome has a stress at 300% elongation of 6.3 MPa or 7.6 MPa, as measured on a compression-molded sample according to ISO 527:2019. In some embodiments, the polyolefin plastome further has a stress at 300% elongation of 8.5 MPa or less.

[0059] In some embodiments, the polyolefin plastome has a Shore D hardness in the range of 37 to 47 or 44 to 46, as measured on a compression-molded sample according to ISO 868:2003.

[0060] In some embodiments, the polyolefin plastome has a tensile permanent deformation (23°C / 100%) in the range of 31 to 43 or 39 to 43 as measured on a compression-molded sample according to ISO 37.

[0061] In some embodiments, the polyolefin plastome has a compression set in the range of 23 to 30 or 23 to 26 (23°C / 100%) as measured on a compression-molded sample according to ISO 815.

[0062] In some embodiments, the polyolefin plastome further has an intrinsic viscosity [η] of 1.2 dl / g or greater as measured in tetrahydronaphthalene at 135 °C, in the range of 1.20 dl / g to 2.10 dl / g, 1.25 dl / g to 2.01 dl / g, 1.30 dl / g to 1.92 dl / g, 1.35 dl / g to 1.83 dl / g, or 1.40 dl / g to 1.75 dl / g.

[0063] In some embodiments, the polyolefin plastic body further has a xylene-soluble content of less than or equal to 20 wt.% based on the total weight of the polyolefin plastic body, in the range of 0.50 wt.% to 20 wt.%, 0.60 wt.% to 10 wt.%, 0.80 wt.% to 5.0 wt.%, 0.90 wt.% to 3.5 wt.%, or 1.0 wt.% to 2.0 wt.%.

[0064] In some embodiments, the polyolefin plastome has a weight-average molecular weight in the range of 40,000 Daltons to 250,000 Daltons, 50,000 Daltons to 225,000 Daltons, 60,000 Daltons to 200,000 Daltons, 70,000 Daltons to 175,000 Daltons, 80,000 Daltons to 150,000 Daltons, or 90,000 Daltons to 125,000 Daltons.

[0065] In some embodiments, the polyolefin plastome further has a molecular weight distribution M of less than or equal to 3.0, less than or equal to 2.8, less than or equal to 2.6, less than or equal to 2.5, or less than or equal to 2.4. w / M n (MWD), where M w It is the weight-average molecular weight and M n These are number-average molecular weights, all measured by GPC (gel permeation chromatography).

[0066] In some embodiments, the polyolefin plastome further has a molecular weight distribution M greater than or equal to 2.0 or greater than or equal to 2.1. w / M n (MWD).

[0067] In some embodiments, the polyolefin plastome further has a molecular weight distribution M of less than or equal to 2.0, less than or equal to 1.9, less than or equal to 1.8, or less than or equal to 1.7, and in all cases greater than or equal to 1.0 or greater than or equal to 1.1. z / M w M w It is the weight-average molecular weight and Mw These are z-average molecular weights, all measured by GPC (gel permeation chromatography).

[0068] In some embodiments, the polyolefin plastome has a molecular weight distribution M greater than or equal to 1.0 or greater than or equal to 1.1. z / M w .

[0069] The polyolefin plastome of claim 0 has a melting enthalpy ΔH of less than or equal to 115 J / g, or in the range of 70 J / g to 115 J / g, 78 J / g to 114 J / g, 85 J / g to 113 J / g, 93 J / g to 111 J / g, or 100 J / g to 110 J / g, as measured by differential scanning calorimetry at a heating rate of 10°C per minute. m .

[0070] In some embodiments, the polyolefin plastome has a melt elasticity (ER) in the range of 0.20 to 0.90.

[0071] In some embodiments, the polyolefin plastome has a composition distribution width index (CDBI) in the range of 50 to 90, as measured by crystallization elution fractionation (CEF).

[0072] In some embodiments, the polyolefin plastic has soluble fractions in the range of 1 to 21, as determined by crystallization elution fractionation (CEF).

[0073] In some embodiments, the polyolefin plastome has a uniformity index (HI) in the range of 80 to 90.

[0074] In some embodiments, the polyolefin plastome has a polydispersity ratio (PDR) in the range of 2.0 to 4.0.

[0075] In some embodiments, the polyolefin plastome has a complex viscosity (Eta) at a frequency of 100 rad / sec in the range of 1.4E+04 to 2.6E+04. 100).

[0076] In some embodiments, the polyolefin plastome has a zero shear viscosity (Eta0) in the range of 3.9E+04 to 2.0E+05.

[0077] In some embodiments, the polyolefin plastide further has a melt temperature T measured by differential scanning calorimetry at a heating rate of 10°C per minute, in the range of 80°C to 110°C, 85°C to 108°C, 90°C to 106°C, 94°C to 104°C, or 99°C to 102°C. m .

[0078] In some embodiments, the polyolefin plastide further has a crystallization temperature T measured by differential scanning calorimetry at a heating rate of 10°C per minute, in the range of 65°C to 90°C, 69°C to 89°C, 74°C to 88°C, 78°C to 87°C, or 82°C to 86°C. c .

[0079] In some embodiments, the polyolefin plastide further satisfies (melting temperature T) m - Crystallization temperature T c ≥14.0℃ and (melting temperature T) m + Crystallization temperature T c ) ≥182.0℃ condition.

[0080] In some embodiments, the polyolefin plastide further has a glass transition temperature (Tg) in the range of -31°C to -20.0°C, -29°C to -20.5°C, -27°C to -21.0°C, -25°C to -21.5°C, or -23°C to -22.0°C, as measured by dynamic mechanical thermometry. g ).

[0081] End-use applications Plastics play a crucial role in the packaging industry, their unique combination of properties enabling the creation of advanced packaging solutions to meet diverse market demands. These materials combine the best of elastomers and plastics, providing unparalleled flexibility, sealing, and durability for a wide range of packaging applications. The focus on packaging applications, particularly in the food and consumer goods sectors, underscores the importance of plastics in enhancing product safety, extending shelf life, and improving aesthetics.

[0082] In heat-sealing applications, plastries excel due to their superior seal integrity and performance over a wide temperature range. This quality is crucial for ensuring that packaging is securely sealed to protect contents from contamination and leakage, while also allowing easy opening by the end consumer. Compared to traditional packaging materials, plastries can form a strong, hermetic seal at lower temperatures, which not only saves energy but also minimizes the risk of heat damage to sensitive products such as food or pharmaceuticals.

[0083] In packaging structures, plastics are often integrated into multilayer films as a key component, imparting flexibility and excellent sealing properties. In these constructions, a thin layer of plastic can be combined with other polyethylene types to form a composite material that balances mechanical strength with excellent elasticity and sealing performance. The lamination sequence and thickness are carefully designed to meet specific functional requirements, including barrier properties, puncture resistance, and transparency.

