Adhesive compositions and adhesive films comprising the same
By combining acrylate prepolymers and polymers, adjusting the molecular weight and glass transition temperature, and adding crosslinking agents, an adhesive composition is prepared that provides high peel strength and chemical resistance in foldable devices, solves the problems of warping and bubbling, and achieves low-temperature stability and high performance.
Patent Information
- Application Number
- CN202580028282.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-25
- Filing Date
- 2025-04-15
- Publication Date
- 2026-11-17
AI Technical Summary
Existing adhesives cannot effectively suppress warping and bubbling during folding in foldable mechanical devices, and their high elastic modulus at low temperatures cannot meet the requirements for high peel strength and chemical resistance.
An adhesive composition is formed by combining acrylate prepolymers and acrylate polymers, adjusting their weight-average molecular weight and glass transition temperature, and adding multifunctional crosslinking agents, photoinitiators, and coupling agents to prepare adhesive films.
It achieves low elastic modulus at low temperatures while providing high substrate peel strength and chemical resistance, suppressing warping and bubbling, and meeting folding test requirements.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention claims priority to Korean Patent Application No. 10-2024-0055141, filed on April 25, 2024, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to adhesive compositions and adhesive films comprising the thereof, and more particularly, to adhesive compositions and adhesive films comprising an acrylate prepolymer and an acrylate polymer, wherein, relative to 100 parts by weight of the acrylate prepolymer, the acrylate polymer comprises more than 2 parts by weight and less than 15 parts by weight of the acrylate polymer. Background Technology
[0003] Typically, display devices may include polarizing plates, retardation plates, and other functional layers made of plate-like material. These layers are attached to a substrate inside the display element using an adhesive medium and can be manufactured in various shapes, such as bent or folded.
[0004] Recently, display devices, such as mobile display devices, are developing towards various deformable forms such as thinner, lighter, and lower-energy-consumption folding or rolling methods, as information technology deepens, becomes more widespread and popular.
[0005] The optical elements and films used in the device are subject to stress during use due to external folding or bending. Such devices typically cannot use conventional optical elements or films directly and require measures to reduce the stress generated during folding or bending.
[0006] Furthermore, when repeated pressure is applied to the device, the adhesive composition securing the device should adhere well to the device. Poor adhesion will cause bubbles or defects.
[0007] Therefore, it is necessary to develop adhesive compositions that have high peel strength suitable for foldable mechanical devices, low elastic modulus at low temperatures, and do not cause defects such as warping or bubbling during folding tests. Summary of the Invention
[0008] Technical issues
[0009] The problem to be solved by the present invention is to provide an adhesive composition that has high peel force, low elastic modulus at low temperature, and does not cause defects such as warping or bubbling during folding tests, suitable for foldable mechanical devices.
[0010] However, the technical problems to be solved by this application are not limited to those mentioned above. Those skilled in the art to which this invention pertains can clearly understand other technical problems not mentioned through the following description.
[0011] Technical solution
[0012] One embodiment of the present invention provides an adhesive composition comprising an acrylate prepolymer and an acrylate polymer, wherein, relative to 100 parts by weight of the acrylate prepolymer, the composition comprises more than 2 parts by weight and less than 15 parts by weight of the acrylate polymer.
[0013] According to one embodiment of the present invention, the weight-average molecular weight (Mw) of the acrylate prepolymer can be 500,000 or more and 3,000,000 or less.
[0014] According to one embodiment of the present invention, the weight-average molecular weight of the acrylate polymer can be 3000 or more and 10000 or less.
[0015] According to one embodiment of the present invention, the glass transition temperature (Tg) of the acrylate polymer can be above 90°C and below 200°C.
[0016] According to one embodiment of the present invention, the adhesive composition may contain one selected from the group consisting of multifunctional crosslinking agents, photoinitiators, coupling agents, and combinations thereof.
[0017] According to one embodiment of the present invention, the adhesive composition may further include a multifunctional crosslinking agent, a photoinitiator, and a coupling agent.
[0018] One embodiment of the present invention provides an adhesive film comprising: a substrate layer; and an adhesive layer comprising an acrylate prepolymer and an acrylate polymer.
