Glass fiber filled thermoplastic flame retardant composition

By adding components such as halogen-free flame retardant salts and polysiloxanes to glass fiber-filled polycarbonate materials, the challenge of achieving the UL94 V-0 rating in thin-walled applications has been solved. This enables high-efficiency flame retardancy and improved mechanical properties of halogen-free flame retardant materials at thicknesses of 1.5 mm or 1.2 mm, making them suitable for thin-walled components in various electronic and electrical equipment.

CN123125281APending Publication Date: 2026-11-17SABIC GLOBAL TECHNOLOGIES BV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202580028471.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-19
Filing Date
2025-04-11
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing glass fiber-filled polycarbonate materials struggle to achieve the UL94 V-0 rating in thin-walled applications, especially at thicknesses of 1.5 mm or 1.2 mm, and require the challenge of halogen-free flame retardants. Furthermore, traditional materials face design limitations during the thinning and miniaturization process.

Method used

A composition comprising aromatic polycarbonate, non-adhesive glass fiber, halogen-free flame retardant salt (such as potassium diphenyl sulfonate), polysiloxane and anti-dripping agent is used to ensure UL94 V-0 rating at a thickness of 1.5 mm or 1.2 mm, and mechanical properties are improved by optimizing component ratios and process conditions.

Benefits of technology

It achieves a UL94 V-0 rating for halogen-free flame retardant materials in thin-wall applications, with excellent mechanical properties and flowability, suitable for thin-walled components of a variety of electronic and electrical devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention relates to a thermoplastic composition comprising, by weight, 79-94 wt% of an aromatic polycarbonate, 5-25 wt% of glass fiber (preferably non-bonded glass fiber), 0.10-0.50 wt% of a halogen-free flame retardant salt, 0.2-5 wt% of a polysiloxane, 0-2 wt% of an anti-dripping agent, and 0-3 wt% of other components, wherein the sum of the components is 100 wt%, and wherein the thermoplastic composition has, or is selectively has, a UL94 V0 rating achieved at 1.5 mm. The invention also relates to an article comprising the thermoplastic composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a thermoplastic composition and articles obtained therefrom. Background Technology

[0002] Glass fiber-filled polycarbonate is used in electrical and electronic applications such as MCE (Microcircuit Engineering) protection, television housings, home cable equipment, and microelectronics. These applications are currently facing trends towards thinning and miniaturization, and design limitations exist in terms of flame retardancy and processability (mold filling). Especially for new applications in 5G devices and microelectronics, new glass fiber-filled flame-retardant polycarbonate compositions are needed to replace metal, glass fiber-filled polyamide, or glass fiber-filled PBT materials. The main challenge lies in achieving a UL94 V-0 rating at very low thicknesses (e.g., 1.5 mm or 1.2 mm) using halogen-free (including PFAS-free) or at least bromine- and chlorine-free flame retardants.

[0003] EP2471854 discloses a glass fiber reinforced polycarbonate resin composition comprising: (A) glass fiber reinforced polycarbonate; (B) a mixture of two organosilicon-based compounds comprising (b1) a siloxane compound and (b2) a silicone-based resin; (C) a metal salt-based flame retardant; and (D) a fluorinated polyolefin-based resin. All embodiments in this document rely on the use of Rimar salt (potassium perfluorobutane sulfonate), a fluorinated material.

[0004] CN103709708 discloses a high-flow, glass fiber-reinforced halogen-free flame-retardant polycarbonate material, characterized in that the material is prepared from the following components and parts by weight: 50-90 parts polycarbonate, 10-30 parts glass fiber, 0-10 parts flow modifier, 0-10 parts compatibilizer, 0.1-1 parts halogen-free flame retardant, 0-2 parts flame retardant synergist, 0.1-1 parts lubricant, and 0.1-1 parts antioxidant. This document does not teach or imply how to formulate compositions that achieve a UL94 V0 rating at a thickness of 1.5 mm or even 1.2 mm.