[0084] Plasticizers are also crucial in the formulation of single-layer films, where they are blended with other polyethylenes to achieve desired performance characteristics. In these applications, the ratio of plasticizers to other PE types is carefully adjusted to enhance the overall properties of the film, particularly in terms of tensile strength, toughness, and heat-sealing properties. Single-layer films containing plasticizer components are highly valued in the packaging industry for their versatility and efficiency in a wide range of sealing applications, from flexible bags to rigid containers.

[0085] The widespread use of plastics in packaging, particularly in heat-sealing applications, reflects their crucial role in providing safe, reliable, and consumer-friendly packaging solutions. Their unique combination of properties allows packaging designers and manufacturers to achieve an optimal balance between performance, aesthetics, and cost-effectiveness, making plastics an indispensable material for the sustainable development of the packaging industry. As the demand for more sophisticated and sustainable packaging options continues to rise, the role of plastics in addressing these challenges is expected to expand, further highlighting their importance in the packaging sector.

[0086] The polyolefin plastics of the present invention can be advantageously compounded with additional polyolefins, particularly ethylene polymers such as ethylene homopolymers, random copolymers, and thermoplastic elastomer polyolefin compositions, to form polyolefin compositions. In some embodiments, the polyolefin composition comprises at least 50% by weight, typically 50% to 95% by weight, of one or more additional polyolefins, and thus comprises 50% by weight or less, typically 5% to 50% by weight, of the ethylene copolymer of the present invention, all percentages relative to the total weight of the ethylene copolymer and one or more additional polyolefins. Practical examples of the additional polyolefins include, but are not limited to, crystalline ethylene homopolymers and those with propylene and / or C4-C 10 Copolymers of α-olefins, such as LDPE, LLDPE, MDPE and HDPE.

[0087] Polyolefin compositions can be manufactured by mixing a polyolefin plastide and an additional polyolefin together, extruding the mixture, and granulating the resulting composition using known techniques and equipment.

[0088] Some implementation schemes This document discloses a first set of embodiments of a polyolefin plastide comprising units derived from ethylene and 1-octene. The polyolefin plastide is produced in a solution polymerization process using the metallocene catalyst disclosed herein. The polyolefin plastide has the following characteristics: a) Measured at 23°C according to ISO 1183-1:2012, at 0.890 g / cm³. 3 Up to 0.910 g / cm 3 0.894 g / cm 3 Up to 0.910 g / cm 30.898 g / cm 3 Up to 0.909 g / cm 3 0.902 g / cm 3 Up to 0.908 g / cm 3 or 0.905 g / cm 3 Up to 0.907 g / cm 3 Density within the range; b) Melt index (2.16 kg, 190 °C) (I2), measured at 190 °C and with a load of 2.16 kg, in the ranges of 0.10 g / 10 min to 3.00 g / 10 min, 0.20 g / 10 min to 2.90 g / 10 min, 0.30 g / 10 min to 2.80 g / 10 min, 0.40 g / 10 min to 2.70 g / 10 min, 0.50 g / 10 min to 2.60 g / 10 min, or 0.60 g / 10 min to 2.50 g / 10 min, according to ISO 1133-1 2012-03; and c) Values ​​in the range of 0.820 to 1.08, 0.825 to 1.035, 0.830 to 0.990, 0.835 to 0.945, or 0.840 to 0.900. 13 The product of the reactivity ratios obtained from the C NMR ternary distribution is r1×r2, where r1 is the reactivity ratio of ethylene to 1-octene, and r2 is the reactivity ratio of 1-octene to ethylene.

[0089] In the second set of embodiments, in addition to the limitations of each embodiment of the first set of embodiments disclosed above, the polyolefin plastic body is further described by one or more of the following: a) Long chain branching index (LCBI) in the range of 0.04 to 0.38, 0.05 to 0.37, 0.06 to 0.36, 0.08 to 0.35, or 0.10 to 0.22; b) Long-chain branching content in the ranges of 0.005 LCB / 1000C to 0.025 LCB / 1000C, 0.006 LCB / 1000C to 0.024 LCB / 1000C, 0.007 LCB / 1000C to 0.023 LCB / 1000C, 0.008 LCB / 1000C to 0.022 LCB / 1000C, 0.009 LCB / 1000C to 0.021 LCB / 1000C, or 0.010 LCB / 1000C to 0.020 LCB / 1000C; or c) Its combination.

[0090] In the third set of embodiments, in addition to the definitions of each embodiment of the first and / or second sets of embodiments disclosed above, the polyolefin plastic body is further described by one or more of the following: a) Melt index (21.6 kg, 190 °C) measured according to ISO 1133-1 2012-03 at 190 °C with a load of 21.6 kg, in the ranges of 5.0 g / 10 min to 45.0 g / 10 min, 7.0 g / 10 min to 44.3 g / 10 min, 9.0 g / 10 min to 43.5 g / 10 min, 11.0 g / 10 min to 42.8 g / 10 min, or 13.0 g / 10 min to 42.0 g / 10 min (I) 21 ); b) Melt flow index (2.16 kg, 230 °C) measured at 230 °C with a load of 2.16 kg, in the ranges of 0.50 g / 10 min to 3.50 g / 10 min, 0.68 g / 10 min to 3.45 g / 10 min, 0.85 g / 10 min to 3.40 g / 10 min, 1.03 g / 10 min to 3.35 g / 10 min, or 1.20 g / 10 min to 3.30 g / 10 min, according to ISO 1133-1 2012-03. c) Melt index (10 kg, 190 °C) measured at 190 °C and with a load of 10.0 kg, according to ISO 1133-1 2012-03, within the ranges of 3.0 g / 10 min to 15.0 g / 10 min, 3.5 g / 10 min to 14.5 g / 10 min, 4.0 g / 10 min to 14.1 g / 10 min, 4.5 g / 10 min to 13.6 g / 10 min, or 5.0 g / 10 min to 13.1 g / 10 min. 10 );or d) Its combination.

[0091] In the fourth group of embodiments, in addition to the definitions of each embodiment of the first, second, and / or third group of embodiments disclosed above, the polyolefin plastic body is further described by one or more of the following: a) I in the range of 17.0 to 28.0, 17.5 to 26.0, 18.0 to 24.0, 18.5 to 22.0, or 19.0 to 20.0 21 The ratio of / I2; b) I in the range of 3.0 to 10.0, 3.8 to 9.3, 4.6 to 8.6, 5.3 to 7.9, or 6.1 to 7.2 10 The ratio of / I2; or c) Its combination.