[0019] According to one embodiment of the present invention, relative to 100 parts by weight of the acrylate prepolymer, it may contain more than 2 parts by weight and less than 15 parts by weight of the acrylate polymer.
[0020] According to one embodiment of the present invention, the peel force of the adhesive film to the substrate can be above 800 gf / inch and below 1300 gf / inch.
[0021] According to one embodiment of the present invention, the haze of the adhesive layer can be less than 1.2%.
[0022] According to one embodiment of the present invention, the energy storage modulus of the adhesive layer at a temperature of -20°C can be 10. 5 Below Pa.
[0023] The effects of the invention
[0024] The adhesive composition of one embodiment of the present invention exhibits higher substrate peel strength than before by adjusting the appropriate content of acrylate prepolymer and acrylate polymer, meets folding test and chemical resistance, and can suppress undesirable phenomena such as warping and bubble formation.
[0025] The adhesive film of one embodiment of the present invention has a low elastic modulus at low temperatures and exhibits high substrate peel strength, meets folding test and chemical resistance requirements, and can suppress undesirable phenomena such as warping and bubble formation. Detailed Implementation
[0026] In this specification, when a part is referred to as "containing" a structural element, unless otherwise stated otherwise, it means that other structural elements may also be included, rather than excluding other structural elements.
[0027] In this specification, "A and / or B" means "A and B or A or B".
[0028] In this specification, when it is mentioned that a structural element is set "on", unless otherwise stated otherwise, it means that other structural elements may be set therein, rather than excluding the setting of other structural elements.
[0029] The present invention will now be described in more detail.
[0030] One embodiment of the present invention includes an adhesive composition comprising an acrylate prepolymer and an acrylate polymer, wherein, relative to 100 parts by weight of the acrylate prepolymer, the composition comprises more than 2 parts by weight and less than 15 parts by weight of the acrylate polymer.
[0031] The adhesive composition of one embodiment of the present invention can exhibit higher substrate peel strength than before by adjusting the appropriate content of acrylate prepolymer and acrylate polymer, meet folding test and chemical resistance, and suppress undesirable phenomena such as warping and bubble formation.
[0032] According to one embodiment of the present invention, the adhesive composition comprises an acrylate prepolymer and an acrylate polymer.
[0033] According to one embodiment of the present invention, the acrylate prepolymer may be a partially polymerized form of the acrylate monomer component.
[0034] According to one embodiment of the present invention, the acrylate polymer may be a copolymer of acrylate monomer components. "(meth)acryloyl" refers to acryloyl and / or methacryloyl.
[0035] According to one embodiment of the present invention, the acrylate monomers may include, for example, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, sec-butyl methacrylate, tert-butyl methacrylate, amyl methacrylate, isoamyl methacrylate, neopentyl methacrylate, n-hexyl methacrylate, heptyl methacrylate, ethylhexyl methacrylate, n-octyl methacrylate, isooctyl methacrylate, nonyl methacrylate, etc. Isononyl acrylate, decyl acrylate, isodecyl acrylate, undecyl acrylate, dodecyl acrylate (i.e., lauryl acrylate), isotridecyl acrylate, tetradecyl acrylate, isotetradecyl acrylate, pentadecyl acrylate, cetyl acrylate, heptadecanyl acrylate, octadecyl acrylate, isooctadecyl acrylate, and nonadecanyl acrylate.
[0036] According to one embodiment of the present invention, for example, the acrylate monomer can be a cycloalkyl methacrylate, a methacrylate having a bicyclic aliphatic hydrocarbon ring, or a methacrylate having three or more aliphatic hydrocarbon rings. For example, a cycloalkyl methacrylate can be cyclopentyl methacrylate, cyclohexyl methacrylate, cycloheptyl methacrylate, and cyclooctyl methacrylate. For example, a methacrylate having a bicyclic aliphatic hydrocarbon ring can be isobornyl methacrylate.
[0037] According to one embodiment of the present invention, the acrylate monomer is a monomer containing a hydroxyl group, and examples include 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 2-hydroxybutyl methacrylate, 3-hydroxypropyl methacrylate, 4-hydroxybutyl methacrylate, 6-hydroxyhexyl methacrylate, 8-hydroxyoctyl methacrylate, 10-hydroxydecyl methacrylate, 12-hydroxylaurate methacrylate, and (4-hydroxymethylcyclohexyl)methacrylate.
