Optical products with high refractive index abrasion-resistant and / or scratch-resistant coatings that are low in sensitivity to environmental conditions.
By using a combination of TiO2 and SnO2 colloidal particles with epoxy silanes and organosilanes, the problems of cracking, peeling and water sensitivity of organic optical products under UV and humidity are solved, providing a highly durable and protective coating.
Patent Information
- Application Number
- CN202580028349.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-19
- Filing Date
- 2025-04-18
- Publication Date
- 2026-11-17
AI Technical Summary
Existing transparent organic optical products are prone to cracking, peeling and water sensitivity under humidity and UV exposure, and traditional hard coatings cannot effectively protect the substrate from the effects of UV light.
A composition containing two high-refractive-index colloids and two organosilanes is used. TiO2 and SnO2 colloidal particles are used as a hard coating, combined with epoxy compounds and silane compounds to form a wear-resistant, scratch-resistant and low-water-sensitivity coating. The water sensitivity of the coating is reduced by controlling the ratio of TiO2 and SnO2 and using a small amount of organic silane groups.
It achieves high durability, low risk of peeling and low water sensitivity of the coating under UV and humidity conditions, while maintaining transparency and good adhesion to the substrate and protecting the substrate from the effects of UV light.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
[0001] This invention relates to curable compositions for preparing transparent abrasion-resistant and / or scratch-resistant coatings, articles coated thereon exhibiting abrasion-resistant and / or scratch-resistant properties, particularly optical lenses and ophthalmic lenses for eyeglasses, and methods for preparing such articles.
[0002] Optical products made of transparent organic materials or plexiglass (which is lighter than mineral glass) are now widely used. However, compared to traditional mineral optical products, organic optical products are more sensitive to scratches and abrasion.
[0003] Typically, the method to increase the abrasion resistance and / or scratch resistance of optical products is to apply a hard coating to their surface. Hard coatings used to protect the surface of plexiglass are typically of the poly(meth)acrylic acid type or based on silane hydrolysis products.
[0004] Application EP 0614957 describes a composition comprising, in a solvent medium, a hydrolysis product of a silane having an epoxy moiety and three alkoxy moieties directly bonded to silicon atoms, a hydrolysis product of a silane having two non-reactive groups bonded to silicon atoms via Si-C bonds and two hydrolyzable moieties directly bonded to silicon atoms, colloidal silica, and an aluminum compound catalyst. However, this hard coating does not provide the substrate with protection against UV light.
[0005] US 6808812 describes a composition for use in abrasion-resistant or scratch-resistant coatings, the composition comprising the reaction product of oxalic acid with an organometallic derivative (preferably a titanate, such as tetraisopropyl titanate), an epoxyalkoxysilane (such as γ-glycidoxypropyltrimethoxysilane (GLYMO)), and optionally a second alkoxysilane (such as dimethyldiethoxysilane (DMDES)).
[0006] JP S59-115366 discloses an optical lens having a cured film made from a mixture of: an epoxyalkoxysilane or a partially hydrolyzed product thereof, a silicon compound or a partially hydrolyzed product thereof (such as tetramethoxysilane or methyltrimethoxysilane), fine inorganic particles with a particle size of 200 nanometers or smaller and a refractive index of 1.6 or larger (such as TiO2 or Al2O3), a metal catalyst and / or a crosslinking agent (such as SnCl2), and optional monomers or polymers (such as epoxy-containing compounds, acrylic-containing compounds, styrene-containing compounds, or melamine-containing compounds). The cured film provides improved properties such as surface hardness, abrasion resistance, chemical resistance, corrosion resistance, and weather resistance.
[0007] Hard coatings containing TiO2 colloidal particles provide protection against UV degradation for photosensitive substrates. However, problems have been observed when titanium dioxide is used as the metal oxide in the hard coating. This phenomenon is known as photoactivation. Titanium dioxide is activated upon receiving light energy (ultraviolet light) and tends to decompose organic substances, such as organosilanes or dyes, contained in the hard coating composition due to its strong oxidizing ability to induce cracks in the coating.
[0008] Furthermore, it is believed that cracks allow water to penetrate into the coating, making it more sensitive to moisture. Hard coatings with insufficient water resistance undergo delamination, thereby reducing the durability of the coating.
[0009] Replacing titanium dioxide with another high-refractive-index material (such as SnO2 or ZrO2) that has no (or low) photocatalytic activity is unsatisfactory. While it reduces the occurrence of cracks, it also eliminates the protection of the substrate from UV light, leading to yellowing or peeling problems after UV exposure.
[0010] Therefore, it is necessary to improve the reliability of abrasion-resistant and / or scratch-resistant coatings under certain humidity and UV exposure conditions.
[0011] Therefore, the object of the present invention is to provide a transparent optical article, particularly an ophthalmic lens, comprising a mineral or plexiglass substrate and a coating thereon that provides scratch resistance and / or abrasion resistance, the coating having high durability, low tendency to form cracks, reduced risk of peeling, low water sensitivity, while still protecting the substrate from UV light and maintaining other properties such as transparency, low haze, and good adhesion to other layers formed on the substrate, which are required for optical applications.
[0012] Another object of the present invention is to provide a method for manufacturing such optical articles, which can be easily integrated into the usual production process of optical articles.
[0013] The inventors discovered that a combination of two high-refractive-index colloids and two organosilanes provides a hard coating that is abrasion-resistant, weather-resistant, and protects UV-sensitive optical substrates. Interestingly, these improvements did not produce significant negative effects on the light diffusion, adhesion, abrasion resistance, and scratch resistance of the hard coating.
[0014] To address the needs of this invention and to overcome the aforementioned shortcomings of the prior art, the applicant provides a curable composition for abrasion-resistant and / or scratch-resistant coatings, the curable composition comprising:
[0015] (a) At least one epoxy compound and / or its hydrolysis product carrying at least one silicon atom, wherein the silicon atom has at least one hydrolyzable group directly attached to the silicon atom and at least one group containing an epoxy functional group attached to the silicon atom via a carbon atom.
[0016] (b) At least one silane compound having formula (II) and / or its hydrolysis product:
[0017]
[0018] Z 1 and Z 2 Independently representing a hydrolyzable group or hydrogen atom, R 1 and R 2 Independently represents a monovalent organic group that is attached to a silicon atom by a carbon atom and does not contain any epoxy groups.
[0019] (c) Colloidal particles of metal oxides or metal-like oxides, including (c1) colloidal particles of titanium oxide and (c2) colloidal particles of tin oxide.
[0020] (d) At least one curing catalyst,
[0021] Compound (b) is present in an amount ranging from 1% to 10% by weight relative to the dry extract of the composition, and wherein tin oxide represented as SnO2 and titanium oxide represented as TiO2 are present in the composition at a weight ratio of TiO2 / (TiO2+SnO2) ranging from 35% to 75%.
[0022] The composition of this invention combines two colloids, TiO2 (which acts as a barrier to protect the UV-sensitive substrate) and SnO2 (which has low or no photocatalytic activity), thereby preventing cracking in the resulting coating while ensuring a high refractive index coating. Furthermore, the use of a small amount of silane (b) carrying two organic groups reduces the water sensitivity of the coating (compared to coatings containing only epoxysilane (a) as the silane compound) and softens the coating matrix, thus preventing it from cracking after polymerization.
[0023] Another object of the present invention is an optical article coated with a wear-resistant and / or scratch-resistant coating obtained from the above composition, and a method thereof for manufacturing the same. Detailed Implementation
[0024] The terms “comprising” (and any of its grammatical variations, such as “including” and “including”), “having” (and any of its grammatical variations, such as “having” and “possessing”), “containing” (and any of its grammatical variations, such as “containing” and “accommodating”), and “including” (and any of its grammatical variations, such as “containing” and “including”) are all open-ended linking verbs. They are used to specify the presence of the stated feature, whole, step, or component or group thereof, but do not exclude the presence or addition of one or more other features, wholes, steps, or components or groups thereof. Therefore, a method or a step in a method that “comprising,” “having,” “containing,” or “including” one or more steps or elements possesses, but is not limited to, possessing only those one or more steps or elements.
[0025] Unless otherwise specified, all figures or expressions relating to quantities of ingredients, ranges, reaction conditions, etc., used herein should be understood to be modified by the term “about” in all cases.