[0092] In the fifth group of embodiments, in addition to the limitations of each embodiment of the first, second, third, and / or fourth group of embodiments disclosed above, the polyolefin plastic body further has one or more of the following: a) The 1-octene content (C8) relative to the weight of the polyolefin plastic body in the range of 10.0 wt.% to 26.0 wt.%, 11.0 wt.% to 23.8 wt.%, 12.0 wt.% to 21.5 wt.%, 13.0 wt.% to 19.3 wt.%, or 14.0 wt.% to 17.0 wt.%. cont ; b) Yield strength of 5.0 MPa, 6.0 MPa, 7.0 MPa, or 7.5 MPa or greater, as measured on a compression-molded sample according to ISO 527:2019, wherein in a further embodiment, the polyolefin plastome further has a yield strength of 10.0 MPa or 8.5 MPa or less. c) A yield elongation greater than or equal to 80% or greater than or equal to 89% as measured on a compression-molded sample according to ISO 527:2019, wherein in a further embodiment, the polyolefin plastic body further has a yield elongation less than or equal to 110% or less than or equal to 101%.

[0093] d) A fracture strength of ≥19 MPa or ≥23.2 MPa measured on a compression-molded sample according to ISO 527:2019, wherein in a further embodiment, the polyolefin plastome further has a fracture strength of ≤43.0 MPa or ≤31.8 MPa. e) An elongation at break of 500%, 522%, or 590% or greater, as measured on a compression-molded sample, according to ISO 527:2019, wherein in a further embodiment, the polyolefin plastome further has an elongation at break of 800% or less or 750% or less. f) Stress at 100% elongation of 5.2 MPa or 7.3 MPa or greater, as measured on the compression-molded sample according to ISO 527:2019, wherein in some embodiments, the polyolefin plastic body further has stress at 100% elongation of 8.3 MPa or less than or equal to 8.1 MPa. g) Stress at 300% elongation of 6.3 MPa or 7.6 MPa or greater than or equal to 6.3 MPa or greater than or equal to 7.6 MPa, as measured on a compression-molded sample according to ISO 527:2019, wherein in some embodiments, the polyolefin plastome further has stress at 300% elongation of 8.5 MPa or less. h) Shore D hardness measured on the compression-molded sample in the range of 37 to 47 or 44 to 46, according to ISO 868:2003; i) Tensile permanent deformation (23°C / 100%) in the range of 31 to 43 or 39 to 43, measured on the compression-molded sample according to ISO 37. j) Compression set in the range of 23 to 30 or 23 to 26 degrees Celsius (23°C / 100%) on the compression-molded sample, as measured according to ISO 815. k) The intrinsic viscosity [η] of 1.2 dl / g or greater in tetrahydronaphthalene, measured at 135 °C, in the range of 1.20 dl / g to 2.10 dl / g, 1.25 dl / g to 2.01 dl / g, 1.30 dl / g to 1.92 dl / g, 1.35 dl / g to 1.83 dl / g, or 1.40 dl / g to 1.75 dl / g; l) Based on the total weight of the polyolefin plastic body, the xylene-soluble content is less than or equal to 20 wt.%, within the range of 0.50 wt.% to 20 wt.%, 0.60 wt.% to 10 wt.%, 0.80 wt.% to 5.0 wt.%, 0.90 wt.% to 3.5 wt.%, or 1.0 wt.% to 2.0 wt.%. m) weight-average molecular weight in the ranges of 40,000 Daltons to 250,000 Daltons, 50,000 Daltons to 225,000 Daltons, 60,000 Daltons to 200,000 Daltons, 70,000 Daltons to 175,000 Daltons, 80,000 Daltons to 150,000 Daltons, or 90,000 Daltons to 125,000 Daltons; Molecular weight distribution M with n) less than or equal to 3.0, less than or equal to 2.8, less than or equal to 2.6, less than or equal to 2.5, or less than or equal to 2.4 w / M n(MWD), where M w It is the weight-average molecular weight and M n These are number-average molecular weights, all measured by GPC (gel permeation chromatography). (o) Molecular weight distribution M greater than or equal to 2.0 or greater than or equal to 2.1 w / M n (MWD); Molecular weight distribution M with p) less than or equal to 2.0, less than or equal to 1.9, less than or equal to 1.8, or less than or equal to 1.7, and in all cases greater than or equal to 1.0 or greater than or equal to 1.1. z / M w M w It is the weight-average molecular weight and M w These are z-average molecular weights, all measured by GPC (gel permeation chromatography). q) Molecular weight distribution M greater than or equal to 1.0 or greater than or equal to 1.1 z / M w ; r) The enthalpy of fusion ΔH, measured by differential scanning calorimetry at a heating rate of 10 °C per minute, is less than or equal to 115 J / g, or falls within the ranges of 70 J / g to 115 J / g, 78 J / g to 114 J / g, 85 J / g to 113 J / g, 93 J / g to 111 J / g, or 100 J / g to 110 J / g. m ; s) Melt elasticity ER in the range of 0.20 to 0.90; t) Composition distribution width index (CDBI) in the range of 50 to 90, measured by crystallization elution fractionation (CEF). u) Soluble fractions in the range of 1 to 21 obtained by crystallization elution fractionation (CEF).

[0094] v) The uniformity index (HI) in the range of 80 to 90; w) Polydispersity ratio (PDR) in the range of 2.0 to 4.0; The complex viscosity (Eta) of x at a frequency of 100 rad / sec in the range of 1.4E+04 to 2.6E+04. 100 ) y) Zero shear viscosity (Eta0) in the range of 3.9E+04 to 2.0E+05. z) The melting temperature T measured by differential scanning calorimetry at a heating rate of 10°C per minute in the ranges of 80°C to 110°C, 85°C to 108°C, 90°C to 106°C, 94°C to 104°C, or 99°C to 102°C. m ; aa) The crystallization temperature T measured by differential scanning calorimetry at a heating rate of 10 °C per minute in the ranges of 65 °C to 90 °C, 69 °C to 89 °C, 74 °C to 88 °C, 78 °C to 87 °C, or 82 °C to 86 °C. c ; (bb) The glass transition temperature (Tb) measured by dynamic mechanical thermometry in the ranges of -31°C to -20.0°C, -29°C to -20.5°C, -27°C to -21.0°C, -25°C to -21.5°C, or -23°C to -22.0°C. g );or cc) any combination thereof.

[0095] In the sixth group of embodiments, in addition to the limitations of each embodiment of the first, second, third, fourth and / or fifth group of embodiments disclosed above, the polyolefin plastome is further characterized by satisfying the following conditions: a) Melting temperature T m - Crystallization temperature T c ≥14.0℃, wherein in some embodiments (melting temperature T) m - Crystallization temperature T c <20.0℃; and b) Melting temperature T m + Crystallization temperature T c ≥182.0℃, wherein in some embodiments (melting temperature T) m + Crystallization temperature T c <250.0℃.

