polyurethane resin powder

By controlling the roundness, stress, and glass transition temperature of polyurethane resin particles, the problem of large hardness variations was solved, resulting in polyurethane resin particles with low environmental dependence, suitable for applications such as synthetic leather.

CN123125253APending Publication Date: 2026-11-17CANON KK
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202580029526.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-09-12
Filing Date
2025-04-09
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing polyurethane resin particles exhibit significant variations in hardness under different environments, lacking low environmental dependence and making it difficult to simultaneously possess both appropriate hardness and low environmental dependence.

Method used

By controlling the average sphericity of polyurethane resin particles, the stress range of compressed particle size under specific conditions, and the glass transition temperature, it is ensured that polyurethane resin particles maintain a rubber state within the commonly used temperature range, reducing changes in hardness.

Benefits of technology

This technology achieves minimal hardness variation in polyurethane resin particles under different environments, exhibiting appropriate hardness and low environmental dependence, making it suitable for applications such as synthetic leather.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

A polyurethane resin powder comprising polyurethane resin particles is provided. The polyurethane resin particles contain polyurethane resin. The polyurethane resin powder is characterized in that: the average sphericity of the polyurethane resin particles contained in the polyurethane resin powder is 0.950 or higher; the stress of the polyurethane resin particles when compressed by 10% of their particle size in an environment of 23°C and 50%RH is 0.25-0.50 mN; and the glass transition temperature of the polyurethane resin particles is below 0°C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to polyurethane resin powder, which comprises polyurethane resin particles blended in coatings, cosmetics, surface modifiers for synthetic leather, etc. Background Technology

[0002] Polyurethane resin particles, whose main component is polyurethane resin, possess excellent hardness properties, such as softness and scratch resistance, in addition to solvent resistance and heat resistance. Therefore, they are widely used in coatings, adhesives, cosmetics, surface modifiers for synthetic leather, and fillers for plastic and rubber products. From the viewpoint of the tactile feel and softness of articles containing polyurethane resin particles, it is important to properly control the hardness of the polyurethane resin particles, and polyurethane resin particles with various controlled hardnesses are disclosed in Patent Documents 1 and 2.

[0003] Reference List

[0004] Patent documents

[0005] Patent Document 1: Japanese Patent Application Publication No. 2007-4142

[0006] Patent Document 2: Japanese Patent Application Publication No. 2018-35249 Summary of the Invention

[0007] The problem the invention aims to solve

[0008] One of the required functions of polyurethane particles is minimal performance variation regardless of season and operating environment (i.e., low environmental dependence on hardness). However, to date, polyurethane resin particles possessing both suitable hardness and low environmental dependence do not exist. Therefore, the object of this invention is to provide a polyurethane resin powder comprising polyurethane resin particles with suitable hardness and low environmental dependence.

[0009] Solution for solving the problem

[0010] A polyurethane resin powder is provided, comprising polyurethane resin particles containing polyurethane resin, wherein the polyurethane resin particles contained in the polyurethane resin powder have an average sphericity of 0.950 or more, and the stress when the polyurethane resin particles are compressed to 10% of their particle size in an environment of 23°C and 50%RH is 0.25 mN or more and 0.50 mN or less, and the polyurethane resin particles have a glass transition temperature of 0°C or less.

[0011] The effects of the invention

[0012] Polyurethane resin powder containing polyurethane resin particles with appropriate hardness and low environmental dependence can be provided. Detailed Implementation Plan

[0013] In this disclosure, unless otherwise stated, expressions indicating a range of values, such as "above XX and below YY" and "XX to YY", refer to a range including both the lower and upper limits as endpoints. When a range of values ​​is represented in a segmented manner, the upper and lower limits of each range can be arbitrarily combined.

[0014] The inventors have discovered that the above-mentioned problem can be solved by controlling the stress of polyurethane resin particles when compressed to 10% of their particle size in an environment of 23°C and 50%RH to a value of 0.25mN or more and 0.50mN or less, and by controlling the glass transition temperature to a value of 0°C or less.

[0015] This disclosure relates to polyurethane resin powder, which includes polyurethane resin particles containing polyurethane resin, wherein the polyurethane resin particles in the polyurethane resin powder have an average sphericity of 0.950 or more, the polyurethane resin particles are compressed to 10% of their particle size in an environment of 23°C and 50%RH with a stress of 0.25 mN or more and 0.50 mN or less, and the glass transition temperature is below 0°C.

[0016] The inventors deduce the following mechanism by which the effects of the present invention are achieved.

[0017] The polyurethane resin particles of this invention have a glass transition temperature below 0°C. That is, the polyurethane resin particles of this invention are in a rubbery state within a practical temperature range. Generally, resins exhibit a large change in hardness in the transition regions from a glassy state to a rubbery state and from a rubbery state to a molten state. On the other hand, resins exhibit a characteristic where, within a temperature range where the resin exists in a glassy or rubbery state without accompanying state transition, the hardness is minimally affected by temperature changes. Since the polyurethane resin particles of this invention are in a rubbery state within a commonly used temperature range of 10°C to 40°C, the hardness is minimally affected by temperature changes. In other words, it exhibits low environmental dependence.

[0018] Furthermore, by appropriately controlling the composition of the polyurethane resin, the stress of the polyurethane resin particles when compressed to 10% of their particle size in an environment of 23°C and 50%RH is 0.25 mN or more and 0.50 mN or less. Therefore, polyurethane resin particles of the present invention, having suitable hardness and low environmental dependence, and ultimately a polyurethane resin powder containing these particles, are achieved.

[0019] The polyurethane resin powder according to the present invention will now be described in more detail.

[0020] The polyurethane resin particles of the present invention preferably have an average roundness of 0.950 or higher. Roundness, as used herein, refers to a value representing the shape of the particle calculated from a projected image of the particle. First, a particle image is captured, its outline is extracted, and the projected area S, perimeter L, etc., are measured. Second, the area S and perimeter L are used to determine the equivalent diameter and roundness. The equivalent diameter is the diameter of a circle having the same area as the projected area of ​​the particle image, and roundness C is defined as a value obtained by dividing the perimeter of the circle determined by the equivalent diameter by the perimeter of the particle projected image, and is calculated using the following expression:

[0021] Circularity C = 2 × (π × S) 1 / 2 / L.

[0022] The roundness of each particle is calculated, and then the roundness range of 0.200 to 1.000 is divided into 800 parts. The arithmetic mean of the obtained roundness values ​​is calculated and defined as the average roundness.

[0023] When the particle image is circular, the roundness is 1, and the greater the unevenness of the outer periphery of the particle image, the lower the roundness value becomes. In other words, a roundness value close to 1 means that the shape is close to a perfect sphere.

[0024] The average roundness is preferably 0.950 or higher. When the average roundness is 0.950 or higher, performance changes caused by particle shape can be suppressed. The average roundness can be controlled by the type of monomer to be used and by changing the manufacturing conditions.

[0025] In the polyurethane resin particles of the present invention, the stress when the polyurethane resin particles are compressed to 10% of their particle size in an environment of 23°C and 50%RH is 0.25 mN or more and 0.50 mN or less, preferably 0.26 mN or more and 0.38 mN or less. That is, this hardness range is precisely the appropriate hardness for the purposes of the present invention. It is said that the range of human skin tactile sensitivity involves 10 to 10. 3 μN input detection and 10 -2 Up to 10 2 The irregularity resolution is within μN, and the appropriate hardness, which is the objective of this invention, is within this range. That is, when the polyurethane resin particles of this invention are used, for example, as a surface modifier for synthetic leather, they can impart the function of "minimizing changes in tactile feel regardless of the usage environment." The stress at 10% of the compressed particle size can be adjusted by the type or molecular weight of the monomers used to manufacture the polyurethane resin particles, the functionality, the composition ratio of each monomer, the type of catalyst, the amount of solvent to be used, etc.