[0026] When an optical article includes one or more surface coatings, the phrase “depositing a coating or layer onto an optical article” means depositing a coating or layer onto the outermost coating of the optical article (i.e., the coating closest to the air).
[0027] In this application, a coating “on” or already deposited on a substrate / coating is defined as a coating that (i) is located above the substrate / coating, (ii) is not necessarily in contact with the substrate / coating, that is, one or more intermediate coatings may be disposed between the substrate / coating and the coating in question (however, preferably in contact with the substrate / coating), and (iii) does not necessarily completely cover the substrate / coating. When “layer 1 is disposed below layer 2”, it is intended to mean that layer 2 is farther from the substrate than layer 1.
[0028] The term "coating" should be understood to mean any layer, stack of layers, or film that can come into contact with a substrate and / or with another coating (e.g., a sol-gel coating or a coating made of pure organic resin). Coatings can be deposited or formed by a variety of methods, including wet processing, gas processing, and film transfer.
[0029] In this application, a layer or compound is referred to as having a high refractive index when the refractive index of the layer or compound is greater than or equal to 1.55, preferably greater than or equal to 1.56, more preferably in the range of 1.57 to 1.65, and even more preferably in the range of 1.58 to 1.62.
[0030] Compound (a)
[0031] The curable composition according to the invention is generally a liquid and contains at least one compound (a) and / or its hydrolysis product, the compound being an epoxy compound carrying at least one silicon atom, the silicon atom having at least one hydrolyzable group directly attached to the silicon atom and at least one group containing an epoxy functional group attached to the silicon atom via a carbon atom.
[0032] Compound (a) is used as a binder. The binder is defined as a film-forming material that can improve the adhesion of the coating to the underlying and / or upper layers, and / or the integrity of the coating.
[0033] Compound (a) preferably has 2 to 6, more preferably 2 or 3, functional groups that produce silanol groups upon hydrolysis. The compound is considered an organic compound and preferably has the formula (I):
[0034] R n' Y m Si(X) 4-n'-m (I)
[0035] Wherein R groups are the same or different and represent monovalent organic groups that are attached to silicon atoms by carbon atoms and do not contain any epoxy groups, Y groups are the same or different and represent monovalent organic groups that are attached to silicon atoms by carbon atoms and contain at least one epoxy group, X groups are the same or different and represent hydrolyzable groups or hydrogen atoms, m and n' are integers such that m equals 1 or 2 and n' + m = 1 or 2.
[0036] Integers n and m define three groups of compounds (I): compounds having the formula RYSi(X)2, compounds having the formula Y2Si(X)2, and compounds having the formula YSi(X)3. Among these compounds, epoxysilanes having the formula YSi(X)3 are preferred.
[0037] These monovalent R groups, bonded to silicon atoms via Si-C bonds, are organic groups. These groups can be, without restriction, saturated or unsaturated hydrocarbon groups, preferably C1-C. 10 Groups, and more preferably C1-C4 groups, such as: alkyl (preferably C1-C4 alkyl, such as methyl or ethyl), aminoalkyl, alkenyl (such as vinyl), C6-C 14 Aryl (e.g., optionally substituted phenyl, particularly phenyl substituted with one or more C1-C4 alkyl groups), benzyl, (meth)acryloyloxyalkyl.
[0038] The most preferred R group is alkyl, especially C1-C4 alkyl, and ideally methyl.
[0039] A “hydrolyzable group” generated from silicon atoms is a chemical group that will transform into an OH group when exposed to hydrolytic conditions. It is noteworthy that SiOH bonds can initially exist in compounds having formula (I), which are considered hydrolysis products in this case. Hydrolysis products also include siloxane salts.
[0040] The term "hydrolysis product" for silane derivatives indicates the fact that, in the context of this invention, the silane derivative may have been at least partially hydrolyzed to form silanol groups, and may have also undergone some degree of crosslinking through the condensation reaction of these silanol groups.
[0041] The X group can be represented independently and without restriction: alkoxy-OR 1 , where R 1 Preferably, it represents a straight-chain or branched alkyl or alkoxyalkyl group, more preferably a C1-C4 alkyl group; acyloxy-OC(O)R 3 , where R 3 Preferably, it represents an alkyl group, more preferably a C1-C6 alkyl group, and even more preferably a methyl or ethyl group; a halogen group such as Cl and Br; an amino group optionally substituted with one or two functional groups such as alkyl or silyl groups, for example an NHSiMe3 group; an alkenyl group such as isopropenyloxy. The hydroxyl group is considered a hydrolyzable group.
[0042] The most preferred epoxy silanes are those in which n'=0, m=1 and X is a C1-C5 alkoxy group, preferably OCH3, in formula (I).
[0043] Monovalent Y groups bonded to silicon atoms via Si-C bonds are organic groups because they contain at least one epoxy functional group, preferably one epoxy functional group. An epoxy functional group refers to a group of atoms in which an oxygen atom is directly bonded to two adjacent or non-adjacent carbon atoms contained in a carbon chain or cyclic carbon system. Among epoxy functional groups, ethylene oxide functional groups are preferred, i.e., saturated three-membered cyclic ether groups.
[0044] Epoxysilane compounds of formula (I) provide a highly cross-linked matrix. Preferred epoxysilanes have organic linkages between Si atoms and epoxy functional groups, which provide a level of flexibility.
[0045] The preferred Y group is a group having formulas III and IV:
[0046]
[0047] Where R 2 It is an alkyl (preferably methyl) or hydrogen atom, ideally a hydrogen atom, a and c are independently integers ranging from 1 to 6, and b is 0, 1 or 2.
[0048] The preferred group having Formula III is γ-glycidoxypropyl (R 2 = H, a = 3, b = 0) and preferably the (3,4-epoxycyclohexyl)alkyl having formula IV is β-(3,4-epoxycyclohexyl)ethyl (c = 1). γ-glycidoxyethoxypropyl (R) can also be used. 2 = H, a = 3, b = 1).
[0049] Preferred epoxysilanes having formula (I) are epoxyalkoxysilanes, and most preferably those having one Y group and three alkoxy X groups. Particularly preferred epoxytrialkoxysilanes are those having formulas V and VI:
[0050]
[0051] Where R 1 It is an alkyl group having 1 to 6 carbon atoms, preferably methyl or ethyl, and a, b, and c are as defined above. In some embodiments, a is 3. In some embodiments, b is 0.
[0052] Examples of such epoxy silanes include, but are not limited to, γ-glycidoxymethyltrimethoxysilane, γ-glycidoxymethyltriethoxysilane, γ-glycidoxymethyltripropoxysilane, γ-glycidoxyethyltrimethoxysilane, γ-glycidoxyethyltriethoxysilane, γ-glycidoxyethyltripropoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropyltripropoxysilane, γ-glycidoxypropylmethyldiethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane. Other useful epoxytrialkoxysilanes are described in patents US 4,294,950, US 4,211,823, US 5,015,523, EP 0614957, US 2009 / 0311518, US 2011 / 0058142 (compounds having formulas I, VII, and VIII) and WO 94 / 10230. Among those silanes, γ-glycidoxypropyltrimethoxysilane (GLYMO) is preferred.
[0053] In one embodiment, the composition comprises at least one compound (a) having the formula RYSi(X)2, where R, Y, and X are as defined above. The compound (a) having the formula RYSi(X)2 can be used as a single compound (a) or as a mixture with one or more other compounds (a), such as a compound (a) having the formula YSi(X)3, where Y is as defined above. In one embodiment, the composition comprises at least one compound (a) having the formula RYSi(X)2 and at least one compound (a) having the formula RYSi(X)2. Compounds (a) having the formula RYSi(X)2 are more hydrophobic than compounds (a) having the formula YSi(X)3 (where r is a monovalent organic group), and they have the ability to limit the sensitivity of the resulting abrasion-resistant and / or scratch-resistant coating to water. Preferred compounds (a) having the formula RYSi(X)2 are γ-glycidoxypropylmethyldiethoxysilane and γ-glycidoxypropylmethyldimethoxysilane.
[0054] In one embodiment of the invention, the hydrolyzable polymerizable compound (a) is hydrolyzed before being mixed with the other components of the composition. Hydrolysis can be carried out as is known in the field of sol-gel processing, as disclosed in FR 2702486 or US4211823. Acidic catalysts such as hydrochloric acid or acetic acid can be used to promote the hydrolysis reaction in the presence of water.