[0096] The following embodiments illustrate the present invention; however, those skilled in the art will recognize that many variations exist within the spirit and scope of the claims. Preferred embodiments are provided below to facilitate a better understanding of the invention. These embodiments should not in any way be construed as limiting or restricting the scope of the invention.

[0097] Example The various embodiments, compositions, and methods provided herein are disclosed in the following examples. These examples are merely illustrative and are not intended to limit the scope of the invention.

[0098] The following analytical methods are used to characterize polymer compositions.

[0099] Test methods density Density was determined according to ISO 1183.

[0100] melt flow rate Melt flow was determined according to ISO 1133-1 2012-03 at the specified temperature and load.

[0101] Shear rheology measurement Shear rheological measurements were performed according to ASTM 4440-95a, characterizing dynamic viscoelastic properties (storage modulus G', loss modulus G'', and complex viscosity). (As a function of the oscillation frequency ω). Rheological measurements were performed using a rotational rheometer (TA Instrument). A 25 mm parallel plate fixture was used. The sample was pressed into a disk (approximately 29 mm in diameter and approximately 1.3 mm thick) using a hot press at 190 °C. An oscillation frequency sweep experiment was applied at 190 °C (from 398.1 rad / s to 0.0251 rad / s). The applied strain amplitude was approximately 10%, and the operating gap was set to 1 mm. A nitrogen flow was applied to the sample chamber to minimize thermal oxidation during the measurement.

[0102] Melt elasticity Melt elasticity (“ER”) was determined as described by R. Shroff and H. Mavridis in “New Measures of Polydispersity from Rheological Data on PolymerMelts” (J. Applied Polymer Science, Vol. 57 (1995), p. 1605). See also U.S. Patents 7,238,754, 6,171,993, and 5,534,472 (column 10, lines 20–30), the teachings of which are incorporated herein by reference in their entirety. Therefore, the storage modulus (G') and loss modulus (G”) were measured. A linear equation was fitted to log G' versus log G” using nine lowest frequency points (five points per decimal frequency) and by least-squares regression. The ER was then calculated according to the following formula: ER=(1.781 x 10 -3 ) x G', Where G" = 5,000 dyn / cm 2 The same procedures and equations used for ER calculations apply to both linear polyolefins and long-chain branched polyolefins.

[0103] 1-Octenene content 13C10 NMR spectra were acquired on a Bruker AV-600 spectrometer equipped with a cryoprobe, which was operated at 160.91 MHz in Fourier transform mode at 120 °C.

[0104] Sδδ peak of carbon (nomenclature according to "through") 13 Monomer sequence distribution in ethylene-propylene rubber measured by C NMR. 3. Use of reaction probability model (Monomer Sequence Distribution in Ethylene-Propylene Rubber Measured by C NMR) 13 C10 NMR. 3. Use of Reaction Probability Mode (CJ Carman, R.A. Harrington, and C.E. Wilkes, *Macromolecules*, 1977, 10, 536) was used as an internal standard at 29.9 ppm. The sample was dissolved in 1,1,2,2-tetrachloroethane-d2 at 120 °C at a concentration of 8% wt / v. Each spectrum was acquired with a 90° pulse, delayed 15 seconds between pulses, and removed using CPD. 1 H- 13 C-coupling. Using a spectral window of 9000 Hz, 512 transients were stored in 32K data points.

[0105] The spectra were assigned according to JC Randal, Macromol. Chem Phys., C29, 201 (1989).

[0106] According to Kakugo ("Carbon-13 NMR determination of monomer sequence distribution in ethylene-propylene copolymers prepared with δ-titanium trichloride-diethyl-aluminum chloride", M. Kakugo, Y. Naito, K. Mizunuma and T. Miyatake, *Macromolecules*, 1982, 15, 1150), modified to account for signal overlap in the spectrum, the ternary distribution was evaluated and the composition determined using the following equation: OOO=100 Tββ / S OOEE=100 Tβδ / S EOE=100 Tδδ / S OEO=100 Sββ / S OEE=100(Sαδ-Tββ-Tβδ-Tδδ) / S EEE=100(0.25 Sγδ+0.5(Sδδ-Tββ-Tβδ-Tδδ)) / S S=Tββ+Tβδ+Tδδ+Sββ+Sαδ-Tββ-Tβδ-Tδδ+0.25 Sγδ+0.5(Sδδ-Tββ-Tβδ-Tδδ) The molar percentage of 1-octene and ethylene content was evaluated using the following equation: 0% mol=100 [EOE+OOE+OOO] E% mol=100 [OEO+OEE+EEE] The weight percentage of 1-octene and ethylene content was evaluated using the following equation: 0% wt. = 0% mol MWO 100 / (E% mol MWE+O% mol MWO) E% wt. = E% mol MWE 100 / (E% mol MWE+O% mol MWO) 1-Hexene and 1-Butene Content This procedure determines the amount of ethyl, butyl, and hexyl branching associated with ethylene-butene, ethylene-hexene, and ethylene-octene copolymers. Based on the spectrum, the type of polymer branching is qualitatively identified according to the position and relative intensity ratio of certain peaks. The peak areas in the spectrum are then integrated to calculate the number of branchings in the polymer chain. Sample preparation is as follows: 0.2–0.3 g of sheet or film is inserted into an NMR tube. 2.5 mL of trichlorobenzene / C6D6 (4:1) solution is added to the NMR tube using a 2.5 mL airtight syringe. The NMR tube is heated to 125 °C and stirred until the sample becomes homogeneous. NMR experiments can begin when the sample appears homogeneous. NMR data are collected using a 500 MHz Varian Oxford NMR spectrometer for high-resolution solution analysis. 13C NMR. NMR spectra were acquired using the following settings: 90° pulses, duration 11 µs, using a Tycko 25 decoupled sequence (Tycko 25 is a 256-pulse sequence generated using a waveform generator to produce soft-shaped pulses), acquisition time 2.5 s, delay time 12.5 s, and number of transients 900. Free induction decay (FID) signals were processed with line broadening (LB) of 1 and baseline correction (BC) was applied. Calculations were based on the spectral region between 0 and 40 ppm in ethylene-butene and ethylene-hexene copolymers. The peak of EEE was used as an internal standard at 30.0 ppm. The total spectrum was integrated and normalized to 100 - total C from ethylene. Average peaks associated with ethyl / butyl / hexyl branching were reported; typically per 1000 TC. The weight percentage of butene was calculated from ethyl branching as Et. Br. / 100 TC × 4. The weight percentage of hexene, calculated from butyl branching, is Bu. Br. / 100TC × 6. The weight percentage of octene, calculated from hexyl branching, is hexyl Br. / 100TC × 8. Insoluble substances in the sample, or any substances with similar chemical shifts to ethyl or butyl branching, can cause inhomogeneities in the sample mixture within the NMR tube and interfere with the ability to produce high-resolution spectra.