[0038] According to one embodiment of the present invention, the acrylate prepolymer can be a partial polymerization of the acrylate monomer. Preferably, the acrylate monomer can be one or more selected from the group consisting of 2-ethylhexyl acrylate (2-EHA), 4-hydroxybutyl acrylate (4-HBA), isobornyl acrylate (IBoA), 2-hydroxyethyl acrylate (HEA), butyl acrylate (BA), cyclohexyl acrylate (CHA), and combinations thereof. More preferably, the acrylate monomer can be one or more selected from the group consisting of 2-ethylhexyl acrylate, 4-hydroxybutyl acrylate, and combinations thereof. Partial polymerization of the acrylate monomer selected from the above can be used to prepare adhesive compositions with excellent physical properties.
[0039] According to one embodiment of the present invention, the acrylate polymer can be a copolymer of the acrylate monomers. Preferably, the acrylate monomers can be one or more selected from the group consisting of ethyl acetate (EAc), isobornyl acrylate (IBOA), dicyclopentyl methacrylate (DCPMA), methyl methacrylate (MMA), ethylhexyl acrylate (EHA), isobornyl acrylate (IBoA), 2-hydroxyethyl acrylate (HEA), butyl acrylate (BA), cyclohexyl acrylate (CHA), 4-hydroxybutyl acrylate (HBA), and combinations thereof. More preferably, the acrylate monomers can be one or more selected from the group consisting of ethyl acetate, isobornyl acrylate, dicyclopentyl methacrylate, methyl methacrylate, and combinations thereof. The acrylate monomers selected from the above can be polymerized to prepare adhesive compositions with excellent physical properties.
[0040] According to one embodiment of the present invention, the acrylate prepolymer comprises more than 2 parts by weight and less than 15 parts by weight of the acrylate polymer relative to 100 parts by weight of the acrylate prepolymer. Specifically, the acrylate polymer may be 3 or more parts by weight and less than 14 parts by weight, 5 or more parts by weight and less than 13 parts by weight, 5 or more parts by weight and less than 12 parts by weight, 5 or more parts by weight and less than 11 parts by weight, or 5 or more parts by weight and less than 10 parts by weight relative to 100 parts by weight of the acrylate prepolymer, as described above, to exhibit higher substrate peel strength than before, meet folding tests and chemical resistance, and suppress defects such as warping and bubbling.
[0041] According to one embodiment of the present invention, the weight-average molecular weight of the acrylate prepolymer can be 500,000 or more and 3,000,000 or less. Specifically, the weight-average molecular weight of the acrylate prepolymer can be 600,000 or more and 2,800,000 or less, 700,000 or more and 2,600,000 or less, 800,000 or more and 2,400,000 or less, 900,000 or more and 2,200,000 or less, 1,000,000 or more and 2,000,000 or less, 1,000,000 or more and 1,800,000 or less, 1,000,000 or more and 1,600,000 or less, 1,000,000 or more and 1,400,000 or less, 1,000,000 or more and 1,200,000 or less, or 1,050,000 or more and 1,150,000 or less. Adhesive compositions with excellent physical properties can be prepared by adjusting the weight-average molecular weight of the acrylate prepolymer within the above ranges.
[0042] According to one embodiment of the present invention, the weight-average molecular weight of the acrylate polymer can be 3000 or more and 10000 or less. Specifically, the weight-average molecular weight of the acrylate polymer can be 3100 or more and 9000 or less, 3200 or more and 8000 or less, 3300 or more and 7000 or less, 3400 or more and 6000 or less, 3500 or more and 5500 or less, 3600 or more and 5400 or less, 3700 or more and 5300 or less, 3800 or more and 5200 or less, 3900 or more and 5100 or less, or 4000 or more and 5000 or less. Adhesive compositions with excellent physical properties can be prepared by adjusting the weight-average molecular weight of the acrylate polymer within the above ranges.