[0055] The aforementioned organofunctional compounds form a silica organosol. After undergoing hydrolysis, they generate an interpenetrating network by forming silanol groups, which can bond with the underlying layer and act as adhesion promoters. They can also act as crosslinking agents for other compounds present in the composition, such as compound (b).
[0056] Although epoxysilanes are typically in their hydrolyzed form, the amount of epoxysilane will conventionally be defined as the weight prior to the initial hydrolysis of the precursor. The hydrolysis of the alkoxy group releases the associated alcohol to form silanol groups, which will spontaneously condense. Preferably, the alkoxysilane is reacted with a stoichiometric amount of water to hydrolyze the hydrolyzable group, typically the alkoxy group.
[0057] The composition preferably contains 10% to 30%, more preferably 15% to 28%, and even more preferably 18% to 27% of compound (a) relative to the total weight of the composition.
[0058] In one embodiment, the composition comprises 75% to 95%, more preferably 80% to 92%, or even more preferably 82% to 90% of the total weight of the polymerizable compounds present in the composition (a).
[0059] The composition preferably comprises 25% to 65%, more preferably 30% to 60%, and even more preferably 35% to 55% of the dry extract of the composition by weight (a).
[0060] Compound (b)
[0061] The curable composition comprises at least one compound (b) for increasing hydrophobicity and / or its hydrolysis product, the compound being a silane compound having formula (II):
[0062]
[0063] Z 1 and Z 2 Independently representing a hydrolyzable group or hydrogen atom, R 1 and R 2 Independently represents a monovalent organic group that is attached to a silicon atom by a carbon atom and does not contain any epoxy groups.
[0064] Monovalent R atoms are attached to silicon atoms via Si-C bonds. 1 and R 2 The group can be, without restriction, a saturated or unsaturated hydrocarbon group, preferably C1-C. 10 Groups, and more preferably C1-C4 groups, such as: alkyl (preferably C1-C4 alkyl, such as methyl or ethyl), aminoalkyl, alkenyl (such as vinyl), C6-C 14 Aryl (e.g., optionally substituted phenyl, particularly phenyl substituted with one or more C1-C4 alkyl groups), benzyl, (meth)acryloyloxyalkyl.
[0065] "Aryl" is an unsaturated hydrocarbon group that contains alternating single and double bonds and obeys Hückel's aromaticity rule.
[0066] The optimal R 1 and R 2 The group is alkyl, especially C1-C4 alkyl, and ideally methyl.
[0067] In one embodiment, R 1 and / or R 2 The group does not contain any groups capable of reacting with silanol groups, such as OH or SiOH groups, or bridging groups other than epoxy groups. In one embodiment, R 1 and / or R 2 The group is an unsubstituted alkyl or aryl group.
[0068] The reaction can be carried out during the hydrolysis of silanes having formula (II) to obtain Z with an OH group. 1 and Z 2The group can be represented independently and without restriction: alkoxy -OR 1 , where R 1 Preferably, it represents a straight-chain or branched alkyl or alkoxyalkyl group, more preferably a C1-C4 alkyl group; acyloxy-OC(O)R 3 , where R 3 Preferably, it represents an alkyl group, more preferably a C1-C6 alkyl group, and even more preferably a methyl or ethyl group; a halogen group such as Cl and Br; an amino group optionally substituted with one or two functional groups such as alkyl or silyl groups, for example an NHSiMe3 group; an alkenyl group such as isopropenyloxy. The hydroxyl group is considered a hydrolyzable group.
[0069] In one embodiment, R in equation (II) 1 and R 2 The group independently represents an alkyl group, and Z 1 and Z 2 The group independently represents the alkoxy group.
[0070] The most preferred compound (b) is the one in which Z 1 and Z 2 Independently representing C1-C5 alkoxy groups, preferably OCH3, and / or R 1 and R 2 Those that independently represent C1-C4 alkyl groups. Preferred silane compounds (b) having formula (II) are dimethyldiethoxysilane, dimethyldimethoxysilane, and methylphenyldimethoxysilane, with dimethyldiethoxysilane (DMDES) being the most preferred. Alternatively, γ-chloropropylmethyldimethoxysilane, vinylmethyldiethoxysilane, vinylmethyldiacetoxysilane, 3-acryloyloxypropylmethyl-dimethoxysilane, 3-acryloyloxypropyl-methylbis(trimethylsiloxy)silane, 3-methacryloyloxypropyl-methyldimethoxysilane, 3-methacryloyloxypropyl-methyldiethoxysilane, 3-methacryloyloxypropyl-bis(trimethylsiloxy)methylsilane, methacryloyloxymethylbis(trimethylsiloxy)methylsilane, 3-aminopropylmethyldimethoxysilane, 3-(2-aminoethyl)aminopropylmethyldimethoxysilane, and 3-aminopropylmethyldiethoxysilane can be used.
[0071] The composition preferably contains 0.5% to 9%, more preferably 1% to 7%, and even more preferably 2% to 5% of the compound (b) relative to the total weight of the composition.
[0072] In one embodiment, the composition comprises 5% to 25%, more preferably 8% to 20%, and even more preferably 10% to 18% of the compound by weight relative to the total weight of the polymerizable compounds present in the composition (b).
[0073] Compound (b) is present in an amount ranging from 1% to 10% by weight relative to the dry extract of the composition, preferably from 2% to 9%, 3% to 7% or 4% to 6% by weight relative to the dry extract of the composition.
[0074] Compound (b) is more hydrophobic than compound (a). Compared to prior art hard coating compositions, a portion of the epoxy silane compound (a) forming the coating matrix has been replaced by the more hydrophobic silane compound (b), thereby reducing the coating's water sensitivity and the likelihood of delamination.
[0075] Without being bound by any theory, it is believed that hard coatings with a matrix formed of epoxy silane compounds (a) (which are hydrophilic) can swell by absorbing water from ambient humidity or sweat, putting one or more of the most vulnerable interfaces of the optical article under stress, thereby causing the coating to peel off.
[0076] In this invention, compounds (a) and (b) are preferably present in the composition at a weight ratio of compound (b) to compound (a) ranging from 8% to 25%, more preferably from 10% to 20%, 12% to 20%, or 13% to 18%.
[0077] In this invention, compounds (a) and (b) are preferably present in the composition in such amounts that the ratio of the dry extract weight of compound (b) to the dry extract weight of compound (a) ranges from 6% to 18%, more preferably from 7% to 16%, 8% to 15% or 9% to 13%.
[0078] This ratio ensures low water sensitivity of the coating.
[0079] Hard coatings prepared from compositions according to the invention containing at least one compound (b) exhibit adhesion, transparency, abrasion resistance and scratch resistance properties that are generally similar to or higher than those obtained from corresponding compositions that do not contain any compound having formula (b), although compound (b) is used in the compositions of the invention at a relatively low concentration.
[0080] Compound (c)
[0081] The curable composition comprises at least one compound (c) comprising colloidal particles of a metal oxide or metal-like oxide, including (c1) colloidal particles of titanium oxide and (c2) colloidal particles of tin oxide.
[0082] These particles increase the hardness of the coating and optionally adjust the refractive index of the resulting coating. They are used in colloidal form.
[0083] The preparation of colloidal particles requires well-known methods. As used herein, "colloid" refers to fine particles (nanoparticles) with an average diameter (or maximum size in the case of elongated particles) less than 150 nm, more preferably less than 100 nm, dispersed in a liquid dispersion medium (aqueous or organic) (such as water, alcohol, ketone, ester, or combinations thereof, preferably alcohols such as methanol, ethanol, or isopropanol). At such low average particle sizes, the transparency of the coating is not affected. Preferred colloidal particle sizes range from 2 to 100 nm, 2 to 50 nm, or 5 to 40 nm. The size of particles in liquids is determined by conventional methods such as light scattering and particle size analysis. The size of particles in solids is determined by tunneling electron microscopy or light scattering.
[0084] Colloidal particles (c1) and / or (c2) may comprise homogeneous or non-homogeneous groups of particles, and may include particles of different sizes, different properties, or both. In this way, users can incorporate multiple particles with various functions to provide a variety of properties depending on the end use of the product.
