Resin compositions, prepregs, laminates, metal-clad laminates, printed circuit boards, and semiconductor packages

By using a phosphorus-based flame retardant and thermosetting resin composition with a styrene skeleton in printed circuit boards, the problems of through-hole deformation and uneven plating caused by resin dissolution are solved, the peel strength of copper foil and resistance to adhesive residue removal are improved, and the structural stability and circuit integrity of printed circuit boards are ensured.

CN123125283APending Publication Date: 2026-11-17RESONAC CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202580029239.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-07-19
Filing Date
2025-07-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing printed circuit boards, the resin components dissolve during the descaling process after through-hole formation, leading to through-hole shape deformation and uneven plating. Furthermore, increasing the content of phosphorus-based flame retardants results in insufficient copper foil peel strength and resistance to descaling.

Method used

A resin composition containing a phosphorus-based flame retardant with a styrene skeleton is used, combined with thermosetting resin and filler, to optimize the resin composition ratio and structure, thereby improving flame retardancy, copper foil peel strength and resistance to adhesive residue removal.

Benefits of technology

This technology achieves improved copper foil peel strength and resistance to adhesive residue removal while maintaining flame retardancy, ensuring the structural stability and circuit integrity of printed circuit boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention provides a resin composition exhibiting excellent flame retardancy, high copper foil peel strength, and high resistance to adhesive residue removal. Furthermore, this invention provides prepregs, laminates, metal-clad laminates, printed circuit boards, and semiconductor packages manufactured using this resin composition. Specifically, the resin composition is a resin composition containing (A) a thermosetting resin and (B) a flame retardant, wherein the (B) flame retardant comprises (B1) a phosphorus-based flame retardant having a styrene backbone.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to resin compositions, prepregs, laminates, metal-clad laminates, printed circuit boards, and semiconductor packages. Background Technology

[0002] In the flame retardancy of materials for printed circuit boards, many studies have taken halogen-free properties into consideration from an environmental perspective. Therefore, in recent years, to impart flame retardancy to materials for printed circuit boards, most researchers have considered halogen-free phosphorus-based flame retardants with high flame retardancy enhancement effects to be preferred (see, for example, Patent Document 1).

[0003] Existing technical documents

[0004] Patent documents

[0005] Patent Document 1: Japanese Patent Application Publication No. 2021-138803 Summary of the Invention

[0006] The problem that the invention aims to solve

[0007] However, the manufacture of printed circuit boards includes forming through-holes for interlayer bonding. These through-holes are formed through processes such as laser processing or drilling, but after these processes, a process to remove residual resin components (so-called desmearing) is typically performed. Because desmearing is performed on the bottom and walls of the through-holes, if a significant amount of resin in the substrate dissolves due to this process, the shape of the through-hole may be significantly deformed. Furthermore, various problems may occur, such as uneven plating coverage due to variations in the wall surface. Therefore, it is necessary to reduce the amount of resin dissolved in the substrate due to desmearing.

[0008] In addition, in printed circuit boards, a peel strength is required that prevents the conductor layers constituting the printed wiring and circuit patterns from peeling off, even when the circuit pattern is miniaturized.

[0009] However, the inventors conducted research and found that if the content of phosphorus-containing flame retardant is increased in order to impart flame retardancy to the material for printed circuit boards, the copper foil peel strength and resistance to descaling of the printed circuit board become insufficient. It is evident that it is difficult to maintain both the copper foil peel strength and resistance to descaling while maintaining the flame retardancy.

[0010] In view of the above, the object of this disclosure is to provide a resin composition exhibiting excellent flame retardancy, high copper foil peel strength, and high resistance to adhesive residue. Furthermore, the object is to provide prepregs, laminates, metal-clad laminates, printed circuit boards, and semiconductor packages manufactured using this resin composition.

[0011] Methods for solving problems

[0012] The inventors conducted research in order to achieve the above objectives, and found that the above objectives can be achieved through this disclosure.

[0013] This disclosure includes the following embodiments [1] to

[13] .

[0014] [1] A resin composition comprising (A) a thermosetting resin and (B) a flame retardant,

[0015] The above-mentioned flame retardant (B) includes (B1) a phosphorus-based flame retardant with a styrene skeleton.

[0016] [2] According to the resin composition described in [1] above, wherein the above-mentioned (B1) component has two or more styrene skeletons.

[0017] [3] According to the resin composition described in [1] or [2] above, wherein the (B1) component has a structural unit represented by the following general formula (B-1).

[0018] [Chemical Formula 1]

[0019]

[0020] (where R) b1 (This refers to organic groups with 1 to 20 carbon atoms.)

[0021] [4] The resin composition according to any one of [1] to [3] above, wherein the content of the above (B1) component is 1 to 25 parts by mass relative to the total amount of the above (A) component and the above (B) component 100 parts by mass.

[0022] [5] The resin composition according to any one of [1] to [4] above, wherein the (A) component comprises at least one selected from epoxy resin, polyimide resin, maleimide compound, phenolic resin, polyphenylene ether resin, bismaleimide triazine resin, cyanate resin, isocyanate resin, benzoxazine resin, oxetane resin, amino resin, unsaturated polyester resin, allyl resin, dicyclopentadiene resin and organosilicon resin.

[0023] [6] The resin composition according to any one of [1] to [5] above, wherein the above-mentioned component (A) comprises at least one selected from maleimide compounds having one or more N-substituted maleimide groups and their derivatives.

[0024] [7] The resin composition according to any one of [1] to [6] above, wherein the above component (A) comprises a siloxane-modified maleimide compound.

[0025] [8] The resin composition according to any one of [1] to [7] above further contains (C) filler.

