Moisture-curing polyurethane adhesives for engineered wood

By using a polyurethane adhesive composition of high molecular weight polyol and low MDI isocyanate, the problems of insufficient heat resistance and mechanical properties of engineered wood are solved, and high-strength and high-efficiency laminated products are manufactured.

CN123125255APending Publication Date: 2026-11-17ARKEMA FRANCE SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202580028692.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-18
Filing Date
2025-04-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Engineered wood has poor heat resistance and mechanical properties, and is expensive. Existing adhesives are not effective in improving its performance.

Method used

A polyurethane adhesive composition with a specific composition, comprising a prepolymer of high molecular weight polyol and low content of MDI isocyanate, combined with appropriate amounts of curing agent and rheology modifier, is used for the manufacture of laminated products.

Benefits of technology

It significantly improves the heat resistance and wet strength of engineered wood, enhances initial bond strength, and is compatible with high-speed manufacturing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention relates to an adhesive composition. The composition may comprise a prepolymer comprising the reaction product of a first polyol and a polymeric isocyanate. The polyol may have a number average molecular weight of at least about 2000 Daltons. The first polyol may also have a hydroxyl functionality of at least about 2.0. The polymeric isocyanate may have a functionality of at least about 2.8, preferably, optionally, a 4,4'-MDI monomer content of less than about 50 wt%, and optionally a 2,4'-MDI monomer content of less than about 30 wt%. Optionally, the adhesive composition may comprise a curing agent having a second polyol. The second polyol may be the same as or different from the first polyol. For embodiments including a curing agent, the weight ratio of prepolymer to curing agent may include up to about 10:1. Based on the amounts of the polymeric isocyanate, the first polyol, and, when present, the second polyol, the wt% of the polymeric isocyanate in the adhesive composition includes greater than 60%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to adhesive compositions for engineered wood products, laminated articles comprising one or more of the adhesive compositions (particularly laminated articles made of engineered wood), and methods for preparing the laminated articles. Background Technology

[0002] Engineered timber is used in a wide range of applications, from residential construction to commercial buildings and industrial products. Some advantages of engineered timber products include:

[0003] Engineered wood can be sustainable. Furthermore, it reduces waste because it utilizes all parts of the tree, even defective parts or scraps left over from cutting lumber to size can be used in products.

[0004] • Polyurethane-based engineered wood can be made into laminated products with high density and different grain patterns in each layer, resulting in greater strength than conventional wood in the desired direction or configuration.

[0005] • Engineered beams can be made in almost any size, and the beams are not limited by the length of the logs.

[0006] However, engineered wood is generally more expensive than conventional wood. Besides the increased cost, the disadvantages of polyurethane-bonded engineered wood products include, at least, generally less-than-ideal heat resistance, often lower than that of conventional wood. Furthermore, engineered wood products may have poorer mechanical properties.

[0007] It has now been found that engineered wood products containing the following adhesive compositions can overcome the above-mentioned disadvantages. Summary of the Invention

[0008] The embodiments disclosed herein relate to an adhesive composition. The composition may comprise (a) a prepolymer comprising the reaction product of a first polyol and a polymeric isocyanate, the first polyol having a number-average molecular weight of at least about 2000 Daltons and a hydroxyl functionality of at least about 2.0, the polymeric isocyanate having a functionality of at least about 2.8, optionally comprising less than about 50 wt% of the 4,4'-monomer MDI, and optionally comprising less than about 30 wt% of the 2,4'-MDI monomer.

[0009] Optionally, the composition may include a curing agent comprising a second polyol. The second polyol may be the same as or different from the first polyol.

[0010] In a particular embodiment that includes a curing agent, the weight ratio of the prepolymer to the curing agent includes up to about 10:1.

[0011] The embodiments disclosed herein may further include laminated articles. The laminated articles may comprise a first substrate and a second substrate. The adhesive composition described above may be sandwiched between the first substrate and the second substrate.

[0012] The embodiments described herein also include a method for preparing a laminated article. In this embodiment, the adhesive composition described above is applied to at least one of a first substrate and a second substrate. The first substrate and the second substrate are pressed together to form a laminated article, wherein the adhesive composition is sandwiched between the first substrate and the second substrate.

[0013] This invention enables the resolution of the aforementioned needs. In particular, the adhesive compositions according to the invention surprisingly offer one or more of the following advantages: enhanced heat resistance, improved wet strength (initial bond strength), compatibility with high-speed manufacturing processes, and combinations of these advantages. Detailed Implementation

[0014] This invention relates to adhesive compositions. Polyurethane adhesives are one exemplary class of adhesives. Polyurethane adhesives can be one-component or two-component adhesives.

