Polyphenylene sulfide resin compositions and molded articles
By mixing non-fibrous inorganic fillers and organosilicon compounds into PPS resin and controlling the particle size distribution, and combining fibrous inorganic fillers and elastomers, the problems of leakage current tracking resistance and thermal shock resistance of PPS resin under high voltage environment are solved, thereby improving safety and design freedom, and making it suitable for lightweighting and miniaturization of electrical and electronic components.
Patent Information
- Application Number
- CN202580027373.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-05-13
- Filing Date
- 2025-05-09
- Publication Date
- 2026-11-17
AI Technical Summary
Existing polyphenylene sulfide (PPS) resins lack sufficient resistance to tracking and thermal shock under high voltage conditions, limiting their application in fields such as electric vehicles.
By mixing non-fibrous inorganic fillers and organosilicon compounds into PPS resin, the standard deviation of its particle size distribution is controlled, and fibrous inorganic fillers and elastomers are added to improve the resin's resistance to tracking and thermal shock.
It achieves safety and design freedom for PPS resin molded products under high voltage environments, ensures that creepage distances meet standards, is suitable for complex-shaped metal insert molded products, and supports the miniaturization and weight reduction of electrical and electronic components.
Smart Images

Figure FT_1 
Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to polyphenylene sulfide resin compositions and their molded articles that exhibit excellent resistance to tracking and thermal shock. Background Technology
[0002] Polyphenylene sulfide (PPS) resin is an engineering plastic with excellent heat resistance, flame retardancy, chemical resistance, electrical insulation, resistance to damp heat, mechanical strength, and dimensional stability. PPS resin can be molded into various molded products, fibers, films, etc. through various molding methods such as injection molding and extrusion molding, and therefore it is used in a wide range of fields such as electrical and electronic components, mechanical components, and automotive components.
[0003] In recent years, with the increasing power of electric vehicles, the heat generation has tended to increase, thus increasing the demand for resin compositions with excellent heat resistance, such as PPS resin.
[0004] In addition, electric vehicles use many metal-embedded resin molded parts such as busbars, current sensors, and power modules. These require resin compositions with excellent resistance to thermal shock, which will not cause cracks in the metal inserts even when the ambient temperature changes.
[0005] On the other hand, PPS resin is inferior to other engineering plastics such as polyamide resin and polyester resin in terms of tracking damage caused by applying high voltage to the surface of insulators.
[0006] Therefore, although PPS resin exhibits excellent properties in terms of heat resistance, flame retardancy, chemical resistance, electrical insulation, resistance to damp heat, mechanical strength, and dimensional stability, its use is limited when exposed to high voltage environments. From the perspective of the increasing output of electric vehicles and their adaptation to fast charging in recent years, there is a trend towards higher rated voltages. Furthermore, from the perspective of component miniaturization and weight reduction, the necessity of ensuring that the creepage distance of components exceeds the necessary creepage distance specified in IEC 60664 is becoming increasingly important. Therefore, PPS resin with excellent resistance to tracking is required.
[0007] To date, attempts have been made to improve the tracking resistance of PPS resin. For example, Patent Document 1 describes improving tracking resistance by adding magnesium hydroxide and an ethylene-vinyl alcohol copolymer to PPS resin. Patent Document 2 describes stabilizing the production of PPS resin with excellent tracking resistance by adding magnesium hydroxide with a high apparent density to PPS resin.
[0008] Existing technical documents
[0009] Patent documents
[0010] Patent Document 1: Japanese Patent Application Publication No. 2014-145006
[0011] Patent Document 2: International Publication No. 2015 / 137228 Summary of the Invention
[0012] The problem that the invention aims to solve
[0013] However, while the resin composition described in Patent Document 1 improves resistance to tracking by incorporating large amounts of magnesium hydroxide and ethylene-vinyl alcohol copolymers, it does not specifically address resistance to thermal shock. Furthermore, it is believed that the compositions specifically shown in the examples, due to the large amount of magnesium hydroxide with small particle size and a small standard deviation in particle size distribution, do not exhibit sufficient resistance to thermal shock.
[0014] While the resin composition described in Patent Document 2 improves resistance to tracking by incorporating a large amount of magnesium hydroxide, it does not specifically describe resistance to thermal shock. Furthermore, it is believed that the resin composition specifically shown in the examples lacks sufficient resistance to thermal shock because it does not incorporate irregularly shaped glass or elastomers.
[0015] In view of the above, the objective of the present invention is to provide a PPS resin composition and its molded articles that have high safety when used in components subjected to high voltage, and do not crack even when used in environments with varying temperatures.
[0016] Problem-solving methods
[0017] To address the aforementioned issues, the present invention employs the following solution:
[0018] [1]. A polyphenylene sulfide resin composition, which is a polyphenylene sulfide resin composition mixed with polyphenylene sulfide resin, has a tracking resistance of 300V or more and a thermal shock resistance of more than 15 cycles when using metal insert molded articles.
[0019] [2]. The polyphenylene sulfide resin composition as described in [1] is a polyphenylene sulfide resin composition in which 20 parts by weight and 170 parts by weight of (B) non-fibrous inorganic filler are mixed with 100 parts by weight of (A) polyphenylene sulfide resin, wherein the standard deviation of the particle size distribution of (B) non-fibrous inorganic filler is 0.22 or more and 10.00 or less.
[0020] [3]. The polyphenylene sulfide resin composition as described in [1] or [2], wherein the (B) non-fibrous inorganic filler is a decomposition endothermic filler.
[0021] [4]. The polyphenylene sulfide resin composition as described in any one of [1] to [3] is mixed with 0.1 parts by weight and 20 parts by weight of organosilicon compound (E) relative to 100 parts by weight of polyphenylene sulfide resin (A).
[0022] [5]. A polyphenylene sulfide resin composition comprising, relative to 100 parts by weight of (A) polyphenylene sulfide resin, 20 parts by weight and 170 parts by weight of (B) non-fibrous inorganic filler, wherein the standard deviation of the particle size distribution of (B) non-fibrous inorganic filler is 0.22 or more and 10.00 or less, and (B) non-fibrous inorganic filler is a decomposition endothermic filler, and relative to 100 parts by weight of (A) polyphenylene sulfide resin, 0.1 parts by weight and 20 parts by weight of (E) organosilicon compound.
[0023] [6]. The polyphenylene sulfide resin composition according to any one of [2] to [5], wherein the average particle size of the (B) non-fibrous inorganic filler is 1.0 μm or more and 50.0 μm or less.
[0024] [7]. The polyphenylene sulfide resin composition according to any one of [1] to [6], wherein the 10%D of the (B) non-fibrous inorganic filler is 0.1 μm or more and 1.2 μm or less.
[0025] [8]. The polyphenylene sulfide resin composition according to any one of [1] to [7] is mixed with 40 parts by weight and 190 parts by weight of fibrous inorganic filler (C) relative to 100 parts by weight of polyphenylene sulfide resin (A).
[0026] [9]. The polyphenylene sulfide resin composition as described in any of [1] to [8], wherein the (C) fibrous inorganic filler is shaped cross-section glass fiber.
[0027]
[10] . The polyphenylene sulfide resin composition according to any one of [1] to [9] is mixed with 1 or more and 40 or less of elastomer (D) relative to 100 parts by weight of polyphenylene sulfide resin (A).
[0028]
[11] . A molded article formed from a polyphenylene sulfide resin composition according to any one of [1] to
[10] .
[0029]
[12] . A metal insert molded article comprising the molded article described in
[11] .
[0030]
[13] . An automotive electrical component comprising the molded article described in
[11] .
[0031]
[14] . An electric drive axle comprising the molded article described in
[11] .
[0032]
[15] . An electric vehicle (xEV) comprising the molded article described in
[11] .
[0033] Invention Effects
[0034] The PPS resin composition of the present invention provides high safety for molded articles when used in components subjected to high voltage. Furthermore, it ensures that the creepage distance of the molded article exceeds the necessary creepage distance specified in IEC 60664. Therefore, molded articles made from the PPS resin composition of this application offer increased design freedom and facilitate miniaturization and weight reduction. Additionally, metal insert molded articles made using the PPS resin composition of the present invention do not crack even when used in environments with varying temperatures, thus making them suitable for various complex shapes of metal insert molded articles.
[0035] The molded articles of the present invention can be well used in automotive electrical components such as current sensors and busbars, and electrical and electronic components such as power semiconductor housings. Attached Figure Description
[0036] Figure 1 This is a schematic diagram of a molded article used for evaluating resistance to thermal shock. Detailed Implementation
[0037] The embodiments of the present invention will be described in detail below.
[0038] (A) PPS resin
[0039] The PPS resin used in the embodiments of the present invention is a polymer having repeating units as shown in the following structural formula.
[0040]
[0041] From the viewpoint of heat resistance, PPS resin is preferably a polymer containing 70 mol% or more, and more preferably 90 mol% or more, of the repeating units shown in the above structural formula. Additionally, less than 30 mol% of the repeating units in the PPS resin may also be composed of repeating units having a structure selected from the following structures.
[0042]
[0043] PPS copolymers that incorporate these structures as part of their structure have a lower melting point, thus making such PPS polymers advantageous in terms of moldability.
[0044] When the total PPS resin composition is set to 100% by weight, the content of (A)PPS resin is preferably 10% by weight or more and 50% by weight or less. The lower limit of the content is more preferably 20% by weight or more, and even more preferably 25% by weight or more. The upper limit of the content is more preferably 40% by weight or less, and even more preferably 35% by weight or less. By setting the content of (A)PPS resin to 10% by weight or more, the proportion of the main resin component responsible for strength in the PPS resin composition increases, thus the weld line tensile strength of the PPS resin composition can be set to 30 MPa or more. By setting the content of (A)PPS resin to 50% by weight or less, the concentration of easily carbonizable PPS resin becomes less in the overall PPS resin composition, thus the tracking resistance of the PPS resin composition can reach 300V or more.