[0026] [9] A prepreg comprising a substrate and a semi-cured product of the resin composition described in any one of [1] to [8] above.

[0027]

[10] A laminate comprising the prepreg described in [9] above.

[0028]

[11] A metal-clad laminate comprising a metal foil and a cured form of the prepreg described in [9] above.

[0029]

[12] A printed circuit board comprising the laminate described in

[10] above or the metal-clad laminate described in

[11] above.

[0030]

[13] A semiconductor package comprising the printed circuit board and semiconductor element described in

[12] above.

[0031] Invention Effects

[0032] According to this disclosure, a resin composition exhibiting excellent flame retardancy, high copper foil peel strength, and high resistance to adhesive residue can be provided. Furthermore, prepregs, laminates, metal-clad laminates, printed circuit boards, and semiconductor packages manufactured using this resin composition can be provided. Detailed Implementation

[0033] In the numerical ranges described in this specification, the upper or lower limit of the numerical range can be replaced with the values ​​shown in the embodiments. Furthermore, the lower and upper limits of the numerical ranges can be arbitrarily combined with the lower or upper limits of other numerical ranges. In expressions such as "AA~BB", the values ​​AA and BB at both ends are included in the numerical range as the lower and upper limits, respectively.

[0034] In this specification, for example, a description such as "10 or more" refers to a value of 10 or more, and this shall apply even if the value differs. Similarly, a description such as "10 or less" refers to a value of 10 or less, and this shall apply even if the value differs.

[0035] Furthermore, unless otherwise specified, each component and material illustrated in this specification may be used individually or in combination with two or more. In this specification, the content of each component in the composition refers to the total amount of the multiple substances present in the composition, unless otherwise specified. This is especially relevant when multiple substances equivalent to each component are present in the composition.

[0036] In this disclosure, "resin component" refers to all components in the solid components constituting the resin composition other than inorganic compounds such as inorganic fillers, which will be described later.

[0037] In this disclosure, "solid component" refers to components other than the organic solvents described later, and components that are liquid at 25°C are also considered solid components.

[0038] The expression "containing XX" as described in this disclosure means either a situation in which XX is capable of reacting, or a situation in which XX is simply contained, where XX has reacted.

[0039] The arbitrary combination of the items described in this disclosure is also included in this disclosure and this embodiment.

[0040] [Resin Composition]

[0041] One embodiment relates to a resin composition comprising (A) a thermosetting resin and (B) a flame retardant, wherein the (B) flame retardant comprises (B1) a phosphorus-based flame retardant having a styrene skeleton.

[0042] The resin composition of this embodiment contains (B1) a phosphorus-based flame retardant having a styrene skeleton, thereby exhibiting excellent flame retardancy, high copper foil peel strength, and high resistance to adhesive residue removal.

[0043] The components contained in the resin composition of this embodiment will be described in detail below.

[0044] <(A) Thermosetting resin>

[0045] Examples of component (A) include epoxy resin, polyimide resin, maleimide compound, phenolic resin, polyphenylene ether resin, bismaleimide triazine resin, cyanate ester resin, isocyanate ester resin, benzoxazine resin, oxetane resin, amino resin (melamine resin, etc.), unsaturated polyester resin, allyl resin, dicyclopentadiene resin, and silicone resin. Preferably, component (A) is selected from one or more of epoxy resin, maleimide compound, phenolic resin, polyphenylene ether resin, cyanate ester resin, and isocyanate ester resin; more preferably, it is selected from one or more of epoxy resin and maleimide compound; and even more preferably, it combines epoxy resin and maleimide compound.

[0046] As component (A), one type can be used alone or two or more types can be used together.

[0047] (Epoxy resin)

[0048] As described above, epoxy resins having two or more epoxy groups per molecule are preferred. Here, epoxy resins are classified as glycidyl ether type epoxy resins, glycidyl amine type epoxy resins, glycidyl ester type epoxy resins, etc. Among these, glycidyl ether type epoxy resins are preferred.

[0049] Epoxy resins are classified into various types based on their main skeleton. These types are further subdivided into: bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, etc. (bisphenol-type epoxy resins); alicyclic epoxy resins such as dicyclopentadiene type epoxy resin; aliphatic chain epoxy resins; phenolic epoxy resins such as phenol-formaldehyde type epoxy resin, cresol-formaldehyde type epoxy resin, bisphenol A-formaldehyde type epoxy resin, bisphenol F-formaldehyde type epoxy resin, phenol-arylalkyl-formaldehyde type epoxy resin, biphenyl-arylalkyl-formaldehyde type epoxy resin, etc. (phenolic resins); naphthalene-type epoxy resin; naphthol-formaldehyde type epoxy resin, naphthol-arylalkyl-formaldehyde type epoxy resin, etc. (naphthalene-containing skeleton epoxy resins); biphenyl-type epoxy resin; phthalimide type epoxy resin; dihydroanthracene type epoxy resin, etc.

[0050] Among them, from the viewpoints of solder heat resistance, electrical insulation reliability and copper foil peel strength, phenolic epoxy resin and naphthalene skeleton epoxy resin are preferred as epoxy resins, phenolic epoxy resin is more preferred, and biphenyl aryl phenolic epoxy resin is even more preferred.

[0051] The weight-average molecular weight of epoxy resin can be 200–1,000, 250–950, or 300–900. If the weight-average molecular weight of epoxy resin is above the lower limit of the above values, it tends to have excellent heat resistance of solder; if it is below the upper limit of the above values, it tends to exhibit low elasticity and flexibility.

[0052] From a compatibility perspective, the epoxy equivalent of epoxy resin can be 150–500 g / eq, 150–450 g / eq, or 200–350 g / eq.