[0015] The adhesive composition (also referred to herein as a "polyurethane adhesive composition") may comprise a prepolymer comprising the reaction product of a first polyol and a polymeric isocyanate. The first polyol may have a number average molecular weight of at least about 2000 Daltons, preferably greater than about 2000 Daltons, preferably at least about 2500 Daltons, preferably at least about 3000 Daltons, more preferably greater than about 3000 Daltons, more preferably at least about 4500 Daltons, more preferably greater than 4500 Daltons, more preferably at least about 6000 Daltons, and even more preferably greater than about 6000 Daltons. Examples of polyols having a number average molecular weight of at least 6000 include Acclaim® 6300, 8200, and 12200, all available from Covestro. The polyol may also have a hydroxyl functionality of at least about 2.0, preferably greater than about 2.5, more preferably greater than about 2.7, even more preferably greater than about 2.8, and further preferably at least about 3.0.

[0016] The polyol is preferably selected from polyether polyols, polyester polyols, and combinations thereof. Useful polyether polyols can be obtained by polymerization of cyclic oxides (e.g., ethylene oxide, propylene oxide, butane oxide, and tetrahydrofuran), or by addition of one or more such oxides to a multifunctional initiator having at least two active hydrogens, said initiator including, for example, water, polyols (e.g., ethylene glycol, propylene glycol, diethylene glycol, cyclohexanediol, glycerol, trimethylolpropane, pentaerythritol and bisphenol A, ethylenediamine, propylenediamine, triethanolamine, and 1,2-propanedithiol). Particularly useful polyether polyols include, for example, polyoxypropylene glycol and triol, poly(ethylene oxide-propylene oxide) glycol and triol obtained by simultaneous or sequential addition of ethylene oxide and propylene oxide to a suitable initiator, and polytetramethylene ether glycol obtained by polymerization of tetrahydrofuran. Preferred examples of polyether polyols include polyalkylene oxides, such as polypropylene oxide, poly(ethylene oxide), and ethylene oxide / propylene oxide copolymers.

[0017] According to another embodiment of this disclosure, the polyester polyol is selected from the group consisting of: polydicarboxylate, polycaprolactone polyol, polycaprolactone, and combinations thereof.

[0018] Useful polyester polyols are prepared from the reaction products of polycarboxylic acids, their anhydrides, their esters, or their halides with a stoichiometric excess of the polyol. Suitable polycarboxylic acids include dicarboxylic acids and tricarboxylic acids, including, for example, aromatic dicarboxylic acids, their anhydrides, and esters (e.g., terephthalic acid, isophthalic acid, dimethyl terephthalate, diethyl terephthalate, phthalic acid, phthalic anhydride, methylhexahydrophthalic acid, methylhexahydrophthalic anhydride, methyltetrahydrophthalic acid, methyltetrahydrophthalic anhydride, hexahydrophthalic acid, hexahydrophthalic anhydride, and tetrahydrophthalic acid). Aliphatic dicarboxylic acids and their anhydrides (e.g., maleic acid, maleic anhydride, succinic acid, succinic anhydride, glutaric acid, glutaric anhydride, adipic acid, hexanoic acid, pimelic acid, octanoic acid, azelaic acid, sebacic acid, chlorogenic acid, 1,2,4-butanetricarboxylic acid, decanedicarboxylic acid, octadecanedicarboxylic acid, dimer acids, dimer fatty acids, trimer fatty acids and fumaric acid), as well as alicyclic dicarboxylic acids (e.g., 1,3-cyclohexanedicarboxylic acid and 1,4-cyclohexanedicarboxylic acid).

[0019] Examples of suitable polyols from which polyester polyols can be derived include aliphatic polyols such as ethylene glycol, propylene glycol (e.g., 1,2-propanediol and 1,3-propanediol), butanediol (e.g., 1,3-butanediol, 1,4-butanediol), pentanediol (e.g., 1,5-pentanediol), 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, neopentanediol, diethylene glycol, triethylene glycol, tetraethylene glycol, and polyethylene glycol. Propylene glycol, polypropylene glycol (e.g., dipropylene glycol and tripropylene glycol), 1,4-cyclohexanediol, 1,4-cyclohexanediol, dimerized glycol, bisphenol A, bisphenol F, hydrogenated bisphenol A, hydrogenated bisphenol F, glycerol, tetramethylene glycol, polytetramethylene glycol, 3-methyl-1,5-pentanediol, 1,9-nonanediol, 2-methyl-1,8-octanediol, trimethylolpropane, glycerol, pentaerythritol, sorbitol, glucose, and combinations thereof.

[0020] Polymeric isocyanates may have a functionality of at least about 2.8, preferably greater than about 2.9, and more preferably at least about 2.95.

