Glass fiber reinforced recycled polyethylene terephthalate compositions and molded articles with improved hydrolysis resistance and enhanced tracking index compared to electrochemical indices.
By adding a combination of epoxidized linseed oil, N,N'-hexane-1,6-dimethylbis(hexahydro-2-oxo-1H-azaphen-1-carboxamide) and dicalcium phosphate to RPET, the problems of hydrolytic degradation and decreased anti-tracking properties of RPET during thermomechanical processing were solved, and the mechanical properties were maintained and the RPET was used in electrical equipment under high temperature and high humidity conditions.
Patent Information
- Application Number
- CN202480080448.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-12-21
- Filing Date
- 2024-12-18
- Publication Date
- 2026-11-17
AI Technical Summary
In the prior art, recycled polyethylene terephthalate (RPET) is easily hydrolyzed and degraded during thermomechanical processing, resulting in loss of mechanical properties. Furthermore, its anti-tracking properties decrease after being reinforced with glass fiber, making it difficult to meet the requirements of advanced applications.
The combination of epoxide-containing compounds, bis-lactams and phosphorus-containing compounds, especially epoxidized linseed oil, N,N'-hexane-1,6-dimethylbis(hexahydro-2-oxo-1H-azaphen-1-carboxamide) and dicalcium phosphate, enhances the hydrolytic stability and anti-tracking properties of RPET.
It significantly improves the hydrolytic stability and anti-tracking properties of RPET, enabling it to maintain its mechanical properties under high temperature and humid conditions, making it suitable for advanced electrical and electronic equipment.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
[0001] This invention relates to compositions comprising recycled polyethylene terephthalate and glass fiber, molded articles, electronic or electrical devices, methods of manufacturing molded articles, and the use of compositions disclosed herein for improving the hydrolytic stability and / or enhancing the relative tracking index level of articles manufactured therefrom.
[0002] Polyethylene terephthalate (PET) is by far the most common thermoplastic polymer resin in the polyester family and has a wide range of applications. Therefore, PET is in large circulation and has been extensively recycled. However, polyesters, such as PET, are prone to degradation via hydrolysis under humid conditions and elevated temperatures. This primarily occurs during the thermomechanical processing of polymers in the presence of moisture, but can also occur during the subsequent use of the resulting product. Hydrolysis of polyesters leads to a decrease in molecular weight and melt viscosity, as well as impaired mechanical properties. These effects severely limit the uses of polyesters and increase the drying costs before polymer processing. In recycled polyesters, such as, particularly, recycled PET (RPET), the disadvantages of hydrolytic degradation are even more pronounced because these polyesters have undergone multiple thermomechanical processing cycles since their initial manufacture.
[0003] Chain extenders are used to restore the mechanical and rheological properties damaged by hydrolytic degradation during thermomechanical processing. Chain extenders are multifunctional compounds that link the end groups of polymer chains together, resulting in polymers with higher molecular weights. The reactivity of the chain extender should be very high to allow the reaction to occur quickly, preferably fast enough to complete this step during extrusion. In the past, a large number of chain extenders with different types of reactions have been developed for polyesters, and these chain extenders are well known in the prior art.
[0004] For example, WO 98 / 47940 A1 describes a bifunctional caprolactam chain extender for the production of high molecular weight polyesters. Similarly, U.S. Patent No. 3,657,191 discloses a composition containing a linear polyester and a diepoxide compound with terminal epoxy groups for increasing the molecular weight of the polyester. Because these chain extenders are highly reactive with the carboxyl end groups of the polyester under extrusion conditions, a common drawback of such compounds is that they often result in a significant, abrupt increase in branched products and / or molecular weight during extrusion. This is especially true when these chain extenders are added at the high levels required for current hydrolysis resistance. Of course, the viscosity increase associated with the increase in molecular weight is often unpredictable, which can also adversely affect performance manufacturing operations such as injection molding. Furthermore, the stabilizing effect is based more on the initial molecular weight increase due to chain growth than on hydrolytic protection present in the final product and throughout its entire service life.
[0005] To expand their applications, polyesters are often reinforced with reinforcing agents such as glass fibers. However, this compromises their electrical insulation properties and makes them prone to tracking. Tracking is the formation of conductive pathways on the polymer surface under specific conditions and voltages. Tracking in polymers can be a source of fire and / or component breakage. Therefore, tracking resistance is often an important safety requirement for materials used in certain electrical or electronic applications. A common method for evaluating the tracking resistance of polymers is to use their Comparative Tracking Index (CTI).
[0006] For example, as disclosed in EP 3323854 B1, polybutylene terephthalate (PBT) resin itself has a very high comparative tracking index (CTI) of 600 V, which is higher than the tracking resistance of polyethylene terephthalate (PET) resin. However, when these polyester resins are compounded with various fillers such as stabilizers, flame retardants, or reinforcing glass fibers to improve mechanical properties, their tracking resistance deteriorates significantly, for example, decreasing to 325 V or even lower, depending on the amount of filler added. However, some applications may require materials with a higher comparative tracking index.
[0007] Therefore, the demand for glass fiber reinforced recycled polyethylene terephthalate (RPET) engineering resin compositions with higher hydrolysis resistance and / or stronger electrical tracking resistance continues to increase, particularly in the area of glass fiber reinforced recycled polyethylene terephthalate resins as described in the prior art.