[0053] (maleimide compound)

[0054] As the aforementioned maleimide compound, it is preferred to include at least one selected from maleimide compounds having one or more (preferably two or more) N-substituted maleimide groups and their derivatives.

[0055] As a maleimide compound having one or more N-substituted maleimide groups, there is no particular limitation, and examples include N-phenylmaleimide, N-(2-methylphenyl)maleimide, N-(4-methylphenyl)maleimide, N-(2,6-dimethylphenyl)maleimide, N-(2,6-diethylphenyl)maleimide, N-(2-methoxyphenyl)maleimide, N-benzylmaleimide, etc., preferably aromatic maleimide compounds having one N-substituted maleimide group bonded to an aromatic ring; 4,4'-diphenylmethane bismaleimide, bis(4-maleimidephenyl) ether, bis(4-maleimidephenyl) sulfone, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, etc. 4-Methyl-1,3-phenylene bismaleimide, m-phenylene bismaleimide, 2,2-bis[4-(4-maleimide phenoxy)phenyl]propane, aromatic bismaleimide containing an indene ring, etc., preferably aromatic bismaleimide compounds having two N-substituted maleimide groups bonded to the aromatic ring; polyphenylmethane maleimide, biphenyl aralkyl maleimide, etc., preferably aromatic polymaleimide compounds having three or more N-substituted maleimide groups bonded to the aromatic ring; N-dodecyl maleimide, N-isopropyl maleimide and N-cyclohexyl maleimide, 1,6-bismaleimide-(2,2,4-trimethyl)hexane, pyrophosphate binder type long-chain alkyl bismaleimide, etc., aliphatic maleimide compounds, etc. From the perspectives of compatibility with other resins, copper foil peel strength, solder heat resistance, low thermal expansion, and mechanical properties, aromatic bismaleimide compounds having two N-substituted maleimide groups bonded to an aromatic ring are preferred, more preferably 4,4'-diphenylmethane bismaleimide, 2,2-bis[4-(4-maleimide phenoxy)phenyl]propane, and aromatic bismaleimides containing an indane ring, and even more preferably 2,2-bis[4-(4-maleimide phenoxy)phenyl]propane.

[0056] Furthermore, in the aforementioned maleimide compounds, "preferably one N-substituted maleimide group bonded to the aromatic ring," "preferably two N-substituted maleimide groups bonded to the aromatic ring," and "preferably three or more N-substituted maleimide groups bonded to the aromatic ring" all preferably have nitrogen atoms bonded to the aromatic ring. Thus, in the aforementioned maleimide compounds, the nitrogen atoms of the preferably N-substituted maleimide groups are bonded to each other via linking groups containing the aromatic ring.

[0057] It should be noted that, as derivatives of maleimide compounds, examples include addition reactions of maleimide compounds having one or more (preferably two or more) of the aforementioned N-substituted maleimide groups with amine compounds such as monoamine compounds and diamine compounds. Examples of the aforementioned monoamine compounds include monoamine compounds with acidic substituents such as o-aminophenol, m-aminophenol, p-aminophenol, o-aminobenzoic acid, m-aminobenzoic acid, p-aminobenzoic acid, o-aminobenzenesulfonic acid, m-aminobenzenesulfonic acid, p-aminobenzenesulfonic acid, 3,5-dihydroxyaniline, and 3,5-dicarboxylated aniline. Examples of the aforementioned diamine compounds include 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylethane, 4,4'-diaminodiphenylpropane, 2,2'-bis(4,4'-diaminodiphenyl)propane, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-diethyl-4,4'-diaminodiphenylmethane, 3,3'-dimethyl-4,4'-diaminodiphenylethane, 3,3'-diethyl-4,4'-diaminodiphenylethane, 4,4'-di... Aminodiphenyl ether, 4,4'-diaminodiphenyl sulfide, 3,3'-dihydroxy-4,4'-diaminodiphenylmethane, 2,2',6,6'-tetramethyl-4,4'-diaminodiphenylmethane, 3,3'-dichloro-4,4'-diaminodiphenylmethane, 3,3'-dibromo-4,4'-diaminodiphenylmethane, 2,2',6,6'-tetrachloro-4,4'-diaminodiphenylmethane, 2,2',6,6'-tetrabromo-4,4'-diaminodiphenylmethane, siloxane diamine, etc.

[0058] A preferred approach is to use derivatives of the aforementioned maleimide compounds that are addition products of maleimide compounds having one or more (preferably two or more) N-substituted maleimide groups and siloxane diamines, i.e., so-called siloxane-modified maleimide compounds.

[0059] As the aforementioned siloxane-modified maleimide compound, the addition reaction product of an aromatic bismaleimide compound siloxane diamine having two N-substituted maleimide groups bonded to an aromatic ring is preferred; more preferably, the addition reaction product of 4,4'-diphenylmethane bismaleimide, 2,2-bis[4-(4-maleimidephenoxy)phenyl]propane, or an aromatic bismaleimide containing an inden ring with a siloxane diamine is preferred; and even more preferably, the addition reaction product of 2,2-bis[4-(4-maleimidephenoxy)phenyl]propane with a siloxane diamine is preferred.

[0060] The weight-average molecular weight (Mw) of the above-mentioned siloxane-modified maleimide compounds is not particularly limited, but is preferably 400 to 10,000, more preferably 1,000 to 5,000, even more preferably 1,500 to 4,000, and particularly preferably 2,000 to 3,000.