[0021] Diphenylmethane diisocyanate is also referred to as MDI in this document. Diphenylmethane diisocyanate (MDI) monomers can exist in the form of a mixture of three isomers (i.e., 4,4'-diphenylmethane diisocyanate (4,4'-MDI), 2,4'-diphenylmethane diisocyanate (2,4'-MDI) and 2,2'-diphenylmethane diisocyanate (2,2'-MDI)).

[0022] The polymeric isocyanate may have a 4,4'-MDI monomer content of less than about 50 wt%, preferably less than about 45 wt%, more preferably less than about 40 wt%, and even more preferably no more than about 35 wt%. The polymeric isocyanate may have a 2,4'-MDI monomer content of less than about 30 wt%, preferably no more than about 25 wt%, more preferably no more than about 20 wt%, even more preferably no more than about 15 wt%, further preferably no more than about 10 wt%, and most preferably no more than about 7 wt%. The MDI ring number distribution of the polymeric isocyanate can be determined by GPC. The ratio of isomers (2,4'-MDI and 4,4'-MDI) in the residual / free bicyclic MDI of the polymeric isocyanate can be determined by LC-QQQ.

[0023] The weight ratio of 4,4'-MDI monomer content to 2,4'-MDI monomer content in the polymeric isocyanate may optionally include greater than about 1:1. Preferred weight ratios may include at least about 5:1, at least about 7:1, at least about 10:1, at least about 15:1, at least about 19:1, and at least about 20:1.

[0024] The total amount of 4,4'-MDI monomer and 2,4'-MDI monomer contained in the polymeric polyisocyanate may optionally include less than about 20 wt%, preferably less than about 10 wt%, more preferably less than about 5 wt%, even more preferably less than about 2 wt%, further preferably less than about 1 wt%, and even more preferably less than about 0.5 wt%.

[0025] In one embodiment, the polymeric isocyanate may have an NCO content of about 10 wt% to about 35 wt% and a viscosity of about 50 mPa·s to about 1000 mPa·s. Alternatively or in combination with the NCO content and viscosity, the polymeric isocyanate may have a 4,4'-MDI monomer content of no more than 65 wt%.

[0026] According to another embodiment of this disclosure, the polymeric isocyanate is selected from the group consisting of polymeric diphenylmethane diisocyanate, polymeric toluene diisocyanate, polymeric tetramethylxylene diisocyanate, and combinations thereof. Advantageously, the polymeric isocyanate comprises or is polymeric diphenylmethane diisocyanate. The prepolymer (part i) may contain other components typically present in the prepolymer portion of a two-component solvent-free binder, such as polymeric isocyanate.

[0027] Polymer isocyanates that can be used in this invention include commercially available polymeric isocyanates such as MONDURMR-5, MONDUR MR Light, MONDUR MRS, MONDUR 448, MONDUR 489 (available from Covestro), and combinations thereof.

[0028] According to another embodiment of this disclosure, the polymeric isocyanate is present in an amount of about 20 wt% to about 30 wt%, or about 30 wt% to about 40 wt%, or about 40 wt% to about 50 wt%, or about 50 wt% to about 60 wt%, or about 60 wt% to about 70 wt%, or about 70 wt% to about 80 wt%, or about 80 wt% to about 90 wt% of the total weight of the prepolymer of the composition.

[0029] Another embodiment of this disclosure includes a polymeric isocyanate containing less than about 10 wt% TDI (toluene diisocyanate). In a particular embodiment, the polymeric isocyanate may contain no more than about 1 wt% TDI, preferably no more than trace amounts, more preferably less than detectable amounts of TDI, and most preferably free of TDI.

[0030] In this text, the term “not greater than trace amounts” preferably refers to amounts of up to 0.02 wt%, such as up to 0.01 wt%, or substantially 0 wt%.

[0031] Optionally, the polymeric isocyanate may contain less than about 10 wt% of aliphatic isocyanate (“AC”). In a particular embodiment, the polymeric isocyanate may contain no more than about 1 wt% of AC, preferably no more than trace amounts, more preferably less than detectable amounts of AC, and most preferably no AC.

[0032] Similarly, in another optional aspect, the polymeric isocyanate contains less than about 10 wt% of HDI (hexamethylene diisocyanate) trimer. In a particular embodiment, the polymeric isocyanate may contain no more than about 1 wt% of HDI trimer, preferably no more than trace amounts, more preferably less than detectable amounts of HDI trimer, and most preferably no HDI trimer.

[0033] The adhesive composition, preferably the prepolymer, may further comprise a second polymeric isocyanate. The second polymeric isocyanate may have a functionality of at least about 2.7, and preferably, the 4,4'-MDI monomer content may include less than about 45%.