[0043] According to one embodiment of the present invention, the glass transition temperature (Tg) of the acrylate polymer can be 90°C or higher and 200°C or lower. Specifically, the glass transition temperature of the acrylate polymer can be 95°C or higher and 195°C or lower, 95°C or higher and 190°C or lower, 95°C or higher and 185°C or lower, 95°C or higher and 180°C or lower, 95°C or higher and 175°C or lower, or 100°C or higher and 175°C or lower. Adhesive compositions with excellent physical properties can be prepared by adjusting the glass transition temperature of the acrylate polymer within the above ranges.
[0044] According to one embodiment of the present invention, the adhesive composition may contain one selected from the group consisting of multifunctional crosslinking agents, photoinitiators, coupling agents, and combinations thereof.
[0045] According to one embodiment of the present invention, the adhesive composition may further comprise a multifunctional crosslinking agent. Adhesive compositions prepared by crosslinking acrylate prepolymers and acrylate polymers with the aforementioned multifunctional crosslinking agent exhibit higher substrate peel strength than before, meet folding tests and chemical resistance, and suppress defects such as warping and bubbling. Examples of the multifunctional crosslinking agent include multifunctional (meth)acrylates. For example, it can be an ester compound of polyols and (meth)acrylic acid, such as polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,2-ethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, etc.; allyl (meth)acrylate, vinyl (meth)acrylate, divinylbenzene, epoxy acrylate, polyester acrylate, polyurethane acrylate, butyl di(meth)acrylate, and hexyl di(meth)acrylate. Preferably, the multifunctional crosslinking agent can be hexanediol diacrylate (HDDA).
[0046] According to one embodiment of the present invention, 100 parts by weight of the acrylate prepolymer may contain 0.05 parts by weight or more and 0.5 parts by weight of the multifunctional crosslinking agent. Specifically, 100 parts by weight of the acrylate prepolymer may contain 0.1 parts by weight or more and 0.45 parts by weight, 0.11 parts by weight or more and 0.4 parts by weight, 0.12 parts by weight or more and 0.35 parts by weight, 0.13 parts by weight or more and 0.3 parts by weight, 0.14 parts by weight or more and 0.25 parts by weight, 0.14 parts by weight or more and 0.2 parts by weight, 0.14 parts by weight or more and 0.18 parts by weight, or 0.14 parts by weight or more and 0.16 parts by weight, preferably 0.15 parts by weight. Adhesive compositions prepared by adjusting the range of the multifunctional crosslinking agent can exhibit higher substrate peel strength than before, meet folding tests and chemical resistance, and suppress undesirable phenomena such as warping and bubble formation.
[0047] According to one embodiment of the present invention, the adhesive composition may further comprise a photoinitiator. The photoinitiator may be any initiator that can initiate the polymerization reaction of the adhesive composition by light irradiation or the like. For example, these could be α-hydroxy ketones (e.g., IRGACURE 184, IRGACURE 500, IRGACURE 2959, DAROCUR 1173; manufactured by Ciba Specialty Chemicals); phenylglyoxylates (e.g., IRGACURE 754, DAROCUR MBF; manufactured by Ciba Specialty Chemicals); benzyl dimethyl ketals (e.g., IRGACURE 651; manufactured by Ciba Specialty Chemicals); α-amino ketones (e.g., IRGACURE 369, IRGACURE 907, IRGACURE 1300; manufactured by Ciba Specialty Chemicals); monoacylphosphine compounds (MAPO) (e.g., DAROCUR TPO, manufactured by Ciba Specialty Chemicals); bisacylphosphine compounds (BAPO) (e.g., IRGACURE 819, IRGACURE 184, IRGACURE 500, IRGACURE 2959, DAROCUR 1173; manufactured by Ciba Specialty Chemicals); monoacylphosphine compounds (MAPO) (e.g., DAROCUR TPO, manufactured by Ciba Specialty Chemicals); diacylphosphine compounds (BAPO) (e.g., IRGACURE 819, IRGACURE 184 ... 819DW; manufactured by Ciba Specialty Chemicals; phosphine oxides (e.g., IRGACURE 2100; manufactured by Ciba Specialty Chemicals); metallocenes (e.g., IRGACURE 784; manufactured by Ciba Specialty Chemicals); iodonium salts (e.g., IRGACURE 250; manufactured by Ciba Specialty Chemicals); and mixtures of one or more of the above compounds (e.g., DAROCUR 4265, IRGACURE 2022, IRGACURE 1300, IRGACURE 2005, IRGACURE 2010, IRGACURE 2020; manufactured by Ciba Specialty Chemicals). One or more of the above compounds may be used, but are not limited thereto.