[0045] Hereinafter, the manufacturing method of the PPS resin used in the embodiments of the present invention will be described, but the method is not limited to the above method as long as the PPS resin with the above structure can be obtained.
[0046] First, the contents of the polyhalogenated aromatic compounds, vulcanizing agents, polymerization solvents, molecular weight regulators, polymerization aids, and polymerization stabilizers used in the manufacturing method will be explained.
[0047] [Polyhalogenated aromatic compounds]
[0048] Polyhalogenated aromatic compounds refer to compounds having two or more halogen atoms in one molecule. Specific examples include p-dichlorobenzene, m-dichlorobenzene, o-dichlorobenzene, 1,3,5-trichlorobenzene, 1,2,4-trichlorobenzene, 1,2,4,5-tetrachlorobenzene, hexachlorobenzene, 2,5-dichlorotoluene, 2,5-dichlorop-xylene, 1,4-dibromobenzene, 1,4-diiodobenzene, and 1-methoxy-2,5-dichlorobenzene, with p-dichlorobenzene being preferred. Alternatively, two or more different polyhalogenated aromatic compounds can be combined to form copolymers, but p-dihalogenated aromatic compounds are preferably used as the main component.
[0049] From the viewpoint of obtaining a PPS resin with a viscosity suitable for processing, the amount of polyhalogenated aromatic compound supplied to the manufacturing process is preferably 0.9 mol or more, more preferably 0.95 mol or more, and even more preferably 1.005 mol or more, relative to 1 mole of vulcanizing agent. Regarding the upper limit, the amount of polyhalogenated aromatic compound is preferably 2.0 mol or less, more preferably 1.5 mol or less, and even more preferably 1.2 mol or less, relative to 1 mole of vulcanizing agent.
[0050] [Vulcanizing agent]
[0051] Examples of sulfiding agents include alkali metal sulfides, alkali metal hydrogen sulfides, and hydrogen sulfide.
[0052] Specific examples of alkali metal sulfides include lithium sulfide, sodium sulfide, potassium sulfide, rubidium sulfide, cesium sulfide, and mixtures of two or more thereof, with sodium sulfide being preferred. These alkali metal sulfides can be used as hydrates or aqueous mixtures or in anhydrous form.
[0053] Specific examples of alkali metal hydrosulfides include sodium hydrosulfide, potassium hydrosulfide, lithium hydrosulfide, rubidium hydrosulfide, cesium hydrosulfide, and mixtures of two or more of these, with sodium hydrosulfide being preferred. These alkali metal hydrosulfides can be used as hydrates or aqueous mixtures, or in anhydrous form.
[0054] Alternatively, alkali metal sulfides can be prepared in situ in the reaction system from alkali metal hydrogen sulfides and alkali metal hydroxides. Furthermore, alkali metal sulfides can be prepared from alkali metal hydrogen sulfides and alkali metal hydroxides and then transferred to a polymerization tank for use.
[0055] Alternatively, alkali metal sulfides can be prepared in situ in the reaction system from alkali metal hydroxides such as lithium hydroxide and sodium hydroxide and hydrogen sulfide. Furthermore, alkali metal sulfides can be prepared from alkali metal hydroxides such as lithium hydroxide and sodium hydroxide and hydrogen sulfide, and then transferred to a polymerization tank for use.
[0056] In this specification, the amount of vulcanizing agent "added" refers to the remaining amount after subtracting the loss of the vulcanizing agent from the actual amount of vulcanizing agent added, in cases where a portion of the vulcanizing agent is lost before the start of the polymerization reaction due to dehydration operations, etc.
[0057] Alternatively, alkali metal hydroxides and / or alkaline earth metal hydroxides may be used in conjunction with a vulcanizing agent. Specific examples of alkali metal hydroxides include, for instance, sodium hydroxide, potassium hydroxide, lithium hydroxide, rubidium hydroxide, cesium hydroxide, and mixtures of two or more of these. Specific examples of alkaline earth metal hydroxides include, for instance, calcium hydroxide, strontium hydroxide, and barium hydroxide. Sodium hydroxide is preferred.
[0058] When using alkali metal hydrogen sulfide as a vulcanizing agent, it is particularly preferable to use alkali metal hydroxide simultaneously. Regarding the amount of alkali metal hydroxide used, the lower limit relative to 1 mole of alkali metal hydrogen sulfide is preferably 0.95 moles or more, more preferably 1.00 moles or more, and even more preferably 1.005 moles or more. Regarding the upper limit relative to 1 mole of alkali metal hydrogen sulfide, it is preferably 1.2 moles or less, more preferably 1.15 moles or less, and even more preferably 1.100 moles or less.
[0059] [Polymerization solvent]
[0060] As polymerization solvents, polar organic solvents are preferred. Specific examples include N-alkylpyrrolidones such as N-methyl-2-pyrrolidone and N-ethyl-2-pyrrolidone; caprolactams such as N-methyl-ε-caprolactam; aprotic organic solvents such as 1,3-dimethyl-2-imidazolium ketone, N,N-dimethylacetamide, N,N-dimethylformamide, hexamethylphosphoric triamine, dimethyl sulfone, and tetramethylene sulfoxide; and mixtures thereof. These polymerization solvents are preferred due to their high reaction stability. Among them, N-methyl-2-pyrrolidone (hereinafter sometimes simply referred to as "NMP") is particularly preferred.
[0061] The amount of organic polar solvent used in the manufacturing process is preferably 2.0 moles or more, more preferably 2.25 moles or more, and even more preferably 2.5 moles or more, relative to 1 mole of vulcanizing agent. The upper limit of the amount of organic polar solvent used is preferably 10 moles or less, more preferably 6.0 moles or less, and even more preferably 5.5 moles or less, relative to 1 mole of vulcanizing agent.
[0062] [Molecular weight regulator]
[0063] In order to form the ends of the generated PPS resin, or to adjust the polymerization reaction and molecular weight, a monohalogenated compound (which may not be an aromatic compound) may be used in combination with the aforementioned polyhalogenated aromatic compounds.
[0064] [Polymerization aids]
[0065] To obtain PPS resin with a high degree of polymerization in a shorter time, using polymerization aids is a preferred method. Here, "polymerization aid" refers to a substance that increases the viscosity of the resulting PPS resin. Specific examples of such polymerization aids include organic carboxylates, water, alkali metal chlorides, organic sulfonates, alkali metal sulfates, alkaline earth metal oxides, alkali metal phosphates, and alkaline earth metal phosphates. They can be used alone or in combination. Among these, compounds selected from organic carboxylates, water, and alkali metal chlorides are preferred. Alkali metal carboxylates are preferred as organic carboxylates, and lithium chloride is preferred as an alkali metal chloride.
[0066] The aforementioned alkali metal carboxylates are compounds represented by the general formula R(COOM)n (where R is an alkyl, cycloalkyl, aryl, alkylaryl, or arylalkyl group having 1 to 20 carbon atoms; M is an alkali metal selected from lithium, sodium, potassium, rubidium, and cesium; and n is an integer from 1 to 3). Alkali metal carboxylates can also be used as hydrates, anhydrous forms, or aqueous solutions. Specific examples of alkali metal carboxylates include, for example, lithium acetate, sodium acetate, potassium acetate, sodium propionate, lithium valerate, sodium benzoate, sodium phenylacetate, potassium p-methylbenzoate, and mixtures thereof.
[0067] Alkali metal carboxylates can also be formed by reacting an organic acid with one or more compounds selected from alkali metal hydroxides, alkali metal carbonates, and alkali metal bicarbonates in approximately stoichiometric amounts. Among the aforementioned alkali metal carboxylates, lithium salts exhibit high solubility in the reaction system and have a significant accelerator effect, but they are expensive. On the other hand, potassium, rubidium, and cesium salts are considered to have insufficient solubility in the reaction system. Therefore, sodium acetate, which is inexpensive and has moderate solubility in the polymerization system, is the most preferred choice.
[0068] When using these alkali metal carboxylates as polymerization aids, the lower limit is preferably 0.01 moles or more relative to 1 mole of the added alkali metal sulfide, more preferably 0.1 moles or more in the sense of obtaining a higher degree of polymerization, and even more preferably 0.2 moles or more. The upper limit is preferably 2 moles or less relative to 1 mole of the added alkali metal sulfide, more preferably 0.6 moles or less in the sense of obtaining a higher degree of polymerization, and even more preferably 0.5 moles or less.
[0069] Furthermore, when water is used as a polymerization aid, the lower limit is preferably 0.3 moles or more relative to 1 mole of alkali metal sulfide, more preferably 0.6 moles or more in the sense of obtaining a higher degree of polymerization, and even more preferably 1 mole or more. The upper limit is preferably 15 moles or less relative to 1 mole of alkali metal sulfide, more preferably 10 moles or less in the sense of obtaining a higher degree of polymerization, and even more preferably 5 moles or less.
[0070] These polymerization aids can of course be used in combination with more than one type. For example, if alkali metal carboxylates and water are used together, the molecular weight of PPS resin can be increased using a smaller amount of alkali metal carboxylates and water.
[0071] The timing of adding these polymerization aids is not specifically specified; they can be added at any point during the preceding steps, at the start of polymerization, or during polymerization, as described later, or they can be added in multiple stages. When using alkali metal carboxylates as polymerization aids, adding them simultaneously with other additives at the start of the preceding steps or at the start of polymerization is preferable from the viewpoint of ease of addition. Furthermore, when using water as a polymerization aid, adding it during the polymerization reaction after the addition of a polyhalogenated aromatic compound is more effective.