[0034] In certain embodiments, the weight ratio of the polymeric polyisocyanate to the second polymeric polyisocyanate may include about 1:6 to about 6:1, preferably about 1:5 to about 5:1, more preferably about 4:1 to about 1:4, and even more preferably about 1:3 to about 3:1. Even more preferably, the weight ratio of the polymeric polyisocyanate to the second polymeric polyisocyanate is less than about 2:1 to about 1:2, and even more preferably about 1:1.

[0035] In another specific embodiment, the combined NCO functionality of the polymeric polyisocyanate and the second polymeric polyisocyanate includes at least about 2.7, preferably at least about 2.75.

[0036] The above disclosure regarding polymeric isocyanates applies to second polymeric isocyanates, and is incorporated herein by reference for second polymeric isocyanates as if fully rewritten herein.

[0037] The adhesive composition may optionally contain a curing agent. The curing agent may contain a second polyol. The second polyol may be the same as or different from the first polyol. In one particular embodiment, the second polyol is different from the first polyol.

[0038] The above description of the first polyol also applies to the second polyol, and the second polyol is incorporated herein by reference, which is considered as a complete rewrite in this document.

[0039] For embodiments that include a curing agent, the weight ratio of the prepolymer to the curing agent may include up to about 10:1, preferably up to about 5:1, more preferably up to about 4:1, more preferably not less than about 1:1, and more preferably not less than about 1.5:1 (such as about 1:1 to about 10:1, or about 1.5:1 to about 10:1, or about 1:1 to about 5:1, or about 1.5:1 to about 5:1, or about 1:1 to about 4:1, or about 1.5:1 to about 4:1).

[0040] The adhesive composition may further comprise up to about 10 wt%, preferably up to about 7 wt%, more preferably up to about 5 wt%, more preferably up to about 4 wt%, even more preferably up to about 3 wt%, even more preferably up to about 2 wt%, and most preferably up to about 1 wt% of a desiccant. A particularly preferred type of desiccant is a molecular sieve. In a preferred embodiment, the desiccant is in the prepolymer.

[0041] The adhesive composition may further contain a rheology modifier (particularly fumed silica), preferably in an amount of 0.5 wt% to 5 wt%, more preferably 0.5 wt% to less than 3 wt%, and typically about 1 wt%, based on the total weight of the adhesive composition.

[0042] The adhesive composition may also contain an amine compound, preferably in the curing agent. Examples of amines may be polyaspartic esters. Suitable types of polyaspartic esters may be monofunctional, difunctional, or trifunctional, such as amines, diamines, or triamines.

[0043] In a particular embodiment, the polyurethane adhesive composition may have a molar ratio of NCO to OH of at least about 7:1, preferably at least about 10:1, more preferably at least about 11:1, more preferably at least about 12:1, more preferably at least about 13:1, more preferably at least about 14:1, more preferably at least about 15:1, and even more preferably not greater than about 19:1 (e.g., about 7:1 to about 19:1, preferably about 10:1 to about 19:1, more preferably about 11:1 to about 19:1, more preferably about 12:1 to about 19:1, more preferably about 13:1 to about 19:1, more preferably about 14:1 to about 19:1, and even more preferably about 15:1 to about 19:1).

[0044] In a particular embodiment, the polyurethane adhesive composition has a weight ratio of polyol to polymeric polyisocyanate of preferably not less than about 1:1.2, more preferably not less than about 1:1.5, and most preferably up to about 1:2.5 (such as about 1:1.2 to about 1:2.5, preferably about 1:1.5 to about 1:2.5).

[0045] Based on the amounts of polymeric isocyanate, the first polyol, and the second polyol (if present), the amount of polymeric isocyanate in the adhesive composition is preferably greater than 60 wt%, more preferably at least about 65 wt%, more preferably greater than about 65 wt%, further preferably not greater than about 80 wt%, even more preferably not greater than about 75 wt%, even more preferably less than about 75 wt% (such as greater than 60 wt% to not greater than about 80 wt%, preferably about 65 wt% to about 75 wt%, more preferably greater than about 65 wt% to less than 75 wt%).

[0046] In embodiments that include a curing agent, the adhesive composition comprises a polyisocyanate isocyanate content of at least about 65 wt%, preferably less than about 75 wt%, of polymeric isocyanate (particularly, from about 65 wt% to less than about 75 wt%).

[0047] The reaction of the first polyol with the polymeric isocyanate can be carried out using a catalyst. The catalyst can be used in an amount of 0.01 wt% to 10 wt%, preferably 0.01 wt% to 3 wt%, particularly 0.05 wt% to 1.0 wt%, based on the total weight of the binder composition.