[0085] In some embodiments, the colloidal particles may be made from a mixture of small-sized particles (e.g., having a diameter of 10 to 15 nm) and large-sized particles (e.g., having a diameter of 30 to 80 nm).
[0086] Colloidal particles of titanium oxide (c1) and colloidal particles of tin oxide (c2) can be introduced into the composition as two different colloids or as a single colloid containing both types of particles.
[0087] In one embodiment, the colloidal particles (c2) include SnO2 particles.
[0088] These particles can be modified by grafting organic groups, especially onto silicon atoms.
[0089] The particles can also be composite oxide particles based on two or more metal oxides or metal-like oxides.
[0090] In one embodiment, the composite particles have a core / shell structure. One or more shells, identical or different metal oxides and / or metal-like oxides, may be formed around the core of the particle. The core may be formed of a single metal oxide or metal-like oxide, or may be a mixture or complex of several metal oxides and / or metal-like oxides. In another embodiment, the composite particles are Janus particles.
[0091] Composite materials can be used, such as SiO2 / TiO2, SnO2 / TiO2, SiO2 / SnO2 / TiO2, SiO2 / ZrO2, SiO2 / TiO2 / ZrO2, SiO2 / SnO2, or TiO2 / SiO2 / ZrO2 / SnO2.
[0092] In one embodiment, the colloidal particles of titanium oxide (c1) comprise composite particles of titanium oxide, which are preferably free of tin oxide. The composite particles are particles of multi-component oxides, wherein the amounts of each oxide can be varied to alter the refractive index of the particles. The composite particles of titanium oxide are preferably composite particles of titanium oxide, zirconium oxide, and silicon oxide, which are preferably free of tin oxide. An example of commercially available colloidal particles having a composite structure based on TiO2, ZrO2, and SiO2 is the core-shell structured colloidal Optolake 1120Z from JGC Catalysts Co., Ltd. ® (S-95 / A8). This colloid is disclosed in JP 2009-197078 as a methanol dispersion sol containing 20 wt% of fine particles of titanium-based composite oxides, which contain titanium, silicon and zirconium (the dry titanium content, expressed as TiO2, is approximately 48.8 wt%).
[0093] In one embodiment, the colloidal particles of titanium oxide and the colloidal particles of tin oxide are different particles. In one embodiment, the curable composition is prepared by adding colloidal particles of titanium oxide (c1) and colloidal particles of tin oxide (c2) to a mixture, respectively. In one embodiment, the colloidal particles of titanium oxide (c1) do not contain tin oxide. In another embodiment, the colloidal particles of tin oxide (c2) do not contain titanium oxide.
[0094] In one embodiment, the colloidal particles of tin oxide (c2) comprise composite particles of tin oxide, which preferably do not contain titanium oxide.
[0095] In one embodiment, colloidal particles of titanium oxide (c1) and colloidal particles of tin oxide (c2) are provided as a composite sol comprising composite particles of titanium oxide and tin oxide, such as composite particles of titanium oxide, tin oxide, zirconium oxide, and silicon oxide. An example of commercially available colloidal particles having a composite structure based on TiO2, SnO2, ZrO2, and SiO2 is the core-shell structured colloidal Optolake 1120Z from Nichibukai Chemicals Co., Ltd. ® (11RU7-A-8). It is disclosed, for example, in patent application JP H11-310755.
[0096] Another example of a commercially available colloid containing TiO2, SnO2, ZrO2 and SiO2 particles is colloid HT-R305M7-20 from Nissan Chemical Industries, disclosed, for example, in US 2019 / 092681.
[0097] Another example of such composite particles of titanium oxide and tin oxide is disclosed in patent application JP 2000-204301, which relates to composite particles consisting of: (i) a core particle of tin oxide and titanium oxide, and (ii) a covering layer covering the core particle, the covering layer being composed of oxides of silicon oxide and zirconium and / or aluminum; particularly composite particles having a core / shell structure having a core of tin oxide and titanium oxide in rutile form and a shell comprising a mixture of silicon oxide and zirconium oxide.
[0098] Hybrid particles having a metallic or metalloid core and at least one polymeric shell can also be used, such as reactive core-shell particles having at least one metal oxide or metalloid as the core and a polymerizable material (such as a prepolymer) as the shell. During coating preparation, the reactive groups of the latter type of particles can react with each other under heat or UV treatment or further crosslink with the reactive materials of the composition (such as polymerizable compounds (a) and / or (b)), thereby providing a dense network and thus a harder substrate surface.
[0099] Compound (c) may comprise colloidal particles of metal oxides or metal-like oxides other than tin oxide and titanium oxide. Non-limiting examples of such oxide colloidal particles include particles of silicon oxide (preferably SiO2), aluminum oxide, zirconium oxide, aluminum-doped silicon oxide, indium-doped tin oxide (ITO), antimony-doped tin oxide (ATO), aluminum-doped zinc oxide, zinc oxide (ZnO), indium oxide (In2O3), Sb2O3, MgO, Sb2O5, Y2O3, Ta2O5, La2O3, Fe2O3, WO3, vanadium pentoxide, cerium oxide, zinc antimonate, indium antimonate, or mixtures of two or more thereof, which are colloidally dispersed in a dispersion medium.
[0100] In a preferred embodiment, compound (c) comprises colloidal particles of silica (such as silicon dioxide). Silica may be present in composite particles with other metal / metal-like oxides or in non-composite particles. Silica colloids are manufactured by DuPont de Nemours under the trade name Ludox. ® Sale.
[0101] In one embodiment, compound (c) comprises colloidal particles of zirconium oxide (such as ZrO2). Zirconia may be present in composite particles with other metal / metal-like oxides or in non-composite particles.
[0102] The composition preferably comprises, by weight, 4% to 25%, more preferably 6% to 20%, even more preferably 8% to 18% or 10% to 15% of colloidal particles of metal oxide or metal-like oxide (excluding the weight of the solvent present in the colloid), i.e., compound (c), relative to the total weight of the composition. Compound (c) is typically present in an amount ranging from 30% to 70%, preferably 35% to 65%, more preferably 37% to 60%, even more preferably 38% to 52% relative to the weight of the dry extract of the composition.
[0103] In this invention, tin oxide (represented by SnO2) and titanium oxide (represented by TiO2) are present in the composition at a weight ratio of TiO2 / (TiO2+SnO2) ranging from 35% to 75%, more preferably 40% to 70%, 44% to 65%, or 46% to 60%. This ratio ensures low yellowing of the coating while preventing cracking, as the presence of tin oxide limits the photocatalytic degradation of organic matter.
[0104] In one embodiment, titanium dioxide, represented by TiO2, is present in the composition in an amount ranging from 10% to 22%, preferably 12% to 20% or 14% to 18% by weight relative to the dry extract of the composition.
[0105] In one embodiment, titanium oxide, represented by TiO2, is present in the composition in an amount ranging from 1% to 11% by weight, preferably from 2% to 9% or from 4% to 7% relative to the total weight of the composition.
[0106] In one embodiment, tin oxide, represented by SnO2, is present in the composition in an amount ranging from 7% to 19%, preferably 9% to 17% or 11% to 16% by weight relative to the dry extract of the composition.
[0107] In one embodiment, tin oxide, represented by SnO2, is present in the composition in an amount ranging from 1% to 10%, preferably 2% to 8% or 3% to 7% by weight relative to the total weight of the composition.
[0108] In one embodiment, silicon dioxide, represented by SiO2, is present in the composition in an amount ranging from 3% to 19%, preferably 4% to 17% or 5% to 15% by weight relative to the dry extract of the composition.
[0109] In one embodiment, silicon dioxide, represented by SiO2, is present in the composition in an amount ranging from 1% to 10%, preferably 1.3% to 8% or 1.5% to 6% by weight relative to the total weight of the composition.
[0110] In one embodiment, zirconium oxide, represented by ZrO2, is present in the composition in an amount ranging from 0.5% to 10%, preferably 1% to 8% or 2% to 6% by weight relative to the dry extract of the composition.
[0111] In one embodiment, zirconium oxide, represented as ZrO2, is present in the composition in an amount ranging from 0.25% to 5%, preferably 0.5% to 4% or 1% to 3% by weight relative to the total weight of the composition.