[0072] [Polymerization stabilizer]
[0073] Polymerization stabilizers can also be used to stabilize the polymerization reaction system and prevent side reactions. Polymerization stabilizers help stabilize the polymerization reaction system and suppress unwanted side reactions. One indicator of side reactions is the formation of thiophenols. The formation of thiophenols can be suppressed by adding polymerization stabilizers. Specific examples of polymerization stabilizers include alkali metal hydroxides, alkali metal carbonates, alkaline earth metal hydroxides, and alkaline earth metal carbonates. Among these, alkali metal hydroxides such as sodium hydroxide, potassium hydroxide, and lithium hydroxide are preferred. Since the aforementioned alkali metal carboxylates also function as polymerization stabilizers, they are considered polymerization stabilizers. Furthermore, when using alkali metal hydrogen sulfides as vulcanizing agents, as mentioned above, it is particularly preferable to use alkali metal hydroxides simultaneously; however, in this case, alkali metal hydroxides in excess relative to the vulcanizing agent can also serve as polymerization stabilizers.
[0074] These polymerization stabilizers can be used individually or in combination of two or more. Regarding the polymerization stabilizer, the lower limit relative to 1 mole of alkali metal sulfide added is preferably 0.02 moles or more, more preferably 0.03 moles or more, and even more preferably 0.04 moles or more. Regarding the upper limit relative to 1 mole of alkali metal sulfide added, it is preferably 0.2 moles or less, more preferably 0.1 moles or less, and even more preferably 0.09 moles or less. If this proportion is too low, the stabilization effect is insufficient; conversely, even if it is too high, it is economically disadvantageous and tends to reduce the polymer yield.
[0075] There is no specific requirement for the timing of adding the polymerization stabilizer. It can be added at any point in time, such as during the preceding process, at the start of polymerization, or during polymerization. Alternatively, it can be added in multiple stages, but adding it simultaneously at the start of the preceding process or at the start of polymerization is preferred from the perspective of ease of addition.
[0076] Next, a preferred method for manufacturing the PPS resin used in the embodiments of the present invention will be specifically described in the order of the pre-process, polymerization reaction process, recycling process and post-process, but it is not limited to this method.
[0077] [Previous Process]
[0078] In the manufacturing process of PPS resin, the vulcanizing agent is usually used in the form of a hydrate. However, it is preferable to heat the mixture containing the organic polar solvent and the vulcanizing agent before adding the polyhalogenated aromatic compound to remove excess water from the system. This process is called the pre-process.
[0079] In addition, as mentioned above, vulcanizing agents can also be used, which are prepared in situ in the reaction system by alkali metal hydrogen sulfide and alkali metal hydroxide, or prepared in a tank different from the polymerization tank. There are no particular limitations on this method; preferably, the alkali metal hydrogen sulfide and alkali metal hydroxide are added to an organic polar solvent under an inert gas atmosphere, at a temperature range of room temperature to 150°C, preferably room temperature to 100°C, and the temperature is raised to at least 150°C, preferably 180 to 260°C, under normal or reduced pressure, to remove water by distillation. Polymerization aids can also be added at this stage. Furthermore, toluene or the like can be added to promote the distillation removal of water.
[0080] The amount of water in the polymerization system during the polymerization reaction is preferably 0.3 to 10.0 moles relative to each mole of vulcanizing agent added. Here, "the amount of water in the polymerization system" refers to the amount obtained by subtracting the amount of water removed from the polymerization system from the amount of water added to the polymerization system. In addition, the water added can be in any form such as water, aqueous solution, or water of crystallization.
[0081] [Polymerization reaction process]
[0082] PPS resin is manufactured by reacting a vulcanizing agent and a polyhalogenated aromatic compound in an organic polar solvent at a temperature range above 200°C and below 290°C. This process is called the polymerization reaction process.
[0083] At the start of the polymerization reaction, it is preferable to mix the organic polar solvent, vulcanizing agent, and polyhalogenated aromatic compound under an inert gas atmosphere, at a temperature above room temperature, preferably above 100°C, and below 240°C, preferably below 230°C. Polymerization auxiliaries may also be added at this stage. The feeding sequence of these raw materials can be sequential or simultaneous.
[0084] The mixture is typically heated to a temperature range of 200°C to 290°C. There are no particular restrictions on the heating rate, but a lower limit is preferably a rate of 0.01°C / min or higher, more preferably 0.1°C / min or higher. An upper limit is preferably a rate of 5°C / min or lower, more preferably 3°C / min or lower.
[0085] Typically, the final temperature is raised to 250–290°C, at which the lower limit of the reaction time is usually 0.25 hours or more, preferably 0.5 hours or more. The upper limit is a reaction time of less than 50 hours, preferably less than 20 hours.
[0086] In the stage before reaching the final temperature, for example, by reacting at 200°C to 260°C for a certain time and then raising the temperature to 270°C to 290°C, it is effective to obtain a higher degree of polymerization. At this time, the reaction time at 200°C to 260°C is usually preferably in the range of 0.25 hours to 20 hours, and more preferably in the range of 0.25 hours to 10 hours.
[0087] Furthermore, to obtain polymers with higher degrees of polymerization, it is sometimes more effective to perform polymerization in multiple stages. When performing polymerization in multiple stages, it is more effective to achieve a conversion rate of 40 mol% or more, and more preferably 60 mol% of the polyhalogenated aromatic compounds in the system at 245°C.
[0088] In addition, the conversion rate of polyhalogenated aromatic compounds (hereinafter referred to as "PHA") is calculated using the following formula. The residual amount of PHA can usually be determined by gas chromatography.
[0089] (A) When polyhalogenated aromatic compounds are added in excess relative to alkali metal sulfides in a molar ratio
[0090] Conversion rate = [PHA addition (moles) - PHA residue (moles)] / [PHA addition (moles) - PHA excess (moles)]
[0091] (B) Other than (A) above
[0092] Conversion rate = [PHA addition amount (moles) - PHA residue amount (moles)] / [PHA addition amount (moles)].
[0093] [Recycling Process]
[0094] In the manufacturing process of PPS resin, after polymerization is completed, solids are recovered from the polymerization reactants containing polymers, solvents, etc. This process is called the recovery process. Any known method can be used for recovery.
[0095] For example, a method can be used to recover the granular polymer by slow cooling after the polymerization reaction is completed. There is no particular limitation on the slow cooling rate, but it is preferably around 0.1°C / min to 3°C / min. It is not necessary to maintain the same slow cooling rate throughout the entire slow cooling process; for example, a method can be used where the polymer particles are cooled slowly at 0.1 to 1°C / min before crystallization, and then at a rate of 1°C / min or higher.
[0096] In addition, performing the above-mentioned recovery under quenching conditions is also a preferred method. Among this recovery method, flash evaporation can be listed as a preferred method. The so-called "flash evaporation" involves removing the polymer reactants from high temperature and high pressure (usually above 250°C and 8 kg / cm³). 2 The above describes a method of flash evaporation in an atmosphere of normal or reduced pressure, whereby the polymer is recovered as a powder while the solvent is being recycled. Here, "flash evaporation" means ejecting the polymer reactants from a nozzle. Specifically, the flash evaporation atmosphere can be nitrogen or water vapor at normal pressure, with a preferred temperature range of 150°C to 250°C.
[0097] [Post-processing steps]
[0098] After PPS resin is produced through the above polymerization and recycling processes, it can undergo acid treatment, hot water treatment, or cleaning with organic solvents. This process is called the post-treatment process.
[0099] The acid treatment process is as follows. There are no particular restrictions on the acid used in the acid treatment of PPS resin, as long as it does not decompose the PPS resin. Examples include acetic acid, hydrochloric acid, sulfuric acid, phosphoric acid, silicic acid, carbonic acid, and propionic acid. Among these, acids selected from acetic acid and hydrochloric acid are more preferred.
[0100] As an acid treatment method, one method is to impregnate the PPS resin in an acid or an aqueous solution of an acid, and stirring or heating may also be performed as needed. For example, when using acetic acid, impregnating the PPS resin powder with an aqueous solution of acetic acid at pH 4 at 80–200°C and stirring for 30 minutes can achieve sufficient results.
[0101] The hot water treatment process is as follows. When treating PPS resin with hot water, it is preferable that the water temperature is 100°C or higher, more preferably 120°C or higher, even more preferably 150°C or higher, and particularly preferably 170°C or higher. Temperatures below 100°C result in minimal expected chemical modification of the PPS resin and are therefore not preferred.
[0102] Furthermore, to avoid undesirable decomposition of end groups, the processing atmosphere is preferably inert. Moreover, to remove residual components, the PPS resin after this hot water treatment operation is preferably rinsed several times with warm water.
[0103] The following applies to cleaning with organic solvents. There are no particular restrictions on the organic solvents used for cleaning PPS resin, as long as they do not decompose the PPS resin. Examples of organic solvents used for cleaning PPS resin include nitrogen-containing polar solvents such as N-methyl-2-pyrrolidone, dimethylformamide, dimethylacetamide, 1,3-dimethylimidazolium ketone, hexamethylphosphoramide, and piperazine; sulfoxide-sulfone solvents such as dimethyl sulfoxide, dimethyl sulfone, and sulfolane; ketone solvents such as acetone, methyl ethyl ketone, diethyl ketone, and acetophenone; ether solvents such as dimethyl ether, dipropyl ether, dioxane, and tetrahydrofuran; halogen solvents such as chloroform, dichloromethane, trichloroethylene, 1,2-dichloroethane, perchloroethylene, monochloroethane, dichloroethane, tetrachloroethane, perchloroethane, and chlorobenzene; alcohol or phenol solvents such as methanol, ethanol, propanol, butanol, pentanol, ethylene glycol, propylene glycol, phenol, cresol, polyethylene glycol, and polypropylene glycol; and aromatic hydrocarbon solvents such as benzene, toluene, and xylene. Among these organic solvents, N-methyl-2-pyrrolidone, acetone, dimethylformamide, and chloroform are particularly preferred. Furthermore, one or more of these organic solvents may be used.