[0026] The polyurethane resin particles of this invention have a glass transition temperature (Tg) below 0°C. When Tg is greater than 0°C and below 40°C, the transition between the glass and rubber states occurs within the practical temperature range, resulting in high environmental dependence and failing to achieve the objectives of this invention. Similarly, in methods that control Tg to temperatures above 40°C, the transition from the glass state does not occur within the practical temperature range, and environmental dependence can be minimized. However, this method is not preferred because the hardness tends to increase to a level higher than that of this invention.

[0027] The Tg of polyurethane resin particles can be adjusted by the type or molecular weight of the monomers used to manufacture the polyurethane resin particles, the functionality, the composition ratio of each monomer, the type of catalyst, and the amount of solvent to be used.

[0028] In particular, Tg is preferably controlled by using a compound having the chemical formula (1) described in detail later.

[0029] The Tg of polyurethane resin particles is preferably below -20°C.

[0030] In pulse NMR measurements of polyurethane resin powder at a measurement temperature of 23°C, the polyurethane resin particles of the present invention were analyzed using hydrogen nuclei via solid-state echo method. 1 H is used as the measuring nucleus to measure the spin-spin relaxation time T2 to determine the echo intensity curve A of the polyurethane resin powder. The echo intensity curve A is decomposed into three components using the least squares method, and the component with the shortest relaxation time is defined as component T. 2s A. When the component T in the polyurethane resin particles 2s The component fraction of A is defined as F s When A[%], F s A is preferably 15 or higher and 90 or lower.

[0031] Component T 2s A is typically referred to as the "hard segment at 23°C," and the component near the crosslinking point in the polyurethane resin that forms the polyurethane resin particles, including the component where a portion of the molecular chain is oriented and stacked, is detected as component T. 2s A.

[0032] By using component T 2s A's component fraction F s By controlling A[%] within the above range, polyurethane resin particles with reduced environmental dependence can be obtained. From the viewpoint of easy control of hardness, the component fraction F s A[%] is more preferably 25% or more and 60% or less, and even more preferably 30% or more and 45% or less.

[0033] Component fraction Fs A[%] can be adjusted by the type or molecular weight of the monomers used to manufacture polyurethane resin particles, as well as their functionality. Specifically, F can be increased by, for example, using monomers in which the molecular chains are easily oriented and stacked, or by adding multifunctional monomer components. s A[%].

[0034] In the polyurethane resin particles of the present invention, when (1) hydrogen nuclei are used 1 H, as a solid-state echo method for measuring the spin-spin relaxation time T2 of a nucleus, was performed in pulsed NMR measurements of polyurethane resin powder at a measurement temperature of 10 °C to determine the echo intensity curve B of the polyurethane resin powder. The echo intensity curve B was decomposed into three components using the least squares method, and the component with the shortest relaxation time among the three components was defined as component T. 2s B, component T 2s The component fraction of B in polyurethane resin powder is defined as F. s B[%] and (2) are used for the use of hydrogen nuclei 1 H, as a solid-state echo method for measuring the spin-spin relaxation time T2 of a nucleus, was performed in pulsed NMR measurements of polyurethane resin powder at a measurement temperature of 40°C to determine the echo intensity curve C of the polyurethane resin powder. The echo intensity curve C was decomposed into three components using the least squares method, and the component with the shortest relaxation time was defined as component T. 2s C, the component T 2s The component fraction of C in the polyurethane resin powder is defined as F. s When C[%], F s B / F s C is preferably 1.0 or higher and 1.5 or lower.

[0035] Component T 2s B is usually referred to as the "hard segment at 10°C", and its component T is... 2s C is usually referred to as the "hard segment at 40°C". The component T in polyurethane resin powder... 2s B and component T 2s The component fractions of C are defined as F. s B and F s C. In this case, if F s B and F s C to F s B / F s A C value between 1.0 and 1.5 means that the amount of the component detected as a hard segment does not change significantly with temperature. Generally, hard segments, due to the orientation and stacking of molecular chains, tend to move easily upon heating. Therefore, a small F... s B / F s C indicates that most of the T component was detected as a hard segment.2s B and component T 2s C represents the component near the crosslinking point.

[0036] F s B / F s C can be adjusted by the type or molecular weight of the monomers used to manufacture the polyurethane resin particles, as well as their functionality. In particular, as mentioned above, it is preferable to add multifunctional monomers to increase the proportion near the crosslinking points.

[0037] F s B / F s The range of C is more preferably less than 1.45, and even more preferably less than 1.40.

[0038] The polyurethane resin particles of the present invention contain polyurethane resin as the main component.

[0039] The main components in this article refer to components containing more than 50% by mass.

[0040] Within the scope of this invention, materials other than polyurethane resins may be included for various purposes. For example, materials such as colorants (e.g., dyes and pigments), UV absorbers, antioxidants, metal powders, and flavorings may be included.

[0041] The polyurethane resin contained in the polyurethane resin particles of the present invention preferably has a partial structure in its molecular structure represented by the following formula (1).

[0042]

[0043] Because polyurethane resins with this structure significantly reduce their orientation regularity, the glass transition temperature can be easily controlled below 0°C.

[0044] In order to incorporate a portion of the structure of chemical formula (1) into the molecular structure of polyurethane resin, it is preferable to use an isocyanate component or a polyol component having the structure of chemical formula (1) as a raw material to synthesize the polyurethane resin. In particular, from the perspective of availability, it is preferable to use a polyol component having the structure of chemical formula (1).

[0045] Specifically, examples of polyol components include polycarbonate polyols of 3-methyl-1,5-propanediol (MPD), polyester polyols of MPD and sebacic acid, polyester polyols of MPD and adipic acid, polyester polyols of MPD and terephthalic acid, and polyester polyols of MPD and isophthalic acid.

[0046] The method for synthesizing the polyurethane resin in the polyurethane resin particles of the present invention is not particularly limited, as long as it is within the scope of the present invention, and the polyurethane resin can be prepared by the following known methods.

[0047] -A one-step method by mixing and reacting the polyol component and the polyisocyanate component; and

[0048] - A method of reacting a prepolymer with isocyanate-terminated groups obtained by reacting a portion of a polyol with an isocyanate, and then reacting it with a chain extender (e.g., a low molecular weight polyol).

[0049] Examples of isocyanate components that can be used to prepare the polyurethane resin in the polyurethane resin particles of the present invention include toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), naphthalene diisocyanate (NDI), dimethylbiphenyl diisocyanate (TODI), hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), terephthalic acid diisocyanate (PPDI), xylene diisocyanate (XDI), tetramethylxylene diisocyanate (TMXDI), cyclohexane diisocyanate, and mixtures thereof. Furthermore, copolymers, isocyanurate types, TMP adduct types, and biuret types of the above components can also be used.

[0050] Examples of polyol components that can be used to prepare the polyurethane resin in the polyurethane resin particles of the present invention include polyether polyols, polyester polyols, polycarbonate polyols, polyolefin polyols, acrylic polyols, and mixtures thereof. In particular, as described above, polyol components having the structure of chemical formula (1) are preferred, especially polycarbonate polyols of 3-methyl-1,5-propanediol (MPD), polyester polyols of MPD and sebacic acid, and polyester polyols of MPD and adipic acid.