[0061] (Content of component (A))

[0062] Relative to the total amount of components (A) and (B) above 100 parts by mass, the content of component (A) is preferably 70 to 99 parts by mass, more preferably 75 to 99 parts by mass, even more preferably 75 to 95 parts by mass, and particularly preferably 80 to 95 parts by mass. If the content of component (A) is above the lower limit mentioned above, there is a tendency to obtain high copper foil peel strength and high solder heat resistance. In addition, if the content of component (A) is below the upper limit mentioned above, the content of component (B) can be increased accordingly, and therefore there is a tendency to improve flame retardancy.

[0063] <(B) Flame retardant>

[0064] In this embodiment, in order to exhibit excellent flame retardancy, high copper foil peel strength and high resistance to descaling, (B) flame retardant includes (B1) a phosphorus-based flame retardant with a styrene skeleton.

[0065] As for the phosphorus-based flame retardant as component (B1), there are no particular limitations as long as it has a styrene skeleton. From the viewpoints of flame retardancy, copper foil peel strength and resistance to glue residue removal, it is preferable to have a phosphorus-based flame retardant with two or more styrene skeletons, more preferably a phosphorus-based flame retardant with two to eight styrene skeletons, even more preferably a phosphorus-based flame retardant with two to five styrene skeletons, and particularly preferably a phosphorus-based flame retardant with three or four styrene skeletons.

[0066] The above-mentioned component (B1) is preferably a phosphazene compound.

[0067] The above-mentioned component (B1) is not particularly limited. From the viewpoints of flame retardancy, copper foil peel strength and resistance to adhesive residue removal, it is preferable to have structural units shown in the following general formula (B-1), more preferably to have 1 to 8 structural units shown in the following general formula (B-1) in 1 molecule, even more preferably to have 2 to 5 structural units shown in the following general formula (B-1) in 1 molecule, and particularly preferably to have 3 or 4 structural units shown in the following general formula (B-1) in 1 molecule.

[0068] [Chemical Formula 2]

[0069]

[0070] (where R) b1 (This refers to organic groups with 1 to 20 carbon atoms.)

[0071] In the above general formula (B-1), R is... b1 Examples of organic groups having 1 to 20 carbon atoms include alkyl groups having 1 to 20 carbon atoms, substituted or unsubstituted aryl groups having 6 to 20 carbon atoms, and combinations thereof.

[0072] It should be noted that R b1 It may or may not contain vinyl.

[0073] As R b1 Examples of alkyl groups having 1 to 20 carbon atoms include methyl, ethyl, propyl, n-butyl, tert-butyl, n-octyl, and n-dodecyl. The alkyl group having 1 to 20 carbon atoms is preferably an alkyl group having 1 to 10 carbon atoms, and more preferably an alkyl group having 1 to 5 carbon atoms.

[0074] As R b1 Examples of aryl groups with 6 to 20 carbon atoms include phenyl, naphthyl, and anthracene. The aryl group with 6 to 20 carbon atoms is preferably an aryl group with 6 to 14 carbon atoms, more preferably an aryl group with 6 to 12 carbon atoms, and even more preferably an aryl group with 6 to 10 carbon atoms.

[0075] R b1 The aryl group with 6 to 20 carbon atoms shown may or may not have substituents. Examples of such substituents include hydroxyl groups, alkyl groups with 1 to 5 carbon atoms, and alkoxy groups with 1 to 5 carbon atoms.

[0076] As R b1 Examples of groups consisting of an alkyl group having 1 to 20 carbon atoms (hereinafter simply referred to as alkyl) and a substituted or unsubstituted aryl group having 6 to 20 carbon atoms (hereinafter simply referred to as aryl) include -alkyl-aryl, -aryl-alkyl, -alkyl-aryl-alkyl, etc. Preferred forms of alkyl and aryl groups are as described above.

[0077] From the viewpoints of flame retardancy, copper foil peel strength and resistance to adhesive residue removal, the structural unit shown in general formula (B-1) is preferably the structural unit shown in general formula (B-2) below.

[0078] [Chemical Formula 3]

[0079]

[0080] From the viewpoints of flame retardancy, copper foil peel strength and resistance to adhesive residue removal, the above-mentioned component (B1) is preferably represented by the following general formula (B-3).

[0081] [Chemical Formula 4]

[0082]

[0083] (where n) b1 (Integers greater than or equal to 3.)

[0084] In general formula (B-3), n b1From the viewpoints of flame retardancy, copper foil peel strength and resistance to adhesive residue removal, the integer value is preferably 3 to 8, more preferably 3 to 5, and even more preferably 3 or 4.

[0085] From the viewpoints of flame retardancy, copper foil peel strength, and resistance to adhesive residue removal, the above-mentioned component (B1) is preferably represented by the following general formula (B-4). The flame retardant represented by the following general formula (B-4) can be obtained from Fushimi Pharmaceutical Co., Ltd.

[0086] [Chemical Formula 5]

[0087]

[0088] (Content of component (B1))

[0089] Relative to the total amount of components (A) and (B) above 100 parts by mass, the content of component (B1) is preferably 1 to 25 parts by mass, more preferably 2 to 20 parts by mass, even more preferably 3 to 18 parts by mass, and particularly preferably 5 to 15 parts by mass. If the content of component (B1) is above the lower limit mentioned above, there is a tendency to exhibit excellent flame retardancy, high copper foil peel strength, and high resistance to descaling. In addition, if the content of component (B1) is below the upper limit mentioned above, there is a tendency to suppress the decrease in glass transition temperature and easily exhibit good solder heat resistance.

[0090] In the resin composition of this embodiment, component (B) may contain a flame retardant other than component (B1), or it may not contain one.

[0091] Flame retardants other than component (B1) include phosphate ester compounds, phosphine compounds, etc.; halogenated flame retardants; metal hydrates, etc.