[0008] One object of the present invention is to overcome these and other disadvantages of the prior art, and in particular to provide glass fiber reinforced recycled polyethylene terephthalate compositions and molded articles comprising such compositions, characterized by improved hydrolytic stability and / or enhanced resistance to tracking. Specifically, one object of the present invention is to provide a glass fiber reinforced recycled polyethylene terephthalate composition having improved hydrolytic stability and enhanced resistance to tracking. Another object of the present invention is to provide an electronic or electrical device comprising or substantially composed of the compositions disclosed herein, and to propose the use of the compositions disclosed herein for improving the hydrolytic stability and / or improving the relative tracking index level of articles manufactured therefrom.
[0009] According to the independent claims, the compositions, molded articles, electronic or electrical devices, manufacturing methods, and uses of the compositions disclosed herein achieve the above and other objectives. The dependent claims define preferred embodiments.
[0010] The compositions according to the present invention comprise at least one recycled polyethylene terephthalate resin, glass fiber, at least one epoxy-containing compound, at least one bis-lactam, and at least one phosphorus-containing compound.
[0011] As used herein, an epoxy-containing compound should be understood as a compound containing at least one epoxy functional group. In particular, the epoxy-containing compound has a molecular weight of less than 3000 g / mol, preferably less than 1500 g / mol, and is not polymerizable.
[0012] Preferred epoxy-containing compounds contain at least three epoxy groups per molecule, more preferably at least four epoxy groups per molecule, and most preferably at least six epoxy groups per molecule. The epoxy-containing compounds can be polymeric or non-polymeric, preferably non-polymeric.
[0013] Polyethylene terephthalate (PET), as used herein and as commonly understood by those skilled in the art, is a semi-aromatic polyester derived from terephthalic acid (or dimethyl terephthalate) and monoethylene glycol, wherein the total mass of the reacted terephthalic acid (or dimethyl terephthalate) and monoethylene glycol accounts for at least 90% of the mass of the reacting monomers forming the polymer. Those skilled in the art will understand that the term "virgin PET" refers to PET produced directly from petrochemical feedstocks and which has not been previously processed or used. Virgin polyethylene terephthalate material refers to non-post-consumer recycled material, and, as determined in the second thermal scan of ASTM D3418 standard procedure 10.1, has a melt peak temperature between 225°C and 255°C when the sample is heated at a rate of 10°C / min.
[0014] As used herein and as commonly understood by those skilled in the art, recycled polyethylene terephthalate (RPET) refers to any PET material derived from recycled materials rather than virgin, unprocessed petrochemical raw materials (i.e., virgin PET). Those skilled in the art will understand that recycled polyethylene terephthalate (RPET) can be prepared, in particular, by depolymerizing polyethylene terephthalate (PET) flakes, amorphous PET (A-PET), crystalline PET (C-PET), PET films, PET fibers, PET textiles, and post-consumer recycled PET (PCR-PET).
[0015] The goal is to reuse recycled polyethylene terephthalate (RPET) in new molded or extruded articles, as using recycled RPET reduces the environmental footprint of the product. However, the reusability of PET has historically been hampered, as thermomechanically recycled RPET is of lower quality than virgin PET, especially after multiple recycling cycles. Therefore, the use of recycled RPET has been largely limited to less demanding applications. In contrast, this invention enables the use of recycled RPET in advanced applications requiring high hydrolytic stability and / or high resistance to electro-tracking.
[0016] As is known to those skilled in the art, lactams are cyclic amides. The structural motif of a lactam can be represented by the following structural formula (1):
[0017]
[0018] In the structural formula (1) shown, n represents the size of the lactam ring, which is usually an integer from 1 to 5. The lactams obtained from this are called α-lactam (three-membered ring), β-lactam (four-membered ring), γ-lactam (five-membered ring), δ-lactam (six-membered ring) and ε-lactam (seven-membered ring), respectively.
[0019] Therefore, dilactams should be understood as any compound having formula (2):
[0020]
[0021] In the shown structural formula (2), n is an integer between 1 and 15, preferably between 4 and 10, and most preferably 5, and R is any functional group or residue that connects the lactam ring, particularly a carbonyl group. At least one lactam ring of the bis-lactam can be substituted and / or fused (condensed) to another ring. The synthesis of compounds according to formula (2) is described in WO 98 / 47940.
[0022] A specific example of a bis-lactam that can be used according to the present invention is a bis-N-acyllactam having formula (3):
[0023]
[0024] Wherein, n is between 1 and 15, preferably between 4 and 10, most preferably an integer of 5, and A is selected from alkyl groups, such as alkylene diamines, especially hexamethylene diamine, or aromatic groups. The synthesis of compounds according to formula (3) is described in EP 0286253 A2.
[0025] Phosphorus-containing compounds as used herein are specifically understood to be metal phosphates, metal phosphonates, or metal hypophosphonates, preferably metal phosphates. In particular, the metal phosphate used in this invention is calcium hydrogen phosphate.