[0048] This disclosure also includes embodiments of laminated articles. The laminated articles comprise a first substrate and a second substrate, and an adhesive composition sandwiched between the first substrate and the second substrate. The adhesive composition may comprise any of the adhesive compositions described above.

[0049] At least one of the first substrate and the second substrate may contain a wood substrate, preferably both the first substrate and the second substrate contain wood substrates (the wood substrates of the first substrate and the second substrate are also referred to as the first wood substrate and the second wood substrate, respectively, in this text). In addition, the wood substrate may contain engineered wood, preferably both the first wood substrate and the second wood substrate contain engineered wood.

[0050] Examples of engineered timber may include any of the following: wood I-joists, glulam beams, structural finger joints, cross-laminated timber (CLT) or laminated veneer lumber (LVL), medium-density fiberboard (MDF), oriented strand board (OSB), plywood, and laminated veneer lumber (LSL).

[0051] In a particular embodiment of the wood-based substrate, at least one of the first substrate and the second substrate may comprise a substrate formed from at least one of compressed sawdust, oriented strand board, and combinations thereof.

[0052] Embodiments of the laminated article may include a primer applied to at least one of a first substrate or a second substrate, the primer being positioned between either the first or second substrate and an adhesive composition. In another specific embodiment, the primer may be applied to both the first and second substrates. A first amount of primer is disposed between the adhesive composition and the first substrate, and a second amount of primer is disposed between the second substrate and the adhesive composition. The first and second amounts of primer may be the same or different. In a specific embodiment, the amount of primer is sufficient to facilitate adhesion between the adhesive and one of the substrates. In a specific embodiment, the weight ratio of the adhesive composition to the primer comprises at least about 2:1, preferably no more than about 20:1 (e.g., about 2:1 to about 20:1).

[0053] In a particular embodiment, when measured according to ASTM D 7247, the laminate exhibits a retention strength of more than about 25%, preferably at least about 30%, more preferably at least about 35%, and even more preferably at least about 40%.

[0054] In other embodiments, the laminated product may pass ICC acceptance standard 14 (“AC14”).

[0055] In another embodiment disclosed herein, the laminated article has an initial strength (wet strength) of at least 150 psi.

[0056] In another specific embodiment, the laminated article can have a tensile strength of at least about 5,333 psi at an ambient temperature (preferably 20-25°C) for less than about 100 minutes, preferably not less than about 60 minutes (e.g., about 60 to at least 100 minutes).

[0057] In another embodiment, the laminated article has a tensile strength of at least about 4000 psi, preferably at least about 4500 psi, more preferably at least about 5000 psi, and even more preferably about 5333 psi. It is typically tested under ambient conditions.

[0058] In another embodiment, the laminate retains more than about 20%, preferably more than about 25%, and more preferably at least about 30% of its strength after exposure to test conditions according to ASTM 7247.

[0059] Unless otherwise stated, all standards mentioned throughout this application are effective as of the date of filing of this application.

[0060] As for "approximately X", it refers to the value of X plus or minus 10%.

[0061] In the context of this invention, the range of values ​​should be understood to include extreme values. For example, the range "0% to 25%" specifically includes the values ​​0% and 25%.

[0062] All the embodiments described above can be combined with each other. In particular, the various components of the composition described above, and especially the preferred embodiments, can be combined with each other.

[0063] The following examples illustrate the present invention but do not limit it.

[0064] Example

[0065] The engineered wood products industry has long used ASTM D7247 to evaluate the performance of adhesives at elevated temperatures. This article uses a slightly modified version of that standard test to evaluate the thermal properties of different samples. The wood used to prepare the test specimens had an annual ring orientation of 45 to 90°, was defect-free, and had a moisture content of 10 to 12% before bonding. Each shear specimen was prepared and cut according to ASTM D905.

[0066] In the modified D7247 test, shear blocks cut from the same ply blank were paired. For each pair, one block was tested for shear strength at ambient temperature, while the other was heated at 428°F for 2 hours and then immediately subjected to a fracture test. The ratio of the strength of the heated sample to the ambient strength of the corresponding pair was considered the percentage of strength retention, and the higher this value, the better the heat resistance. The percentage of wood failure of the shear blocks tested at elevated temperatures is another indicator of heat resistance; the higher the percentage of wood failure, the better the heat resistance. For comparison, shear blocks cut from the wood used for the ply were also tested, and their percentage of strength retention values ​​indicated how much strength the wood itself retained after exposure to 428°F for 2 hours.