[0092] (Content of component (B))

[0093] Relative to the total amount of component (A) and component (B) of 100 parts by mass, the content of component (B), i.e., the total content, is preferably 1 to 30 parts by mass, more preferably 1 to 25 parts by mass, even more preferably 5 to 25 parts by mass, and particularly preferably 5 to 20 parts by mass. By setting the content of component (B) to the lower limit or above, there is a tendency to easily obtain excellent flame retardancy. Furthermore, if the content of component (B) is below the upper limit, there is a tendency to achieve low thermal expansion.

[0094] It should be noted that when the resin composition of this embodiment contains a flame retardant other than component (B1) as component (B), the content of the flame retardant other than component (B1) is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, even more preferably 5 parts by mass or less, and particularly preferably 1 part by mass or less, relative to the total amount of component (A) and component (B) above 100 parts by mass. There is no particular limitation on the lower limit value, and it can be 0.1 parts by mass or more, or 0.5 parts by mass or more.

[0095] <(C) Packing>

[0096] The resin composition of this embodiment may further contain (C) filler.

[0097] As for filler (C), there are no particular limitations, but inorganic fillers are preferred from the viewpoint of ensuring low thermal expansion and flame retardancy. Examples of inorganic fillers include silica, alumina, titanium dioxide, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, calcium silicate, calcium oxide, magnesium oxide, aluminum nitride, aluminum borate whiskers, boron nitride, and silicon carbide. Filler (C) can be used alone or in combination with two or more types. Among these, silica is preferred from the perspectives of low relative permittivity and low coefficient of linear expansion. Examples of silica include synthetic silica synthesized by wet or dry methods, crushed silica, and fused silica.

[0098] (C) The filler may be a filler that has undergone coupling treatment. As the coupling agent used in the above-mentioned coupling treatment, a silane coupling agent is preferred. Examples of silane coupling agents include aminosilane-based coupling agents, epoxysilane-based coupling agents, phenylsilane-based coupling agents, alkylsilane-based coupling agents, alkenylsilane-based coupling agents, alkynylsilane-based coupling agents, and organosilicon oligomer-based coupling agents. One of these can be used alone, or two or more can be used in combination.

[0099] The average particle size of component (C) is preferably 0.1 to 2.5 μm, more preferably 0.2 to 1.5 μm, and even more preferably 0.3 to 0.8 μm. If the average particle size of component (C) is above the lower limit mentioned above, the filler is easily dispersed in the resin varnish and therefore tends to be less prone to agglomeration. If it is below the upper limit mentioned above, component (C) tends to settle less easily in the resin varnish.

[0100] In this embodiment, the average particle size refers to the particle size at a point that corresponds to 50% of the volume when the total volume of the particles is set to 100% and a cumulative degree distribution curve based on particle size is obtained. This can be measured using a particle size distribution measuring device that uses laser diffraction scattering.

[0101] (C) Content of component

[0102] When the resin composition of the present embodiment contains component (C), the content of component (C) is not particularly limited. Based on 100 parts by mass of the total amount of the aforementioned component (A) and the aforementioned component (B), it is preferably 30 to 300 parts by mass, more preferably 50 to 250 parts by mass, further preferably 70 to 200 parts by mass, particularly preferably 100 to 200 parts by mass, and most preferably 130 to 170 parts by mass. When the content of component (C) is at or above the aforementioned lower limit value, there is a tendency that low thermal expansibility is enhanced and sufficient solder heat resistance can be obtained. When the content of component (C) is at or below the aforementioned upper limit value, there is a tendency that the heat resistance and the like possessed by component (A) and the flame retardancy possessed by component (B) can be easily obtained.

[0103] <(D) Curing Accelerator>

[0104] The resin composition of the present embodiment may contain (D) a curing accelerator. As the component (D), one type may be used alone, or two or more types may be used in combination.

[0105] For example, when the aforementioned component (A) contains an epoxy resin, the component (D) is not particularly limited, and preferably contains one or more selected from amine compounds and imidazole-based compounds, and more preferably contains an imidazole-based compound.

[0106] Examples of the aforementioned amine compound include dicyandiamide, diaminodiphenylethane, guanylurea and the like.

[0107] Examples of the aforementioned imidazole-based compound include 2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-phenylimidazolium trimellitate, benzimidazole, isocyanate-blocked imidazole (for example, an addition reactant of hexamethylene diisocyanate resin and 2-ethyl-4-methylimidazole, etc.) and the like.

[0108] (Content of Component (D))

[0109] When the resin composition of the present embodiment contains component (D), the content of component (D) is not particularly limited. Based on 100 parts by mass of the total amount of the aforementioned component (A) and the aforementioned component (B), it is preferably 0.01 to 10 parts by mass, more preferably 0.03 to 2 parts by mass, and further preferably 0.1 to 1 part by mass.

[0110] <Other Components>

[0111] The resin composition of this embodiment may contain, as needed, crosslinking agents, flame retardants, rubber-based elastomers, conductive particles, coupling agents, flow modifiers, antioxidants, heat stabilizers, antistatic agents, pigments, leveling agents, defoamers, ion traps, etc. These other components may be of known composition.

[0112] When the resin composition of this embodiment contains the other components described above, their content is preferably 0.1 to 10 parts by mass relative to 100 parts by mass of the total amount of component (A) and component (B) described above, more preferably 0.1 to 5 parts by mass, and even more preferably 0.1 to 3 parts by mass.

[0113] The resin composition of this embodiment can be in a state of being dissolved or dispersed in an organic solvent, that is, in the state of a so-called "resin varnish". Hereinafter, the resin composition containing an organic solvent will sometimes be referred to as a resin varnish.