[0005] WO2007 / 094932 discloses a flame retardant composition comprising: (i) 100 parts by weight of polycarbonate; (ii) about 0.0001 to about 0.2 parts by weight of aromatic sulfonate; (iii) about 0.002 to about 0.2 parts by weight of aromatic sulfonate; and (iv) optionally about 0.05 to about 2 parts by weight of siloxane oligomer, wherein a molded sample of the composition is capable of achieving a UL94 V0 rating at a thickness of 3.0 mm.

[0006] Purpose

[0007] One object of the present invention is to provide an improved glass fiber reinforced thermoplastic composition having excellent mechanical and flame-retardant properties. In particular, an object of the present invention is to provide a bromine- and chlorine-free thermoplastic composition suitable for thin-walled applications. Summary of the Invention

[0008] In a first aspect, the present invention relates to a thermoplastic composition comprising a weight based on the thermoplastic composition.

[0009] a) 79-94% by weight of aromatic polycarbonate,

[0010] b) 5-25% by weight of glass fiber, preferably non-bonded glass fiber.

[0011] c) 0.10-0.50% by weight of a halogen-free flame retardant salt, preferably an alkali metal salt of an aromatic sulfonic acid, more preferably a potassium salt of diphenyl sulfone sulfonic acid (KSS) or a sodium salt of toluenesulfonic acid (NaTS) or a combination thereof.

[0012] d) 0.2-5% by weight of polysiloxane,

[0013] e) 0-2% by weight, preferably 0.2-1% by weight, of an anti-dripping agent, and

[0014] f) 0-3% by weight of other components,

[0015] The sum of components a)-f) is 100% by weight, and the thermoplastic composition has or is selectively achieved a UL94 V0 rating at 1.5 mm, preferably at 1.2 mm.

[0016] In a second aspect, the present invention relates to an article comprising the thermoplastic composition.

[0017] The corresponding embodiments of the thermoplastic composition are also applicable to articles according to the invention. Detailed Implementation

[0018] The present invention will now be described in detail.

[0019] Definition List

[0020] The following definitions are used to define the subject matter in this specification and claims. Other terms not listed below are intended to have their commonly accepted meaning in the art.

[0021] As used in this specification, "non-adhesive glass fiber" refers to glass fiber coated with a sizing agent composition that results in poor adhesion between the coated glass fiber and the polycarbonate matrix; in other words, the glass fiber is non-adhesive relative to the aromatic polycarbonate. Individual fibers of the glass fiber filler may not exhibit affinity to the polymer matrix. The term "glass" herein refers broadly to natural or synthetic materials whose main component is silicon dioxide (SiO2) or silica.

[0022] As used in this specification, "adhesive glass fiber" refers to glass fiber coated with a sizing agent composition that results in good / improved adhesion between the coated glass fiber and the polycarbonate matrix; in other words, the glass fiber is adhesive to the aromatic polycarbonate. Individual fibers of the glass fiber filler may exhibit affinity to the polycarbonate resin matrix. This affinity, among many other forces, can be attributed to the glass sizing agent.

[0023] The term "halogen-free flame retardant salt" as used in this specification refers to a flame retardant in salt form that does not contain halogen atoms; in other words, it is free of bromine, chlorine, fluorine, and iodine. Some flame retardants are bromine- and chlorine-free but do contain fluorine, such as Rimar salts (potassium salts of fluoroalkyl sulfonates and perfluorobutane sulfonates). These are not consistent with this invention. This invention relates to...

[0024] thermoplastic composition

[0025] The thermoplastic composition of the present invention comprises the following components: a) one or more aromatic polycarbonates, b) one or more glass fibers, c) one or more halogen-free flame-retardant salts, and d) one or more polysiloxanes. Optionally, the thermoplastic composition further comprises e) one or more anti-dripping agents and f) one or more other components. The sum of components a)-f) is 100% by weight of the thermoplastic composition.