[0067] Comparative Examples 1-5 and Test Example AE

[0068] Table 1 Comparative Examples

[0069]

[0070] Table 2 Embodiments of the Invention

[0071]

[0072] Table 2A Properties of Polymerized Isocyanates

[0073]

[0074] To determine the 4,4'-MDI and 2,4'-MDI monomer contents in polymeric isocyanates, polymeric isocyanate samples were analyzed by GPC (oligopore column, set at 35°C, THF mobile phase, flow rate 1 mL / min) to determine the MDI ring number distribution of polymeric isocyanates (PMDI). The ratio of isomers (2,4'-MDI and 4,4'-MDI) in the residual / free two-ring MDI in the submitted samples was determined by LC-QQQ (triple quadrupole LC / MS system operated in SRM / MRM mode). Two preparations of the samples were derivatized to form diethylcarbamate of unreacted MDI for analysis.

[0075] Table 3. Improved ASTM D 7247 test results

[0076]

[0077] The embodiments of the present invention exhibit significantly better heat resistance than these comparative embodiments, as indicated by a much higher percentage of retained strength and a much higher percentage of wood failure.

[0078] aspect

[0079] In addition to the claimed subject matter, summary of invention, and detailed description, the disclosed subject matter also includes the following aspects. Preferably, the adhesive composition disclosed herein can be a one-component or two-component polyurethane adhesive.

[0080] The first aspect includes an adhesive composition, preferably a polyurethane adhesive composition. The adhesive composition may comprise a prepolymer comprising the reaction product of a first polyol and a polymeric isocyanate. The polyol may have a number average molecular weight of at least about 2000 Daltons, preferably greater than about 3000 Daltons, more preferably greater than 4500 Daltons, and even more preferably greater than about 6000 Daltons. The first polyol may also have a hydroxyl functionality of at least about 2.0, preferably greater than about 2.5, preferably greater than about 2.7, even more preferably greater than about 2.8, and further preferably at least about 3.0.

[0081] The polymeric isocyanate may have a functionality of at least about 2.8, preferably greater than about 2.9, and more preferably at least about 2.95. The polymeric isocyanate may also have a 4,4'-MDI monomer content of less than about 50 wt%, preferably less than about 45 wt%, more preferably less than about 40 wt%, and even more preferably no more than about 35 wt%. The polymeric isocyanate may further have a 2,4'-MDI monomer content of less than about 30 wt%, preferably no more than about 25 wt%, more preferably no more than about 20 wt%, even more preferably no more than about 15 wt%, more preferably no more than about 10 wt%, and most preferably no more than about 7 wt%. Optionally, the total wt% of the 4,4'-MDI monomer content and the 2,4'-MDI monomer content contained in the polymeric polyisocyanate includes less than about 20 wt%, preferably less than about 10 wt%, more preferably less than about 5 wt%, even more preferably less than about 2 wt%, further preferably less than about 1 wt%, and even more preferably less than about 0.5 wt%.

[0082] Optionally, the adhesive composition may include a curing agent comprising a second polyol. The second polyol may be the same as or different from the first polyol.

[0083] For embodiments that include a curing agent, the weight ratio of the prepolymer to the curing agent may include up to about 10:1, preferably up to about 5:1, and more preferably not less than about 1:1.

[0084] Based on the amount of polymeric isocyanate, the first polyol, and, when present, the second polyol, the wt% of polymeric isocyanate in the adhesive composition may include greater than 60%, preferably at least about 65%, more preferably greater than 65%, further preferably not greater than about 80%, even more preferably not greater than about 75%, and even more preferably less than 75%.

[0085] In the second aspect (which may be applied to the first aspect), the adhesive composition may have a molar ratio of NCO to OH of at least about 10:1, preferably at least about 11:1, more preferably at least about 12:1, more preferably at least about 13:1, more preferably at least about 14:1, more preferably at least about 15:1, and even more preferably up to about 19:1.

[0086] In the third aspect (which may be applied to the adhesive composition of any of the foregoing aspects), the adhesive composition further comprises up to about 5 wt%, preferably up to about 4 wt%, even more preferably up to about 3 wt%, even more preferably up to about 2 wt%, and most preferably up to about 1 wt% of molecular sieve.

[0087] In the fourth aspect (which may apply to any of the aforementioned aspects), the second polyol differs from the first polyol.

[0088] In the fifth aspect (which may be applied to any of the foregoing aspects), the isocyanate content of the adhesive composition includes at least about 65% polymeric isocyanate.

[0089] The sixth aspect may be applied to any of aspects 1 to 5, wherein the adhesive composition further comprises (c) a second polymeric isocyanate, and the functionality of the second polymeric isocyanate comprises at least about 2.7.