[0112] The phrase "represented by..." or "converted to" indicates that a metal or metal-like oxide, such as tin oxide or titanium oxide, does not necessarily exist as a single oxide in the composition, but can exist in a mixture of composite oxides, especially when composite particles of oxides are used. Therefore, for practical reasons, the weight of a metal or metal-like oxide such as tin oxide or titanium oxide can be indicated by representing the titanium or tin component (or other oxide component) as TiO2 or SnO2, respectively. Clearly, when the colloid (c1) contains colloidal particles of TiO2 and (c2) contains colloidal particles of SnO2, conversion is not necessary.
[0113] In one embodiment, the ratio (weight of dry extract of colloidal titanium dioxide particles) / (weight of dry extract of colloidal titanium dioxide particles + weight of dry extract of colloidal tin oxide particles) ranges from 50% to 85%, more preferably 55% to 80%, 60% to 75%, or 65% to 75%. Such a ratio ensures low yellowing of the coating while preventing cracking.
[0114] Compound (d)
[0115] The curable composition comprises at least one compound (d) that is a curing catalyst. A catalyst is a system used to accelerate the polymerization reaction that occurs (i.e., the condensation and / or crosslinking reaction of epoxy compounds and / or siloxane compounds). It is typically a thermally activated condensation catalyst.
[0116] Preferred catalysts found to enable the composition to cure at sufficiently low temperatures (preferably ≤ 110°C, more preferably ≤ 100°C) without damaging the underlying substrate or adversely affecting other coatings or coating components include (strong) acid catalysts designed for ring-opening polymerization of cyclic ether groups (such as Lewis acids disclosed in US 2013 / 274381), ammonium salts of metal anions, and aluminum-based compounds.
[0117] In a preferred embodiment, the catalyst (d) is selected from aluminum chelates, aluminum acylates, aluminum alkoxides, and aluminum siloxy compounds. When using those aluminum compounds, the composition preferably does not contain other epoxy ring-opening catalysts, such as acid catalysts or ammonium salts of metal anions.
[0118] Aluminum acylates, siloxyaluminum compounds, and aluminum alkoxides each have the preferred general formula Al(OC(O)R). n (OR') 3-n Al(OC(O)R) n (OSiR"3) 3-n And Al(OSiR"3) n (OR') 3-n R and R' are straight-chain or branched alkyl groups containing 1 to 10 carbon atoms, R'' is a straight-chain or branched alkyl group containing 1 to 10 carbon atoms, a phenyl moiety, or an acylated moiety having the formula OC(O)R, wherein R is as just defined above, and n is an integer from 1 to 3. Preferably, R' is isopropyl or ethyl, and R and R'' are methyl.
[0119] Aluminum chelates can be formed by reacting aluminum alkoxides or aluminum acylates with chelating agents (such as acetylacetone, ethyl acetoacetate, or diethyl malonate) that do not contain nitrogen or sulfur and contain oxygen as a coordinating atom. These can be selected from aluminum acetylacetone (denoted as Al(AcAc)3), aluminum monoacetoacetate·diacetylacetone, aluminum diacetoacetate·monoacetylacetone, di-n-butoxy-ethyl monoacetoacetate, and diisopropoxy-ethyl monoacetoacetate. Other examples of useful catalysts are given in patent EP 0614957. When the catalyst is an aluminum chelate, the coating composition preferably contains an organic solvent with a boiling temperature in the range of 70°C to 140°C at atmospheric pressure, such as ethanol, isopropanol, ethyl acetate, methyl ethyl ketone, or tetrahydropyran.
[0120] Other metal complex catalysts, such as iron acetylacetonate or zinc acetylacetonate, can also be used.
[0121] The catalyst is typically used in an amount ranging from 0.01% to 5% by weight, preferably from 0.1% to 3.5% by weight, and more preferably from 0.2% to 3% by weight, based on the weight range of the composition.
[0122] The compositions of the present invention advantageously further contain a small amount, preferably 0.005% to 1% by weight based on the total weight of the composition, more preferably 0.02% to 0.8%, and even more preferably 0.05% to 0.5%, of at least one nonionic or ionic surfactant. Surfactants are important for good wetting of the substrate, thereby producing a satisfactory final coating appearance. The surfactant may include, for example, polyether-modified polydimethylsiloxane, poly(alkylene glycol)-modified polydimethylsiloxane, or polyheptamethylsiloxane or fluoroalkyl-modified polysiloxane. Preferred surfactants are polyether-modified polydimethylsiloxanes such as BYK supplied by BYK Chemicals. ® -3752, Fluorinated surfactants such as Novec from 3M ® FC-4434 (a nonionic surfactant containing fluorinated aliphatic polymer esters), Unidyne from CIBA TM NS-9013 and EFKA ® 3034 (Fluorocarbon modified polysiloxane). Useful fluorinated surfactants are disclosed in WO 2010 / 076314.
[0123] In addition to one or more solvents present in the colloidal component (c), the composition typically contains at least one solvent. The at least one solvent present in the composition is preferably an alcohol (such as an alkanol (methanol, ethanol, propanol…)) or a diol monoether (e.g., Dowanol PM from Dow Chemical). ® Solvents may be ketones (such as methyl ethyl ketone), propylene carbonate, or water. The solvent is preferably an organic solvent (such as methanol or ketone) or a water-alcohol mixture.
[0124] The total amount of solvent depends on the components used, the type of optical article, and the coating process. The purpose of the solvent is to achieve good surface wetting and a specific coating viscosity range determined by the coating equipment used to achieve a particular coating thickness range. The solvent or solvent mixture typically constitutes 25% to 80% of the composition by weight, preferably 35% to 75%, more preferably 50% to 65%.
[0125] The compositions according to the invention contain, in general, 20%-50%, preferably 25%-45%, more preferably 30%-40% by weight of solids (the weight of the dry extract relative to the weight of the composition).
[0126] The dry extract weight content of the compound in the composition indicates the content of that compound in the final coating. The dry extract weight can be calculated based on the theoretical dry extract weight, as disclosed in US 2012 / 0295084 or EP 614957. Typically, for hydrolyzable silane compounds, it is expressed as Q...k SiO (4-k) / 2 The unit represents the calculated weight, where Q is the organic part directly bonded to silicon atoms via Si-C bonds, k is 0, 1, 2, or 3, and Q k SiO (4-k) / 2 By Q k SiR''' (4-k) The hydrolysis of produces Si-R''', which yields Si-OH upon hydrolysis.
[0127] Dry extracts can also be determined experimentally. A dry extract of a compound or composition is the total weight of the compound or composition after complete removal of volatile substances in an oven at 100°C to 110°C, preferably at 100°C. Dry extracts are also known as solids content, expressed as a percentage of non-volatile material by weight, or % NVM. Conventional procedures for determining solids take 60 minutes in an oven at 105°C to 110°C and require pre- and post-weighing of the sample pan and sample (ASTM names: D2369 and D2926-80). Procedures using a commercial Mark 3 solids analyzer from Sartorius or a SMART Turbo™ from CEM take only 2 to 10 minutes, depending on the volatile / moisture content and viscosity of the material.
[0128] In addition to the main components (a), (b), (c), and (d), the composition may further comprise a variety of additives in conventional proportions for polymerizable compositions. These additives include additional curing / crosslinking agents (e.g., silane coupling agents or comonomers such as polyamines, polythiols, polyols, and polycarboxylic acids), photochromic agents, lubricants, rheology modifiers, flow and leveling additives, wetting agents, defoamers, stabilizers, pH adjusters, dyes, pigments, UV absorbers, and free radical scavengers (such as hindered amine light stabilizers and antioxidants).
[0129] Its advantages are numerous and include applicability to most substrates with good adhesion, especially plastic substrates, as well as the production of optical products with high transmittance, low haze, improved abrasion and / or scratch resistance (compared to the same optical products without the abrasion and / or scratch-resistant coating), increased durability, resistance to breakage throughout the wear process, while maintaining excellent adhesion of the coating.
[0130] The present invention also relates to the abrasion-resistant and / or scratch-resistant coating itself, independent of the substrate to which it is coated.
[0131] The present invention also relates to an optical article comprising a substrate having at least one main surface coated with an abrasion-resistant and / or scratch-resistant coating, wherein the abrasion-resistant and / or scratch-resistant coating is formed from a curable composition as described above. It will sometimes be referred to in this patent application as a "hard coating composition".
[0132] The wear-resistant and / or scratch-resistant coating according to the invention preferably has a refractive index greater than or equal to 1.5, more preferably greater than or equal to 1.55 or 1.60.