[0107] Intrinsic viscosity (Tables 3A and 3B) The sample was dissolved in tetrahydronaphthalene at 135°C and then poured into a capillary viscometer. The viscometer tube (Ubbelohde type) was surrounded by a cylindrical glass sleeve; this setup allows for temperature control using a circulating thermostatic liquid. The downward passage of the meniscus was timed by a photoelectric device.

[0108] When the meniscus passes in front of the upper lamp, it activates a counter with a quartz crystal oscillator. The counter stops when the meniscus passes the lower lamp, and the outflow time is recorded: this is converted to an intrinsic viscosity value using the Huggins equation (Huggins, ML, *Journal of the American Chemical Society*). (J. Am. Chem. Soc) (1942, 64, 2716), assuming that the flow time of the pure solvent is known under the same experimental conditions (same viscometer and same temperature). The intrinsic viscosity is determined using a single polymer solution.

[0109] Melting temperature T m enthalpy of fusion ΔH m and crystallization temperature T c According to ISO 11357-3:2018, T is determined by differential scanning calorimetry (DSC). m ΔH m and T c .

[0110] A sample weighing 13 ± 1 mg was heated to 200 ± 1 °C at a rate of 10 °C / min and held at 200 ± 1 °C for 5 min in a nitrogen stream. It was then cooled to -90 ± 2 °C at a rate of 20 °C / min and held at that temperature for 5 min. The sample was then melted again to 200 ± 1 °C at a heating rate of 10 °C / min. Melt scans were recorded to obtain thermograms, and the temperatures corresponding to the peaks were read. The temperature corresponding to the strongest melting peak recorded during the second melting was taken as the melting temperature. The enthalpy of fusion ΔH was measured at the strongest melting peak. m Obviously, if only one peak is detected, the melting temperature and ΔH... m Both are provided by such peaks (i.e., measured at such peaks). To determine the enthalpy of fusion ΔH m, A baseline is constructed by connecting the two closest points where the endothermic peak of melting deviates from the baseline. The enthalpy of fusion (ΔH) is then calculated by integrating the area between the DSC heat flow record signal and the constructed baseline. m ).

[0111] Crystallization temperature T c Calculations based on cooling operation. During cooling, the polymer crystallizes, exhibiting an exothermic peak. Crystallization temperature T. c This corresponds to the strongest peak recorded for an exothermic event.

[0112] Crystallization elution fractionation (CEF) The chemical composition distribution of the polymer resin was analyzed using a CEF instrument (Polymer Char, Valencia, Spain). Prior to CEF testing, insoluble fractions and particles were filtered from the PCR resin using an external filtration system (EFS) set to 160°C from the Polymer Char. Approximately 24 mg of material was weighed into a 10 mL vial and sealed for CEF measurement. The dissolution process was automated using an Agilent autosampler. CEF experiments were performed automatically using the CEF instrument controller software. The sample was dissolved in 8 mL of 1,2,4-trichlorobenzene (TCB) containing 300 ppm butylated hydroxytoluene as an antioxidant and dissolved at 160°C for 1 hour. Subsequently, 400 µL of sample was injected into the CEF column (set to 105°C), and crystallization and elution steps were applied. During the crystallization step (cooling from 105°C to 30°C at a cooling rate of 2°C / min), a small flow of TCB (approximately 42 µL / min) was used to aid polymer fractionation and minimize co-crystallization within the polymer. The material crystallized in the CEF column was then eluted in a heating step (from 30 °C to 160 °C at a heating rate of 4 °C / min), while the TCB flow rate was increased to the elution flow rate (1 mL / min). The concentration and composition of the eluted material were measured using an online IR detector (at 160 °C).

[0113] Glass transition temperature T was determined by DMTA (Dynamic Mechanical Thermal Analysis). g A molded specimen measuring 20 mm × 5 mm × 1 mm was fixed onto a DMTA machine for tensile stress testing. The frequency of the sinusoidal oscillation was fixed at 1 Hz. DMTA converted the elastic response of the specimen from -100℃ (glassy state) to 130℃ (softening point). In this way, the elastic response versus temperature curve can be plotted. In DMTA, the elastic modulus of a viscoelastic material is defined as the ratio of stress to strain, and is also defined as the complex modulus E. =E'+iE''. DMTA can separate the two components E' and E'' through their resonance, and can plot the curves of E' (elastic component), E'' (loss modulus), and E'' / E'=tan δ (damping coefficient) against temperature. Glass transition temperature T g Assume the temperature at the maximum value of the curve tan=(δ) E'' / E' with respect to temperature.

[0114] Determination of the product r1×r2 of reactivity ratios According to CJ Carman, R.A. Harrington, and C.E. Wilkes, *Macromolecules*, 10, 536 (1977), the following expression is used from... 13 The product of the C NMR triplet distribution yields the reactivity ratio: Where O indicates a 1-octene unit and E indicates an ethylene unit.

[0115] The same NMR apparatus and measurement conditions were used as those for the determination of comonomer content.

[0116] Xylene soluble fractions Mix 2.5 g of polymer with 250 cm 3 o-Xylene was introduced into a glass flask equipped with a cooler and a magnetic stirrer. The temperature was raised from room temperature to the boiling point of the solvent (135°C) over 30 minutes. The resulting clear solution was then refluxed and stirred for another 30 minutes. The sealed flask was then kept in a constant temperature water bath at 25°C for 30 minutes to allow crystallization of the insoluble (XI) portion of the sample. The solid thus formed was filtered through rapid filter paper. A 100 cm⁻¹ filter was then used. 3 The filtered liquid was poured into a pre-weighed aluminum container and heated on a hot plate under a nitrogen atmosphere to remove the solvent by evaporation. The container was then kept in an oven at 80°C under vacuum until dry, and subsequently weighed after reaching constant weight.

[0117] Therefore, the weight percentages of polymers soluble and insoluble in xylene at 25°C were calculated.

[0118] Tensile properties Under the following conditions, the tensile modulus, yield tensile stress, tensile stress at break, elongation at break, and elongation at yield of the sheet material prepared by compression molding were measured.