[0048] According to one embodiment of the present invention, relative to 100 parts by weight of the acrylate prepolymer, the photoinitiator may comprise 0.1 parts by weight and 0.8 parts by weight. Specifically, relative to 100 parts by weight of the acrylate prepolymer, the photoinitiator may be 0.12 parts by weight and 0.7 parts by weight, 0.14 parts by weight and 0.6 parts by weight, 0.16 parts by weight and 0.5 parts by weight, 0.18 parts by weight and 0.4 parts by weight, 0.2 parts by weight and 0.35 parts by weight, 0.22 parts by weight and 0.3 parts by weight, or 0.24 parts by weight and 0.26 parts by weight, preferably 0.25 parts by weight. By adjusting the weight of the photoinitiator within the above range to initiate the polymerization reaction of the adhesive composition, it is possible to achieve higher substrate peel strength than before, meet folding tests and chemical resistance, and suppress undesirable phenomena such as warping and bubble formation.
[0049] According to one embodiment of the present invention, the adhesive composition may further include a coupling agent. The coupling agent can improve heat resistance and moisture resistance by enhancing the adhesion and bonding stability of the adhesive, and can also improve bonding reliability even after long-term placement under harsh conditions. For example, the coupling agent may be γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, γ-glycidoxypropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, γ-methacryloyloxypropyltrimethoxysilane, γ-methacryloyloxypropyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, 3-isocyanopropyltriethoxysilane, γ-acetoacetylpropyltrimethoxysilane, γ-acetoacetylpropyltriethoxysilane, β-cyanoacetyltrimethoxysilane, β-cyanoacetyltriethoxysilane, acetoxyacetyltrimethoxysilane, etc., and one or more of the above compounds may be used. Preferably, a silane coupling agent containing an acetoacetate group or a β-cyanoacetate group is used, but it is not limited thereto.
[0050] According to one embodiment of the present invention, the coupling agent may be 0.05 parts by weight or more and 0.5 parts by weight or less relative to 100 parts by weight of the acrylate prepolymer, preferably 0.1 parts by weight or more and 0.3 parts by weight or less, and more preferably 0.2 parts by weight. Adjusting the weight of the coupling agent within the above range can improve the adhesion and bonding stability of the adhesive, thereby increasing the bonding reliability.
[0051] According to one embodiment of the present invention, the adhesive composition may further comprise a multifunctional crosslinking agent, a photoinitiator, and a coupling agent. As described above, the adhesive composition may exhibit higher substrate peel strength than before by further comprising a multifunctional crosslinking agent, a photoinitiator, and a coupling agent, thereby meeting folding tests and chemical resistance requirements, and suppressing defects such as warping and bubble formation.
[0052] According to one embodiment of the present invention, an adhesive film is included, comprising: a substrate layer; and an adhesive layer comprising an acrylate prepolymer and an acrylate polymer.
[0053] The adhesive film of one embodiment of the present invention has a low elastic modulus at low temperatures and exhibits high substrate peel strength, meets folding test and chemical resistance requirements, and can suppress undesirable phenomena such as warping and bubble formation.
[0054] According to one embodiment of the present invention, the substrate layer may be a resin film. Specifically, it may contain polyesters such as polyethylene terephthalate (PET), polycarbonates, polyolefins, polyimides, and other plastic materials.
[0055] According to one embodiment of the present invention, relative to 100 parts by weight of the acrylate prepolymer, it may contain more than 2 parts by weight and less than 15 parts by weight of the acrylate polymer.
[0056] According to one embodiment of the present invention, the contents concerning the acrylate prepolymer and the acrylate polymer are the same as those described above.