[0026] UL rating

[0027] The thermoplastic composition has or is selectively equipped with a UL94V0 rating, achieved at 1.5 mm, preferably at 1.2 mm.

[0028] An important requirement for this thermoplastic composition is its excellent performance in terms of safety / flammability. UL94 is a safety testing standard for the flammability of plastic materials used in equipment and appliance components, and is a US standard for plastic flammability. This test measures the tendency of a material to extinguish or spread a flame once the specimen is ignited. According to the invention, the rating must be V-0 (V-zero), meaning that flaming combustion on a vertical specimen ceases within 10 seconds. UL ratings can be measured at different thicknesses, which can cause significant variations in the rating. The thicker the specimen, the better the UL rating. For the present invention, a V-0 rating is required for thin specimens with a thickness of 1.5 mm, or even more preferably 1.2 mm. This allows the thermoplastic composition to be used in thin-walled applications.

[0029] HDT

[0030] Heat distortion temperature (HDT) is a measure of a polymer's resistance to deformation under a given load when the temperature rises. It is the temperature at which the polymer deforms under a specified load. Other names for this indicator include "Deflection Temperature Under Load" (DTUL) or "Heat Deflection Temperature Under Load" (HDTUL). HDT is measured according to ISO 75 / Af, 80 × 10 × 4, sp = 64 mm.

[0031] In one embodiment, the thermoplastic composition has, or is selected to have, a heat distortion temperature (HDT) of at least 130°C, preferably at least 132°C.

[0032] Detailed Implementation Plan

[0033] In one specific embodiment, the thermoplastic composition comprises a weight based on the composition.

[0034] a) 79-94% by weight of aromatic polycarbonate (preferably 79.0-94.0% by weight),

[0035] b) 7-13% by weight of non-bonded glass fiber (preferably 7.0-13.0% by weight),

[0036] c) 0.15-0.30% by weight of a halogen-free flame retardant salt, preferably a potassium salt of diphenyl sulfone sulfonic acid (KSS).

[0037] d) 0.8-1.5% by weight of polysiloxane,

[0038] e) 0.2-1% by weight of anti-dripping agent (preferably 0.20-1.0% by weight),

[0039] f) 0-3% by weight of other components (preferably 0.0-3.0% by weight).

[0040] Aromatic polycarbonate

[0041] The thermoplastic composition comprises (as component a) one or more aromatic polycarbonates in an amount of 79 to 94 by weight based on the total weight of the thermoplastic composition.

[0042] In one embodiment, the thermoplastic composition comprises one or more bisphenol A polycarbonates as aromatic polycarbonates, preferably bisphenol A homopolymers. In another embodiment, the thermoplastic composition does not contain any other polymer components.

[0043] In one embodiment, the melt volume rate (MVR) of the thermoplastic composition is 6 to 20 cc / 10 min, for example 7 to 20 cc / 10 min, preferably 10 to 15 cc / 10 min, measured according to ISO 1133 at 300°C and 1.2 kg load.

[0044] In one embodiment, the aromatic polycarbonate is a blend of two or more aromatic polycarbonates with different weight-average molecular weights, preferably a blend of a first polycarbonate with a melt volumetric rate (MVR) of 3 to 10 cc / 10 min and a second polycarbonate with a melt volumetric rate (MVR) of 20 to 35 cc / 10 min, the MVR being measured according to ISO 1133 at 300°C and a 1.2 kg load.

[0045] Even more preferably, the aromatic polycarbonate is a blend of a first bisphenol A polycarbonate homopolymer with a melt volumetric rate (MVR) of 3 to 10 cc / 10 min and a second bisphenol A polycarbonate homopolymer with a melt volumetric rate (MVR) of 20 to 35 cc / 10 min, the MVR being measured according to ISO 1133 at 300°C and 1.2 kg load.