[0133] The optical articles prepared according to the present invention are transparent optical articles, preferably optical lenses or lens blanks, and more preferably ophthalmic lenses or lens blanks. The ophthalmic lenses may be polarized lenses with or without corrective function, or tinted sunglass lenses.
[0134] Optical articles may be coated with an abrasion-resistant and / or scratch-resistant coating according to the invention on their convex main surface (front), concave main surface (back / rear), or both surfaces, but preferably on the convex (front) main surface, to avoid multiple reflections of light reaching the lens. As used herein, in the case of ophthalmic lenses, the back of the substrate is intended to refer to the surface closest to the wearer's eye when the article is in use. It is typically concave. Conversely, the front of the substrate is the surface furthest from the wearer's eye when the article is in use. It is typically convex. Optical articles may also be plano articles.
[0135] In an embodiment, the optical article according to the invention is coated with an abrasion-resistant and / or scratch-resistant coating according to the invention on two surfaces (front main surface and rear main surface). The coatings may be the same or different.
[0136] In this document, the term "lens" refers to an organic or inorganic glass lens, including a lens substrate, which may be coated with one or more coatings having different properties.
[0137] The term "ophthalmic lens" is used to refer to a lens that is fitted into an eyeglass frame, for example, to protect the eyes and / or correct vision. The lens may be selected from afocal lenses, monofocal lenses, bifocal lenses, trifocal lenses, and progressive lenses. While ophthalmic optics is a preferred area of this invention, it should be understood that the invention can be applied to other types of optical articles, such as lenses for optical instruments used in photography or astronomy, optical aiming lenses, eye protection goggles, optical components of lighting systems, etc.
[0138] In this specification, unless otherwise specified, an optical article / material shall be understood to be transparent when no significant loss of contrast is perceived when an image is viewed through it, i.e., when image formation is obtained through the optical article without adversely affecting the quality of the image. Unless otherwise specified, this definition of the term "transparent" may be applied to all objects as so defined in this specification.
[0139] In the context of this invention, "substrate" should be understood to mean an uncoated substrate and typically has two main surfaces. The substrate can in particular be an optically transparent material having the shape of an optical article (e.g., an ophthalmic lens destined for mounting on eyeglasses). In this context, the term "substrate" should be understood to mean the basic building material of an optical lens, and more particularly, an ophthalmic lens. This material acts as a support for a stack of one or more coatings or layers.
[0140] The substrate can be made of inorganic glass or plexiglass, preferably plexiglass. Plexiglass can be a thermoplastic material (such as polycarbonate and thermoplastic polyurethane) or a thermosetting (crosslinked) material, such as diethylene glycol bis(allyl carbonate) polymers and copolymers (especially CR-39 from PPG Industries). ® Preferred materials for lens substrates include thermosetting polyurethanes, polysulfuric esters (preferably polysulfuric ester resins with a refractive index of 1.60 or 1.67), polyepoxides, polycyclic sulfides (such as polycyclic sulfides with a refractive index of 1.74), and substrates based on poly(meth)acrylates and copolymers, such as substrates containing (meth)acrylate polymers and copolymers derived from bisphenol A, polysulfo(meth)acrylates, and copolymers thereof and blends thereof. Preferred materials for lens substrates are polycarbonate (PC), diethylene glycol bis(allyl carbonate) polymers, and substrates obtained from thermosetting polysulfuric ester resins, which are sold by Mitsui Toatsu Chemicals Co., Ltd. under the MR series, particularly MR-6. ® MR-7 ® and MR-8 ® Resins. These latter substrates and the monomers used in their preparation are particularly described in patents US 4,689,387, US 4,775,733, US 5,059,673, US 5,087,758 and US 5,191,055.
[0141] The present invention is particularly effective when applied to lens substrates obtained from cyclic sulfides, and preferably polycyclic sulfides.
[0142] The present invention further relates to a method for manufacturing an optical article as described herein, the method comprising:
[0143] (i) Providing an optical article comprising a substrate having at least one main surface,
[0144] (ii) Optionally, an impact-resistant primer coating is deposited on the surface.
[0145] (iii) Depositing a curable composition for an abrasion-resistant and / or scratch-resistant coating as previously described on the surface produced by step (i) or (ii),
[0146] (iv) Curing the composition deposited in step (iii) to obtain a cured abrasion-resistant and / or scratch-resistant coating.
[0147] The coating or coating composition can be deposited onto the surface of the optical article by liquid phase deposition or lamination according to any suitable method, starting from the above-described liquid coating composition, and then dried, pre-cured, or cured at a temperature typically around 70°C–100°C, if necessary. The application of the composition can be performed without limitation by spin coating, dip coating, spraying, brushing, roller coating, or flow coating. Spin coating and dip coating are preferred. The drying / curing step is preferably carried out using heat or ultraviolet radiation and includes solvent evaporation, curing of the reactive epoxy compound, and crosslinking.
[0148] The thickness of the cured abrasion- and / or scratch-resistant coating can be adapted to the specific application required and typically ranges from 0.5 to 50 µm, preferably 1 to 20 µm or 1 to 10 µm, more preferably 1.5 to 10 µm, and even more preferably 2 to 5 µm. The coating thickness can be easily adjusted by changing the solvent concentration of the claimed composition and the coating conditions (e.g., the pull-up speed in the case of deposition by dip coating). The longer the pull-up time, the thinner the final dry coating will be.
[0149] The main surface of the substrate may be coated with several functional coatings to improve its optical and / or mechanical properties. The functional coatings used herein may be selected without limitation from the following: impact-resistant coatings, antireflective coatings, polarizing coatings, photochromic coatings, antistatic coatings, antifog coatings (hydrophobic and / or oleophobic coatings), antifog coatings, precursors to antifog coatings, or stacks of two or more such coatings.
[0150] If the substrate is coated with at least one surface coating, the abrasion-resistant and / or scratch-resistant coating according to the invention can be deposited on the bare substrate or on the outermost coating of the substrate.
[0151] In a preferred embodiment, at least one main surface of the optical article is sequentially coated with an impact-resistant primer coating and an abrasion-resistant and / or scratch-resistant coating as disclosed in this invention.
[0152] Impact-resistant coatings, preferably impact-resistant primer coatings, can be any coating typically used to improve the impact resistance of finished optical products. Furthermore, this coating usually promotes the adhesion of additional layers in the final product to the substrate, particularly the adhesion of abrasion-resistant and / or scratch-resistant coatings.
[0153] By definition, an impact-resistant coating is a coating that improves the impact resistance of an optical product compared to an identical optical product without an impact-resistant coating.
[0154] Typical impact-resistant coatings are based on (meth)acrylic acid and polyurethane, which optionally contain fillers such as metal or metal-like oxide particles.
[0155] Preferred primer compositions include: thermoplastic polyurethane-based compositions, such as those described in patents JP 63-141001 and JP 63-87223; poly(meth)acrylic primer compositions, such as those described in patent US 5015523; thermosetting polyurethane-based compositions, such as those described in patent EP 0404111; and compositions based on poly(meth)acrylic latex or polyurethane latex, such as those described in patents US 5,316,791 and EP 0680492.
[0156] Preferred primer compositions are polyurethane-based compositions and latex-based compositions, particularly polyurethane latex, poly(meth)acrylic latex, and polyester latex, and combinations thereof.
[0157] The primer coating and abrasion-resistant and / or scratch-resistant coating may be selected from those described in application WO 2007 / 088312.
[0158] The impact-resistant coating composition can be deposited onto the surface of an optical article using any classic method such as spin coating, dip coating, or flow coating, and then dried or cured at a temperature of about 70°C–100°C.
[0159] The thickness of the impact-resistant coating in the final optical product is typically in the range of 0.2 to 2.5 μm, preferably 0.5 to 1.5 μm.
[0160] Antireflective coatings can be any antireflective coating traditionally used in the field of optics, particularly ophthalmic optics. It is also well known that antireflective coatings traditionally comprise single-layer or multi-layer stacks of dielectric materials (typically one or more metal oxides) and / or sol-gel materials and / or organic / inorganic layers, as described in WO 2013 / 098531. These are preferably multilayer coatings comprising layers with a high refractive index (HI) and layers with a low refractive index (LI).