[0114] Examples of organic solvents mentioned above include ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; aromatic hydrocarbon solvents such as toluene and xylene; ester solvents such as methoxyethyl acetate, ethoxyethyl acetate, butoxyethyl acetate, and ethyl acetate; amide solvents such as N-methylpyrrolidone, formamide, N-methylformamide, and N,N-dimethylacetamide; and alcohol solvents such as methanol, ethanol, ethylene glycol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, triethylene glycol, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, propylene glycol monopropyl ether, and dipropylene glycol monopropyl ether. One organic solvent can be used alone, or two or more can be used in combination.

[0115] The concentration of solid components in the varnish is preferably 10-70% by mass, more preferably 20-60% by mass, and even more preferably 35-60% by mass.

[0116] [Prepreg]

[0117] The prepreg of this embodiment comprises a substrate and a semi-cured product of the resin composition of this embodiment. Here, the expression "semi-cured product comprising a substrate and a resin composition of this embodiment" refers to a substance formed by semi-curing (B-stage) while the resin composition is impregnated in the substrate. Here, in this specification, B-stage refers to the state of forming the B-stage as defined in JIS K 6900 (1994).

[0118] The prepreg can be manufactured, for example, by impregnating or coating a varnish-like resin composition of this embodiment onto a substrate and then heating and drying it, thereby semi-curing (B-stage curing) the resin composition.

[0119] As a method for impregnating or coating a resin composition onto a substrate, the following hot-melt method or solvent method can be used.

[0120] The hot melt method is a method in which the resin composition does not contain organic solvents, (1) temporarily coated onto a coated paper with good peelability to the resin composition, and laminated onto a substrate, or (2) directly coated onto the substrate using a die coater.

[0121] On the other hand, the solvent method is as follows: the resin composition contains an organic solvent, the substrate is immersed in the obtained resin composition, thereby allowing the resin composition to penetrate the substrate, and then it is dried.

[0122] As the substrate, woven fabrics, non-woven fabrics, and other fiber substrates are commonly used, with woven fabrics being preferred. Alternatively, sheet-like fiber substrates are also preferred.

[0123] Examples of materials that can be used as fiber substrates include inorganic fibers such as glass, alumina, asbestos, boron, silica, alumina glass, silica glass, Tyranno, silicon carbide, silicon nitride, and zirconium oxide; organic fibers such as aromatic polyamides, polyetheretherketones, polyetherimides, polyethersulfones, carbon, and cellulose; and blends thereof. Among these, inorganic fibers are preferred, and glass fibers are more preferred. That is, woven fabrics of glass fibers, i.e., glass cloth, are preferred as substrates.

[0124] The thickness of the substrate is preferably 5–200 μm, but can be 10–100 μm or 20–50 μm. By setting the thickness of the substrate below the above upper limit, dimensional changes due to temperature variations, moisture absorption, etc., during the manufacturing process can be reduced.

[0125] There are no particular limitations on the manufacturing conditions of the prepreg. If it is a solvent method, the organic solvent used in the resin varnish should preferably evaporate by more than 80% by mass in the obtained prepreg.

[0126] The drying temperature after impregnating or coating the resin composition onto the substrate is preferably 80–180°C, more preferably 100–140°C, and the drying time is appropriately set taking into account the gelation time of the resin composition.

[0127] The content of solid components derived from the resin composition in the prepreg of this embodiment is not particularly limited, but is preferably 30 to 90% by mass, more preferably 35 to 80% by mass, even more preferably 40 to 70% by mass, and particularly preferably 45 to 60% by mass. If the content of solid components derived from the resin composition in the prepreg is within the above range, there is a tendency to obtain good formability when producing laminates.

[0128] The thickness of the prepreg in this embodiment is not particularly limited; it can be 10–200 μm, 10–150 μm, or 10–100 μm.

[0129] [Laminated laminates, metal-clad laminates]

[0130] The laminate in this embodiment is a laminate containing a cured prepreg of this embodiment. Here, the laminate in this embodiment is also a laminate containing a cured resin composition of this embodiment.

[0131] Furthermore, the metal-clad laminate of this embodiment is a metal-clad laminate comprising a cured metal foil and the prepreg of this embodiment. Here, the metal-clad laminate of this embodiment is also a metal-clad laminate comprising a cured metal foil and the resin composition of this embodiment.

[0132] Metal-clad laminates can be manufactured, for example, by overlapping the adhesive surfaces of both sides of a single prepreg or the two sides of a laminate formed by stacking two or more (preferably 2 to 20) prepregs with a metal foil, and then heating and pressing the laminate under vacuum at a temperature preferably 130 to 260°C, more preferably 180 to 250°C, and even more preferably 210 to 250°C, and at a pressure of 0.5 to 10 MPa, preferably 1 to 5 MPa.

[0133] Examples of metal foils used in metal-clad laminates include copper foil, aluminum foil, tin foil, tin-lead alloy (solder) foil, and nickel foil. In addition, composite foils with a three-layer structure (using nickel, nickel-phosphorus, nickel-tin alloy, nickel-iron alloy, lead, or lead-tin alloy as intermediate layers, with 0.5–15 μm and 10–300 μm copper layers on both sides) and two-layer composite foils (combining aluminum and copper foil) can also be used.

[0134] As a metal foil, copper foil and aluminum foil are preferred, with copper foil being more preferred.

[0135] The thickness of the metal foil can be set to the thickness typically used for laminates, for example, 1 to 200 μm.