[0046] In one embodiment, the aromatic polycarbonate is a blend of two polycarbonates, preferably a blend of two bisphenol A polycarbonate homopolymers, more preferably having different MVRs as directly discussed above, wherein the ratio (also referred to as the proportion) of the two polycarbonates is 10:90 to 90:10, for example 20:80 to 80:20, or 30:70 to 70:30, or 40:60 to 60:40, for example 50:50.

[0047] Fiberglass

[0048] The thermoplastic composition comprises (as component b) one or more glass fibers in an amount of 5-25% by weight based on the total weight of the thermoplastic composition. In one embodiment, the amount of glass fibers is 5 to 15% by weight, preferably 7 to 13% by weight.

[0049] In one embodiment, the composition comprises non-bonded glass fibers. In another embodiment, substantially all glass fibers in the thermoplastic composition are non-bonded glass fibers.

[0050] Glass fibers can be selected from E-glass, S-glass, AR-glass, T-glass, D-glass, and R-glass, particularly from E-glass, S-glass, and combinations thereof, and more particularly from E-glass or EC glass. Glass fibers can be manufactured using standard processes, such as steam or air blowing, flame blowing, and mechanical drawing. Exemplary glass fibers for polycarbonate reinforcement are manufactured by mechanical drawing.

[0051] In the preparation of unbonded or bonded glass fibers, multiple filaments can be formed simultaneously, sized with a coating agent, and then bundled into a so-called filament bundle. Alternatively, the filaments can be bundled first, and then sized. The amount of sizing agent is typically sufficient to bond the glass filaments into a continuous filament bundle, ranging from about 0.1 to about 5% by weight or about 0.1 to 2% by weight based on the weight of the glass fibers. Typically, it can be about 1.0% by weight based on the weight of the glass fibers.

[0052] Glass fibers can be continuous or chopped. In some instances, glass fibers are chopped glass fibers in the form of chopped bundles, for example, with lengths from about 0.3 mm to about 10 cm, specifically from about 0.5 mm to about 5 cm, more specifically from about 1.0 mm to about 2.5 cm, for example from 0.2 mm to 20 mm, or from about 0.2 mm to about 10 mm.

[0053] Glass fibers can have circular (or annular), flat, or irregular cross-sections. The width or diameter of unbonded glass fibers can be from about 1 to about 20 µm, or from about 5 to about 20 µm, or from about 5 to about 15 µm.

[0054] Flame retardant salt

[0055] The thermoplastic composition contains (as component c) one or more halogen-free flame retardant salts in an amount of 0.10 to 0.50 by weight based on the total weight of the thermoplastic composition.

[0056] Preferably, the flame retardant salt is an alkali metal salt of an aromatic sulfonic acid, such as a potassium salt. In one embodiment, the flame retardant salt is a potassium salt of diphenyl sulfone sulfonic acid (KSS) or a sodium salt of toluenesulfonic acid (NaTS), or a combination thereof.

[0057] In one embodiment, a salt that is bromine-free, chlorine-free, and free of perfluoroalkyl sulfonates is involved.

[0058] Polysiloxane

[0059] The thermoplastic composition comprises (as component d) one or more polysiloxanes in an amount of 0.2 to 5% by weight based on the total weight of the thermoplastic composition. When more than one polysiloxane is present, the above amount is the total amount of all polysiloxanes.

[0060] In one embodiment, the polysiloxane is a homopolymer of siloxane (i.e., organosilicon) containing a silicon-oxygen backbone with organic groups, such as methyl groups, attached to the silicon atoms.

[0061] In one embodiment, the polysiloxane is in liquid form. In one embodiment, the polysiloxane of the present invention does not include polysiloxanes coated on or otherwise loaded onto solid materials, such as polysiloxane-treated talc.

[0062] Anti-dripping agent

[0063] The thermoplastic composition optionally includes (as component e) one or more anti-dripping agents in an amount of 0 to 2% by weight, preferably 0.2 to 1% by weight, based on the total weight of the thermoplastic composition.