[0026] Surprisingly, the study found that a combination of at least one epoxy-containing compound, at least one bis-lactam, and at least one phosphorus-containing compound imparts significantly improved hydrolytic stability and excellent comparative tracking index to glass fiber-reinforced recycled polyethylene terephthalate resin. This is contrary to expectations, particularly regarding hydrolytic stability, as previous literature such as EP 2184311 A1 reported that the use of carbonyl bis-caprolactams and other carbonyl lactams in polyesters leads to an increased hydrolysis rate of the corresponding polyester film, rather than improved hydrolytic stability. Instead, the inventors found that not only does the use of bis-lactams (and especially N,N′-hexane-1,6-dimethylbis(hexahydro-2-oxo-1H-azaphen-1-carboxamide), hereinafter referred to as "CBA") not hinder the obtaining of polyesters with improved hydrolytic stability, but also that the use of CBA contributes to obtaining polyesters with enhanced resistance to tracking.
[0027] Unwilling to be bound by theory, the addition reaction of the carboxylic acid group with the epoxy group produces the corresponding hydroxyalkyl ester. The hydroxyl group of the hydroxyalkyl ester can then be captured by reaction with one or both of bis-lactams and metal phosphates.
[0028] In a preferred embodiment of the composition according to the invention, at least one epoxy-containing compound is an epoxidized fatty acid ester.
[0029] Epoxidized fatty acid esters are preferred because these compounds are non-toxic, have high-temperature stability, and their migration behavior in the polymer matrix can be modulated by the acid used. Furthermore, their use is also preferred from a sustainability and environmental protection perspective, as they are based on renewable raw materials.
[0030] The epoxidized fatty acid ester is preferably selected from flaxseed oil, soybean oil, sunflower oil, safflower oil, tung oil, sesame oil, corn oil, sesame oil, cottonseed oil, castor oil, olive oil, peanut oil, rapeseed oil, coconut oil, babassu oil, palm oil, and fish oil. Most preferably, the epoxidized fatty acid ester is epoxidized flaxseed oil. Epoxidized flaxseed oil can be represented by the following exemplary structure (4):
[0031]
[0032] Epoxidized linseed oil (ELO; CAS No. 8016-11-3) is available, for example, from Valtris Specialty Chemicals under the trade name Lankroflex. TM L is obtained.
[0033] Epoxidized linseed oil was found to be particularly suitable and effective in enhancing hydrolytic stability, while also giving recycled polyethylene terephthalate resins an excellent comparative tracking index.
[0034] In a preferred embodiment of the composition according to the invention, at least one of the bis-lactams in the composition is carbonylbiscaprolactam or N,N'-hexane-1,6-dimethylbis(hexahydro-2-oxo-1H-azaphen-1-carboxamide) or both. CBA (CAS No. 5888-87-9) is readily available and is sold by Brüggemann as a polymerization activator under the trade name Bruggolen®. It exists in granular form and melts above 70°C, which allows for dust-free and safe processing.
[0035] In a preferred embodiment, at least one epoxy-containing compound is selected from epoxidized fatty acid esters, ethylene-n-butyl acrylate-glycidyl methacrylate (EBA-GMA) terpolymer, ethylene-methyl acrylate-glycidyl methacrylate (EMA-GMA) copolymer, and methyl methacrylate-butadiene-styrene (MBS) copolymer. At least one bis-lactam is one or two of carbonylbiscaprolactam and N,N'-hexane-1,6-dimethylbis(hexahydro-2-oxo-1H-azaphen-1-carboxamide), and at least one phosphorus-containing compound is one or two of dicalcium phosphate and hydroxyapatite.
[0036] Such compositions are characterized by particularly high resistance to electro-tracking and excellent hydrolytic stability.
[0037] The polymer composition is particularly preferred if it contains epoxidized linseed oil, N,N'-hexane-1,6-dimethylbis(hexahydro-2-oxo-1H-azaphen-1-carboxamide) and dicalcium phosphate.
[0038] As will be detailed in the comparative experiments, the composition containing epoxidized linseed oil, N,N'-hexane-1,6-dimethylbis(hexahydro-2-oxo-1H-azaphen-1-carboxamide) (CBA) and dicalcium phosphate exhibits particularly good resistance to hydrolysis and electro-tracking.
[0039] In a preferred embodiment of the compositions disclosed herein, at least one of the phosphorus-containing compounds is selected from metal phosphates, metal phosphonates, and metal hypophosphonates. In a particularly preferred embodiment of the compositions disclosed herein, the phosphorus-containing compound is at least one of calcium hydrogen phosphate and hydroxyapatite.
[0040] Based on the total weight of the composition, the total amount of epoxy compounds in the composition can be from 0.1 to 5% by weight. Preferably, based on the total weight of the composition, the total amount of epoxy compounds in the composition is from 0.5 to 3% by weight. In particular, based on the total weight of the composition, the total amount of epoxidized fatty acid esters in the composition can be from 0.1 to 5% by weight, preferably from 0.5 to 3% by weight.
[0041] Within the aforementioned range, a significant chain extension effect will occur without an uncontrollable tendency to form gels.