[0119] The machine platen is set to 180°C. Aluminum foil is laid on a steel plate, and a 150×150 mm template is placed on top. 100 g of polymer granules is used to fill the cavity of the template. Another aluminum foil and steel plate are used to complete the sandwich structure. The sandwich is introduced into the hot platen of the compression molding machine. The platen is closed without applying any pressure, and the sample is heated for 5 min. Then, a pressure of 50 bar is applied to the sample for 5 min, while maintaining the temperature of the hot platen at 180 ± 1°C. After the heat treatment, the platen is cooled at 15°C / min, and the sandwich is removed when the platen temperature is below 30°C. A polymer sheet is thus obtained, from which suitable test specimens are machined.

[0120] Tensile modulus: ISO 527 / 1+2:2019.

[0121] Yield tensile stress and fracture tensile stress: ISO 527:2019.

[0122] Elongation at break and elongation at yield: ISO 527:2019.

[0123] Stress at 100% elongation and stress at 300% elongation: ISO 527:2019.

[0124] Shaw Brothers D: ISO 868:2003.

[0125] (23℃ tensile permanent deformation %) - ISO 37 A 50×2×2 mm specimen was tested at 23±1℃. The specimen was stretched on a brass bow with 200% elongation and held in that position for 10 min. Then, the specimen was removed and allowed to stand for another 10 min. Finally, the length of the specimen was measured again. The tensile permanent deformation was then calculated as follows: Tensile permanent deformation % = [(L - L0) / L0] 100, where L0 = the original length of the specimen, and L = the final length of the specimen after the procedure.

[0126] Compression set at 23°C (@25%) - ISO 815 A circular specimen with a diameter of 28.67 mm and a thickness of 12.7 mm is required. The specimen is flattened between two flanges with a diameter of 130 mm, a thickness of 14 mm, and a bore-to-axis spacing of 100 mm. The flanges are used to apply a force of 400 lbs to the specimen, corresponding to a 28 mm spring flattening. First, the specimen is flattened between the two flanges to 25% of its original thickness. The apparatus is maintained at 23°C for 22 hours. Finally, the specimen is removed, allowed to stand for 30 min, and the thickness is measured again. The compression set is calculated as follows: Compression set (%) = [(t0-t1) / (t0-t2)] 100, where t0 = original thickness, t1 = final measured thickness, and t2 = thickness of the sample after 25% compression (75% of the original thickness).

[0127] Overall polydispersity measure PDR, or “total polydispersity measure,” is determined as described by R. Shroff and H. Mavridis in “New Measures of Polydispersity from Rheological Data on Polymer Melts” (J. Applied Polymer Science, Vol. 57 (1995), pp. 1605, 1619, Equation 27), where G… ref,1 =1.95 10 4 dyn / cm 2 And log 10 (G ref,3 / G ref,1 =2. The same procedure and equations used for PDR calculations are applied to both linear polyolefins and long-chain branched polyolefins.

[0128] Complex viscosity at a frequency of 0.1 rad / sec and complex viscosity at a frequency of 100 rad / sec ratio It is used as an additional measure of shear sensitivity, and therefore as an additional measure of the rheological width or polydispersity of polymer melts.

[0129] molecular weight Molecular weight distribution (“MWD”) and average molecular weight (number-average molecular weight M) n Weight-average molecular weight Mw and z-average molecular weight M z The determination was performed using high-temperature Polymer Char gel permeation chromatography (“GPC”), also known as size exclusion chromatography (“SEC”), equipped with a filter-based infrared detector IR5, a four-capillary differential bridge viscometer, and a Wyatt 18-angle light scattering detector. n M w M z MWD and short-chain branching (SCB) spectra were reported using an IR detector, while the long-chain branching parameter g' was determined using a combination of a viscometer and an IR detector at 145 °C. Based on the hydrodynamic magnitude in 1,2,4-trichlorobenzene (TCB), polymer fractionation was performed using three Agilent PLgel Olexis GPC columns at 145 °C with 300 ppm of the antioxidant butylated hydroxytoluene (BHT) as the mobile phase. 16 mg of polymer was weighed into 10 mL vials and sealed for GPC measurements. The dissolution process was automated in an Agilent autosampler (in 8 mL TCB) at 160 °C with continuous shaking for 1 hour. During dissolution, 20 µL of heptane was also injected into the vial as a flow marker. After dissolution, 200 µL of the solution was injected into the GPC column. The GPC column was calibrated based on twelve monodisperse polystyrene (PS) standards ranging from 578 g / mol to 3,510,000 g / mol (provided by PSS). Comonomer compositions (or SCB profiles) are reported based on different calibration profiles obtained using a series of relatively narrow polyethylene profiles (polyethylene comonomers with 1-hexene and 1-octene were provided by Polymer Char, while polyethylene comonomers with 1-butene were synthesized internally), with known CH3 / 1000 total carbon values ​​determined by established solution NMR techniques. Data were analyzed using GPC one software. The long-chain branching parameter g' was determined by the following equation: g'=[η] / [η] lin in,[ η [ ] is the average intrinsic viscosity of the polymer (Tables 4A and 4B), which is derived by summing the slices on the GPC spectrum, as follows: Where c i It is the concentration of a specific slice obtained from an IR detector, and This is the intrinsic viscosity of the slice, measured from a viscometer detector. [η] lin Using the Mark-Hovink equation for linear high-density polyethylene (HDPE) ) is obtained from an IR detector, where M iThis refers to the viscosity-average molecular weight, K, and... This is the Mark-Hovink constant for linear polymers; specifically for linear polyethylene, K = 0.000374. =0.7265, while for linear polypropylene, K=0.00041, =0.6570.

[0130] Zero shear viscosity It was determined by fitting the dynamic complex viscosity to the Sabia equation for the radian frequency, as described by Shroff and Mavridis (1999) in “A Long Chain Branching Index for Essentially Linear Polyethylenes” (Macromolecules, Vol. 32, pp. 8454-8464) (included in Appendix B), the contents of which are incorporated herein by reference in their entirety.

[0131] Long chain branching LCBI was determined using Equation 13: Equation 13 and its application are described in Shroff and Mavridis’s (1999) “A Long Chain Branching Index for Essentially Linear Polyethylenes” (Macromolecules, Vol. 32, pp. 8454-8464), the contents of which are incorporated herein by reference in their entirety.