[0064] In one implementation, the anti-dripping agent is polytetrafluoroethylene (PTFE) or PTFE-coated styrene-acrylonitrile copolymer (TSAN). These types of anti-dripping agents are so-called PFAS compounds. Perfluorinated and polyfluoroalkyl substances (PFAS) are synthetic chemicals used in many products, but are currently under review for environmental reasons. Reducing the amount of PFAS used is desirable.

[0065] Other components

[0066] The thermoplastic composition optionally contains (as component f) one or more other components in an amount of 0 to 3 by weight based on the total weight of the thermoplastic composition.

[0067] In one embodiment, the other components include plasticizers, antistatic agents, impact modifiers, colorants, antioxidants, release agents, UV absorbers, lubricants, or foaming agents, or combinations of two or more thereof.

[0068] Products / Applications

[0069] In one embodiment, the articles of manufacture are selected from the group consisting of: aerospace and aircraft components, (electric) vehicle components, electrical and electronic components, energy production and storage components, communication infrastructure or infrastructure components, sports and leisure articles, building components, and industrial components.

[0070] Examples of aerospace and aircraft components include rudders, elevators, fuselages, landing gear doors, wing leading and trailing edge components, fuel tanks, and floors. Examples of (electric) vehicle components include automotive parts such as air deflectors and spoilers, intake manifolds, battery housings and covers, bumpers and bumper beams, cylinder head covers (e.g., valves, rocker arms, camshafts), window / sunroof frames, front grille opening panels, headlight housings for forward-facing headlights, heat shields (e.g., engines, transmissions), pillars, and covers; or marine (e.g., superyachts, racing boats, workboats, and recreational boats) components such as hulls, frames, keels, masts, poles and sails, carbon fiber winch drums, shafting, bearings, propellers, commercial hatch covers, exhaust systems, and superstructures.

[0071] Examples of electrical and electronic components are electrical housings, power outlets, battery housings—for example, for smartphones, computers or other electrical devices—microprocessors, (miniature or small) circuit breakers, circuit protection devices, and the housings or components of personal computers and (5G) industrial computers.

[0072] Examples of energy production and storage components include turbine blades and rotor blades for onshore and offshore wind turbines, multifunctional energy storage composites (MESCs), hydrogen tanks for aerospace, hydrogen fuel cells, and battery cells.

[0073] Examples of communication infrastructure components include 5G infrastructure and components of mobile devices, such as antenna systems.

[0074] Examples of infrastructure components are those used to reinforce concrete (e.g., bridges) or to replace steel reinforcement (e.g., in bridge decks or other outdoor concrete pavement structures).

[0075] Examples of sports and leisure products include fishing rods, tennis rackets, kayak paddle shafts / axles, windsurfing masts and boards, hockey sticks, kites, and bicycle handlebars, as well as niche applications such as fairings for recumbent bicycles.

[0076] Examples of building components include interior or exterior building panels, pipes, conduits, and storage tank installations.

[0077] Examples of industrial components are pipe, conduit, and storage tank installations used in i) (chemical) manufacturing plants, ii) oil and gas extraction, processing, and transportation, or iii) (waste) water treatment.

[0078] Those skilled in the art, upon studying the accompanying drawings, this disclosure, and the appended claims, can understand and implement other variations of the disclosed embodiments when practicing the claimed invention. In the claims, the word "comprising / including" does not exclude other elements or steps, and the indefinite articles "a" or "an" do not exclude a plurality. The fact that certain means are described in mutually different dependent claims does not indicate that a combination of these means cannot be used to produce advantageous effects. The scope of the invention is defined by the appended claims. One or more objects of the invention are achieved by the appended claims.

[0079] Example

[0080] The present invention is further illustrated below with reference to embodiments. These embodiments are merely exemplary and should not be regarded as limiting the present invention.

[0081] Table 1: Materials used in the examples

[0082]

[0083] method

[0084] Melt volumetric rate (MVR) was measured according to ISO 1133 at 300°C under a 1.2 kg load and a residence time of 5 minutes. The granules were dried at 100°C for 4 hours. MVR is expressed in cubic centimeters (cc or cm³) of polymer melt. 3 ) / 10-minute report.