[0136] It should be noted that in the laminate and metal-clad laminate of this embodiment, the prepreg (more specifically, the resin composition in the prepreg) has undergone C-stepping to become a cured product. In other words, it can also be said that the laminate of this embodiment contains a C-stepped prepreg, and the metal-clad laminate of this embodiment contains a C-stepped prepreg and a metal foil. Here, in this specification, C-stepping refers to forming a C-step state as defined in JIS K6900 (1994).

[0137] Printed Circuit Board

[0138] The printed circuit board of this embodiment includes the laminate or metal-clad laminate of this embodiment. The printed circuit board of this embodiment does not necessarily need to include the laminate or metal-clad laminate as is. For example, it may include the laminate or metal-clad laminate in a state in which circuit forming processes such as hole forming, metal plating, and metal foil etching have been performed on the laminate or metal-clad laminate.

[0139] The printed circuit board of this embodiment can be manufactured as follows: using the laminate or metal-clad laminate of this embodiment, circuit formation processing based on hole processing, metal plating processing, metal foil etching, etc. is performed by known methods, and further multilayer processing is performed as needed, thereby manufacturing the board.

[0140] [Semiconductor package]

[0141] The semiconductor package of this embodiment includes the printed circuit board and semiconductor elements of this embodiment. In other words, the semiconductor package of this embodiment is formed by mounting semiconductor elements on the printed circuit board of this embodiment.

[0142] The semiconductor package of this embodiment can be manufactured as follows: semiconductor components such as semiconductor chips and memory are mounted on a predetermined position on the printed circuit board of this embodiment using known methods, and the semiconductor components are sealed with a sealing resin or the like.

[0143] Example

[0144] The following examples illustrate this implementation method in detail. However, this implementation method is not limited to the following examples.

[0145] It should be noted that, in each case, the weight-average molecular weight (Mw) was determined by the following method.

[0146] The conversion was performed using gel permeation chromatography (GPC) based on a standard curve using standard polystyrene. The standard curve used standard polystyrene: TSK standard POLYSTYRENE (Type: A-2500, A-5000, F-1, F-2, F-4, F-10, F-20, F-40) [manufactured by Tosoh Corporation], approximated using a cubic formula. The determination conditions for GPC are shown below.

[0147] Device:

[0148] Pump: L-6200 type [Manufactured by Hitachi High-Technologies Co., Ltd.]

[0149] Detector: L-3300 RI [Manufactured by Hitachi High-Technologies Co., Ltd.]

[0150] Column oven: L-655A-52 [manufactured by Hitachi High-Technologies Co., Ltd.]

[0151] Columns: Protective columns: "TSK Guardcolumn HHR-L" + column; "TSKgel G4000HHR" + "TSKgel G2000HHR" (all manufactured by Tosoh Corporation)

[0152] Column dimensions: 6.0×40mm (protective column), 7.8×300mm (column)

[0153] Eluent: Tetrahydrofuran

[0154] Sample concentration: 30 mg / 5 mL

[0155] Injection volume: 20μL

[0156] Flow rate: 1.00 mL / min

[0157] Measurement temperature: 40℃

[0158] [Manufacturing Example 1: Manufacturing of siloxane-modified maleimide compounds]

[0159] 100 g of a diamine-terminated siloxane (Shin-Etsu Chemical Industry Co., Ltd., X-22-161A, amino functional group equivalent: 800 g / mol), 450 g of 2,2-bis[4-(4-maleimide phenoxy)phenyl]propane, and 550 g of propylene glycol monomethyl ether were added to a 2 L reaction vessel equipped with a thermometer, stirrer, moisture meter with reflux condenser, and capable of heating and cooling. The reaction was carried out at 120 °C for 3 hours to produce a liquid containing a siloxane-modified maleimide compound. The weight-average molecular weight (Mw) of the obtained modified maleimide resin was 2,500.

[0160] Example 1, Comparative Examples 1-3

[0161] (Preparation of resin compositions and resin varnishes)

[0162] The components shown in Table 1 were combined in the proportions shown in Table 1 (the proportions in Table 1 are the mass parts of the solid components) and mixed in methyl ethyl ketone to obtain a resin composition (resin varnish) with a non-volatile component (solid component concentration) of 50% by mass.

[0163] (Prepreg preparation)

[0164] The resin varnish prepared in each example was impregnated into glass cloth T2118 (manufactured by Nitto Boki Co., Ltd.), and then dried by heating at 120°C for 5 minutes, thereby obtaining the prepreg.

[0165] (Fabrication of double-sided copper-clad laminate)

[0166] A double-sided copper-clad laminate was fabricated by overlapping 12μm thick electrolytic copper foil "3EC-M3-VLP-12" (manufactured by Mitsui Metals & Mining Co., Ltd.) on both sides of four overlapping prepregs, so that the bonding surface is attached to the prepregs, and then heating and pressing under vacuum pressing conditions of 240°C and 3MPa for 80 minutes.

[0167] The obtained double-sided copper-clad laminate was evaluated according to the following evaluation method. The results are shown in Table 1.

[0168] [Evaluation Method]

[0169] (1) Flame retardancy

[0170] The double-sided copper-clad laminates obtained in each example were immersed in a 10% by mass solution of ammonium persulfate as a copper etching solution to remove the copper foil. Afterward, they were cut to produce five evaluation substrates, each measuring 1.3 cm × 12.5 cm. A vertical burning test (UL94 flammability test) was performed on the five evaluation substrates. The burning time was measured by exposing each substrate to a flame, and the average burning time of the five evaluation substrates was determined as an indicator of flame retardancy. The average burning time is preferably less than 10 seconds.