[0042] Alternatively or additionally, the total amount of dilactams in the composition may be 0.1 to 5% by weight, based on the total weight of the composition. Preferably, the total amount of dilactams in the composition is 0.5 to 2% by weight, based on the total weight of the composition. In particular, the total amount of one or both of carbonylbiscaprolactam and N,N'-hexane-1,6-dimethylbis(hexahydro-2-oxo-1H-azaphen-1-carboxamide) in the composition may be 0.1 to 5% by weight, preferably 0.5 to 2% by weight, based on the total weight of the composition.
[0043] Below 0.1% by weight, the effect is too small, while a content exceeding 5% by weight leads to gelation and a sharp increase in viscosity during extrusion. In particular, it has been found that the properties of the compositions according to the invention, namely hydrolytic stability and comparative tracking index (CTI), are best when the total amount of bislactams in the polymer composition is 0.5 to 2% by weight, based on the total weight of the composition, because a decrease in the comparative tracking index (CTI) of the resulting compositions is found, especially at higher bislactam contents.
[0044] Alternatively or additionally, the total amount of phosphorus-containing compounds in the composition may be 0.1 to 5% by weight, based on the total weight of the composition. Preferably, the total amount of phosphorus-containing compounds in the composition is 0.1 to 2.5% by weight, based on the total weight of the composition. In particular, the total amount of one or both of dicalcium phosphate and hydroxyapatite in the composition may be 0.1 to 5% by weight, preferably 0.1 to 2.5% by weight, based on the total weight of the composition.
[0045] Based on the total weight of the composition, the total amount of at least one recycled polyethylene terephthalate resin contained in the composition may be 40 to 90% by weight, preferably 50 to 80% by weight.
[0046] The above content range allows for the addition of other fillers and additives as needed to enable its function.
[0047] In a preferred embodiment, the composition is substantially free of any other semi-aromatic polyesters other than recycled polyethylene terephthalate.
[0048] The composition contains at least glass fiber as a reinforcing agent. Based on the total weight of the composition, the glass fiber is preferably present in the composition at an amount of 5 to 80% by weight. Based on the total weight of the composition, the reinforcing agent is more preferably present in the composition at an amount of 10 to 50% by weight, and most preferably at an amount of 25 to 40% by weight. When the composition is used in non-injection molded composites, a higher reinforcing agent content in the composition, especially 50% by weight or higher, is particularly important.
[0049] In a preferred embodiment, the compositions disclosed herein comprise at least one additional reinforcing agent selected from mineral fillers and natural fillers. Specifically, the mineral filler may be at least one selected from whiskers, kaolin, calcined kaolin, wollastonite, talc, chalk, glass beads, amorphous silica, asbestos, calcium silicate, calcium metasilicate, magnesium carbonate, powdered quartz, mica, barium sulfate, and feldspar. The natural filler may preferably be kenaf.
[0050] Compared to unreinforced polyester matrices, fiber-reinforced polyesters exhibit higher strength at all temperatures. Observations have shown that, based on the total weight of the composition, the thermomechanical properties of the compositions disclosed herein, particularly tensile strength and modulus of elasticity, increase when the fiber volume content increases to a maximum of 50% by weight. However, based on the total weight of the composition, these properties decrease when the fiber content exceeds 50% by weight. On the other hand, tensile elongation and impact energy values decrease with increasing fiber content. In summary, adding reinforcing agents, i.e., the sum of glass fibers and optionally other reinforcing agents, in amounts of 10 to 50% by weight based on the total weight of the composition, is a suitable range for effectively improving the thermomechanical properties of the compositions disclosed herein. For non-injection molded composites, such as profile or film extrusion, pultrusion, prepreg, vacuum forming, or compression molding, this range can even be extended to 5 to 80% by weight based on the total weight of the composition.
[0051] The glass fibers used with the compositions disclosed herein can be conventional glass fibers known in the art. There are no particular limitations on the cut length, diameter, or shape of the glass fibers. For example, the glass fibers can be cylindrical fibers, cocoon-shaped fibers, and fibers with an elliptical cross-section. There are also no particular limitations on the glass cutting method used when cutting glass filaments or rovings into chopped strands of specified lengths.
[0052] There are no particular restrictions on the type of glass used, but from a quality perspective, E glass or corrosion-resistant glass containing zirconium in its composition is especially preferred.
[0053] Furthermore, to improve the interfacial properties between the glass fiber and the resin matrix, it is advantageous to use glass fibers that have been surface-treated with an organic treatment agent (surface treatment agent), such as a silane compound including an aminosilane compound or an epoxy compound. There are no particular limitations on the surface treatment agent, and any conventional surface treatment agent can be used advantageously.
[0054] Typically, the compositions disclosed herein contain at least one epoxy-containing compound and at least one bis-lactam, which already possess relatively high impact strength, and the impact strength can be further improved by using known toughening agents.
[0055] In some embodiments, the composition further comprises 0.5 to 15 weight percent of at least one toughening agent, based on the total weight of the composition.
[0056] As used herein, “toughening agent” should be understood as a reagent that, when added to recycled polyethylene terephthalate resin, increases the impact strength of injection-molded elements substantially composed of said recycled polyethylene terephthalate resin, particularly when the impact strength is measured using the Charpy notched impact strength test according to ISO 179.
[0057] Toughening agents, also known as impact modifiers, can be reactive or non-reactive toughening agents. In some embodiments, the composition may contain both reactive and non-reactive toughening agents. Preferably, the composition according to the invention contains a reactive toughening agent.