[0057] According to one embodiment of the present invention, the peel force of the adhesive film to the substrate can be 800 gf / inch or more and 1300 gf / inch or less. Specifically, the peel force of the adhesive film to the substrate can be 810 gf / inch or more and 1271 gf / inch or less, 820 gf / inch or more and 1270 gf / inch or less, 830 gf / inch or more and 1269 gf / inch or less, 840 gf / inch or more and 1268 gf / inch or less, 850 gf / inch or more and 1267 gf / inch or less, 860 gf / inch or more and 1266 gf / inch or less, or 868 gf / inch or more and 1266 gf / inch or less. Durability can be improved by adjusting the peel force of the adhesive film to the substrate within the above range.
[0058] According to one embodiment of the present invention, the haze of the adhesive layer can be less than 1.2%. Specifically, the haze of the adhesive layer can be 0.48% or more and 1.1% or less, 0.49% or more and 1.0% or less, 0.49% or more and 0.9% or less, or 0.49% or more and 0.81% or less. Optical properties can be improved by adjusting the haze of the adhesive layer within the above range.
[0059] According to one embodiment of the present invention, the energy storage modulus of the adhesive layer at a temperature of -20°C can be 10. 5 Below Pa. Specifically, the storage modulus of the adhesive layer at a temperature of -20°C can be 9 × 10⁻⁶. 4 Pa or higher and 10 5 Below 90500Pa, above 90500Pa and below 99000Pa, above 90600Pa and below 98000Pa, above 90700Pa and below 97000Pa, above 90800Pa and below 96000Pa, above 90842Pa and below 95454Pa. Detailed Implementation
[0060] Hereinafter, embodiments will be described in detail to specifically illustrate the present invention. However, the embodiments of the present invention can be modified into many other forms, and the scope of the present invention should not be construed as limited to the embodiments described below. The embodiments in this specification are provided to more fully illustrate the present invention to those skilled in the art.
[0061] Preparation Example
[0062] Synthesis Example 1: Acrylate Prepolymer (A)
[0063] 80 parts by weight of 2-ethylhexyl acrylate, 20 parts by weight of 4-hydroxybutyl acrylate, and 0.05 parts by weight of photopolymerization initiator (trade name: Irgacure) were added to the polymerization reactor. ® 184), 0.015 parts by weight of the molecular weight regulator dodecyl mercaptan. Then, nitrogen gas was introduced and the mixture was stirred for 20 minutes. After 20 minutes, it was directly exposed to ultraviolet light for partial polymerization to obtain an acrylate prepolymer (A, 100 parts by weight) with a molecular weight (Mw) of 1.1 million.
[0064] Synthesis Example 2: Acrylate Polymers (B)
[0065] In a polymerization reactor, 100 parts by weight of isobornyl acrylate and 7 parts by weight of dodecanethiol (a molecular weight regulator) were added to 100 parts by weight of ethyl acetate. Nitrogen gas was then introduced and the mixture was stirred at 70°C for 40 minutes. After 40 minutes, the internal temperature of the polymerizer was maintained at 70°C, and 0.2 parts by weight of V-65 (2,2'-azobis(2,4-dimethylvaleronitrile)) was added as a thermal polymerization initiator. Two hours after the first initiator addition, another 0.2 parts by weight of the thermal polymerization initiator was added. Five hours after the second initiator addition, the reaction was terminated. The polymerized resin was then placed in an oven at 120°C to evaporate the remaining monomers and additives to obtain a solid acrylate polymer (B) with a molecular weight (Mw) of 5000. Under these conditions, the glass transition temperature was 100°C.
[0066] Synthesis Example 3: Acrylate Polymers (C)
[0067] In a polymerization reactor, 100 parts by weight of dicyclopentyl methacrylate and 7 parts by weight of dodecanethiol (a molecular weight regulator) were added to 100 parts by weight of ethyl acetate. Nitrogen gas was then introduced and the mixture was stirred at 70°C for 40 minutes. After 40 minutes, the internal temperature of the polymerizer was maintained at 70°C, and 0.2 parts by weight of V-65 (2,2'-azobis(2,4-dimethylvaleronitrile)) was added as a thermal polymerization initiator. Two hours after the first initiator addition, another 0.2 parts by weight of the thermal polymerization initiator was added. Five hours after the second initiator addition, the reaction was terminated. The polymerized resin was then placed in an oven at 120°C to volatilize the remaining monomers and additives to obtain a solid acrylate polymer (C) with a molecular weight (Mw) of 4500. Under these conditions, the glass transition temperature was 175°C.