[0085] The flammability rating (V0 flammability test) was conducted according to the procedure outlined in Underwriters Laboratories Notice 94, "Flammability Testing of Plastic Materials, UL 94". According to this procedure, materials can be classified as V0, V1, or V2 based on test results obtained from samples of specified thickness. Samples were prepared using standard ASTM molding standards according to the UL 94 test procedure. It should be noted that when a V0 rating is given for a specified thickness, a V0 rating can also be obtained at greater thicknesses. Samples were aged at 23 ± 2°C and 50% relative humidity for 48 hours, or at 70°C for 168 hours, and then subjected to vertical burning. The criteria for each flammability classification tested are described below.

[0086] V0: In samples placed with their long axis at a 180-degree angle to the flame, after the ignition flame is removed, the longest duration of flaming combustion and / or smoldering does not exceed 10 seconds. Vertically placed samples do not produce burning particles dripping from the absorbent cotton, and no sample burns to the clamping fixture after flaming combustion or heating. The criteria for V-0 flammability classification are: single flame time ≤ 10 seconds, and total flame time of 5 samples ≤ 50 seconds.

[0087] V1 and V2: In samples placed with their long axis at a 180-degree angle to the flame, after the ignition flame is removed, the average time for flaming combustion and / or smoldering does not exceed 30 seconds. For V1, vertically placed samples do not produce burning droplets that ignite the absorbent cotton. The V2 standard is the same as V1, except that it allows flame droplets that ignite the cotton. The criteria for V-1 flammability classification are: single flame time ≤ 20 seconds, and total flame time of 5 samples ≤ 250 seconds. The criteria for V-2 flammability classification are: single flame time ≤ 30 seconds, and total flame time of 5 samples ≤ 250 seconds.

[0088] Heat distortion temperature (HDT) measurements were performed according to ISO 75 / Af-1:2020 (Method A, flat) on an 80 mm × 10 mm × 4 mm unannealed specimen with a span of 64 mm, a load of 1.8 MPa, and a heating rate of 120°C / h. Results were reported in degrees Celsius.

[0089] Unnotched cantilever beam impact strength (“UNII”) was measured according to ISO 180:2019 on an 80 mm × 10 mm × 4 mm spline at 23 ± 2°C using an 11 joule pendulum. Results are expressed in kJ / m. 2 Report to the unit.

[0090] Tensile modulus (TM) measurements were performed using a universal testing machine (UTM) in accordance with ISO 527-1:2019 as a stress-strain test at speeds of 1 mm / min (extensometer) and 5 mm / min (test speed), and results were reported in MPa.

[0091] Extrusion process of blends

[0092] The ZSK-25 mixer is used, equipped with a 1040 mm cylinder and a 3 mm double-strand die head with a die head temperature of 280°C. The following temperature profiles are used: Zone 1 (feed) 40°C; Zone 2 170°C; Zone 3 220°C; Zone 4 240°C; Zones 5-6 255°C; Zone 7 270°C; Zones 8-10 280°C. The screw speed is 300 rpm, the output is 9-10 kg / h, the torque is 60-65%, the vacuum is -0.08 MPa, and the side feeder is located in Zone 6.

[0093] The injection molding process for glass fiber filled polycarbonate flame-retardant resin is shown in the table below.

[0094] Table 2: Injection Molding Process Conditions

[0095]

[0096] The effect of using polysiloxane

[0097] To demonstrate the effect of using polysiloxane as a synergist in combination with a halogen-free flame retardant in glass fiber-filled thermoplastic compositions, five thermoplastic compositions were prepared: Comparative Example 1 (CE1) contained no flame retardant or synergist; Comparative Example 2 (CE2) used KSS as a flame retardant but contained no synergist; Comparative Example 3 (CE3) used KSS as a flame retardant and kaolin as a synergist; Comparative Example 4 (CE4) used KSS as a flame retardant and PPZ as a synergist; and Invention Example 1 (IE1) used KSS as a flame retardant and polysiloxane as a synergist. These compositions were tested for UNII, HDT, UL-94 at 1.5 mm and 1.2 mm, and the MVR was measured. Table 3 below shows the compositions and results.