[0058] Reactive toughening agents are preferred for reinforcing polyesters because they form a stable dispersed phase by grafting onto the polyester matrix. In contrast, non-reactive toughening agents can be dispersed into polyester resins through vigorous mixing, but may agglomerate downstream of the mixer.
[0059] Preferably, the toughening agent is selected from the following: methacrylate-butadiene-styrene copolymer, acrylate elastomer, acrylonitrile-styrene-acrylate copolymer, acrylonitrile-butadiene-styrene copolymer, high-rubber grafted acrylonitrile-butadiene-styrene copolymer, acrylate-olefin copolymer, polysiloxane rubber, polysiloxane-acrylic rubber, ethylene-propylene non-conjugated diene elastomer, acrylonitrile-styrene-ethylene-propylene non-conjugated diene elastomer, ethylene-methyl methacrylate-glycidyl methacrylate copolymer, ethylene-n-butyl acrylate-co-glycidyl methacrylate (EBA-GMA) terpolymer rubber, and combinations thereof. Even more preferably, the toughening agent is selected from the following: methacrylate-butadiene-styrene copolymer, acrylate-olefin copolymer, ethylene-methyl methacrylate-glycidyl methacrylate copolymer, ethylene-n-butyl acrylate-co-glycidyl methacrylate (EBA-GMA) terpolymer rubber, and combinations thereof.
[0060] The toughening agents mentioned above have proven to be particularly suitable because they are generally readily available and impart exceptionally high impact strength to polyester resins when measured according to the Charpy notch test (ISO 179).
[0061] The comparative tracking index (CTI) value of the composition may be at least 450V. Preferably, the comparative tracking index (CTI) value of the composition is at least 550V. In particular, the compositions disclosed herein that contain 5 to 80 weight percent, preferably 10 to 50 weight percent, and most preferably 25 to 40 weight percent of glass fiber based on the total weight of the polymer composition have a comparative tracking index (CTI) value of at least 450V, preferably at least 550V.
[0062] CTI can be determined using the measurement method specified in the third edition of IEC (International Electrotechnical Commission) 60112. Specifically, CTI is measured using a 0.1% by mass aqueous solution of ammonium chloride and platinum electrodes. A specified number of drops (100 drops) of this ammonium chloride aqueous solution is dropped onto each test piece, and the voltage at which none of the test pieces (n=S) break down is measured and recorded as CTI.
[0063] One or more conventional additives may be added to the compositions disclosed herein. For example, flame retardants and flame retardant synergists may be added to improve flame retardancy. Preferred flame retardants used with the present invention are phosphorus-containing flame retardants, such as metal phosphates, metal phosphonates, and metal hypophosphites, due to their plasticizing effect, thermal stability, and dual use as nucleating agents in semi-aromatic polyester resins. Additionally or alternatively, antioxidants and heat stabilizers may be added for the purpose of improving heat resistance. UV stabilizers may be added to reduce degradation and discoloration. Other additives include fillers, inert fillers, viscosity modifiers, nucleating agents, colorants and dyes, lubricants, plasticizers, and release agents.
[0064] In one specific embodiment, the composition may consist essentially of the following:
[0065] - At least one recycled polyethylene terephthalate resin, in a weight percentage of 40 to 89%;
[0066] - 5 to 80% by weight, preferably 10 to 50% by weight, and most preferably 25 to 40% by weight of glass fiber;
[0067] - 0.1 to 5% by weight, preferably 0.5 to 2% by weight, of at least one bis-lactam, particularly carbonylbiscaprolactam or N,N'-hexane-1,6-dimethylbis(hexahydro-2-oxo-1H-azaphen-1-carboxamide) or both;
[0068] - 0.1 to 5% by weight, preferably 0.5 to 3% by weight, of at least one epoxide-containing compound, particularly at least one epoxidized fatty acid ester, preferably epoxidized linseed oil; and
[0069] - 0.1 to 5% by weight, preferably 0.1 to 2.5% by weight, of at least one phosphorus-containing compound, particularly at least one metal phosphate;
[0070] All figures above are based on the total weight of the composition.
[0071] Optionally, the above embodiments may include an additional 0.5 to 15 weight percent of at least one toughening agent. Again, weight percent refers to the total weight of the composition including the toughening agent.
[0072] This composition is characterized by enhanced hydrolytic stability and excellent resistance to tracking. Furthermore, this composition is very stable and resistant to dielectric breakdown, and therefore can be advantageously used in the manufacture of electrical or electronic products intended for use under extreme conditions.
[0073] The metal phosphate is preferably at least one of calcium hydrogen phosphate (CaHPO4) and hydroxyapatite (Ca5(PO4)3OH) because they are non-toxic, generally readily available, and effective as flame retardants. Furthermore, the inventors have found that the aforementioned metal phosphate provides the compositions disclosed herein with a higher relative tracking index and improved hydrolytic stability.
[0074] The objectives described herein are further achieved by molded articles comprising the compositions disclosed herein.
[0075] As used herein, the term "shaped article" specifically includes bulk material intended for melting in an extruder. Such bulk material is also referred to by those skilled in the art as pellets or cuts.