[0051] Examples of chain extenders that can be used to prepare the polyurethane resin in the polyurethane resin particles of the present invention include, for example, bifunctional low molecular weight diols such as ethylene glycol and 1,4-butanediol, trifunctional low molecular weight triols such as trimethylolpropane, and mixtures thereof.

[0052] The aforementioned isocyanate compounds can react with various polyols in the presence of excess isocyanate groups to pre-form isocyanate-terminated prepolymers. As these isocyanate compounds, materials end-capped with various end-capping agents such as isocyanate-based MEK oximes can be used.

[0053] The polyurethane resin contained in the polyurethane resin particles of the present invention is preferably a polymer comprising a composition of a polyisocyanate having an isocyanurate structure, a difunctional polyol and a polyol with more than three functions.

[0054] The degree of crosslinking of the entire polyurethane resin particles can be improved by using polyisocyanates with isocyanurate structures, and the hardness and component fraction F of the polyurethane resin particles can also be improved. s A[%] can be easily controlled within the above range.

[0055] Regarding the polyol components, it is preferable to use a combination of difunctional polyols and polyols with trifunctionality or higher.

[0056] The combined use of polyols with trifunctionality or higher further increases the degree of crosslinking and makes it easy to control the hardness within an appropriate range.

[0057] More preferably, the polyol with trifunctionality or higher is preferably a polyol with tetrafunctionality or higher. By using a polyol with tetrafunctionality or higher, regions with high cross-linking degree, i.e., hard segments, can be locally formed in the molecular structure. Even when seeking to suppress environmental dependence by increasing the cross-linking degree based on polyurethane resin particles through the local arrangement of hard segments, the resin itself will harden too much, and the hardness of the polyurethane resin particles can be easily controlled within the aforementioned range.

[0058] In particular, polyols with four or more functions are more preferably ethylenediamine modified with propylene oxide.

[0059] Bifunctional polyols can be widely available polyols as described above, but in particular, polycarbonate polyols are preferred for the purpose of improving the abrasion resistance of polyurethane resin particles.

[0060] The molecular weight of the bifunctional polyol to be used is preferably 1,000 or more and 10,000 or less. When the molecular weight is within this range, the distance between crosslinking points can be appropriately adjusted, and the polyurethane resin particles are prevented from becoming too hard or unfavorably too soft. A molecular weight of 3,000 or more and 6,000 or less is more preferred.

[0061] The mixing ratio of the polyisocyanate component reacting with the polyol component is preferably within a certain range, such that the ratio of isocyanate groups based on 1.0 hydroxyl groups of the polyol is in the range of 2.0 to 15.0.

[0062] More preferably, the ratio is 4.0 to 10.0, and even more preferably 5.0 to 7.5.

[0063] <Manufacturing Method>

[0064] There are no particular limitations on the method used to manufacture the polyurethane resin particles of the present invention, and widely known methods for manufacturing polyurethane resin particles can be used. In particular, it is desirable to produce polyurethane resin particles by granulation in an aqueous medium, such as suspension polymerization and solution suspension, because it is easy to control the shape and diameter of the polyurethane resin particles to be obtained.

[0065] As an example of a preferred manufacturing method, the suspension polymerization method will be described below.

[0066] <Preparation of Carbamate Monomer Compositions>

[0067] In this method, monomers of the aforementioned polyurethane resin, such as polyisocyanates and polyols, along with other materials, are mixed to prepare a urethane monomer composition. There are no particular limitations on the mixing method, and a uniformly dissolved and / or dispersed urethane monomer composition can be obtained using commonly used stirring devices, homogenizers, or ultrasonic dispersers.

[0068] The carbamate monomer composition preferably further contains a catalyst for controlling the rate of carbamate condensation and the binding form. Well-known catalysts can be used as the catalyst for carbamate condensation.

[0069] Examples of catalysts include organotin compounds such as dibutyltin dilaurate, dibutyltin diacetate, dibutyltin dithiocarboxylic acid, dibutyltin dimaleate, dioctyltin dithiocarboxylic acid, and tin octenate; organolead compounds such as lead octenate; monoamines such as triethylamine and dimethylcyclohexylamine; diamines such as tetramethylethyldiamine, tetramethylpropylenediamine, and tetramethylhexanediamine; triamines such as pentamethyldiethylenetriamine, pentamethyldipropylenetriamine, and tetramethylguanidine; cyclic amines such as triethylenediamine, dimethylpiperazine, methylethylpiperazine, methylmorpholine, dimethylaminoethylmorpholine, and dimethylimidazole; alkanolamines such as dimethylaminoethanol, dimethylaminoethoxyethanol, trimethylaminoethylethanolamine, methylhydroxyethylpiperazine, and hydroxyethylmorpholine; and ether amines such as bis(dimethylaminoethyl) ether and ethylene glycol bis(dimethyl)aminopropyl ether. These catalysts can be used alone or in combination of two or more. In particular, from the perspective of controlling the degree of crosslinking, catalysts commonly referred to as allophanation catalysts or isocyanurate catalysts are preferred.

[0070] The urethane monomer composition preferably contains an organic solvent for adjusting the viscosity of the urethane monomer composition. The organic solvent is preferably one that can be uniformly mixed in the urethane monomer composition and does not inhibit the polymerization reaction.

[0071] Examples of solvents include aromatic hydrocarbon-based solvents such as toluene, xylene, ethylbenzene, and tetrahydronaphthalene; aliphatic or alicyclic hydrocarbon-based solvents such as n-hexane, n-heptane, petroleum solvent oil, and cyclohexane; halogen-based solvents such as methyl chloride, methyl bromide, methyl iodide, dichloromethane, carbon tetrachloride, trichloroethylene, and perchloroethylene; ester or ester ether-based solvents such as ethyl acetate, butyl acetate, methoxybutyl acetate, methyl acetate cellosolve, and ethyl acetate cellosolve; and ether-based solvents such as diethyl ether, tetrahydrofuran, and dioxane. Alkane, ethyl cellosolve, butyl cellosolve, and propylene glycol monomethyl ether; ketone solvents, such as acetone, methyl ethyl ketone, methyl isobutyl ketone, di-n-butyl ketone, and cyclohexanone; alcohol solvents, such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, tert-butanol, 2-ethylhexanol, and benzyl alcohol; amide solvents, such as dimethylformamide and dimethylacetamide; sulfoxide solvents, such as dimethyl sulfoxide; heterocyclic compound solvents, such as N-methylpyrrolidone; and mixtures of two or more of these solvents.

[0072] Increasing the amount of organic solvent reduces the viscosity of the urethane monomer composition, which reduces the particle size of the dispersed droplets during the subsequent granulation process, and the resulting polyurethane resin particles tend to have a reduced average particle size.

[0073] <Preparation of Aqueous Media>

[0074] In this process, an aqueous medium is prepared as the medium into which the urethane monomer composition is added and dispersed.

[0075] Aqueous media may contain inorganic or organic dispersants and stabilizers.

[0076] Known dispersion stabilizers can be used as dispersion stabilizers.

[0077] Examples of inorganic dispersion stabilizers include phosphates such as hydroxyapatite, tricalcium phosphate, dicalcium phosphate, magnesium phosphate, aluminum phosphate, and zinc phosphate; carbonates such as calcium carbonate and magnesium carbonate; metal hydroxides such as calcium hydroxide, magnesium hydroxide, and aluminum hydroxide; sulfates such as calcium sulfate and barium sulfate; calcium metasilicate; bentonite; silica; and alumina.