[0068] Synthesis Example 4: Acrylate Polymers (D)
[0069] In a polymerization reactor, 60 parts by weight of dicyclopentyl methacrylate, 40 parts by weight of methyl methacrylate, and 7 parts by weight of dodecanethiol (a molecular weight regulator) were added to 100 parts by weight of ethyl acetate. Nitrogen gas was then introduced and the mixture was stirred at 70°C for 40 minutes. After 40 minutes, the internal temperature of the polymerizer was maintained at 70°C, and 0.2 parts by weight of V-65 (2,2'-azobis(2,4-dimethylvaleronitrile)) was added as a thermal polymerization initiator. Two hours after the first initiator addition, another 0.2 parts by weight of the thermal polymerization initiator was added. Five hours after the second initiator addition, the reaction was terminated. The polymerized resin was then placed in an oven at 120°C to volatilize the remaining monomers and additives to obtain a solid acrylate polymer (D) with a molecular weight (Mw) of 4000. Under these conditions, the glass transition temperature was 140°C.
[0070] Examples and Comparative Examples
[0071] Example 1
[0072] An adhesive composition was prepared by combining 0.15 parts by weight of hexanediol diacrylate as a multifunctional crosslinking agent, 0.2 parts by weight of coupling agent (KBM 403, manufactured by Shin-Etsu), 0.25 parts by weight of photoinitiator (Irgacure 651, manufactured by Ciba Specialty Chemicals), and 5 parts by weight of acrylate polymer (B) with 100 parts by weight of the partially polymerized acrylate prepolymer (A) prepared in Example 1.
[0073] Next, the prepared coating liquid was applied to the release-treated polyethylene terephthalate film (XD500P, Toray Advanced Materials, thickness: 75 μm) using a rod coater, and the thickness after ultraviolet (UV) curing was 125 μm. Then, the film was cured by irradiating it with a UV lamp for 5 minutes to prepare the adhesive film.
[0074] Examples 2 to 4 and Comparative Examples 1 to 3
[0075] Except for changing the composition of the adhesive composition as shown in Table 1 below, the adhesive film was prepared in the same manner as in Example 1.
[0076] [Table 1]
[0077]
[0078] Content range: parts by weight
[0079] Multifunctional crosslinking agent: Hexanediol diacrylate
[0080] Coupling agent: KBM 403, manufactured by Shin-Etsu Chemical Co., Ltd.
[0081] Photoinitiator: Irgacure 651, manufactured by Ciba Specialty Chemicals.
[0082] Experimental Example
[0083] The physical properties of the adhesive films prepared in the embodiments and comparative examples were measured according to the methods described below.
[0084] 1. Measure the peel force of the substrate.
[0085] The adhesive film prepared in the above embodiments and comparative examples was cut into 25mm×20cm (horizontal×vertical) sizes. After peeling off the release film, it was applied to stainless steel (SUS 304) by using a 2kg pressure roller to reciprocate 5 times. After 20 minutes, the peel force was measured using a tensile testing machine at a peel speed of 300mm / min and a peel angle of 180°.
[0086] 2. Methods for measuring elastic modulus
[0087] The adhesive compositions prepared in the examples and comparative examples were prepared into adhesive layers with a thickness of approximately 1 mm. Next, the adhesive between the release films was cut into cylindrical specimens of 8 mm × 1 mm (= diameter × thickness), and the storage modulus at -20°C was measured using a dynamic rheological property measuring instrument (ARES, RDA, TA Instruments Inc.) while applying shear stress between parallel plates at a frequency of 1 Hz.
[0088] 3. Measuring optical properties
[0089] Transmittance / Haze: After the prepared adhesive layer was attached to a 1.1 T glass surface in the form of glass / adhesive layer / glass, the haze was measured using an NDH 5000 (Nippon Denshoku).
[0090] 4. Penetration distance of artificial sebum (chemical resistance)
[0091] After the adhesive compositions prepared in the examples and comparative examples were attached to glass, they were cut into 25mm × 25mm pieces to prepare test pieces. Then, the test pieces were immersed in artificial sebum (ESTASAN 3580, Kosher Corporation) for 10 minutes, and the penetration distance of the artificial sebum through the side of the test piece (i.e., the adhesive interface between the adhesive layer and the glass) was measured using vernier calipers.