[0076] In many cases, it is desirable to color molded articles or granules formed therefrom. For example, in electrical applications, polymer compositions with orange, red, green, blue, dark gray, or black colors are often used to mark or classify products.
[0077] Therefore, the molded article may further comprise one or a combination of organic and inorganic pigments. The pigment may, in particular, be carbon black.
[0078] The desired effect is to incorporate carbon black as a pigment to provide dark gray or black. The compositions disclosed herein alleviate the problems that arise after adding carbon black, namely, the decrease in the tracking index and the occurrence of tracking at lower voltages.
[0079] The molded articles disclosed herein can be used alone as molding granules or blended with other polymers. The granules can be used to produce fibers, films, and coatings, as well as injection-molded or extruded articles, particularly for end-use applications requiring improved hydrolysis resistance. However, in one specific embodiment of the invention, the molded articles disclosed herein are not intended for the production of polyester films.
[0080] The compositions disclosed herein can be molded into articles or parts using methods known to those skilled in the art. Preferred methods are commonly used molding methods such as injection molding, extrusion molding, compression molding, foam molding, blow molding, vacuum forming, injection blow molding, rotational molding, calendering, and solution casting.
[0081] The present invention also achieves the stated object by providing an electronic or electrical device comprising or substantially composed of the compositions disclosed herein.
[0082] The electronic or electrical equipment may be a charging gun, inverter, circuit breaker, sensor, relay, electromagnetic coil, connector, electrical box, electronic container and / or switch.
[0083] The beneficial effects of such articles and electronic or electrical devices are substantially the same as those of the compositions disclosed herein.
[0084] The present invention also achieves the stated object by providing a method for manufacturing a molded article comprising the compositions disclosed herein and at least one epoxidized fatty acid ester as disclosed herein.
[0085] Generally, the compositions disclosed herein can be obtained by blending all component materials using any blending method. It is preferable to mix the components and make them as homogeneous as possible. As a specific example, a mixer such as a blender, kneader, or roller extruder is used to mix all component materials homogeneously to obtain a polymer resin composition. Alternatively, a portion of the material can be mixed in a mixer, and then the remaining material can be added and further mixed until homogeneous. Furthermore, alternatively, the material can be pre-dry-mixed, then melted and kneaded using a heated extruder until homogeneous, and then extruded into strips, which are then cut to the desired length to become slurry. The latter method can be particularly used to prepare masterbatches for later mixing with more polymer resin.
[0086] However, according to the manufacturing method disclosed herein, epoxidized fatty acid esters (particularly epoxidized linseed oil) and bis-lactams (particularly carbonyl biscaprolactam and / or N,N'-hexane-1,6-dimethylbis(hexahydro-2-oxo-1H-azaphen-1-carboxamide)) are added to and fused with at least one of at least one recycled polyethylene terephthalate resins. At least one phosphorus-containing compound present in the compositions disclosed herein may be added to a mixture comprising epoxidized fatty acid esters, bis-lactams, and at least one recycled polyethylene terephthalate resin, or added to and fused with at least one of at least one recycled polyethylene terephthalate resins.
[0087] Preferably, the epoxidized fatty acid ester and the bis-lactam are premixed and added to and fused with at least one of the recycled polyethylene terephthalate resins of the compositions disclosed herein.
[0088] In this way, a sudden increase in viscosity during extrusion can be avoided particularly effectively because both compounds are present in the extruder and can be used to recover all of the polyethylene terephthalate resin in the composition.
[0089] The present invention also achieves the stated object by using compositions disclosed herein to improve the hydrolytic stability of articles made therefrom and / or to improve the comparative tracking index (CTI) value.
[0090] In particular, the hydrolytic stability of articles made therefrom and / or the comparative tracking index (CTI) value of articles made therefrom can be improved by using a composition as disclosed herein comprising at least one of an epoxidized fatty acid ester, carbonyl biscaprolactam and N,N'-hexane-1,6-dimethylbis(hexahydro-2-oxo-1H-azaphen-1-carboxamide) and at least one of calcium hydrogen phosphate and hydroxyapatite.
[0091] Comparative Example
[0092] The following comparative examples are intended to illustrate the inventive effects of the present invention. Unless otherwise stated, all quantities are based on the total weight of the respective compositions:
[0093] serial number INV1 INV2 RPET resin 61.00 61.00 60.00 Fiberglass 30.00 30.00 30.00 antioxidants 0.50 0.50 0.50 lubricant 0.50 0.50 0.50 toughening agent 3.00 3.00 3.00 Epon 1002 0.50 0.50 0.50 ELO 2.50 2.50 2.50 <![CDATA[CaHPO4]]> 2.00 1.00 2.00 CBA C20P - 1.00 1.00
[0094] The materials used in the above comparative examples are as follows:
[0095] RPET resin: recycled PET flakes (intrinsic viscosity 0.64 dL / g), trade name Monflakes®, purchased from Montello SpA.
[0096] Glass fiber: ECS 03 T-187H, purchased from Nippon Electric Glass. Short-cut filaments from E-glass, designed to reinforce engineering thermoplastics such as PBT and PET.
[0097] Antioxidant: Pentaerythritol tetra[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionate (CAS No. 6683-19-8), trade name Irganox® 1010, purchased from BASF.