[0171] (2) Copper foil peel strength

[0172] The copper foil of the double-sided copper-clad laminate obtained in each example was partially etched to form a copper foil line with a width of 3 mm, which was used as a test piece. The load when the copper foil line was peeled off at a speed of 50 mm / min in a direction at 90° relative to the bonding surface was measured, and the obtained value was used as an indicator of the copper foil peel strength. If the peel load is 0.6 kN / m or more, it is judged to be a high copper foil peel strength. In addition, an improvement of 0.1 kN / m is very useful in industry.

[0173] (3) Resistance to glue residue removal

[0174] The double-sided copper-clad laminates obtained in each example were immersed in copper etching solution to prepare 40mm×40mm test pieces with the copper foil removed.

[0175] The test piece was treated at 70°C for 5 minutes using a swelling treatment solution, "Swelling Dip Securiganth P" (manufactured by Atotech Japan Co., Ltd.). Next, after washing with water at room temperature for 2 minutes, it was roughened by treatment at 80°C for 10 minutes using a roughening solution, "ConcentrateCompact CP" (manufactured by Atotech Japan Co., Ltd.). Then, after washing with water at 50°C for 2 minutes, it was neutralized by treatment at 40°C for 5 minutes using a neutralization solution, "Reduction Solution Securiganth P500" (manufactured by Atotech Japan Co., Ltd.), and finally washed with water at room temperature for 5 minutes before drying.

[0176] The amount of weight reduction of the degummed residue is calculated based on the difference between the dry weight before and after the degummed residue treatment (dry weight before degummed residue treatment - dry weight after degummed residue treatment), and the obtained value is used as an indicator of degummed residue resistance.

[0177] The smaller the weight reduction of the adhesive residue, the higher the resistance to adhesive residue removal.

[0178] [Table 1]

[0179]

[0180] It should be noted that the detailed information of the components in Table 1 is as follows.

[0181] [(A) Ingredient]

[0182] • Maleimide compound 1: The siloxane-modified maleimide compound prepared in Example 1

[0183] • Epoxy Resin 1: “EPICLON (registered trademark) NC-3000H”, biphenyl aryl phenolic epoxy resin (manufactured by Nippon Kayaku Co., Ltd.), epoxy equivalent: 280~300g / eq

[0184] [(B) Component]

[0185] • Phosphorus-based flame retardant 1: A phosphorus-based flame retardant with a styrene skeleton having the following structure, manufactured by Fushimi Pharmaceutical Co., Ltd.

[0186] [Chemical Formula 6]

[0187]

[0188] (n) 1 (Integers between 3 and 8.)

[0189] • Phosphorus-based flame retardant 2: "Rabitle FP-110", a phosphorus-based flame retardant with the following structure, manufactured by Fushimi Pharmaceutical Co., Ltd.

[0190] [Chemical Formula 7]

[0191]

[0192] (n) 2 (Integers between 3 and 8.)

[0193] • Phosphorus-based flame retardant 3: "Rabitle FP-400", a phosphorus-based flame retardant with the following structure, manufactured by Fushimi Pharmaceutical Co., Ltd.

[0194] [Chemical Formula 8]

[0195]

[0196] (n) 3 (Integers between 3 and 8.)

[0197] • Phosphorus-based flame retardant 4: Phosphorus-based flame retardant "HCA" with the following structure, manufactured by Sanko Co., Ltd.

[0198] [Chemical Formula 9]

[0199]

[0200] [(C) component]

[0201] • Filler 1: Molten spherical silica treated with silane coupling, with an average particle size of 0.5 μm

[0202] [(D) component]

[0203] • Curing accelerator 1: Isocyanate masked imidazole “G-8009L” (manufactured by Daiichi Kogyo Pharmaceutical Co., Ltd.)

[0204] As shown in Table 1, the copper-clad laminates of the embodiments using the resin composition of this embodiment exhibit excellent flame retardancy, high copper foil peel strength, and high resistance to descaling.

Claims

1. A resin composition comprising (A) a thermosetting resin and (B) a flame retardant, The flame retardant (B) comprises (B1) a phosphorus-based flame retardant having a styrene skeleton.

2. The resin composition according to claim 1, wherein, The (B1) component has two or more styrene skeletons.

3. The resin composition according to claim 1, wherein, The (B1) component has the structural unit shown in the following general formula (B-1), In the formula, R b1 Organic groups that have 1 to 20 carbon atoms.

4. The resin composition according to claim 1, wherein, The content of component (B1) is 1 to 25 parts by mass relative to the total amount of component (A) and component (B) of 100 parts by mass.

5. The resin composition according to claim 1, wherein, The (A) component comprises at least one selected from epoxy resin, polyimide resin, maleimide compound, phenolic resin, polyphenylene ether resin, bismaleimide triazine resin, cyanate ester resin, isocyanate ester resin, benzoxazine resin, oxetane resin, amino resin, unsaturated polyester resin, allyl resin, dicyclopentadiene resin and organosilicon resin.

6. The resin composition according to claim 1, wherein, The (A) component comprises at least one selected from maleimide compounds having one or more N-substituted maleimide groups and their derivatives.

7. The resin composition according to claim 1, wherein, The component (A) contains a siloxane-modified maleimide compound.

8. The resin composition according to claim 1, further comprising (C) filler.

9. A prepreg comprising a substrate and a semi-cured product of the resin composition of claim 1.

10. A laminate comprising the prepreg of claim 9.

11. A metal-clad laminate comprising a metal foil and a cured form of the prepreg of claim 9.

12. A printed circuit board comprising the laminate of claim 10 or the metal-clad laminate of claim 11.

13. A semiconductor package comprising the printed circuit board and semiconductor element as described in claim 12.

Citation Information

Patent Citations

  • Resin composition, and carrier-attached resin film, prepreg, laminate, printed wiring board and semiconductor device including the same

    JP2021138803A