[0090] The seventh aspect applies to aspect 6, wherein the content of the 4,4'-MDI monomer in the second polymeric isocyanate is less than about 45%.

[0091] The eighth aspect may be applied to aspect 6 or 7, wherein the adhesive composition has a weight ratio of a polymeric polyisocyanate to a second polymeric polyisocyanate comprising about 1:6 to about 6:1, preferably about 1:5 to about 5:1, more preferably about 4:1 to about 1:4, and even more preferably about 1:3 to about 3:1.

[0092] In the ninth aspect (which may be applied to any of aspects 6, 7 or 8), the combined NCO functionality of the polymeric polyisocyanate and the second polymeric polyisocyanate comprises at least about 2.7, preferably at least about 2.75.

[0093] In the tenth aspect (which may be applied to any of the foregoing aspects), the weight ratio of polyol to polymeric polyisocyanate includes not less than about 1:1.2, preferably not less than about 1:1.5, more preferably not less than about 1:2.0, and even more preferably up to about 1:2.5.

[0094] In the eleventh aspect (which may be applied to any of the foregoing aspects), the adhesive composition further comprises a desiccant.

[0095] In the twelfth aspect (which may be applied to any of the foregoing aspects), the adhesive composition comprises a one-component polyurethane adhesive.

[0096] The thirteenth aspect includes a laminated article comprising a first substrate and a second substrate, and an adhesive composition sandwiched between the first substrate and the second substrate. The adhesive composition comprises an adhesive composition from any of the preceding aspects.

[0097] In the fourteenth aspect, the laminated article of aspect 13 may further include a residual amount of primer on at least one of the first substrate or the second substrate, the primer being located between the first substrate and the second substrate and the adhesive composition.

[0098] The fifteenth aspect includes the laminated article of aspect 13, wherein the weight ratio of the adhesive composition to the primer comprises at least about 2:1, preferably not more than about 20:1.

[0099] The sixteenth aspect applies to any one of aspects 13 to 15, wherein at least one of the first substrate and the second substrate comprises a wood substrate, preferably wherein both the first substrate and the second substrate comprise a wood substrate.

[0100] The seventeenth aspect is applicable to laminates of aspect 16, wherein the wood substrate comprises engineered wood, preferably both the first wood substrate and the second wood substrate comprise engineered wood.

[0101] The eighteenth aspect applies to any one of aspects 13 to 17 above, wherein at least one of the first substrate and the second substrate comprises a substrate formed of at least one of compressed sawdust, oriented strand board, and combinations thereof.

[0102] The nineteenth aspect may be applied to any of aspects 13 to 18 above, wherein when measured according to ASTM D 7247, the laminate exhibits a retention strength of more than about 25%, preferably at least about 30%, more preferably at least about 35%, and even more preferably at least about 40%.

[0103] The twentieth aspect may apply to any of aspects 13 to 19, wherein the laminated articles pass ICC acceptance standard 14 (“AC14”).

[0104] In aspect 21, laminated articles of any of aspects 13-20 may have an initial strength (wet strength) of at least 150 psi.

[0105] In aspect 22, the laminated article of any of aspects 13-21 achieves a strength of at least about 5000 psi, preferably at least about 5300 psi, at ambient temperature for less than about 100 minutes.

[0106] In aspect 23 (which may apply to aspect 22), time includes not less than 60 minutes.

[0107] In aspect 24 (which may apply to aspects 13-23), the laminated article retains more than about 20%, preferably more than about 25%, and more preferably at least about 30% of its strength after exposure to test conditions according to ASTM 7247.

[0108] The twenty-fifth aspect includes a method for preparing a laminated article, the method comprising the step of applying an adhesive composition from any of aspects 1 to 12 to at least one of a first substrate and a second substrate. The method further comprises adhering the first substrate to the second substrate, wherein the adhesive composition is disposed between the first substrate and the second substrate.

[0109] The twenty-seventh aspect may be applied to aspects 25 or 26, further comprising applying a primer to at least one of the first substrate or the second substrate.

[0110] The 28th aspect may be applied to any of aspects 25-27, wherein the failure rate of the method includes no more than about 15%, preferably no more than about 10%, more preferably no more than about 5%, and most preferably less than about 1%.

Claims

1. An adhesive composition comprising (a) a prepolymer and (b) optionally a curing agent, said prepolymer comprising i. a reaction product of a first polyol and ii. a polymeric isocyanate, The first polyol has a number average molecular weight of at least about 2000 Daltons, preferably greater than about 3000 Daltons, more preferably greater than about 4500 Daltons, and even more preferably greater than about 6000 Daltons, and a hydroxyl functionality of at least about 2.0, preferably greater than about 2.5, more preferably greater than about 2.7, even more preferably greater than about 2.8, and even more preferably at least about 3.