[0098] Release agent: PETS L342, pentaerythritol tetrastearate, purchased from Faci.
[0099] Lubricant: Oxidized polyethylene wax (CAS No. 68441-17-8), trade name Licowax® PED 521, purchased from Clariant.
[0100] Toughening agent: Ethylene-n-butyl acrylate-co-glycidyl methacrylate (EBA-GMA) (CAS No. 51541-08-3), trade name LOTADER® AX 8750, purchased from Arkema.
[0101] Epon 1002: Bisphenol-A polyepoxy resin with a functionality of 2 (CAS No. 25036-25-3), trade name EPON. TM 1002F was purchased from Hexion.
[0102] ELO: Epoxidized Flaxseed Oil (CAS No. 8016-11-3), trade name Lankroflex TM L, purchased from Valtris Specialty Chemicals.
[0103] CaHPO4: High-pressure compacted, directly compressible porous anhydrous dicalcium phosphate (Dicalcium phosphate), purchased from Sigma-Aldrich.
[0104] CBA C20P: Bruggolen® C20P, N,N'-hexane-1,6-dimethylbis(hexahydro-2-oxo-1H-azaphen-1-carboxamide) (CAS No. 5888-87-9), purchased from Brüggemann.
[0105] method
[0106] The thermomechanical properties and anti-scratch properties of the formulations listed in the table above were studied. For RPET, the formulation was melt-processed using a 40mm twin-screw extruder suitable for glass fiber reinforced PET composites. The temperature distribution in the extruder heating zone was 285℃-280℃-280℃-275℃-275℃-270℃-265℃-265℃ (along the conveying direction), the screw speed was 200 RPM, and the output was approximately 100 kg / hour. The die temperature used for injection molding to produce tensile test specimens was set at 110℃.
[0107] Tensile properties were measured according to ISO 527-2. Hydrolysis resistance was determined by placing the tensile specimen (RPET) in pressure cooker steam at 121°C for 48 hours. This test is referred to as the "Pressure Cooker Test" (PCT) in the table below. The treated specimen was then placed under ambient conditions for at least 24 hours, followed by tensile property determination according to ISO 527-2 as described above. The relative tracking resistance, i.e., the relative tracking index (CTI), of the formulation was determined according to IEC 60112.
[0108] result
[0109] If the above formula is tested according to the method described in this article, the following values can be obtained:
[0110] serial number INV1 INV2 Molded and dried state Fracture stress [MPa] 112 119 128 48 hours later / 121°C, PCT Fracture stress [MPa] 43 52 62 Retention rate [%] 38 44 48 Electro-tracking CTI [V] 275 325 375
[0111] The RPET test results show that the hydrolytic stability of the formulations "INV1" and "INV2" according to the present invention is improved. This formulation comprises a combination of recycled polyethylene terephthalate resin, glass fiber, the epoxy-containing compound EBA-GMA and epoxidized linseed oil, the bis-lactam CBA, and the phosphorus-containing compound dicalcium phosphate. Increasing the content of the phosphorus-containing compound dicalcium phosphate improves hydrolytic stability (as shown by higher fracture stress and retention values) and resistance to electrical tracking (as shown by the higher CTI values of "INV1" and "INV2" compared to "REF"). However, the improved hydrolytic stability and resistance to electrical tracking are only achieved in the presence of other components of the present invention, including CBA.
Claims
1. A composition comprising at least one recycled polyethylene terephthalate resin, glass fiber, at least one epoxy-containing compound, at least one bis-lactam, and at least one phosphorus-containing compound.
2. The composition of claim 1, wherein, At least one of the epoxy-containing compounds is an epoxidized fatty acid ester, wherein the fatty acid ester is preferably selected from flaxseed oil, soybean oil, sunflower seed oil, safflower oil, tung oil, sesame oil, cottonseed oil, castor oil, olive oil, peanut oil, rapeseed oil, coconut oil, babassu oil, palm oil, and fish oil, and most preferably, the epoxidized fatty acid ester is epoxidized flaxseed oil.
3. The composition according to claim 1 or 2, wherein, At least one of the bis-lactams is carbonylbiscaprolactam or N,N'-hexane-1,6-dimethylbis(hexahydro-2-oxo-1H-azaphen-1-carboxamide) or both.
4. The composition according to any one of the preceding claims, wherein, At least one of the phosphorus-containing compounds is selected from metal phosphates, metal phosphonates, and metal hypophosphonates, preferably at least one of calcium hydrogen phosphate and hydroxyapatite.
5. The composition according to any one of the preceding claims, wherein, Based on the total weight of the composition, the total amount of epoxy-containing compounds in the polymer composition, particularly the total amount of epoxidized fatty acid esters, is 0.1 to 5% by weight, preferably 0.5 to 3% by weight, and / or, based on the total weight of the composition, the total amount of bis-lactams in the composition, particularly carbonylbiscaprolactam and one or both of N,N'-hexane-1,6-dimethylbis(hexahydro-2-oxo-1H-azaphen-1-carboxamide), is 0.1 to 5% by weight, preferably 0.5 to 2% by weight, and / or, based on the total weight of the composition, the total amount of phosphorus-containing compounds in the composition, particularly one or both of dicalcium phosphate and hydroxyapatite, is 0.1 to 5% by weight, preferably 0.1 to 2.5% by weight.