[0104] One method of cleaning using organic solvents is impregnating PPS resin in an organic solvent, with appropriate stirring or heating as needed. There are no particular limitations on the cleaning temperature when cleaning PPS resin with organic solvents; any temperature from room temperature to approximately 300°C can be selected. Higher cleaning temperatures tend to result in higher cleaning efficiency, but generally, a cleaning temperature of room temperature to 150°C is sufficient to achieve adequate results. Cleaning can also be carried out in a pressure vessel under pressure at a temperature above the boiling point of the organic solvent.
[0105] As a post-processing step, it is preferable to perform any one of acid treatment, hot water treatment, or cleaning with organic solvents. From the viewpoint of removing impurities, it is preferable to use two or more treatments together.
[0106] In embodiments of the present invention, PPS resin in which alkali metals or alkaline earth metals such as Ca are introduced may also be used. Examples of methods for introducing alkali metals and / or alkaline earth metals include adding alkali metal salts and / or alkaline earth metal salts at any time before, during, or after the aforementioned preceding process; adding alkali metal salts and / or alkaline earth metal salts into the polymerization reactor at any time before, during, or after the polymerization process; and adding alkali metal salts and / or alkaline earth metal salts at any time at the beginning, middle, or end of the aforementioned cleaning process.
[0107] PPS resin can also be used after polymerization by heating in an oxygen atmosphere or by adding crosslinking agents such as peroxides and heating to perform thermal oxidative crosslinking treatment, thereby increasing its molecular weight.
[0108] When dry heat treatment is performed for the purpose of increasing molecular weight through thermal oxidative crosslinking, the lower limit of the temperature is preferably 160°C or higher, more preferably 170°C or higher. The upper limit of the temperature is preferably 260°C or lower, more preferably 250°C or lower. Furthermore, the oxygen concentration is preferably 5% by volume or higher, more preferably 8% by volume or higher. There is no particular limitation on the upper limit of the oxygen concentration, but approximately 50% by volume is the limit. The lower limit of the treatment time is preferably 0.5 hours or higher, more preferably 1 hour or higher, more preferably 2 hours or higher. The upper limit of the treatment time is preferably 100 hours or lower, more preferably 50 hours or lower, more preferably 25 hours or lower.
[0109] Alternatively, dry heat treatment can be performed to inhibit thermal oxidative crosslinking and remove volatile components. The preferred temperature is in the range of 130–250°C, more preferably in the range of 160–250°C. Furthermore, the oxygen concentration at this temperature is preferably less than 5% by volume, more preferably less than 3% by volume. The minimum treatment time is preferably 0.5 hours or more, more preferably 1 hour or more. The maximum treatment time is preferably 50 hours or less, more preferably 20 hours or less, and more preferably 10 hours or less.
[0110] The heat treatment apparatus can be a conventional hot air dryer or a rotary or stirring-blade heating device. For more efficient and uniform processing, a rotary or stirring-blade heating device is preferred.
[0111] From the viewpoint of improving the fluidity and toughness of PPS resins during molding and processing, it is preferable that the melt flow rate (MFR) measured according to the ASTM-D1238-70 method at a test temperature of 315.5°C and a load of 5000g is in the range of 80g / 10min or more and 6100g / 10min or less. Alternatively, multiple PPS resins with different MFRs can be used in combination.
[0112] (B) Non-fibrous inorganic fillers
[0113] The PPS resin composition of the present invention preferably contains (B) a non-fibrous inorganic filler.
[0114] The standard deviation of the particle size distribution of the (B) non-fibrous inorganic filler mixed in the PPS resin composition of the present invention is preferably 0.22 or more and 10.00 or less, more preferably 0.23 or more and 9.50 or less, and even more preferably 0.24 or more and 9.00 or less. The standard deviation of particle size distribution referred to here is the standard deviation defined on a logarithmic scale based on the particle size distribution measured by laser diffraction and scattering. If the standard deviation of the particle size distribution of the non-fibrous inorganic filler is 0.22 or more, the tracking resistance of the PPS resin composition can be 300V or more even when the average particle size of the non-fibrous inorganic filler is large. Furthermore, even when the average particle size of the non-fibrous inorganic filler is small, the thermal shock resistance of the metal insert molded article using the PPS resin composition can be 15 cycles or more. The reasons why the PPS resin composition exhibits preferred characteristics because the standard deviation of the particle size distribution of the non-fibrous inorganic filler is within the above range are not yet certain, but are speculated as follows. Small-particle-size non-fibrous inorganic fillers have a large specific surface area, thus significantly improving resistance to tracking. On the other hand, large-particle-size non-fibrous inorganic fillers, due to their greater spacing within the resin composition, are believed to benefit more from the resin's inherent toughness. It is speculated that when the standard deviation of the particle size distribution is within the aforementioned range, the effects of small and large particle sizes of the non-fibrous inorganic fillers will synergistically enhance each other. If the standard deviation of the particle size distribution of the non-fibrous inorganic filler is below 10.00, there will be no adverse effects due to the breakage or defects of coarse non-fibrous inorganic fillers, which is therefore preferable. Resistance to tracking and thermal shock will be described later.
[0115] (B) The average particle size of the non-fibrous inorganic filler is preferably 1.0 μm or more and 50.0 μm or less. The lower limit of the average particle size is more preferably 1.1 μm or more, and even more preferably 1.2 μm or more. The upper limit of the average particle size is more preferably 45.0 μm or less, and even more preferably 40.0 μm or less. If the average particle size of the non-fibrous inorganic filler is 1.0 μm or more, the thermal shock resistance of the metal insert molded article using the PPS resin composition can be 15 cycles or more. The reason for exhibiting high thermal shock resistance within the above range is not yet certain, but it is speculated that this is because, within this range, the non-fibrous inorganic fillers in the resin composition are spaced far apart, thus maximizing the effect of the resin's inherent toughness. If the average particle size of the non-fibrous inorganic filler is 50.0 μm or less, the tracking resistance of the PPS resin composition can be 300V or more. Furthermore, the average particle size mentioned here is the volume average particle size obtained from the particle size distribution measured by laser diffraction and scattering.
[0116] (B) The 10%D of the non-fibrous inorganic filler is preferably 0.1 μm or more and 1.2 μm or less. The lower limit of 10%D is more preferably 0.2 μm or more, and even more preferably 0.3 μm or more. The upper limit of 10%D is more preferably 1.1 μm or less, and even more preferably 1.0 μm or less. Furthermore, 10%D as used here refers to a particle size smaller than 10% by volume in the total particle size distribution determined by laser diffraction and scattering. If the 10%D of the non-fibrous inorganic filler is 0.1 μm or more, the resistance to thermal shock of the metal insert molded article using the PPS resin composition can be 15 cycles or more. When the 10%D of the non-fibrous inorganic filler is 1.2 μm or less, the tracking resistance of the PPS resin composition can be 300V or more. The reason why the PPS resin composition exhibits high resistance to thermal shock is uncertain because (B) the non-fibrous inorganic filler 10%D is within the above range. However, it is speculated that this is because within this range, there is a certain amount of non-fibrous inorganic filler with small particle size, large surface area, and great effect on improving resistance to tracking, thus the effect on improving resistance to tracking will be greater.
[0117] (B) One type of non-fibrous inorganic filler may be used, but it is preferable to use two or more in combination, which makes it easier to adjust the standard deviation of particle size distribution, average particle size, and 10%D to an appropriate range. When mixing two types of non-fibrous inorganic fillers, it is preferable to mix non-fibrous inorganic fillers with an average particle size of less than 2 μm and non-fibrous inorganic fillers with an average particle size of more than 2 μm in a weight ratio of 1:10 to 10:1, more preferably 1:9 to 9:1.
[0118] The PPS resin composition of the present invention preferably contains 20 parts by weight or more and 170 parts by weight or less of a non-fibrous inorganic filler (B) relative to 100 parts by weight of (A) PPS resin. The content of the non-fibrous inorganic filler (B) is more preferably 40 parts by weight or more, more preferably 50 parts by weight or more, even more preferably 60 parts by weight or more, and even more preferably 70 parts by weight or more. When the amount of the non-fibrous inorganic filler is 20 parts by weight or more, the tracking resistance of the PPS resin composition can be 300V or more. When the amount of the non-fibrous inorganic filler is 170 parts by weight or less, the thermal shock resistance of the metal insert molded article using the PPS resin composition can be 15 cycles or more.
[0119] Specific examples of non-fibrous inorganic fillers (B) include: fullerenes; silicates such as talc, wollastonite, zeolite, sericite, mica, kaolin, clay, pyrophyllite, bentonite, asbestos, and aluminosilicates; metal oxides such as silicon dioxide, magnesium oxide, aluminum oxide, zirconium oxide, titanium oxide, and iron oxide; metal hydroxides such as magnesium hydroxide, aluminum hydroxide, and calcium hydroxide; carbonates such as calcium carbonate, magnesium carbonate, and dolomite; sulfates such as calcium sulfate and barium sulfate; glass beads, glass flakes, glass powder, ceramic beads, boron nitride, silicon carbide, carbon black, silicon dioxide, and graphite. From the viewpoint of resistance to tracking in PPS resin compositions, decomposition endothermic fillers such as magnesium hydroxide, magnesium carbonate, aluminum hydroxide, and calcium borate, which cause endothermic reactions upon decomposition, and fillers with high thermal conductivity, can suppress the heating of PPS resin compositions and are less likely to cause tracking phenomena, and are therefore particularly preferred.