[0098] Table 3: Effects of using polysiloxanes as synergists and other synergists

[0099]

[0100] The results clearly demonstrate that the combination of halogen-free flame retardant (KSS) with polysiloxane as a synergist provides very robust flame retardancy, achieving a V-0 value at 1.2 mm, and exhibiting high HDT and fairly good flowability.

[0101] The amount of flame retardant material used

[0102] Experiments were conducted to optimize the amount of flame-retardant material used; in other words, to achieve good flame-retardant performance while reducing the amount used.

[0103] To demonstrate the effect of the amount of flame retardant material in glass fiber-filled thermoplastic compositions, thermoplastic compositions were prepared: Invention Example 3a (IE3a) contained 0.2% by weight of KSS, and Invention Example 4 (IE4) contained 0.3% by weight of KSS. These compositions were tested under UNII, HDT, UL-94 at 1.5 mm and 1.2 mm, and the MVR was measured.

[0104] In addition, compositions without the UV stabilizer (STAB 2) were prepared. These compositions (IE2 and IE3b) were tested for UNII, HDT, UL-94 at 1.5 mm and 1.2 mm, and the MVR was measured. Table 4 below shows the compositions and results for all these examples.

[0105] Table 4: Effect of UV stabilizer usage and flame retardant dosage

[0106]

[0107] The results clearly demonstrate that a flame retardant dosage of more than 0.1% by weight is required to provide the desired UL94 rating.

[0108] Evaluation of different polycarbonate blends

[0109] Experiments were conducted to optimize the type of polycarbonate. To demonstrate whether the type of polycarbonate had an impact, five thermoplastic compositions were prepared: Invention Examples 5a-c (IE5a, IE5b, and IE5c) for interfacial PC and Invention Examples 6a-b (IE6a and IE6b) for melt-processed PC. Three different interfacial PC blends were tested, each with a different ratio of high-MVR to low-MVR components; one composition also contained a UV stabilizer. Two different melt-processed PC blends were tested, one with a quencher and one without. The five compositions were tested for UNII, HDT, and UL-94 at 1.5 mm 1.2 mm, and the MVR was measured. The compositions and results are shown in Table 5 below.

[0110] Table 5: Effects of using different PC blends

[0111]

[0112] The results clearly demonstrate that all blends of PC, whether produced by the interfacial or melt-process method, offer excellent flame retardant properties and high HDT over a wide range of MVR values.

[0113] Optimization of anti-dripping agent dosage

[0114] Experiments were conducted to optimize the amount of anti-dripping agent. To demonstrate the effect of anti-dripping agent dosage, four thermoplastic compositions were prepared: Invention Examples IE7a-d (IE7a, IE7b, IE7c, and IE7d). These four compositions were tested for UL-94 at UNII, HDT, 1.5 mm, and 1.2 mm, and the MVR was measured.

[0115] Table 6: Effects of using different dosages of anti-drip agent

[0116]

[0117] The above results clearly demonstrate that even at lower anti-dripping agent dosages, sufficient to good flame retardant results and high HDT can be obtained.

[0118] Effects of different types of polysiloxanes

[0119] Experiments were conducted to optimize the type of polysiloxane. To demonstrate the effects of different types of polysiloxanes, six thermoplastic compositions were prepared: Examples 8a-b (IE8a, IE8b), Examples 9a-b (IE9a, IE9b), and Examples 10a-b (IE10a, IE10b). These six compositions were tested for UNII, HDT, UL-94 at 1.5 mm and 1.2 mm, and the MVR was measured.