0. The polymeric isocyanate a. It has a functionality of at least about 2.8, preferably greater than about 2.9, and more preferably at least about 2.

95. b. Optionally, the 4,4'-MDI monomer content includes less than about 50 wt%, preferably less than about 45 wt%, more preferably less than about 40 wt%, and even more preferably no more than about 35 wt%. c. Optionally, the 2,4'-MDI monomer content includes less than about 30 wt%, preferably no more than about 25 wt%, more preferably no more than about 20 wt%, even more preferably no more than about 15 wt%, further preferably no more than about 10 wt%, and most preferably no more than about 7 wt%. d. Optionally, the weight ratio of the 4,4'-MDI monomer content to the 2,4'-MDI monomer content includes a ratio greater than about 1:1, such as at least about 5:1, preferably at least about 7:1, more preferably at least about 10:1, even more preferably at least about 15:1, further preferably at least about 19:1, and even more preferably at least about 20:

1. e. Optionally, the total wt% content of the 4,4'-MDI monomer and the 2,4'-MDI monomer contained in the polymeric polyisocyanate comprises less than about 20 wt%, preferably less than about 10 wt%, more preferably less than about 5 wt%, even more preferably less than about 2 wt%, further preferably less than about 1 wt%, and even more preferably less than about 0.5 wt%. The curing agent comprises a second polyol, wherein the second polyol may be the same as or different from the first polyol. in, When the curing agent is present, the weight ratio of the prepolymer to the curing agent includes at most about 10:1, preferably at most about 5:1, more preferably at most about 4:1, and more preferably not less than about 1.5:

1. Wherein, based on the amount of the polymeric isocyanate, the first polyol and the second polyol when present, the wt% of the polymeric isocyanate in the adhesive composition includes greater than 60%, preferably at least about 65%, more preferably greater than 65%, further preferably not greater than about 80%, even more preferably not greater than about 75%, even more preferably less than 75%.

2. The adhesive composition according to claim 1, wherein the molar ratio of NCO to OH comprises at least about 7:1, preferably at least about 10:1, more preferably at least about 15:1 and even more preferably at most about 19:

1.

3. The adhesive composition according to any one of the preceding claims further comprises up to about 10 wt%, preferably up to about 7 wt%, even more preferably up to about 5 wt%, further preferably up to about 4 wt%, and most preferably up to about 2 wt% of molecular sieve.

4. The adhesive composition according to any one of the preceding claims, wherein the second polyol is different from the first polyol.

5. The adhesive composition according to any one of the preceding claims, wherein the polymeric isocyanate constitutes at least about 65 wt% of the adhesive composition.

6. The adhesive composition according to any one of the preceding claims, further comprising (iii) a second polymeric isocyanate, wherein the functionality of the second polymeric isocyanate comprises at least about 2.

7.

7. The adhesive composition of claim 6, wherein the 4,4'-MDI monomer content of the second polymeric isocyanate comprises less than about 45%.

8. The adhesive composition according to any one of claims 6 or 7, wherein the weight ratio of the polymeric polyisocyanate to the second polymeric polyisocyanate comprises about 1:6 to about 6:1, preferably about 1:5 to about 5:1, more preferably about 1:4 to about 4:1, more preferably about 1:3 to about 3:1, and even more preferably about 1:2 to less than about 2:1, and even more preferably about 1:

1.

9. A laminated article comprising a first substrate and a second substrate, and a composition sandwiched between the first substrate and the second substrate, wherein the composition comprises an adhesive composition according to any one of the preceding claims and an optional primer.

10. The laminated article according to claim 9, wherein the weight ratio of the adhesive composition to the primer comprises at least about 2:1, preferably not more than about 20:

1.

11. The laminated article according to any one of claims 9 or 10, wherein at least one of the first substrate and the second substrate comprises a wood substrate, preferably wherein both the first substrate and the second substrate comprise a wood substrate.

12. The laminated article according to claim 11, wherein the wood substrate comprises engineered wood, preferably both the first substrate and the second substrate comprise wood substrates containing engineered wood.

13. The laminated article according to any one of claims 9 to 12, wherein at least one of the first substrate and the second substrate comprises a substrate formed of at least one of compressed sawdust, oriented strand board, and combinations thereof.

14. The laminated article according to any one of claims 9 to 13, wherein, when measured according to ASTM D 7247, the laminated article exhibits a retention strength of more than about 25%, preferably at least about 30%, more preferably at least about 35%, and even more preferably at least about 40%.

15. The laminated article according to any one of claims 9 to 14, wherein the laminated article passes ICC Acceptance Standard 14 ("AC14").