[0078] Examples of organic dispersants include polyvinyl alcohol, gelatin, methylcellulose, methyl hydroxypropyl cellulose, ethylcellulose, sodium salts of carboxymethyl cellulose, polyacrylic acid and its salts, and starch.

[0079] When using inorganic compounds as dispersion stabilizers, commercial products can be used as is, but to obtain finer particles, inorganic compounds can be generated in an aqueous medium.

[0080] For example, when using calcium phosphate such as hydroxyapatite and tricalcium phosphate, aqueous solutions of phosphate and calcium salts can be mixed under high stirring conditions.

[0081] Aqueous media may contain surfactants. Known surfactants can be used as surfactants. Examples of surfactants include anionic surfactants, such as sodium dodecylbenzenesulfonate and sodium oleate; cationic surfactants; amphoteric surfactants; and nonionic surfactants.

[0082] The particle size of the resulting polyurethane resin particles can be controlled by adjusting the amount of this dispersant. Increasing the amount of dispersant reduces the particle size of the dispersed droplets during subsequent granulation, resulting in a tendency for the average particle size of the obtained polyurethane resin particles to decrease.

[0083] <Granulation Process>

[0084] In this process, an aqueous dispersion medium and a urethane monomer composition are supplied to a granulation apparatus in a specific ratio to prepare a granulating liquid in which droplets of the urethane monomer composition are dispersed in the aqueous dispersion medium. There are no particular limitations on the method used to supply the aqueous dispersion medium and the urethane monomer composition, and the aqueous dispersion medium and the urethane monomer composition can be supplied separately. Alternatively, the aqueous dispersion medium and the urethane monomer composition can be pre-mixed and then supplied. The droplet size of the urethane monomer composition can be controlled by appropriately adjusting the shear force applied to the granulating liquid. The shear force can be controlled by the type of disperser to be used and operating conditions such as the rotational speed. Increasing the shear force applied to the granulating liquid reduces the droplet size in subsequent granulation processes, resulting in a tendency for the average particle size of the obtained polyurethane resin particles to decrease.

[0085] The granulation process can be a batch system or a cyclic system, and the appropriate choice can be made.

[0086] <Condensation and Desolventizing Processes>

[0087] In this process, the granulation liquid is heated to promote the condensation of the urethane monomer composition and to prepare a dispersion of polyurethane resin particles. In the condensation process of this invention, a standard stirred tank with controllable temperature can be used. The condensation temperature can be constant from start to finish, but it can be increased during the latter half of the polymerization step to obtain the desired molecular weight distribution.

[0088] To further remove impurities, such as unreacted monomers and solvents, the aqueous medium can be partially removed by distillation after condensation. Distillation can be carried out at atmospheric pressure or under reduced pressure.

[0089] (Separation and purification process)

[0090] In this process, polyurethane resin particles are separated and purified from the dispersion of dispersed polyurethane resin particles to prepare the polyurethane resin particles of the present invention. The polyurethane resin particles are separated from the liquid phase using conventional solid-liquid separation methods. In this case, to remove the dispersing stabilizer adhering to the surface of the polyurethane resin particles, the polyurethane resin particle dispersion can be treated with acid, alkali, or another treatment agent.

[0091] The resulting polyurethane resin particles are dried using known drying methods as needed.

[0092] The volume average particle size of the polyurethane resin particles of the present invention is preferably 5.0 μm or more and 50.0 μm or less, more preferably 10.0 μm or more and 50.0 μm or less. When the volume average particle size is within this range, the polyurethane resin particles are easy to process into powder and also easy to disperse, which makes it easier to uniformly impart functionality to the product.

[0093] In order to control the volume average particle size within the above range, an additional procedure can be performed, for example, to classify the particles using an air classifier and remove particles that deviate from the desired particle size distribution as unspecified particles.

[0094] <Measurement Method>

[0095] The method for measuring physical properties according to this disclosure will then be described.

[0096] (Stress when polyurethane resin particles are compressed to 10% of their particle size)

[0097] The stress when polyurethane resin particles are compressed to 10% of their particle size can be calculated from the load-deformation rate curve obtained through indentation testing. Specifically, the "NS-A100" microparticle crushing force measuring device (manufactured by Nano Seeds Corporation) is used. The specific method for measuring the load-deformation rate curve is as follows.

[0098] Measurements were performed in a laboratory environment of 23°C and 50%RH, while the sample stage attached to the temperature control device was maintained at 23.0°C.

[0099] Polyurethane resin particles were applied to the sample stage, and measurements were taken after the sample stage was set to the above temperature and held for more than 10 minutes.

[0100] In the measurement, a flat indenter with a pressure of 0.072 mN / μm attached to the device was used as the indenter.

[0101] Measurements were performed by setting the indentation depth to 40 μm and the indenter movement speed to 0.5 μm / s. The indentation data was set to 3001.

[0102] The particles used for measurement were selected as polyurethane resin particles that existed individually on the screen used for measurement via a microscope attached to the device. However, to minimize the error in displacement, particles with a particle size (D) within the range of volume average particle size (Dv) ± 0.5 μm (Dv - 0.5 μm ≤ D ≤ Dv + 0.5 μm) were selected. The major and minor axes of the polyurethane resin particles were measured using software attached to the device, and the value obtained by [(major axis + minor axis) / 2] was defined as the particle size D (μm) of the measured particle. The volume average particle size (Dv) was measured using a CDA-1000X (manufactured by Sysmex Corporation) via the method described later.

[0103] In the measurement, any 100 polyurethane resin particles with a particle size D (μm) that meets the above requirements are selected and measured.

[0104] The analysis was performed using the "A100 Strain Analysis Graphical Generation Tool" attached to the "NS-A100" microparticle crushing force measuring device. The "Graphic Generation" menu was selected to choose the measurement data, and the load and deformation were output as analysis data. The deformation rate was derived by dividing the obtained deformation by the particle size D (μm) before measurement to obtain a load-deformation rate curve. The load at the point where the deformation rate was 10% was read from the obtained load-deformation rate curve.

[0105] The above measurements and analyses were performed on 100 polyurethane resin particles, and the arithmetic mean was calculated as the stress when the polyurethane resin particles in this invention were compressed to 10% of their particle size.

[0106] The same measurements were performed by controlling the temperature of the sample stage to 10.0℃ and 40.0℃, and the stress of the polyurethane resin particles when compressed by 10% of their particle size at each temperature was calculated.

[0107] (Glass transition temperature of polyurethane resin particles)

[0108] The glass transition temperature (Tg) was measured using a differential scanning calorimeter "Q2000" (manufactured by TA Instruments) according to ASTM D3418-82. Temperature compensation of the device's detection unit was achieved using the melting points of indium and zinc, while heat compensation was achieved using the heat of fusion of indium.

[0109] Specifically, approximately 3 mg of polyurethane resin powder was accurately weighed and placed in an aluminum pan. Using an empty aluminum pan as a reference, the temperature was increased at a rate of 10 °C / min within a measurement temperature range of -80 °C to 200 °C. During the measurement, the temperature was raised to 200 °C, then lowered to -80 °C, and then raised again. The intersection of the differential thermal curve and the line representing the midpoint between the baselines before and after the specific heat change occurring during this second heating process was defined as the glass transition temperature of the polyurethane resin particles.

[0110] (F of polyurethane resin particles) s A, F s B and F s (Measurement of C)

[0111] F of polyurethane resin particles s A is made using hydrogen nuclei 1 The results of pulse NMR measurements using H as the measurement nucleus are calculated as follows.