[0120] Furthermore, it is preferable to use non-fibrous inorganic fillers after surface treatment. Examples of compounds used for surface treatment include vinyl silane compounds such as vinyltriethoxysilane and vinyltrichlorosilane; epoxy silane compounds such as γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; and γ-(2-aminoethyl)aminopropylmethyldimethoxysilane, γ-(2-aminoethyl... Aminopropyltrimethoxysilane compounds such as aminopropyltrimethoxysilane and γ-aminopropyltrimethoxysilane; alkoxysilane compounds containing isocyanate groups such as γ-isocyanate-propyltriethoxysilane, γ-isocyanate-propylmethyldimethoxysilane, γ-isocyanate-propylmethyldiethoxysilane, γ-isocyanate-propylethyldimethoxysilane, γ-isocyanate-propylethyldiethoxysilane, and γ-isocyanate-propyltrichlorosilane; methacryloyloxysilane compounds such as 3-methacryloyloxypropylmethyldimethoxysilane, 3-methacryloyloxypropylmethyldiethoxysilane, and 3-methacryloyloxypropyltriethoxysilane; and long-chain fatty acids or long-chain fatty alcohols such as stearic acid, oleic acid, linalic acid, and stearyl alcohol. In particular, the use of "non-fibrous inorganic fillers that have been surface-treated with compounds selected from vinyl silane compounds, epoxy silane compounds, amino silane compounds, isocyanate silane compounds, and methacryloxy silane compounds" is preferred from the viewpoint of inhibiting aggregation in the composition or molded article, from the viewpoint of resistance to tracking due to the good dispersion and increased surface area of the non-fibrous inorganic filler, and from the viewpoint of improved mechanical strength due to the increased interfacial strength between the non-fibrous inorganic filler and the resin.
[0121] (C) Fibrous inorganic filler
[0122] The PPS resin composition of the present invention preferably contains (C) a fibrous inorganic filler.
[0123] The PPS resin composition of the present invention preferably contains 40 parts by weight or more and 190 parts by weight or less of (C) fibrous inorganic filler, more preferably 60 parts by weight or more and 190 parts by weight or less, relative to 100 parts by weight of (A) PPS resin. When the amount of fibrous inorganic filler is 40 parts by weight or more, the effect of improving the mechanical properties of the resin is particularly significant, and therefore the resistance to thermal shock of metal inserts molded using the PPS resin composition can be 15 times or more. When the amount of fibrous inorganic filler is 190 parts by weight or less, the fluidity of the PPS resin composition during melting can be maintained.
[0124] Specific examples of (C) fibrous inorganic fillers include glass fibers, carbon fibers, carbon nanotubes, carbon nanohorns, potassium titanate whiskers, zinc oxide whiskers, calcium carbonate whiskers, wollastonite whiskers, aluminum borate whiskers, aramid fibers, alumina fibers, silicon carbide fibers, ceramic fibers, asbestos fibers, gypsum fibers, and metal fibers. Alternatively, the surface of the fibrous inorganic filler can be pretreated with coupling agents such as isocyanate compounds, organosilane compounds, organotitanate compounds, organoborane compounds, and epoxy compounds before use.
[0125] In order to improve the rigidity of the material, (C) the fibrous inorganic filler is preferably selected from either glass fiber or carbon fiber, and from the viewpoint of material cost, glass fiber is more preferred. Furthermore, from the viewpoint of thermal shock resistance measured using metal insert molded articles made with PPS resin compositions, irregularly shaped glass fibers are preferred. The reason is unclear, but it can be speculated that irregularly shaped glass fibers have the effect of reducing dimensional changes and anisotropy of the resin composition, thus suppressing the impact caused by dimensional changes and anisotropy during thermal cycling. In addition, molded articles made with resin compositions containing irregularly shaped glass have improved surface smoothness compared to molded articles made with resin compositions containing round cross-section glass with low anisotropy, and are therefore preferred from the viewpoint of resistance to tracking. Irregularly shaped glass fibers are glass fibers with a flat cross-section. For irregularly shaped glass fibers, the ratio of the major axis (the longest straight distance of the cross section) to the minor axis (the longest straight distance in the direction perpendicular to the major axis) (hereinafter sometimes simply referred to as the flatness ratio) in the cross section obtained by cutting the glass fiber perpendicular to the length direction is more preferably 1.3 to 10.0.
[0126] (D) Elastomer
[0127] The PPS resin composition of the present invention preferably includes (D) an elastomer. An elastomer is a material that has rubber-like elasticity. Examples of elastomers include thermoplastic elastomers such as olefin-based (co)polymers and styrene-based (co)polymers, as well as thermosetting elastomers such as silicone elastomers and fluoropolymers.
[0128] The PPS resin composition of the present invention preferably contains 1 part by weight or more and 40 parts by weight or less of (D) elastomer relative to 100 parts by weight of (A) PPS resin, more preferably 2 parts by weight or more and 35 parts by weight or less. When the amount of elastomer is 1 part by weight or more, the stress-relieving and toughness-improving effects of the resin composition are easily exhibited, and therefore the thermal shock resistance of the metal insert molded article using the PPS resin composition can be 15 times or more. In addition, since the (D) elastomer is not easily carbonized, the tracking resistance of the PPS resin composition can reach 300V or more. When the amount of elastomer is 40 parts by weight or less, the flame retardancy of the PPS resin composition can be maintained.
[0129] As the (D) elastomer, it is preferably an olefin copolymer having an epoxy group (D-1). Relative to 100 parts by weight of (A) PPS resin, it is preferably contained in 1 to 40 parts by weight of the olefin copolymer having an epoxy group (D-1), more preferably 2 to 35 parts by weight.
[0130] (D-1) Epoxy-based olefin copolymers can be obtained by introducing epoxy-containing monomer components (containing functional groups) into polymers such as "ethylene, propylene, 1-butene, 1-pentene, 1-octene, 4-methyl-1-pentene, isobutene, etc., either individually or by polymerizing two or more of them; copolymers of α-olefins with α,β-unsaturated acids and their alkyl esters such as acrylic acid, methyl acrylate, ethyl acrylate, butyl acrylate, methacrylic acid, methyl methacrylate, ethyl methacrylate, butyl methacrylate, etc.; for example, ethylene-propylene copolymers (" / " indicates copolymerization, the same below), ethylene / 1-butene copolymers, ethylene / 1-hexene copolymers, ethylene / 1-octene copolymers, ethylene / methyl acrylate copolymers, ethylene / ethyl acrylate copolymers, ethylene / butyl acrylate copolymers, ethylene / methyl methacrylate copolymers, ethylene / ethyl methacrylate copolymers, ethylene / butyl methacrylate copolymers", etc. Examples of functionalized components include epoxy-containing monomers such as glycidyl acrylate, glycidyl methacrylate, ethyl glycidyl acrylate, itaconic acid glycidyl acrylate, and citraconic acid glycidyl acrylate. There are no particular limitations on the methods for introducing these functionalized components; methods such as copolymerizing the functionalized components during the copolymerization of monomers constituting the olefin (co)polymer, or grafting the functionalized components into the olefin (co)polymer using a free radical initiator, are also possible. Specific examples of epoxy-containing olefin copolymers obtained by introducing functionalized components into olefin (co)polymers that are particularly useful include ethylene / propylene-g-glycidyl methacrylate copolymers ("g" indicates grafting, the same applies hereinafter), ethylene / 1-butene-glycidyl methacrylate copolymers, ethylene / glycidyl acrylate copolymers, ethylene / glycidyl methacrylate copolymers, ethylene / methyl acrylate / glycidyl methacrylate copolymers, and ethylene / methyl methacrylate / glycidyl methacrylate copolymers. Alternatively, epoxy-containing olefin copolymers, which use other monomers as copolymerizing components besides glycidyl esters of α-olefins such as ethylene and propylene and α,β-unsaturated acids, are preferred.
[0131] From the viewpoint of resistance to thermal shock and tracking, in order to reduce the dispersion diameter of the (D) elastomer in the PPS resin composition, an olefin copolymer containing a structure derived from glycidyl esters of α,β-unsaturated acids is preferred as the (D) elastomer, and an ethylene / methyl acrylate / glycidyl methacrylate copolymer is more preferred. As a lower limit for the content of glycidyl ester structural units derived from α,β-unsaturated acids, from the viewpoint of thermal shock resistance, when the total resin composition is 100 parts by weight, it is preferably 0.01 parts by weight or more, and more preferably 0.03 parts by weight or more. As an upper limit for the content of glycidyl ester structural units derived from α,β-unsaturated acids, from the viewpoint of melt flowability, when the total resin composition is 100 parts by weight, it is preferably less than 0.15 parts by weight, and more preferably 0.10 parts by weight or less.
[0132] Furthermore, in this invention, the (D) elastomer preferably contains an elastomer that does not have epoxy groups (D-2). Relative to 100 parts by weight of the (A) PPS resin, it is preferable to contain 1 to 40 parts by weight of the elastomer that does not have epoxy groups (D-2), more preferably 2 to 35 parts by weight.
[0133] As the (D) elastomer, combining (D-1) an olefin copolymer with epoxy groups and (D-2) an elastomer without epoxy groups can reduce the dispersion diameter of the (D) elastomer in the PPS resin composition, and is therefore preferred from the viewpoint of resistance to thermal shock and tracking.
[0134] As a specific example of an elastomer (D-2) that does not have an epoxy group, an elastomer having at least one functional group selected from carboxyl, anhydride, hydroxyl, amino, epoxy, and isocyanate groups can be used, especially an elastomer without polar functional groups. Alternatively, if the elastomer does not have an epoxy group, it can also be a thermoplastic elastomer such as an olefin-based (co)polymer or a styrene-based (co)polymer. Alternatively, it can be a thermosetting elastomer such as an organosilicon elastomer or a fluorinated elastomer.
[0135] (D-2) An elastomer without epoxy groups, which, from the viewpoint of resistance to thermal shock in the use of metal insert molded articles, can maintain toughness and low elastic modulus even at low temperatures, so the glass transition temperature is preferably below -20°C, and more preferably below -30°C.