[0120] Table 7: Effects of using different types of polysiloxanes

[0121]

[0122] The above results clearly demonstrate that both types of PC can achieve excellent flame retardancy and high HDT using SG 1 and SG 2, both DMS polymers. The composite containing SG 1 exhibits toughness behavior in both interfacial and melt-processed PC. The composite containing SG 2 and SG 3 exhibits toughness behavior only in interfacial PC.

Claims

1. A thermoplastic composition comprising, by weight based on the thermoplastic composition, a) 79-94% by weight of aromatic polycarbonate, b) 5-25% by weight of glass fiber, preferably non-bonded glass fiber. c) 0.10-0.50% by weight of a halogen-free flame retardant salt, preferably an alkali metal salt of an aromatic sulfonic acid, more preferably a potassium salt of diphenyl sulfone sulfonic acid (KSS) or a sodium salt of toluenesulfonic acid (NaTS) or a combination thereof. d) 0.2-5% by weight of polysiloxane, e) 0-2% by weight, preferably 0.2-1% by weight, of an anti-dripping agent, and f) 0-3% by weight of other components, The sum of components a)-f) is 100% by weight, and the thermoplastic composition has or is selectively achieved a UL94 V0 rating at 1.5 mm, preferably at 1.2 mm.

2. The thermoplastic composition according to claim 1, having or selectively having a heat distortion temperature (HDT) of at least 130°C, preferably at least 132°C.

3. The thermoplastic composition according to claim 1 or 2, having or selectively having a melt volume rate (MVR) of less than 10 cc / 10 min.

4. The thermoplastic composition according to any one of the preceding claims, wherein the aromatic polycarbonate is a bisphenol A polycarbonate, preferably a bisphenol A homopolymer; preferably wherein the thermoplastic composition does not contain any polymer component as other components.

5. The thermoplastic composition according to any one of the preceding claims, wherein the amount of glass fiber is 5-15% by weight, preferably 7-13% by weight.

6. The thermoplastic composition according to any one of the preceding claims, wherein the polysiloxane is a homopolymer of a siloxane, preferably a homopolymer of a dimethylsiloxane.

7. The thermoplastic composition according to any one of the preceding claims, wherein the other components comprise a plasticizer, an antistatic agent, an impact modifier, a colorant, an antioxidant, a release agent, a UV absorber, a lubricant, or a foaming agent, or a combination of two or more thereof.

8. The thermoplastic composition according to any one of the preceding claims has a melt volumetric rate (MVR) of 6 to 20 cc / 10 min, preferably 7 to 20 cc / 10 min, more preferably 10 to 15 cc / 10 min, measured according to ISO 1133 at 300°C and under a 1.2 kg load.

9. The thermoplastic composition according to any one of the preceding claims, wherein the aromatic polycarbonate is a blend of two or more aromatic polycarbonates having different weight-average molecular weights, preferably a blend of a first polycarbonate with a melt volumetric rate (MVR) of 3 to 10 cc / 10 min and a second polycarbonate with a melt volumetric rate (MVR) of 20 to 35 cc / 10 min, the MVR being measured according to ISO 1133 at 300°C and 1.2 kg load.

10. The thermoplastic composition according to any one of the preceding claims, comprising, by weight of the composition, a) 79 to 94% by weight of aromatic polycarbonate, b) 7-13% by weight of non-bonded glass fiber, c) 0.15-0.30% by weight of a halogen-free flame retardant salt, preferably a potassium salt of diphenyl sulfone sulfonic acid (KSS). d) 0.8-1.5% by weight of polysiloxane, e) 0.2-1% by weight of anti-dripping agent, f) 0-3% by weight of other components.

11. An article comprising the thermoplastic composition according to claims 1-10.

12. The article of claim 11, wherein the article is selected from the group consisting of: aerospace and aircraft components, (electric) vehicle components, electrical and electronic components, energy production and storage components, communication infrastructure or infrastructure components, sports and leisure articles, building components, and industrial components.

Citation Information

Patent Citations

  • Glass fiber reinforced polycarbonate resin composition with excellent flame retardancy

    EP2471854A1