[0112] Place 1 gram of polyurethane resin powder in a sample tube and perform pulsed NMR measurements using the following equipment and conditions:

[0113] - Equipment: Minispec MQ20 ​​(manufactured by Bruker);

[0114] - Measurement mode: Solid-state echo;

[0115] - Scan: 64;

[0116] - Recycle delay: 1 second;

[0117] -90° pulse length: 2.78 microseconds;

[0118] -180° pulse length: 5.46 microseconds;

[0119] - Acquisition rate: 1.5 to 4 milliseconds (adjusted appropriately based on the measured relaxation curve); and

[0120] -Measured temperature: 23℃.

[0121] The obtained echo intensity curve was automatically fitted to three components using the standard software TDNMR-A. The component with the shortest relaxation time among the three components was defined as component T. 2s A, and the component T in the polyurethane resin particles 2s The component fraction of A is defined as F s A[%].

[0122] When three-component separation is not possible, two-component separation is performed, and the component with the shorter relaxation time is used as component T. 2s Similarly, component fractions F are calculated for A.s A[%].

[0123] The echo intensity curves measured at a temperature of 10°C using the same method were automatically fitted to three components using the standard software TDNMR-A. The component with the shortest relaxation time among the three components was defined as component T. 2s B, and component T 2s The component fraction of B in polyurethane resin particles is defined as F. s B[%].

[0124] Furthermore, the echo intensity curves measured at a temperature of 40°C were automatically fitted to three components using the standard software TDNMR-A. The component with the shortest relaxation time among the three components was then defined as component T. 2s C, and component T 2s The component fraction of C in polyurethane resin particles is defined as F. s C[%].

[0125] (Measurement of volume average particle size of polyurethane resin powder)

[0126] The volume average particle size (Dv) of the polyurethane resin particles was calculated as follows. As the measuring device, a particle counter "CDA-1000X" (manufactured by Sysmex Corporation) equipped with a 100μm pore tube based on the pore resistance method was used. The measurement conditions were set and the measurement data analyzed using the accompanying dedicated software "CDA-1000X" (manufactured by Sysmex Corporation).

[0127] As an aqueous electrolyte solution used in the measurement, for example, "CELLPACK" (manufactured by Sysmex Corporation) can be used.

[0128] The dedicated software is set up as follows before measurement and analysis.

[0129] On the "Measurement Conditions Settings" screen of the dedicated software, the total count is set to 50,000, the number of measurement repetitions is set to 1, and the measurement mode is set to total count (unlimited).

[0130] The specific measurement method is as follows.

[0131] (1) Place approximately 150 mL of electrolyte solution in a dedicated round-bottom glass beaker, place the beaker on the sample stage, and stir with a stirring propeller at 500 rpm. Then, click "Blank Check Measurement" in the dedicated software to start the measurement and verify that the count is less than 500. When the count is above 500, repeat the washing of the beaker and the well.

[0132] (2) Place approximately 30 mL of the electrolyte aqueous solution into a 100 mL flat-bottomed glass beaker. Add approximately 0.3 mL of a diluted solution prepared by diluting the dispersant "Contaminon N" (a 10% by mass aqueous solution of neutral detergent, composed of nonionic surfactants, anionic surfactants and organic detergent builders, with a pH of 7, used for cleaning precision measuring equipment, manufactured by FUJIFILM Wako Pure Chemical Corporation) to approximately three times its mass using ion-exchanged water.

[0133] (3) Prepare an ultrasonic dispersion system “Ultrasonic Dispensing System Tetra150” (manufactured by Nikkaki Bios Co., Ltd.), which has two built-in oscillators with a 180-degree phase difference and an oscillation frequency of 50 kHz, and has an electrical output of 120 W. Place approximately 3.3 L of ion-exchanged water into the water tank of the ultrasonic dispersion system, and add approximately 2 mL of Contaminon N to the water tank.

[0134] (4) Place the beaker from (2) above into the beaker fixing hole of the ultrasonic dispersion device and operate the ultrasonic dispersion device. Adjust the height of the beaker so that the resonance state of the liquid surface of the electrolyte aqueous solution in the beaker reaches its maximum value.

[0135] (5) Approximately 10 mg of polyurethane resin particles were gradually added to the electrolyte aqueous solution in the beaker from step (4) above, while simultaneously being irradiated and dispersed with ultrasound. The ultrasonic treatment was continued for another 60 seconds. During ultrasonic dispersion, the water temperature in the tank was appropriately controlled between 10°C and 40°C.

[0136] (6) Using a pipette, add the electrolyte aqueous solution containing the polyurethane resin particles dispersed in (5) to the round-bottom beaker in (1) set in the sample holder above to adjust the measurement concentration to about 6%. Perform the measurement until the number of particles reaches 50,000.

[0137] (7) Use dedicated software attached to the equipment to analyze the measurement data to calculate the volume average particle size (Dv).

[0138] (Measurement of the average sphericity of polyurethane resin powder)

[0139] The average sphericity of polyurethane resin powder was measured using a flow particle image analyzer “FPIA-3000” (manufactured by Sysmex Corporation) under the measurement and analysis conditions used during the calibration operation.

[0140] The specific measurement method is as follows. First, place approximately 20 mL of pre-removed solid impurities from an ion-exchanged water solution into a glass container. Add approximately 0.2 mL of a diluted solution prepared by diluting the dispersant "ContaminonN" (a 10% by mass aqueous solution of neutral detergent, composed of nonionic surfactants, anionic surfactants, and organic detergent builders, with a pH of 7, used for cleaning precision measuring equipment, manufactured by FUJIFILM Wako Pure Chemical Corporation) to approximately three times its mass. Then, add approximately 0.02 g of the measurement sample and disperse the mixture using an ultrasonic dispersion device for 2 minutes to obtain a dispersion for measurement. In this case, cool appropriately so that the temperature of the dispersion is above 10°C and below 40°C. As an ultrasonic dispersion device, a benchtop ultrasonic cleaner / disperser (e.g., "VS-150" (manufactured by VELVO-CLEAR)) with an oscillation frequency of 50 kHz and an electrical output of 150 W is used. A predetermined amount of ion-exchanged water is placed in the water tank, and approximately 2 mL of ContaminonN is added to the water tank.

[0141] In the measurements, a flow cytometer equipped with an objective lens "UPlanApro" (magnification: 10×, numerical aperture: 0.40) was used, and a particle sheath "PSE-900A" (manufactured by Sysmex Corporation) was used as the sheath fluid. The dispersion prepared according to the above procedure was introduced into the flow cytometer, and 3,000 polyurethane resin particles were measured using both HPF measurement mode and total count mode. The average sphericity of the polyurethane resin particles was determined by limiting the binarization threshold during particle analysis to 85% and restricting the analyzed particle size to a spherical equivalent diameter greater than 1.985 μm and less than 39.69 μm.

[0142] During the measurement, before starting the measurement, the focus is automatically adjusted using standard latex particles (e.g., "RESEARCH AND TEST PARTICLES LatexMicrosphere Suspensions 5200 A" manufactured by Duke Scientific Corporation, diluted with deionized water). Subsequently, focus adjustment is preferably performed every 2 hours after the start of the measurement.

[0143] When the volume average particle size is greater than 40 μm and the average roundness is calculated by the above method, the polyurethane resin powder is observed with a scanning electron microscope, and the projected area S, perimeter L, etc. of the polyurethane resin particles are measured based on the observed image using the image processing software "ImageJ".