[0136] (E) Organosilicon compounds
[0137] From the viewpoint of resistance to tracking and resistance to thermal shock in metal insert moldings, it is preferable to add an organosilicon compound (E) that can improve the hydrophobicity of the PPS resin composition and has a stress-relieving effect. An organosilicon compound is an organosilicon compound in which silicon is directly bonded to an organic group, etc., with a siloxane bond as its backbone. Known organic groups that are directly bonded to silicon include methyl, ethyl, phenyl, vinyl, trifluoropropyl, and combinations thereof. These known organosilicon compounds can be used without particular limitation. Alternatively, organosilicon compounds in which a portion of the organic group is replaced by a substituent having an epoxy group, amino group, polyether group, carboxyl group, mercapto group, ester group, chloroalkyl group, alkyl group with three or more carbon atoms, hydroxyl group, etc., can also be used. Organosilicon compounds are classified into silicone oils, organosilicon elastomers, and organosilicon resins according to their degree of crosslinking. Furthermore, organosilicon elastomers also belong to (D) elastomers, but are treated as (E) organosilicon compounds in this invention. While any type of organosilicon compound can be used, organosilicon elastomers with high crosslinking degree and low decomposition are particularly preferred from the viewpoints of workability, resistance to tracking, resistance to thermal shock, and tensile strength of weld lines. Furthermore, micronized organosilicon compounds with an average particle size of 0.1–80 μm exhibit good dispersibility, excellent workability, and are more effective.
[0138] The amount of the organosilicon compound (E) relative to 100 parts by weight of the PPS resin (A) is preferably 0.1 to 20 parts by weight, more preferably 0.1 to 15 parts by weight, and even more preferably 0.5 to 15 parts by weight. From the viewpoint of improving resistance to tracking and thermal shock resistance of molded articles using metal inserts, an addition amount of 0.1 parts by weight or more is preferred. If the addition amount is 20 parts by weight or less, it is preferable from the viewpoint of maintaining the mechanical strength of the resin composition and reducing gas generation.
[0139] (F) Organosilanes
[0140] In the PPS resin composition used in this invention, to improve mechanical strength, toughness, etc., without impairing the effects of this invention, a silane compound having at least one functional group selected from epoxy, amino, isocyanate, hydroxyl, mercapto, and urea groups may be added. Specific examples of such compounds include epoxy-containing alkoxysilane compounds such as γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; mercapto-containing alkoxysilane compounds such as γ-mercaptopropyltrimethoxysilane and γ-mercaptopropyltriethoxysilane; and γ-ureopropyltriethoxysilane, γ-ureopropyltrimethoxysilane, and γ-(2-ureoethyl) Alkoxysilane compounds containing urea groups, such as aminopropyltrimethoxysilane; alkoxysilane compounds containing isocyanate groups, such as γ-isocyanate-propyltriethoxysilane, γ-isocyanate-propylmethyldimethoxysilane, γ-isocyanate-propylmethyldiethoxysilane, γ-isocyanate-propylethyldimethoxysilane, γ-isocyanate-propylethyldiethoxysilane, and γ-isocyanate-propyltrichlorosilane; alkoxysilane compounds containing amino groups, such as γ-(2-aminoethyl)aminopropylmethyldimethoxysilane, γ-(2-aminoethyl)aminopropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, and γ-aminopropyltriethoxysilane; and alkoxysilane compounds containing hydroxyl groups, such as γ-hydroxypropyltrimethoxysilane and γ-hydroxypropyltriethoxysilane. Among them, alkoxysilane compounds having at least one functional group selected from epoxy, amino, isocyanate, and hydroxyl groups can improve the dispersibility of (B) non-fibrous inorganic filler and (D) elastomer in the PPS resin composition, and enhance the interfacial strength between (B) non-fibrous inorganic filler and (C) fibrous inorganic filler and PPS resin. Therefore, they are particularly preferred in terms of obtaining excellent resistance to tracking, resistance to thermal shock, and tensile strength of weld lines. The suitable addition amount of this silane compound is preferably in the range of 0.05 to 5 parts by weight relative to 100 parts by weight of PPS resin.
[0141] The PPS resin composition used in this invention may also be mixed with other resins without impairing the effects of this invention. There are no particular limitations on the composable resins; specific examples include polyamides; polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polycyclohexanediol terephthalate, and polynaphthalene terephthalate; polyethylene, polypropylene, polytetrafluoroethylene, polyamide-imide, polyacetal, polyimide, polyetherimide, polyethersulfone, polysulfone resin, polyarylsulfone resin, polyketone resin, polyaryl ester resin, liquid crystal polymers, polyetherketone resin, polythioetherketone resin, polyetheretherketone resin, and polyamide-imide resin.
[0142] Without impairing the effects of the present invention, other components may be added to the PPS resin composition of the present invention, such as antioxidants, heat stabilizers (hindered phenols, hydroquinones, phosphorus compounds, phosphites, amines, sulfur compounds and their substitutes, etc.); weathering agents (resorcinols, salicylates, benzotriazoles, benzophenones, hindered amines, etc.); release agents and lubricants (lignite acid and its metal salts, its esters, its half-esters, stearyl alcohol, stearamide, stearate esters, diurea, polyethylene wax, etc.); pigments (cadmium sulfide, phthalocyanine, carbon black for coloring, etc.); dyes (nigrossine (aniline black) dye, etc.). Plasticizers (octyl paraben, N-butylbenzenesulfonamide, etc.); antistatic agents (alkyl sulfate anionic antistatic agents, quaternary ammonium cationic antistatic agents, nonionic antistatic agents such as polyoxyethylene sorbitan monostearate, betaine amphoteric antistatic agents, etc.); flame retardants (e.g., red phosphorus, phosphate esters, melamine cyanurate, ammonium polyphosphate, brominated polystyrene, brominated polyphenylene ether, brominated polycarbonate, brominated epoxy resin, or combinations of such brominated flame retardants with antimony trioxide, etc.); heat stabilizers; slip agents such as calcium stearate, aluminum stearate, and lithium stearate; strength improvers such as bisphenol A type bisphenol epoxy resin, phenolic varnish type epoxy resin, and cresol-phenolic varnish type epoxy resin; conventional additives such as UV inhibitors, colorants, flame retardants, and foaming agents. Antioxidants and heat stabilizers (hindered phenols, hydroquinones, phosphorus compounds, phosphites, amines, sulfur compounds, and their substitutes, etc.) are preferably used. Phosphorus antioxidants and hindered phenolic antioxidants are more preferred. If the mixing amount of the above compounds exceeds 20 parts by weight of the total resin composition, the original properties of the PPS resin may be impaired; therefore, it is preferably 20 parts by weight or less, and more preferably 10 parts by weight or less.
[0143] There are no particular limitations on the preparation method of the PPS resin composition of the present invention. Representative examples include feeding the raw materials into a commonly known melt mixer such as a single-shaft or bi-shaft extruder, a Banbury mixer, a kneader, and a mixing roller, and mixing them at a temperature of 280–380°C. There are also no particular limitations on the mixing order of the raw materials. Any method can be used, such as mixing all the raw materials and then melt-mixing them as described above; mixing a portion of the raw materials and then melt-mixing them as described above, followed by melting-mixing the remaining raw materials; or mixing a portion of the raw materials and then melting-mixing them in a single-shaft or bi-shaft extruder using a side feeder, etc. Furthermore, for small amounts of additive components, other components can be mixed and granulated using the methods described above, and then added before molding.
[0144] The PPS resin composition of the present invention obtained in this way can be used for various molding processes such as injection molding, extrusion molding, blow molding, and transfer molding, but it is particularly suitable for injection molding.
[0145] The PPS resin composition of the present invention preferably has a tensile elongation of 1.0% or more. This makes it suitable for parts such as snap-fit shapes that are subject to deformation during use. Furthermore, if the tensile elongation is 1.0% or more, the resistance to thermal shock of the molded article using metal inserts can reach 15 cycles or more. The tensile elongation in the present invention is a value measured according to ISO 527-1,-2 (2012).
[0146] The PPS resin composition of the present invention preferably has a weld line tensile strength of 30 MPa or more, more preferably 34 MPa or more, and more preferably 38 MPa or more. This increases the strength of the weld line, which is the weakest part of the molded article, making the molded article less prone to damage and improving its reliability. The measurement method will be described later.
[0147] The tracking resistance of the PPS resin composition of the present invention was evaluated by means of the comparative tracking index, as determined in accordance with IEC 60112 (2003). A higher comparative tracking index indicates higher tracking resistance.
[0148] The PPS resin composition of the present invention must have a tracking resistance of 300V or higher, preferably 400V or higher, as measured according to IEC 60112 (2003). This reduces the likelihood of tracking damage when using the PPS resin composition of this application on components subjected to high voltage (400V or higher), thus improving the safety of the molded article. Furthermore, it ensures that the creepage distance of the molded article is above the necessary creepage distance specified in IEC 60664. Therefore, the design freedom of molded articles made from the PPS resin composition of this application is increased, making it easier to achieve miniaturization and weight reduction. If the tracking resistance of the PPS resin composition is less than 300V, tracking damage easily occurs on the surface of the molded article made from the PPS resin composition, making it unsafe for use in components subjected to high voltage.
[0149] In the PPS resin composition of the present invention, the thermal shock resistance of the metal insert molded article, as measured by the method described later, must be at least 15 cycles, preferably at least 20 cycles. This ensures that when the PPS resin composition of the present application is used in metal insert molded articles, cracks are less likely to occur, allowing for good use. If the thermal shock resistance of the PPS resin composition is less than 15 cycles, resin cracks may easily occur when the metal insert molded article made of the PPS resin composition is used in areas subject to varying ambient temperatures (approximately -40°C to 130°C).