[0132] Long-chain branching frequency, characterized by the ratio of long-chain branching numbers per thousand carbon atoms, or LCB / 10 3 C was determined using the method of Janzen and Colby (J. Janzen and RH Colby, “Diagnosing long-chain branching in polyethylenes,” Journal of Molecular Structure, Vol. 485-486, August 10, 1999, pp. 569-583), employing equations (2-3) from the above references and the constants in Table 2. Specifically, the zero-shear viscosity at 190 °C was determined. Determined by extrapolating complex viscosity data via the Sabia equation, as described separately. Weight-average molecular weight Mw Determined via GPC. Using these two parameters, along with the methods of Janzen and Colby, the long-chain branching frequency LCB / 10 was determined. 3 C can be numerically determined such that all three parameters (η0, M) are equal. w and LCB / 10 3 The material satisfies equations (2-3) in the aforementioned references. The Janzen and Colby method predicts the zero-shear viscosity of the material compared to that of a perfectly linear polymer with the same average molecular weight (LCB / 10). 3 The ratio of zero shear viscosity (C=0) In LCB / 10 3 C exhibits its maximum value at a certain value, and therefore for For each value, there are two levels or values, LCB / 10. 3 C makes this ratio possible. For the purposes of this calculation, in Always choose LCB / 10 for a given ratio. 3 The minimum value of C.

[0133] Composition distribution width index The CDBI, or “Composition Distribution Width Index,” is determined by TREF / CEF and defined in U.S. Patent No. 5,382,630, the teachings of which are incorporated herein by reference in their entirety.

[0134] Uniformity Index The HI, or “uniformity index,” is determined by CEF and is defined in U.S. Patent No. 5,798,427, the teaching of which is incorporated herein by reference in its entirety.

[0135] Test materials Table 1 shows a list of representative polyolefin plastics of the present invention as well as various commercial polymers, with which the polyolefin plastics described herein are compared and contrasted in the following examples.

[0136] Table 1 Examples 1-29 were prepared using the catalysts and processes described below.

[0137] Preparation of metallocene catalyst (A-1) dimethylsilyl (2,4,7-Trimethyl-1-indenyl)-7-(2,5-Dimethyl-cyclopentano[1,2-b:4,3-b']-dithiophene) Zirconium dichloride (A-1) was prepared according to Example 32 of PCT Publication WO2001 / 47939A1.

[0138] Preparation of catalytic solution Under a nitrogen atmosphere, 8.1 L of a 4.5% wt / v TIBA cyclohexane solution (1.84 mol TIBA) and 760 mL of a 30% wt / wt MAO toluene solution (3.65 mol MAO) were loaded into a 20 L jacketed glass reactor equipped with an anchor stirrer and stirred at room temperature for about 1 hour.

[0139] After this time, add metallocene A-1 (1.6 g, 2.75 mmol) and dissolve it with stirring for about 30 minutes.

[0140] The final solution is discharged from the reactor into a cylinder through a filter to remove solid residues (if any).

[0141] The solution has the following composition: polymerization Polymerization was carried out continuously in a pilot plant containing a stirred reactor, wherein cyclohexane constituted the liquid medium. The reaction temperatures and pressures, hydrogen to ethylene ratios, and amounts of solution, ethylene, and 1-octene in the reactors of Examples 1-10 are shown in Table 2 below, to produce the polyolefin plastides shown in Table 3.

[0142] Table 2 Table 3A shows the characteristic parameters of polyolefin polymers POP1-POP7. POP1-POP7 correspond to the polymerization conditions shown in Table 2 (Examples 1-7).

[0143] Table 3A Table 3B is a continuation of Table 3A, showing the characteristic parameters of polyolefin polymers POP8-POP10 and comparative polymers P1-P3. POP8-POP10 correspond to the polymerization conditions shown in Table 2 (Examples 8-10). Examples 11-13 show the characteristic parameters of comparative polymers P1-P3, which are mentioned in Table 1 above.

[0144] Table 3B Examples 14-17 in Table 4A show the characteristic parameters of polyolefin polymers POP4 and POP7, while Examples 18-21 show the characteristic parameters of comparative polymers P1-P4. POP4 and POP7 correspond to the polymerization conditions shown in Table 2 (Examples 4 and 7). Comparative polymers P1-P4 are mentioned in Table 1 above.

[0145] Table 4A Table 4B is a continuation of Table 4A. Examples 22-28 in Table 4B show the characteristic parameters of comparative polymers P5-P11. Comparative polymers P5-P11 are mentioned in Table 1 above.

[0146] Table 4B Figure 1 The results show that the comonomer content of the polyolefin plastomers POP4 and POP7, as disclosed herein, is relatively constant over polymer chain lengths ranging from approximately 4.25 to approximately 5.50 on a log 10 (MW) scale, similar to that of the comparative polymer P5. However, the comonomer content of the comparative polymer P5 is higher than 20 wt.%, while that of the polyolefin plastomers POP4 and POP7 is lower than 20 wt.%. The difference between the polyolefin plastomers POP4 and POP7 and the comparative polymers P6 and P7 is that P6 and P7 exhibit a significant decrease in comonomer content with increasing polymer chain length.

[0147] Figure 2 The complex viscosity (η) of the polymer of the present invention and the comparative polymer is shown. The curve showing how the frequency changes. Figure 2 The curves in the figure have been normalized to MI at 1.0 dg / min. When comparing the viscosity curves (complex viscosity, or η) of different polymer melts... When considering the relationship between viscosity and frequency (or ω), it should be understood that both molecular weight and polydispersity affect the viscosity level and the shape of the viscosity curve. Figure 2 The representation attempts to "normalize and eliminate" the molecular weight effect, so that only polydispersity differences affect the shape of the curve. This procedure involves normalizing the original η... The relationship with ω can be simply redrawn as (MI x η) The graph shows the relationship between (ω / MI), where MI is the melt index of the material. In practice, this representation “shifts” each viscosity curve to the common MI=1 for all comparative materials. The curves for the polyolefin plastomers POP4 and POP7 disclosed herein are flatter than those for the comparative polymers P5, P6, and P7. This means that the complex viscosity of polyolefin plastomers POP4 and POP7 varies less with frequency, indicating an improved balance between viscous and elastic properties relative to the comparative polymers P5, P6, and P7 within the test range. Such materials are considered to have viscoelastic properties but exhibit dominant viscous or elastic behavior that is least affected by frequency variations.

[0148] Figure 3This displays the differential weight fraction (dw / dt) relative to temperature change during analysis (in GPC or TREF). In the context of GPC or TREF, this represents the concentration of the polymer fraction eluted or separated from the column at a specific temperature. Elution temperature refers to the temperature at which a specific fraction of the polymer elutes from the chromatographic column in GPC or TREF. Elution temperature provides information about the polymer's composition, molecular weight, and branching. In TREF, it is particularly used for separating and analyzing polyolefins based on their crystallinity or branching structure.

[0149] The high, narrow peaks in the curves of polyolefin plastomers POP4 and POP7 indicate uniform molecular characteristics, such as molecular weight and / or specific structural features like crystallinity. This level of uniformity indicates consistent material properties and characteristics across a variety of applications. In contrast, the broader, lower peaks of polymers P5, P6, and P7 indicate greater heterogeneity in molecular weight and / or compositional characteristics among these polymers. The high uniformity of the polyolefin plastomers disclosed herein can facilitate the customization of polymer materials for specific applications.