[0144] The roundness of each individual polyurethane resin particle is determined using the following expression based on the obtained area S and perimeter L:

[0145] Circularity C = 2 × (π × S) 1 / 2 / L.

[0146] The same procedure was performed on 100 polyurethane resin particles, and the average value was defined as the average roundness.

[0147] (Molecular structure analysis of polyurethane resin)

[0148] Through pyrolysis GC / MS, ATR-IR, 1 H-NMR or 13 C-NMR analysis is used to determine the molecular structure of polyurethane resin in polyurethane resin particles. When the structure cannot be specified by any single analysis, a combination of multiple analyses is used to determine the structure. Typical measurement methods are shown below.

[0149] [Pyrolysis GC / MS]

[0150] - Pyrolysis unit: JPS-700 (Japan Analytical Industry Co., Ltd.);

[0151] - Decomposition temperature: 590℃;

[0152] -GC / MS device: Focus GC / ISQ (Thermo Fisher Scientific Inc.);

[0153] - Column: HP-5MS, length: 60m, inner diameter: 0.25mm, membrane thickness: 0.25μm;

[0154] -Inlet temperature: 200℃;

[0155] - Flow pressure: 100 kPa;

[0156] - Split: 50 mL / min;

[0157] -MS ionization: EI; and

[0158] - Ion source temperature: 200℃, mass range 45-650.

[0159] Mass spectrometry analysis of the components of resin decomposition products generated when the resin is pyrolyzed under the above conditions is used to identify the types of structural compounds.

[0160] [ATR-IR]

[0161] The structure was analyzed under the following conditions using measurements taken with a Fourier transform infrared spectrometer (Spectrum One: manufactured by PerkinElmer, Inc.) equipped with a universal ATR sampling accessory:

[0162] - Infrared light (λ=5μm), incident angle: 45°;

[0163] -ATR crystal: Ge ATR crystal (refractive index = 4.0);

[0164] -scope

[0165] Starting point: 4,000cm -1 ,

[0166] End: 650cm -1 (Ge ATR crystal);

[0167] -duration

[0168] Number of scans: 16

[0169] Resolution: 4.00cm -1 ;and

[0170] - Advanced: With CO2 / H2O correction.

[0171] [ 1 H-NMR]

[0172] - Measuring equipment: FT NMR equipment JNM-EX400 (manufactured by JEOL Ltd.);

[0173] - Measurement frequency: 400 MHz;

[0174] - Pulse condition: 5.0 μs;

[0175] - Frequency range: 10,500 Hz;

[0176] - Cumulative number: 64 times;

[0177] -Measured temperature: 30℃; and

[0178] - Sample: Prepared as follows: Place 50 mg of polyurethane resin powder into a sample tube with an inner diameter of 5 mm, add deuterated chloroform (CDCl3) as a solvent, and dissolve it in a thermostat at 40 °C.

[0179] The results of the analysis 1 H-NMR charts are used for structural analysis of polyurethane resins.

[0180] Structural analysis of polyurethane resins can also be performed through analysis 13 This is done using C-NMR charts.13 C-NMR charts are similarly obtained by using... 13 C is obtained by measuring a measurement core with a single-pulse mode.

[0181] Example

[0182] The invention will now be described in more detail using examples and comparative examples. The invention is not limited to the following examples within its scope. In the following description of the examples, unless otherwise stated, the term "part" is based on mass.

[0183] <<Preparation of Polyurethane Resin Powder 1>>

[0184] <Preparation of Aqueous Medium 1>

[0185] Dispersant Metalose 65SH-50 (a cellulose derivative manufactured by Shin-Etsu Chemical Co., Ltd.) was dissolved in ion-exchanged water to obtain a concentration of 4.0% by mass, thus obtaining aqueous medium 1.

[0186] <Preparation of Carbamate Monomer Composition 1>

[0187] Place the following materials in the plastic container corresponding to the rotation and revolution mixer (ARV-310P, manufactured by THINKY Corporation):

[0188] -Kuraray polyol C-3090 (poly[(3-methyl-1,5-pentanediol:1,6-hexanediol) carbonate], polycarbonate polyol, manufactured by Kuraray Co., Ltd., molecular weight: 3000, OHV=20): 54.1 parts by weight;

[0189] - Sannix NP-300 (propylene oxide modified ethylenediamine, manufactured by Sanyo Chemical, Ltd., OHV=151): 2.9 parts by weight; and

[0190] -Methyl ethyl ketone (MEK): 33.3 parts by weight.

[0191] Mix for 60 seconds at 2000 rpm using a rotation and revolution mixer.

[0192] Then, quickly weigh the following materials in the container:

[0193] -Duranate TKA100 (hexamethylene diisocyanate polyisocyanate (isocyanurate product), manufactured by Asahi Kasei Corporation, NCO%=21.8): 43.0 parts by weight; and

[0194] -TOYO-CAT RX-5 (tertiary amine catalyst, manufactured by Tosoh Corporation): 2,000 ppm (relative to the total amount of isocyanate and polyol).

[0195] The mixture was remixed for 90 seconds at 2000 rpm and 0.2 kPa using a rotation and revolution mixer to obtain urethane monomer composition 1.

[0196] Since the reaction of the urethane monomer composition 1 is carried out even at room temperature, it is arranged so that the time until the subsequent granulation process can begin is as short as possible.

[0197] <Granulation Process>

[0198] In a reaction vessel equipped with a stirrer, 266.7 parts by mass of aqueous medium 1 were weighed, and the temperature was adjusted to 30°C.

[0199] Continue stirring the inside of the reaction vessel at 1,000 rpm with a stirrer, add 133.3 parts by weight of the urethane monomer composition, and continue stirring for 60 minutes to obtain granulated liquid 1.

[0200] <Condensation and Desolventizing Process>

[0201] After the granulation process is completed, the temperature is raised to 70°C while the container holding the granulation liquid 1 is stirred at 200 rpm, and the condensation process continues for 5 hours. In addition, while stirring at 200 rpm, the temperature is raised to 100°C, and the desolventizing process continues for 5 hours to obtain dispersion 1.

[0202] <Separation and Purification Process>

[0203] After the desolventization process is completed, the solid components are filtered from dispersion 1, thoroughly washed with deionized water, and then dried in a vacuum at 30°C for 24 hours to obtain polyurethane resin powder 1 containing polyurethane resin particles.

[0204] The physical properties and compositional analysis results of the obtained polyurethane resin powder 1 are shown in Table 3.

[0205] <<Preparation of Polyurethane Resin Powder 2 to 10>>

[0206] Except for the changes in materials and manufacturing conditions as shown in Tables 1 and 2, polyurethane resin powders 2 to 10 were prepared by the same method used to manufacture polyurethane resin powder 1. The physical properties and compositional analysis results of the resulting polyurethane resin powders 2 to 10 are shown in Table 3.

[0207] [Table 1]

[0208]

[0209] Each symbol in Table 1 represents the following:

[0210] -TPA100: Durnate TPA100 (a polyisocyanate of hexamethylene diisocyanate (isocyanurate esterification product), manufactured by Asahi Kasei Corporation, NCO%=23.1);

[0211] -TMA100: Durnate TMA100 (a polyisocyanate of hexamethylene diisocyanate (isocyanurate esterification product), manufactured by Asahi Kasei Corporation, NCO%=23.2);

[0212] -C-1090: Kuraray polyol C-1090 (poly[(3-methyl-1,5-pentanediol:1,6-hexanediol) carbonate], polycarbonate polyol, manufactured by Kuraray Co., Ltd., molecular weight: 1,000, OHV=112.0);

[0213] -P-6010: Kuraray polyol P-6010 (poly((3-methyl-1,5-pentanediol)-alt-(adipic acid)), polyester polyol, manufactured by Kuraray Co., Ltd., molecular weight: 6,000, OHV=19.7); and

[0214] -TMP: Trimethylolpropane.