[0150] In addition, the thermal shock resistance of this invention, such as Figure 1 As shown, metal-embedded test pieces with intentionally created welds by setting a hole in the center were used to evaluate the resistance to thermal shock during thermal shock treatment based on the number of treatments in which cracks appeared at the weld. The number of treatments in which cracks appeared indicates the crack resistance of the weld; a higher number of treatments indicates higher resistance to thermal shock.
[0151] The welded portion has weak mechanical strength due to the orientation of the fibrous inorganic filler, making it prone to breakage. However, the PPS resin composition of the present invention has high resistance to thermal shock at the welded portion, making it suitable for molded articles of various shapes, especially metal inserts. Furthermore, the metal inserts of the present invention are integrally molded from a metal component and the PPS resin composition. These metal inserts are well-suited for applications such as current sensors, busbars, and other automotive electrical components, as well as power semiconductor housings and other electrical and electronic components. These components can be appropriately mounted on electric drive axles (eAxle) or electric vehicles (xEVs). An electric drive axle (eAxle) is a drive system in electric vehicles where the motor, inverter, and reducer are integrated. Electric vehicles (xEVs) are a general term for electric vehicles, including battery electric vehicles (BEVs), hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), and fuel cell electric vehicles (FCEVs).
[0152] As applicable uses of the PPS resin composition of the present invention, examples include electrical and electronic components such as power semiconductor housings (e.g., power modules), sensors, civilian connectors, relay housings, coil frames, capacitors, various terminal boards, insulating boards, and small motors; automotive and vehicle-related components such as distributors, starter switches, starter relays, transmission wiring harnesses, fuel-related solenoid valve coils, fuse connectors, electrical component insulating boards, terminal blocks, stepper motor rotors, electromagnetic coil frames, engine oil filters, ignition device housings, vehicle speed sensors, current sensors, busbars, capacitor housings, and cable sheaths; and various other applications such as vehicle electrical components.
[0153] Example
[0154] The following examples illustrate the invention in more detail, but the invention is not limited to the description of these examples.
[0155] [Evaluation method for PPS resin manufactured in the reference example]
[0156] (1) Melt Flow Rate (MFR)
[0157] The test was conducted according to ASTM-D1238-70 at a test temperature of 315.5℃ and a load of 5000g.
[0158] However, for low viscosity polyphenylene sulfide resins, the MFR is calculated by the following method. The ER (Extrusion Rate) of the polyphenylene sulfide resin is determined according to ASTM-D1238-70 at a test temperature of 315.5°C and a load of 345g, and the MFR value is calculated by the following formula (1).
[0159] Formula (1) MFR=15.8×4.4×ER
[0160] [Reference Example 1]
[0161] 8.27 kg (70.00 mol) of 47.5% sodium hydrosulfide, 2.91 kg (69.80 mol) of 96% sodium hydroxide, 11.45 kg (115.50 mol) of N-methyl-2-pyrrolidone (NMP), and 10.5 kg of deionized water were added to a 70°C high-pressure vessel equipped with a stirrer and a bottom valve. Nitrogen gas was introduced under normal pressure, and the mixture was gradually heated to 245°C over approximately 3 hours. After distilling off 14.78 kg of water and 0.28 kg of NMP, the reaction vessel was cooled to 200°C. The residual water content in the system, including water consumed by NMP hydrolysis, was 1.06 mol per mole of alkali metal sulfide added. Additionally, the amount of hydrogen sulfide escaping was 0.02 mol per mole of alkali metal sulfide added.
[0162] Then, 10.48 kg (71.27 mol) of p-dichlorobenzene and 9.37 kg (94.50 mol) of NMP were added. The reaction vessel was sealed under nitrogen atmosphere, and the temperature was increased from 200 °C to 270 °C at a rate of 0.6 °C / min with stirring at 240 rpm. After reacting at 270 °C for 100 minutes, the bottom valve of the autoclave was opened, and the contents were flash-evaporated into a vessel equipped with a stirrer for 15 minutes while pressurizing with nitrogen. The mixture was then stirred at 250 °C for a period of time to remove most of the NMP, yielding a solid.
[0163] The obtained solid and 76 liters of ion-exchanged water were placed in an autoclave equipped with a stirrer and stirred and washed at 70°C for 30 minutes. The mixture was then filtered through a glass filter using suction. Next, 76 liters of ion-exchanged water heated to 70°C were injected into the glass filter for suction filtration to obtain a filter cake.
[0164] The resulting filter cake and 90 liters of deionized water were added to an autoclave equipped with a stirrer, and acetic acid was added to adjust the pH to 7. After purging the autoclave with nitrogen, the temperature was raised to 192°C and maintained for 30 minutes. The autoclave was then cooled, and the contents were removed.
[0165] The contents were filtered through a glass filter by suction, and then 76 liters of ion-exchange water at 70°C were injected. The mixture was then filtered again by suction to obtain a filter cake. The filter cake was dried at 120°C under a nitrogen stream to obtain dried PPS.
[0166] The obtained PPS resin was subjected to thermal oxidation treatment by heating at 220°C and 2% oxygen concentration for 12 hours. The resulting PPS had an ER of 67 g / 10 min, which translates to an MFR of 4658 g / 10 min.
[0167] [Reference Example 2]
[0168] To a 70°C high-pressure reactor equipped with a stirrer and a bottom valve, add 8.27 kg (70.00 mol) of 47.5% sodium hydrosulfide, 2.94 kg (70.63 mol) of 96% sodium hydroxide, 11.45 kg (115.50 mol) of N-methyl-2-pyrrolidone (NMP), 0.513 kg (6.25 mol) of sodium acetate, and 3.82 kg of deionized water. The reactor was slowly heated to 245°C under normal pressure with nitrogen purging for approximately 3 hours. After distilling off 8.09 kg of water and 0.28 kg of NMP, the reactor was cooled to 200°C. The residual water content in the system, including water consumed by NMP hydrolysis, was 1.06 mol per mole of alkali metal sulfide added. Additionally, the amount of hydrogen sulfide escaping was 0.02 mol per mole of alkali metal sulfide added.
[0169] Then, 10.34 kg (70.32 mol) of p-dichlorobenzene and 9.37 kg (94.50 mol) of NMP were added. The reaction vessel was sealed under nitrogen atmosphere, and the temperature was increased from 200 °C to 270 °C at a rate of 0.6 °C / min with stirring at 240 rpm. The reaction was carried out at 270 °C for 140 minutes. Then, 2.67 kg (148.4 mol) of water was injected while cooling from 270 °C to 250 °C over 15 minutes. Next, the mixture was slowly cooled from 250 °C to 220 °C over 75 minutes, then quenched to near room temperature, and the contents were removed.
[0170] The contents were diluted with approximately 35 liters of NMP to form a slurry. After stirring at 85°C for 30 minutes, the slurry was filtered through an 80-mesh metal screen (0.175 mm pores) to obtain a solid. The obtained solid was washed with approximately 35 liters of NMP and filtered again. The process of diluting the obtained solid with 70 liters of deionized water, stirring at 70°C for 30 minutes, and filtering through an 80-mesh metal screen to recover the solid was repeated three times. The obtained solid and 32 g of acetic acid were diluted with 70 liters of deionized water, stirred at 70°C for 30 minutes, and filtered through an 80-mesh metal screen. The obtained solid was then diluted with 70 liters of deionized water, stirred at 70°C for 30 minutes, and filtered through an 80-mesh metal screen to recover the solid. The resulting solid was dried at 120°C under a nitrogen stream to obtain dried PPS. The MFR of the obtained PPS was 600 g / 10 minutes.
[0171] The raw materials used in the examples and comparative examples are shown below.
[0172] (A) PPS resin
[0173] PPS-1: PPS resin polymerized by the method described in Reference Example 1
[0174] PPS-2: PPS resin polymerized by the method described in Example 2.
[0175] (B) Non-fibrous inorganic fillers
[0176] B-1: Surface-treated magnesium hydroxide (Kisuma 5P manufactured by Kyowa Chemical Industry Co., Ltd., treated with silane coupling agent)
[0177] B-2: Surface-treated magnesium hydroxide (EP1 vinyl silane treated product manufactured by Shinjima Chemical Industry Co., Ltd.)
[0178] B-3: Surface-treated magnesium hydroxide (EP3 vinylsilane treated product manufactured by Shinjima Chemical Industry Co., Ltd., standard deviation of particle size distribution: 0.29, average particle size: 4.0 μm, 10%D: 1.38 μm)
[0179] B-4: Surface-treated magnesium hydroxide (S-4, fatty acid + vinyl silane treatment, manufactured by Kamitsu Chemical Industry Co., Ltd.)
[0180] B-5: Surface-treated magnesium hydroxide (Kisuma 5L manufactured by Kyowa Chemical Industry Co., Ltd., treated with silane coupling agent)
[0181] B-6: Surface-treated magnesium hydroxide (manufactured by Huber-Engineered-Materials, Magnifin (registered trademark) H-5A, vinylsilane treatment).
[0182] (C) Fibrous inorganic filler
[0183] C-1: Short-cut glass fiber (CSG 3PA 830 S manufactured by Nitto Boshoku Co., Ltd., 3mm long, 7μm short diameter, 28μm long diameter, flatness ratio 4)
[0184] C-2: Chopped glass fiber (manufactured by Nippon Electric Glass Co., Ltd., T-760H; length 3mm, average fiber diameter 10.5μm, flatness ratio 1)
[0185] C-3: Short-cut glass fiber (manufactured by Nitto Boshoku Co., Ltd., CSG3PA9886; length 3mm, short diameter 7μm, long diameter 28μm, flatness ratio 4).
[0186] (D) Elastomer
[0187] D-1: Ethylene-glycidyl methacrylate-methyl acrylate copolymer (Sumitomo Chemical Co., Ltd. Bondfast (registered trademark) 7M; ethylene 67% by mass, glycidyl methacrylate 6% by mass, methyl acrylate 27% by mass)
[0188] D-2: Ethylene-1-octene copolymer (manufactured by Dow Chemical Company, Engage (registered trademark) 8842; glass transition temperature -61°C).