[0150] Figure 4 The results show that the LCB of polyolefin plastomers POP4 and POP7 is less than that of the comparative polymer P5. The difference between polyolefin plastomers POP4 and POP7 and the comparative polymers P6 and P7 is that P6 and P7 have a much higher density.

[0151] In summary, the data are believed to indicate that the polyolefin plastomers disclosed herein possess a unique structure that provides a new and useful balance of properties.

[0152] For the sake of brevity, this document only explicitly discloses certain ranges. However, in addition to the ranges listed, any lower bound can be combined with any upper bound to list ranges not explicitly listed, and a range from any lower bound can be combined with any other lower bound to list ranges not explicitly listed, just as a range from any upper bound can be combined with any other upper bound to list ranges not explicitly listed. Additionally, even if not explicitly stated, a range includes every point or individual value between its endpoints. Therefore, each point or individual value can be combined as its own lower or upper bound with any other point or individual value or any other lower or upper bound to list ranges not explicitly listed.

[0153] While the invention and its advantages have been described in detail, it should be understood that various changes, substitutions, and modifications may be made herein without departing from the spirit and scope of the invention as defined by the appended claims. All patents, test procedures, and other documents referenced in this application are incorporated herein by reference in their entirety in all jurisdictions where such incorporation is permissible. Furthermore, the scope of this application is not intended to be limited to specific embodiments of the processes, machines, means, methods, and / or steps described in the specification. As will be readily understood by those skilled in the art from the disclosure of this invention, according to the invention, processes, machines, means, methods, and / or steps that are currently existing or subsequently developed can be utilized to perform substantially the same function or achieve substantially the same results as the corresponding embodiments described herein. Therefore, the appended claims are intended to include such processes, machines, means, methods, and / or steps within their scope.

Claims

1. A polyolefin plastic body comprising units derived from ethylene and 1-octene, said polyolefin plastic body having: a) Measured at 23°C according to ISO 1183-1:2012, at 0.890 g / cm³. 3 Up to 0.910 g / cm 3 Density within the range; b) Melt index (2.16 kg, 190 °C) measured at 190 °C with a load of 2.16 kg, in the range of 0.10 g / 10 min to 3.00 g / 10 min, according to ISO 1133-1 2012-03; and c) From the range of 0.820 to 1.08 13 The product of the reactivity ratios obtained from the C NMR ternary distribution is r1×r2, where r1 is the reactivity ratio of ethylene to 1-octene, and r2 is the reactivity ratio of 1-octene to ethylene.

2. The polyolefin plastic body according to claim 1, further comprising: a) Long chain branching index (LCBI) in the range of 0.04 to 0.38; b) Long-chain branching content in the range of 0.005 LCB / 1000C to 0.025 LCB / 1000C; or c) Its combination.

3. The polyolefin plastic body according to claim 1, further comprising: a) Melt index (21.6 kg, 190 °C) measured at 190 °C and with a load of 21.6 kg, in the range of 5.0 g / 10 min to 45.0 g / 10 min, according to ISO 1133-1 2012-03. 21 ); b) Melt flow index (MFR) in the range of 0.50 g / 10 min to 3.50 g / 10 min (2.16 kg, 230 °C) measured at 230 °C and with a load of 2.16 kg, according to ISO 1133-1 2012-03. c) Melt index (10 kg, 190 °C) measured at 190 °C and with a load of 10.0 kg, in the range of 3.0 g / 10 min to 15.0 g / 10 min, according to ISO 1133-1 2012-03. 10 );or d) Its combination.

4. The polyolefin plastide according to claim 3, wherein: a) I 21 The ratio of I2 is in the range of 17.0 to 28.0; b)I 10 The ratio of I / I2 is in the range of 3.0 to 10.0; or c) Its combination.

5. The polyolefin plastic body according to claim 1, further comprising a 1-octene content (C8) in the range of 10.0 wt.% to 26.0 wt.% relative to the weight of the polyolefin plastic body. cont .

6. The polyolefin plastome according to claim 1, further having an elongation at break of 500% or greater as measured on a compression-molded sample according to ISO 527:2019.

7. The polyolefin plastide according to claim 1, further having an intrinsic viscosity [η] of 1.2 dl / g or greater as measured in tetrahydronaphthalene at 135°C.

8. The polyolefin plastic body according to claim 1, further comprising a xylene-soluble content of less than or equal to 20 wt.% based on the total weight of the polyolefin plastic body.

9. The polyolefin plastome according to claim 1, further comprising a molecular weight distribution M of less than or equal to 3.

0. w / M n (MWD), where M w It is the weight-average molecular weight and M n These are number-average molecular weights, all measured by GPC (gel permeation chromatography).

10. The polyolefin plastome according to claim 9, further comprising a molecular weight distribution M greater than or equal to 2.0 or greater than or equal to 2.

1. w / M n (MWD).

11. The polyolefin plastome according to claim 1, further comprising a molecular weight distribution M of less than or equal to 2.

0. z / M w M w It is the weight-average molecular weight and M w These are z-average molecular weights, all measured by GPC (gel permeation chromatography).

12. The polyolefin plastome according to claim 11, further comprising a molecular weight distribution M greater than or equal to 1.0 or greater than or equal to 1.

1. z / M w .

13. The polyolefin plastide according to claim 1, having a melting enthalpy ΔH of less than or equal to 115 J / g, as measured by differential scanning calorimetry at a heating rate of 10°C per minute. m .

14. The polyolefin plastome according to claim 1, having a melt elasticity ER in the range of 0.20 to 0.

90.

15. The polyolefin plastide according to claim 1, having a melt temperature T in the range of 80°C to 110°C, as measured by differential scanning calorimetry at a heating rate of 10°C per minute. m .

16. The polyolefin plastide according to claim 1, wherein (melting temperature T) m – Crystallization temperature T c ≥14.0℃, and (melting temperature T) m + Crystallization temperature T c ≥182.0℃.

17. The polyolefin plastide according to claim 1, further having a glass transition temperature (Tg) in the range of -31°C to -20.0°C as measured by dynamic mechanical thermometry. g ).

Citation Information

Patent Citations

  • Linear ethylene interpolymer blends of interpolymers having narrow molecular weight and composition distribution

    US5382630A

  • Vanadium-containing catalyst system

    US5534472A

  • Ethylene polymers having enhanced processability

    US5798427A

  • Enhanced-impact LLDPE with a shear modifiable network structure

    US6171993B1

  • Solid state process to modify the melt characteristics of polyethylene resins and products

    US7238754B1