[0215] [Table 2]

[0216]

[0217] Each symbol in Table 2 represents the following:

[0218] -90SH-100: Metolose 90SH-100 (a cellulose derivative manufactured by Shin-Etsu Chemical Co., Ltd.).

[0219] <Polyurethane Resin Powder 11>

[0220] Art Pearl C300T, manufactured by Negami Chemical Institute Co., Ltd., was used as polyurethane resin particles 11.

[0221] The physical properties of polyurethane resin powder 11 are shown in Table 3.

[0222] <Polyurethane Resin Powder 12>

[0223] Art Pearl U600T, manufactured by Negami Chemical Institute Co., Ltd., was used as polyurethane resin particles 12.

[0224] The physical properties of polyurethane resin powder 12 are shown in Table 3.

[0225] <Polyurethane Resin Powder 13>

[0226] Art Pearl CE400T, manufactured by Negami Chemical Institute Co., Ltd., was used as polyurethane resin particles 13.

[0227] The physical properties of polyurethane resin powder 13 are shown in Table 3.

[0228] <Polyurethane Resin Powder 14>

[0229] Weigh the following materials in a four-necked separable flask equipped with a 1000 mL jacket:

[0230] - Polyurethane thermoplastic elastomer ("Elastollan" 1180A10, manufactured by BASF Japan Ltd., weight average molecular weight: 130,000, soft segment content: 88%): 17.5g;

[0231] - Polyvinyl alcohol (“Gohseno” GL-05, manufactured by Nippon Synthetic Chemical Industry Co., Ltd., weight average molecular weight: 11,000): 35.0 g; and

[0232] N-methyl-2-pyrrolidone as an organic solvent: 297.5g.

[0233] The temperature of the separable flask was raised to 80°C, and the mixture was stirred at 450 rpm for 2 hours using a spiral ribbon stirrer to form an emulsion. Subsequently, 350 g of ion-exchanged water, acting as a poor solvent, was added dropwise via a liquid transfer pump at a rate of 2.91 g / min. After the complete addition of the ion-exchanged water, the temperature was lowered while stirring to obtain a white dispersion 20. The obtained dispersion 20 was centrifuged at 7500 G for 15 minutes for solid-liquid separation, and then 250 g of ion-exchanged water was added to wash the slurry at 80°C for 30 minutes. Subsequently, the slurry was filtered under reduced pressure, and the slurry washing and filtration under reduced pressure were repeated, with 300 g of ion-exchanged water added to obtain slurry 14. The obtained slurry 14 was lyophilized to obtain polyurethane resin powder 14.

[0234] The physical properties of the obtained polyurethane resin powder 14 are shown in Table 3.

[0235] [Table 3]

[0236]

[0237] Each symbol in Table 3 represents the following:

[0238] -PC: Polycarbonate skeleton; and

[0239] -PES: Polyester skeleton.

[0240] Items marked with "○" are those for which the corresponding structure was detected and compositional analysis was performed; items marked with "-" are those for which the corresponding structure was not detected and compositional analysis was performed; and items marked with a slash are those for which neither physical property measurement nor compositional analysis was performed.

[0241] <Examples 1 to 8 and Comparative Examples 1 to 6>

[0242] Evaluation samples, including the obtained polyurethane resin powders 1 to 14, were prepared as follows and evaluated from the perspectives of environmental dependence and abrasion resistance, as Examples 1 to 8 and Comparative Examples 1 to 6.

[0243] The evaluation results are shown in Table 4.

[0244] (Paint production)

[0245] - Polyurethane resin: 100 parts by weight (CRISVON NY-373, manufactured by DIC);

[0246] - 100 parts by weight for each type of polyurethane resin powder;

[0247] - High molecular weight silicone oil: 2 parts by weight (silicone oil, KP340, manufactured by Shin-Etsu Silicone Co., Ltd.);

[0248] - Fine-grained silica: 12 parts by weight (Nippsil E220, manufactured by Nihon Silica Kogyo KK, average particle size: 1.5 μm); and

[0249] - Solvent: 1,000 parts by weight (IPA / DMF / ethyl acetate mixture).

[0250] The above materials are thoroughly mixed to produce a coating.

[0251] (Evaluation of sample production)

[0252] An olefin-based thermoplastic elastomer (a mixture of PP / PE / EPDM in a 36 / 28 / 36 ratio) was molded into an 800 μm thick sheet as the substrate. A coating was applied to achieve a dry weight of 20 g / m². 2 The amount of product is applied to the surface of the substrate and then dried in a hot air drying oven at 100°C for 3 minutes to produce an evaluation sample.

[0253] <Tactile Impression Evaluation>

[0254] The obtained evaluation samples were left to stand for 24 hours in environments of 15°C and 10%RH, 23°C and 50%RH, and 30°C and 80%RH, and then the tactile sensation and environmental dependence were evaluated:

[0255] A: The hardness difference between 10℃ and 40℃ is less than 0.20, and almost no difference in tactile feel with the environment is detected;

[0256] B: The hardness difference between 10℃ and 40℃ is greater than 0.20 and less than 0.24, and a slight difference in tactile sensation with the environment is sensed;

[0257] C: The hardness difference between 10℃ and 40℃ is greater than 0.25 and less than 0.30, and the difference in tactile sensation with the environment is sensed; and

[0258] D: The difference in hardness between 10℃ and 40℃ is greater than 0.30, and the tactile feel is significantly different.

[0259] <Compressing 10% stress in an environment of 23°C and 50%RH>

[0260] The measured stress under 10% compression in an environment of 23°C and 50%RH was evaluated based on the following evaluation criteria:

[0261] A: Stress above 0.26mN and below 0.38mN;

[0262] B: Stress greater than 0.25 mN and less than 0.26 mN, or stress greater than 0.38 mN and less than 0.50 mN; and

[0263] C: Stress less than 0.25mN or stress greater than 0.50mN.

[0264] <Abrasion Resistance>

[0265] Five layers of gauze (The Japanese Pharmacopoeia) were adhered to the obtained evaluation sample under a certain load, and subjected to a predetermined number of reciprocating rubs at a stroke of 100 mm. The condition of the particles after rubbing was observed using SEM, and the degree of particle degradation was evaluated according to the following criteria:

[0266] A: The changes in particle diameter and aspect ratio are each less than 3.0%;

[0267] B: The changes in particle diameter and aspect ratio are each greater than 3.0% and less than 5.0%; and

[0268] C: The changes in particle diameter and aspect ratio are each greater than 5.0%.

[0269] [Table 4]

[0270]

[0271] This disclosure relates to the following components.

[0272] (Component 1)

[0273] A polyurethane resin powder comprising polyurethane resin particles, wherein

[0274] The polyurethane resin particles comprise polyurethane resin.

[0275] The polyurethane resin powder contains polyurethane resin particles with an average sphericity of 0.950 or higher.

[0276] The polyurethane resin particles, when compressed to 10% of their particle size in an environment of 23°C and 50%RH, exhibit a stress of ≥0.25mN and ≤0.50mN.

[0277] The polyurethane resin particles have a glass transition temperature below 0°C.