[0189] (E) Organosilicon compounds
[0190] E-1: Silica powder loaded with dimethyl silicone oil (manufactured by Dow Toray Co., Ltd., DOWSILTREFIL (registered trademark) F-202).
[0191] E-2: Organosilicon elastomer powder (manufactured by Dow Toray Co., Ltd., DOWSIL EP-2601, epoxy modified).
[0192] (F) Organosilanes F-1: β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane (manufactured by Shin-Etsu Chemical Industry Co., Ltd., KBM-303).
[0193] (G) Other resins G-1: Nylon 610 (manufactured by Toray Industries, Inc., CM2021).
[0194] The evaluation and measurement methods used in the examples and comparative examples are shown below.
[0195] [Standard deviation of particle size distribution of non-fibrous inorganic fillers, average particle size, 10%D]
[0196] 20 mg of a non-fibrous inorganic filler was added to 5 mL of a 0.2 w / v sodium hexametaphosphate aqueous solution and dispersed for 3 minutes using an ultrasonic cleaner. The resulting dispersion was then measured using a particle size distribution measuring apparatus (SALD-2100) manufactured by Shimadzu Corporation, and the standard deviation, volume average particle size, and 10%D were calculated. The standard deviation is expressed on a logarithmic scale. Furthermore, when multiple non-fibrous inorganic fillers were mixed in the examples and comparative examples, the mixtures prepared at the specified mixing ratios (by weight) were used for the measurements.
[0197] [Resistance to tracking]
[0198] A square plate (80mm × 80mm × 3.0mm thickness) injection molded using a Sumitomo Heavy Industries, Ltd. injection molding machine (SE50DUZ-C160) at a barrel temperature of 320°C and a mold temperature of 130°C was used as the test sample. The maximum voltage that would not cause tracking damage was determined according to IEC 60112, 4th edition. A 0.1% ammonium chloride aqueous solution was used as the electrolyte.
[0199] [Resistance to thermal shock]
[0200] In the mold of an injection molding machine (SE30D) manufactured by Sumitomo Heavy Industries, Ltd., a 50mm×35mm×5mm box-type metal insert 1 (material: SUS430) with two holes in the center is installed. Under the conditions of injection speed 70mm / s, filling time 0.5s, injection pressure, holding pressure at injection pressure × 0.6 for 5s, barrel temperature 320℃, and mold temperature 130℃, injection molding is performed from gate 2 to obtain... Figure 1 The metal insert molded article 3 is shown. A thermal shock treatment was performed by treating the metal insert molded article 3 at 130°C for 1 hour, followed by treatment at -40°C for 1 hour, as one cycle. Every 10 cycles, the presence of cracks was visually checked. The average number of cycles until cracks appeared was calculated as N=3. This test piece is a test piece with an intentionally created weld section by setting a hole in the central part, intended to determine the thermal shock resistance of the weld section.
[0201] [Tensile strength, tensile elongation]
[0202] Test specimens conforming to ISO 20753 (2008) were produced using a Sumitomo Heavy Industries injection molding machine (SE75DUZ-C250) at a resin temperature of 310°C and a mold temperature of 140°C. Tensile strength and elongation at break (fracture point) were determined according to ISO 527-1 / -2 at a support distance of 114 mm and a tensile speed of 5 mm / min.
[0203] [Tensile strength of welded wire]
[0204] Type IV test pieces as specified in ASTM-D638 were injection molded using a Sumitomo Heavy Industries SE75DUZ-C250 injection molding machine at a resin temperature of 320°C and a mold temperature of 150°C. Tensile strength and elongation at break (fracture point) were determined according to ISO 527-1.2, with a support distance of 65 mm and a tensile speed of 5 mm / min. This test piece was designed to intentionally create a weld joint in the center by allowing resin to flow from both ends, intended for determining the strength of the weld joint.
[0205] [Examples 1-13, Comparative Examples 1-8]
[0206] Using a TEX30α twin-screw extruder manufactured by Nippon Steel Corporation, set to a barrel temperature of 300°C and a screw speed of 200 rpm, (A) PPS resin, (B) non-fibrous inorganic filler, (C) fibrous inorganic filler, (D) elastomer, (E) organosilicon compound, (F) organosilane compound, and (G) other resins were melt-blended according to the weight ratios described in Tables 1 and 2. (A) PPS resin, (B) non-fibrous inorganic filler, (D) elastomer, (E) organosilicon compound, (F) organosilane compound, and (G) other resins were added from the feed inlet to achieve a molten state, while (C) fibrous inorganic filler was added from the side feeder of the twin-screw extruder. The resin discharged from the extruder was granulated using a pulverizer and hot-air dried overnight at 120°C, followed by various molding processes and evaluations.
[0207] It is evident that in Examples 1-13, by setting the standard deviation, average particle size, and 10%D of the particle size distribution of the (B) non-fibrous inorganic filler within a specified range, the raw material formulation was optimized, resulting in excellent resistance to tracking and thermal shock in the metal insert molded articles. The PPS resin composition of this embodiment can be safely used in molded articles or metal insert molded articles subjected to high voltage, such as automotive parts or electrical and electronic components.
[0208] The PPS resin composition of Comparative Example 1 has poor resistance to thermal shock because the standard deviation of the particle size distribution of the non-fibrous inorganic filler (B) is very small.
[0209] The PPS resin composition of Comparative Example 2 has poor resistance to thermal shock because the particle size distribution of the (B) non-fibrous inorganic filler has a small standard deviation and a small average particle size.
[0210] The PPS resin composition of Comparative Example 3 has poor resistance to tracking because it does not contain (B) non-fibrous inorganic fillers and (E) organosilicon compounds.
[0211] The PPS resin composition of Comparative Example 4 has poor resistance to tracking and thermal shock because the particle size distribution of (B) non-fibrous inorganic filler has a small standard deviation, the amount of which is mixed is small, and it does not contain (E) organosilicon compounds.
[0212] The PPS resin composition of Comparative Example 5 has poor resistance to thermal shock because (C) the fibrous inorganic filler is not a glass with an irregular cross section.
[0213] The PPS resin composition of Comparative Example 6 has poor resistance to thermal shock because (B) the non-fibrous inorganic filler has a small standard deviation in particle size distribution, and does not contain (D) elastomers or (E) organosilicon compounds.
[0214] The PPS resin composition of Comparative Example 7 has poor resistance to thermal shock because the standard deviation of the particle size distribution of the (B) non-fibrous inorganic filler is small.
[0215] The PPS resin composition of Comparative Example 8 has poor resistance to thermal shock because it does not contain (E) organosilicon compounds.
[0216] Explanation of symbols in attached drawings
[0217] 1. Metal inserts
[0218] 2. Gate
[0219] 3. Molded metal inserts
[0220]
[0221]
Claims
1. A polyphenylene sulfide resin composition, which is a polyphenylene sulfide resin composition mixed with polyphenylene sulfide resin, having a tracking resistance of 300V or higher and a thermal shock resistance of more than 15 cycles for metal insert molded articles.
2. The polyphenylene sulfide resin composition according to claim 1 is a polyphenylene sulfide resin composition in which 20 parts by weight and 170 parts by weight of (B) non-fibrous inorganic filler are mixed with 100 parts by weight of (A) polyphenylene sulfide resin, wherein the standard deviation of the particle size distribution of (B) non-fibrous inorganic filler is 0.22 or more and 10.00 or less.
3. The polyphenylene sulfide resin composition according to claim 2, wherein the (B) non-fibrous inorganic filler is a decomposition endothermic filler.
4. The polyphenylene sulfide resin composition according to claim 1, wherein 0.1 parts by weight and 20 parts by weight of organosilicon compound (E) are mixed with 100 parts by weight of polyphenylene sulfide resin (A).
5. A polyphenylene sulfide resin composition comprising, relative to 100 parts by weight of (A) polyphenylene sulfide resin, 20 parts by weight and 170 parts by weight of (B) a non-fibrous inorganic filler, wherein the standard deviation of the particle size distribution of (B) the non-fibrous inorganic filler is 0.22 or more and 10.00 or less, and (B) the non-fibrous inorganic filler is a decomposition endothermic filler, and relative to 100 parts by weight of (A) polyphenylene sulfide resin, 0.1 parts by weight and 20 parts by weight of (E) an organosilicon compound.
6. The polyphenylene sulfide resin composition according to claim 2 or 5, wherein the average particle size of the (B) non-fibrous inorganic filler is 1.0 μm or more and 50.0 μm or less.
7. The polyphenylene sulfide resin composition according to claim 2 or 5, wherein the 10%D of the (B) non-fibrous inorganic filler is 0.1 μm or more and 1.2 μm or less.
8. The polyphenylene sulfide resin composition according to claim 1 or 5, wherein, relative to 100 parts by weight of (A) polyphenylene sulfide resin, there are 40 parts by weight and 190 parts by weight of (C) fibrous inorganic filler.
9. The polyphenylene sulfide resin composition of claim 8, wherein the (C) fibrous inorganic filler is irregularly shaped glass fiber.
10. The polyphenylene sulfide resin composition according to claim 1 or 5, wherein, relative to 100 parts by weight of (A) polyphenylene sulfide resin, there is a mixture of 1 part by weight and 40 parts by weight of (D) elastomer.
11. A molded article formed from the polyphenylene sulfide resin composition of claim 1 or 5.
12. A metal insert molded article comprising the molded article of claim 11.
13. An automotive electrical component comprising the molded article of claim 11.
14. An electric drive axle comprising the molded article of claim 11.
15. An electric vehicle (xEV) comprising the molded article of claim 11.
Citation Information
Patent Citations
High-strength polyarylenesulfide-based composition
JP2014145006A
Polyarylene sulfide resin composition, method for producing same, and molded body
WO2015137228A1