[0161] The structure and preparation of the antireflective coating are described in more detail in patent applications WO 2010 / 109154, WO 2011 / 080472, WO 2012 / 153072 and WO 2012 / 076714.
[0162] The antifouling coating is preferably deposited on the outer layer of the antireflective coating. Generally, its thickness is less than or equal to 10 nm, preferably in the range of 1 to 10 nm, more preferably 1 to 5 nm. The antifouling coating is typically a fluorosilane or fluorosilazane type coating, preferably containing a fluoropolyether portion and more preferably a perfluoropolyether portion. More detailed information about these coatings is disclosed in WO 2012076714.
[0163] The optical article according to the invention preferably has a relative light transmittance factor Tv of 80% or higher, more preferably 85% or higher, more preferably 87% or higher, and even better 89% or higher in the visible spectrum.
[0164] Optical articles of the present invention, made from the optical materials according to the present invention, may be coated with an antireflective coating at one or both air / substrate interfaces. In such embodiments, the Tv factor is preferably in the range of 87% to 99%, more preferably 90% to 98%, and even better 92% to 97%.
[0165] The system’s Tv factor, also known as “light transmittance”, is defined as in standard NF EN 1836 and is associated with an average value in the wavelength range of 380–780 nm, which is weighted according to the sensitivity of the eye at each wavelength in this range and is measured under D65 illumination conditions (daylight).
[0166] The optical articles according to the present invention have satisfactory color characteristics, which can be quantified by the yellowness index Yi. The whiteness of the optical materials of the present invention can be quantified by colorimetric measurement based on the CIE tristimulus values X, Y, and Z as described in standard ASTM E 313-05, using reflectance measurements at a light source C and an observer at 2°. The yellowness index Yi is calculated according to ASTM method E313 using the relationship Yi = (127.69 X - 105.92 Z)) / Y, where X, Y, and Z are CIE tristimulus values. The optical articles according to the present invention preferably have a low yellowness index Yi, i.e., less than 12 or 10, more preferably less than 6, and even better less than 4, as measured according to the above standards.
[0167] The following examples illustrate the invention in more detail, but not in a limiting manner. Unless otherwise stated, all thicknesses disclosed in this application refer to physical thicknesses. Percentages given in tables are weight percentages. Unless otherwise specified, refractive indices mentioned herein are expressed at a wavelength of 550 nm at 25°C.
[0168] Example
[0169] 1. General Procedure
[0170] The optical components used in the example include: ORMA optical fiber with a refractive index of 1.50 and a diopter of -2.00 from Essilor. ® Lens substrate; or a polycarbonate substrate with a refractive index of X and a diopter of -2.00; or a polycyclic sulfide substrate with a refractive index of 1.74 and a diopter of -4.00 (all having a diameter of 65 mm and a thickness of 1.2 mm).
[0171] The substrate of the optical article is sequentially coated with a primer coating with a refractive index of 1.6 and a wear-resistant and / or scratch-resistant coating according to the present invention.
[0172] The primer coating is formed from a coating composition having 20% by weight of dry extract and containing a polyurethane emulsion (U5200 from Alberdingk Boley), a ZrO2-based colloid (SZR-CW from Sakai Chemical Industry), deionized water, and Coatosil 77 as a surfactant.
[0173] In Examples 1-3, the abrasion-resistant and / or scratch-resistant coating compositions comprise, as compound (a), γ-glycidoxypropyltrimethoxysilane (from Dynasylan Corporation), as compound (b), dimethyldiethoxysilane (from Wacker Corporation), as compound (c1), Optolake 1120ZS-95 / A8 (from Nichibukai Chemical Co., Ltd.) (approximately 20.6% by weight of dry extract, average particle size 10 nm), as titanium dioxide colloid (c2), HX-400M7-20 (from Nissan Chemical Industries, Ltd.) (approximately 40.4% by weight of dry extract, average particle size 5 nm), as polymerization catalyst compound (d), aluminum acetylacetonate Al(AcAc)3, as solvent, methyl ethyl ketone, and BYK 3752 as surfactant.
[0174] Example 4 contains the same components, except that titanium oxide colloid (c1) and tin oxide colloid (c2) are both represented by HT-R305M7-20 from Nissan Chemical Industries, Ltd. (approximately 30% by weight of dry extract, average particle size 20 to 25 nm).
[0175] Optolake 1120Z S-95 / A8 is a colloidal dispersion containing 20% by weight of titanium-based composite oxide particles. This colloid contains titanium oxide, zirconium oxide, and silicon oxide dispersed in methanol.
[0176] HX-400M7-20 is a colloidal dispersion containing, by weight, tin oxide (between 30% and 40%, denoted as SnO2), silicon oxide (a small amount, denoted as SiO2), and methanol (approximately 60%).
[0177] HT-R305M7-20 is a colloidal dispersion containing, by weight, titanium oxide (between 10% and 20%, denoted as TiO2), tin oxide (between 2% and 10%, denoted as SnO2), silicon oxide, zirconium oxide, and methanol (approximately 70%).
[0178] Formulation of abrasion-resistant and / or scratch-resistant coatings
[0179] 0.1 N hydrochloric acid was slowly added to Glymo over 15 minutes. Hydrolysis was carried out by stirring at a temperature below 40°C. After hydrolysis for at least 1 hour, DMDES was added to the reaction mixture and stirred for 15 minutes. Then, colloid Optolake 1120Z S-95 / A8 (or HT-R305M7-20 for Example 4) was slowly added over 30 minutes, followed by colloid HX-400M7-20. After adding the colloids, the reaction mixture was stirred for 18–20 hours. Aluminum acetylacetonate was added to the reaction mixture and stirred for 30 minutes. Methyl ethyl ketone and surfactant BYK 3752 were added over 30 minutes. After further stirring for 1 hour, the reaction mixture was filtered and recovered. The viscosity of the dry extract and the recovered solution was measured.
[0180] Deposition conditions for abrasion-resistant and / or scratch-resistant coatings
[0181] Each coating composition was deposited by dip coating onto both sides of a lens substrate that had previously been cleaned with diluted NaOH (500 rpm for 5 s, then 1000 rpm for 10 s), at a pull-up speed of 2.5–3.0 mm / s. The resulting wet coatings were typically pre-cured at 70°C for 12 minutes and post-cured at 100°C–110°C for 3 hours. The (dry) coating thickness of the primer was 0.8 µm, and the (dry) coating thickness of the abrasion-resistant and / or scratch-resistant coating with a refractive index of 1.6 was 2.6 ± 0.5 µm.
[0182] 2. Evaluation of coating performance
[0183] a) Evaluate the resistance to photodegradation (UV) of the coating of the present invention after exposure to sunlight conditions under Q-sun testing. The Q-sun test includes introducing the prepared article into a Q-SUN test. ® The Xe-3 xenon lamp chamber, purchased from Q-LAB, reproduces the full spectrum of sunlight and operates at a chamber temperature of 40°C (0.68 W / m²). 2The convex surfaces of the coatings were exposed to irradiation at the following conditions: blackboard temperature 60°C, initial relative humidity: ambient humidity (i.e., approximately 50%); for 24 h or 80 h. After these time periods, optionally, the appearance of cracks in the hard coatings was determined after subjecting the articles to accelerated aging conditions (stored in a climate chamber at 65°C and 90% relative humidity for 24 h). The first condition assessed the contribution of UV to crack initiation, and the second condition assessed the combined contribution of UV and water to crack initiation.
[0184] b) At Q-SUN ® After irradiation for 80 hours in an Xe-3 xenon lamp chamber using the same parameters as described above, the residual color of the UV-sensitive substrate was measured. The yellowness index Yi of the prepared optical article was calculated by measuring the CIE tri-color stimulus values X, Y, and Z on a white background using a Cary 60 spectrophotometer at a reflectance of 2° observer (light source C) and a Cary 60 spectrophotometer, as described in standard ASTM E 313-05. The residual color is the difference between Yi before and after exposure. Lower values are better.
[0185] c) Abrasion resistance and haze were determined as disclosed in WO 2012 / 173596. Specifically, abrasion resistance was measured by the sand Bayer test according to ASTM F735-81. Haze was measured according to ASTM D1003-00 on a BYK-Gardner Haze-Gard XL-211 Plus apparatus. Since haze is a measure of the percentage of transmitted light that is axially scattered by more than 2.5° from the incident light, a lower haze value indicates a lower degree of turbidity. Generally, for the optical articles described herein, a haze value of less than or equal to 0.3% is acceptable, and more preferably less than or equal to 0.2%.