6. The composition according to any one of the preceding claims, wherein, Based on the total weight of the composition, the at least one recycled polyethylene terephthalate resin is present in an amount of 40 to 90 percent by weight, preferably 50 to 80 percent by weight.
7. The composition according to any one of the preceding claims, wherein, Based on the total weight of the composition, the amount of glass fiber in the composition is 5 to 80% by weight, more preferably 10 to 50% by weight, and most preferably 25 to 40% by weight.
8. The composition according to any one of the preceding claims further comprises at least one toughening agent at a weight percentage of 0.5 to 15% based on the total weight of the polymer composition.
9. The composition of claim 8, wherein, The toughening agent is selected from glass fiber, methacrylate-butadiene-styrene copolymer, acrylate elastomer, acrylonitrile-styrene-acrylate copolymer, acrylonitrile-butadiene-styrene copolymer, high-rubber grafted acrylonitrile-butadiene-styrene copolymer, acrylate-olefin copolymer, polysiloxane rubber, polysiloxane-acrylic rubber, ethylene-propylene non-conjugated diene elastomer, acrylonitrile-styrene-ethylene-propylene non-conjugated diene elastomer, ethylene-methyl methacrylate-glycidyl methacrylate copolymer, ethylene-n-butyl acrylate-co-glycidyl methacrylate (EBA-GMA) terpolymer rubber and combinations thereof. Preferably, the toughening agent is selected from methacrylate-butadiene-styrene copolymer, acrylate-olefin copolymer, ethylene-methyl methacrylate-glycidyl methacrylate copolymer, ethylene-n-butyl acrylate-co-glycidyl methacrylate (EBA-GMA) terpolymer rubber and combinations thereof.
10. The composition according to any one of the preceding claims, in particular according to claim 7, wherein, The comparative tracking index (CTI) of the polymer composition, as measured by IEC 60112, is at least 450 V, preferably at least 550 V.
11. The composition according to any one of the preceding claims, which is substantially composed of: - At least one recycled polyethylene terephthalate resin, in a weight percentage of 40 to 89%; - 5 to 80% by weight, preferably 10 to 50% by weight, and most preferably 25 to 40% by weight of glass fiber; - 0.1 to 5% by weight, preferably 0.5 to 2% by weight, of at least one bis-lactam, particularly carbonylbiscaprolactam or N,N'-hexane-1,6-dimethylbis(hexahydro-2-oxo-1H-azaphen-1-carboxamide) or both; - 0.1 to 5% by weight, preferably 0.5 to 3% by weight, of at least one epoxy compound, particularly at least one epoxidized fatty acid ester, preferably epoxidized linseed oil; - 0.1 to 5% by weight, preferably 0.1 to 2.5% by weight, of at least one phosphorus-containing compound, particularly at least one metal phosphate; - Optionally, 0.5 to 15% by weight of at least one toughening agent; All of the above are based on the total weight of the polymer composition.
12. A molded article, particularly for bulk materials melted in an extruder, comprising the composition according to any one of claims 1 to 11.
13. An electronic or electrical device comprising a component comprising or substantially consisting of a composition according to any one of claims 1 to 11.
14. The apparatus of claim 13, wherein, The equipment includes a charging gun, inverter, circuit breaker, sensor, relay, electromagnetic coil, connector, electrical box, electronic container and / or switch.
15. A method of manufacturing a shaped article, the shaped article comprising the composition according to any one of claims 1 to 11, wherein, The epoxidized fatty acid ester, particularly epoxidized linseed oil, and the dilactam, particularly carbonyl biscaprolactam and / or N,N'-hexane-1,6-dimethylbis(hexahydro-2-oxo-1H-azaphen-1-carboxamide), are added to and fused with at least one of the at least one recycled polyethylene terephthalate resins, and wherein the at least one phosphorus-containing compound is added to a mixture comprising the epoxidized fatty acid ester, the dilactam, and the recycled polyethylene terephthalate resin, or is added to and fused with at least one of the at least one recycled polyethylene terephthalate resins, preferably, the epoxidized fatty acid ester and the dilactam are premixed and added to and fused with at least one of the at least one semi-aromatic polyester resins.
16. Use of the composition according to any one of claims 1 to 11 for improving the hydrolytic stability of articles made therefrom and / or for enhancing the comparative tracking index (CTI) value of said articles, said composition particularly comprising at least one of at least an epoxidized fatty acid ester, carbonyl biscaprolactam and N,N'-hexane-1,6-dimethylbis(hexahydro-2-oxo-1H-azaphen-1-carboxamide), and at least one of calcium hydrogen phosphate and hydroxyapatite.
Citation Information
Patent Citations
The stabilization of dye images produced in photographic materials
EP0286253A1
Biaxially oriented epoxidised fatty acid derivatives containing hydrolysis resistant polyester film and a chain extender and method for production of same and use of same
EP2184311A1
Polybutylene terephthalate resin composition
EP3323854B1
Process for the modification of terminal groups of polyesters
US3657191A
High-molecular polyamide
WO1998047940A1