[0278] (Component 2)

[0279] According to the polyurethane resin powder constituting 1, wherein

[0280] In pulse NMR measurements of the polyurethane resin particles at a measurement temperature of 23°C,

[0281] When using hydrogen nuclei 1 When H is used as a solid-state echo method to measure the spin-spin relaxation time T2 of the nucleus to determine the echo intensity curve A of the polyurethane resin particles,

[0282] The echo intensity curve A is decomposed into three components using the least squares method.

[0283] The component with the shortest relaxation time among the three components is defined as component T. 2s A, and

[0284] The component T in the polyurethane resin particles 2s The component fraction of A is defined as F s A[%],

[0285] Component fraction F s A is 15 or higher and 90 or lower.

[0286] (Component 3)

[0287] According to the polyurethane resin powder constituting 1 or 2, wherein

[0288] In pulse NMR measurements of the polyurethane resin particles at a measurement temperature of 10°C,

[0289] When using hydrogen nuclei 1 When H is used as a solid-state echo method to measure the spin-spin relaxation time T2 of the nucleus to determine the echo intensity curve B of the polyurethane resin particles,

[0290] The echo intensity curve B is decomposed into three components using the least squares method.

[0291] The component with the shortest relaxation time among the three components is defined as component T. 2s B, and

[0292] The component T in the polyurethane resin particles 2s The component fraction of B is defined as F s B[%]; and

[0293] In pulse NMR measurements of the polyurethane resin particles at a measurement temperature of 40°C,

[0294] When using hydrogen nuclei 1 H is used as a solid-state echo method to measure the spin-spin relaxation time T2 of the nucleus to determine the echo intensity curve C of the polyurethane resin particles.

[0295] The echo intensity curve C is decomposed into three components using the least squares method.

[0296] The component with the shortest relaxation time among the three components is defined as component T.2s C, and

[0297] The component T in the polyurethane resin particles 2s The component fraction of C is defined as F s C[%],

[0298] F s B / F s C is 1.0 or higher and 1.5 or lower.

[0299] (Component 4)

[0300] The polyurethane resin powder according to any one of compositions 1 to 3, wherein the polyurethane resin particles have a volume average particle size of 10.0 μm or more and 50.0 μm or less.

[0301] (Component 5)

[0302] The polyurethane resin powder according to any one of compositions 1 to 4, wherein the polyurethane resin particles have an average sphericity of 0.950 or higher.

[0303] (Composition 6)

[0304] According to any one of the following formulations, the polyurethane resin powder has a partial structure represented by the following formula (1):

[0305] .

[0306] (Component 7)

[0307] The polyurethane resin particles according to any one of compositions 1 to 6, wherein the polyurethane resin is a polymer containing a composition of a polyisocyanate having an isocyanurate structure, a difunctional polyol and a trifunctional or higher polyol.

[0308] (Composition 8)

[0309] According to the polyurethane resin particles of composition 7, wherein the bifunctional polyol is a polycarbonate polyol.

[0310] (Composition 9)

[0311] According to the polyurethane resin particles constituting 7 or 8, wherein the trifunctional or higher polyol is a tetrafunctional or higher polyol.

[0312] (Composition 10)

[0313] According to the polyurethane resin particles of composition 9, wherein the tetrafunctional or higher polyol is ethylenediamine modified with propylene oxide.

[0314] (Composition 11)

[0315] According to any one of the polyurethane resin powders comprising 1 to 10, the stress of the polyurethane resin particles when compressed to 10% of their particle size in an environment of 23°C and 50%RH is 0.26 mN or more and 0.38 mN or less.

[0316] This invention is not limited to the embodiments described above, and various changes and modifications can be made without departing from the spirit and scope of the invention. Therefore, the appended claims are used to define the scope of the invention.

[0317] This application claims the benefit of Japanese Patent Application No. 2024-069696, filed on April 23, 2024, and Japanese Patent Application No. 2024-158662, filed on September 12, 2024, the entire contents of which are incorporated herein by reference.

Claims

1. A polyurethane resin powder comprising polyurethane resin particles, wherein... The polyurethane resin particles comprise polyurethane resin. The polyurethane resin particles, when compressed to 10% of their particle size in an environment of 23°C and 50%RH, exhibit a stress of ≥0.25mN and ≤0.50mN. The glass transition temperature of the polyurethane resin particles is below 0°C.

2. The polyurethane resin powder according to claim 1, wherein... In pulse NMR measurements of the polyurethane resin particles at a measurement temperature of 23°C, When performing the measurement using hydrogen nuclei 1 H as measuring nuclei a solid echo method measuring the spin-spin relaxation time T2 to determine an echo intensity curve A of the polyurethane resin particles, The echo intensity curve A is decomposed into three components using the least squares method. The component with the shortest relaxation time among the three components is defined as component T 2s A, and Fraction T in the polyurethane resin particles 2s Fraction F of A is defined as F s at A [%], Component score F s A is 15 or more and 90 or less.

3. The polyurethane resin powder according to claim 1, wherein... In pulse NMR measurements of the polyurethane resin particles at a measurement temperature of 10°C, When performing the measurement using hydrogen nuclei 1 H as measuring nuclei a solid echo method to measure spin-spin relaxation time T2 is performed to determine an echo intensity curve B of the polyurethane resin particles, The echo intensity curve B is decomposed into three components using the least squares method. The component with the shortest relaxation time among the three components is defined as component T 2s B, and Fraction T in the polyurethane resin particles 2s Fraction F of B is defined as F s at B [%]; and In pulse NMR measurements of the polyurethane resin particles at a measurement temperature of 40°C, When using hydrogen nuclei 1 H is used as a solid-state echo method to measure the spin-spin relaxation time T2 of the nucleus to determine the echo intensity curve C of the polyurethane resin particles. The echo intensity curve C is decomposed into three components using the least squares method. The component with the shortest relaxation time among the three components is defined as component T. 2s C, and The component T in the polyurethane resin particles 2s The component fraction of C is defined as F s When C[%], F s B / F s C is 1.0 or higher and 1.5 or lower.

4. The polyurethane resin powder according to any one of claims 1 to 3, wherein, The volume average particle size of the polyurethane resin particles is greater than 10.0 μm and less than 50.0 μm.

5. The polyurethane resin powder according to any one of claims 1 to 3, wherein the average sphericity of the polyurethane resin particles is 0.950 or higher.

6. The polyurethane resin powder according to any one of claims 1 to 3, wherein... The polyurethane resin has a partial structure represented by the following formula (1): 。 7. The polyurethane resin particles according to claim 1, wherein, The polyurethane resin is a polymer comprising a composition of a polyisocyanate having an isocyanurate structure, a difunctional polyol, and a polyol with or greater than three functionalities.

8. The polyurethane resin particles according to claim 7, wherein the bifunctional polyol is a polycarbonate polyol.

9. The polyurethane resin particles according to claim 7 or 8, wherein the polyol with three or more functions is a polyol with four or more functions.

10. The polyurethane resin particles according to claim 9, wherein the polyol with more than one tetrafunctional function is ethylenediamine modified with propylene oxide.

11. The polyurethane resin powder according to claim 1, wherein, The stress of the polyurethane resin particles when compressed to 10% of their particle size in an environment of 23°C and 50%RH is greater than 0.26mN and less than 0.38mN.

Citation Information

Patent Citations

  • Resin particle for spacer of liquid crystal display panel

    JP2007004142A

  • Polymer fine particle

    JP2018035249A

  • Toner storage container, developing device, process cartridge, and image forming apparatus

    JP2024069696A

  • Game machine

    JP2024158662A