[0186] d) The transmittance factor Tv in the visible spectrum was measured from the wearer's perspective in transmission mode (incident angle: 0°) using a Cary 4000 spectrophotometer from Hunter, with the back (concave) side of the lens (1.2 mm thick at the center) facing the detector and light entering on the front side of the lens. Tv was measured under D65 illumination conditions (daylight).
[0187] e) The yellowness index Yi of the prepared optical article is calculated by measuring the CIE tri-color stimulus values X, Y, Z as described in standard ASTM E 313-05 on a white background using a Cary 60 spectrophotometer under reflectance measurements at a light source C with an observer at 2°. A low yellowness index Yi indicates high whiteness.
[0188] In another test, the evolution of the yellowness index Yi of hard-coated optics was measured after 80 h of Q-Sun testing. A lower evolution was better.
[0189] f) Wet Adhesion Test (Cross-Cut Test): This test measures the water sensitivity of the coating. According to ASTM D3359-93, the cross-cut adhesion test measures the coating's adhesion by cutting a series of five lines spaced 1 mm apart through the coating with a razor blade, followed by cutting a second series of five lines spaced 1 mm apart perpendicular to the first series, creating a cross-cut pattern of 25 squares. After blowing away any dust formed during the crisscrossing process with an airflow, the product is placed in boiling water for 30 minutes, removed from the bath, and stored at room temperature for 60 minutes. Then, transparent cellophane tape (3M Scotch) is applied. ® Apply n° 600) to the crisscross pattern, press firmly down, and then quickly pull it off the coating in a direction perpendicular to the coating surface. Then repeat the application and removal of fresh tape four more times. Adhesion is rated as follows (0 is the best adhesion, 1-4 are medium adhesion, and 5 is the worst adhesion):
[0190]
[0191] The water sensitivity of the coating was also investigated through storage tests. Optical products were stored in a climate chamber at 65°C and 90% relative humidity. The adhesion test was performed daily until failure (score = 5). Products could be ranked based on the number of days before failure (longer is better).
[0192] 3. Results
[0193] Examples C1 to C7 show that tin oxide, represented by SnO2, and titanium oxide, represented by TiO2, should be present in the composition at a weight ratio of TiO2 / (TiO2+SnO2) ranging from 35% to 75%. If this weight ratio is too low (Examples C1, C2), corresponding to a low amount of TiO2 used, the resulting optical article will have insufficient UV exposure resistance and yellowing will be observed. If this weight ratio is too high (Examples C6, C7), corresponding to a high amount of TiO2 used, cracks will be observed in the abrasion-resistant and / or scratch-resistant coating after UV exposure of the optical article.
[0194] The amounts of components in the coating compositions of Examples C1 to C7 are suitable for having a coating with a refractive index of 1.6 in each case.
[0195]
[0196] ( (Weight of dry extract of colloidal titanium oxide particles) / (Weight of dry extract of colloidal titanium oxide particles + Weight of dry extract of colloidal tin oxide particles).
[0197] Examples C7, C4, and 1-4 show that the silane compound (compound (b)) of formula (II) should be present in an amount ranging from 1% to 10% by weight relative to the dry extract of the composition. If the amount of compound (b) is too low (Examples C7, C4), the coating becomes too water-sensitive. If the amount of compound (b) is too high (data not shown), the resulting optical article has insufficient abrasion resistance, and the haze becomes too significant, indicating reduced transparency. The UV sensitivity, transmittance, and yellowness index of the optical article are not affected by the amount of silane compound (b).
[0198] weight
[0199]
[0200] N / A: Not available
[0201] dry weight
[0202]
[0203] ( (Weight of dry extract of colloidal titanium oxide particles) / (Weight of dry extract of colloidal titanium oxide particles + Weight of dry extract of colloidal tin oxide particles).
[0204] The optical products of Examples 1-4 have low diffusion levels, low yellowness, low UV sensitivity, low water sensitivity, and maintain satisfactory abrasion resistance.
Claims
1. A curable composition for abrasion-resistant and / or scratch-resistant coatings, comprising: (a) At least one epoxy compound and / or its hydrolysis product carrying at least one silicon atom, wherein the silicon atom carries at least one hydrolyzable group directly attached to the silicon atom and at least one group containing an epoxy functional group attached to the silicon atom via a carbon atom. (b) At least one silane compound having formula (II) and / or its hydrolysis product: Z 1 and Z 2 Independently representing a hydrolyzable group or hydrogen atom, R 1 and R 2 Independently represents a monovalent organic group that is attached to the silicon atom by a carbon atom and does not contain any epoxy groups. (c) Colloidal particles of metal oxides or metal-like oxides, including (c1) colloidal particles of titanium oxide and (c2) colloidal particles of tin oxide. (d) At least one curing catalyst, Compound (b) is present in an amount ranging from 1% to 10% by weight relative to the dry extract of the composition. Furthermore, tin oxide represented by SnO2 and titanium oxide represented by TiO2 are present in the composition at a weight ratio of TiO2 / (TiO2+SnO2) ranging from 35% to 75%.
2. The curable composition according to claim 1, wherein, Compound (a) is present in an amount ranging from 25% to 65% by weight relative to the dry extract of the composition.
3. The curable composition according to any one of the preceding claims, wherein, Compound (b) is present in an amount ranging from 3% to 7% by weight relative to the dry extract of the composition.
4. The curable composition according to any one of the preceding claims, wherein, Compound (c) is present in an amount ranging from 30% to 70% by weight relative to the dry extract of the composition.
5. The curable composition according to any one of the preceding claims, wherein, Titanium oxide, represented as TiO2, is present in an amount ranging from 10% to 22% by weight relative to the dry extract of the composition.
6. The curable composition according to any one of the preceding claims, wherein, Tin oxide, represented as SnO2, is present in an amount ranging from 7% to 19% by weight relative to the dry extract of the composition.
7. The curable composition according to any one of the preceding claims, wherein, The colloidal particles of titanium oxide (c1) include composite particles of titanium oxide, preferably composite particles of titanium oxide, zirconium oxide and silicon oxide.
8. The curable composition according to any one of the preceding claims, wherein, Compound (a) is a compound having the following formula: R n' Y m Si(X) 4-n'-m (I) Wherein R groups are the same or different and represent monovalent organic groups that are attached to the silicon atom by a carbon atom and do not contain any epoxy groups, Y groups are the same or different and represent monovalent organic groups that are attached to the silicon atom by a carbon atom and contain at least one epoxy functional group, X groups are the same or different and represent hydrolyzable groups or hydrogen atoms, and m and n' are integers such that m equals 1 or 2 and n' + m = 1 or 2.
9. The curable composition according to any one of the preceding claims, wherein, The colloidal particles of titanium oxide and the colloidal particles of tin oxide are different particles.
10. The curable composition according to any one of the preceding claims, wherein, The colloidal particles of the titanium oxide (c1) do not contain tin oxide.
11. The curable composition according to any one of the preceding claims, wherein, The silane compound (b) having formula (II) is selected from dimethyldiethoxysilane, dimethyldimethoxysilane and methylphenyldimethoxysilane.
12. The curable composition according to any one of the preceding claims, wherein, The curable composition is prepared by adding colloidal particles of titanium oxide (c1) and colloidal particles of tin oxide (c2) to the mixture, respectively.
13. An optical article comprising a substrate having at least one main surface coated with an abrasion-resistant and / or scratch-resistant coating, wherein the abrasion-resistant and / or scratch-resistant coating is formed from a curable composition according to any one of claims 1 to 12.
14. The optical article according to claim 13, wherein, The wear-resistant and / or scratch-resistant coating has a thickness ranging from 1 to 10 μm.
15. The optical article according to claim 13 or 14, further defined as an optical lens, preferably an ophthalmic lens.
Citation Information
Patent Citations
Process for producing plastic lens
EP0404111A2
Abrasion-resistant coating compositions containing hydrolised silanes and aluminium compounds; coated articles resistant to abrasion and shocks
EP0614957A1
Process for improving impact resistance of coated plastic substrates
EP0680492A1
Abrasion-resistant coating compositions containing hydrolised silanes and aluminium compounds