[0092] O: The penetration distance of artificial sebum is ≤0.3mm.
[0093] △: 0.3mm < penetration distance of artificial sebum ≤ 0.7mm,
[0094] X: 0.7mm < penetration distance of artificial sebum.
[0095] 5. Folding Test
[0096] The folding test was conducted as follows: a laminate made by bonding an adhesive between two polyimide films of about 100 μm was cut into a rectangular shape with a horizontal side length of about 8 cm and a vertical side length of about 18 cm to prepare a test piece.
[0097] The test was performed using a folding test device (Flexigo, model name: Foldy-100-1C).
[0098] The previously cut test piece is attached to a unit in the testing machine that can be folded with a radius of curvature of 1R. The test is repeated 200,000 times in a chamber ranging from 25°C to 85°C. After the sample is recovered, defects such as bubble formation, peeling / delamination, and coating cracking are observed visually. The occurrence of any one of these defects is rated as X; if none of the defects occur, the rating is O.
[0099] [Table 2]
[0100]
[0101] As shown in Table 2, it can be confirmed that the adhesive films prepared in Examples 1 to 4 of the present invention contain more than 2 parts by weight and less than 15 parts by weight of acrylate polymer relative to 100 parts by weight of acrylate prepolymer. The peel strength of the adhesive film to the substrate is greater than 800 gf / inch and less than 1300 gf / inch. The haze of the adhesive layer is less than 1.2%. The storage modulus value of the adhesive layer at a temperature of -20°C is greater than 10. 5 Below Pa, it shows higher substrate peel strength than before, meets folding test and chemical resistance, and no defects such as warping and bubbling occurred.
[0102] Conversely, it can be confirmed that if acrylate polymers are not included, as in Comparative Example 1, the folding test and chemical resistance are not met, and defects such as warping and bubbling occur.
[0103] Furthermore, it can be confirmed that if the weight percentage of the acrylate polymer deviates from the appropriate range, as in Comparative Examples 2 and 3, defects such as warping and bubbles will occur due to failure to meet the folding test requirements.
[0104] Therefore, the adhesive composition and adhesive film comprising the present invention specifically comprise an acrylate prepolymer and an acrylate polymer, comprising more than 2 parts by weight and less than 15 parts by weight of the acrylate polymer relative to 100 parts by weight of the acrylate prepolymer, exhibiting high substrate peel strength, meeting folding test and chemical resistance requirements, and suppressing adverse phenomena such as warping and bubble formation.
Claims
1. An adhesive composition, characterized in that, Includes acrylate prepolymers and acrylate polymers. The acrylate prepolymer comprises more than 2 parts by weight and less than 15 parts by weight of the acrylate polymer relative to 100 parts by weight of the acrylate prepolymer.
2. The adhesive composition according to claim 1, characterized in that, The weight-average molecular weight of the acrylate prepolymer is above 500,000 and below 3 million.
3. The adhesive composition according to claim 1, characterized in that, The weight-average molecular weight of the acrylate polymer is above 3000 and below 10000.
4. The adhesive composition according to claim 1, characterized in that, The glass transition temperature of the acrylate polymer is above 90°C and below 200°C.
5. The adhesive composition according to claim 1, characterized in that, The adhesive composition comprises one selected from the group consisting of multifunctional crosslinking agents, photoinitiators, coupling agents, and combinations thereof.
6. The adhesive composition according to claim 1, characterized in that, The adhesive composition further comprises a multifunctional crosslinking agent, a photoinitiator, and a coupling agent.
7. An adhesive film, characterized in that, include: Substrate layer; as well as Adhesive layer, The adhesive layer comprises an acrylate prepolymer and an acrylate polymer.
8. The adhesive film according to claim 7, characterized in that, The acrylate prepolymer comprises more than 2 parts by weight and less than 15 parts by weight of the acrylate polymer relative to 100 parts by weight of the acrylate prepolymer.
9. The adhesive film according to claim 7, characterized in that, The adhesive film has a peel force to the substrate of 800 gf / inch or more and 1300 gf / inch or less.
10. The adhesive film according to claim 7, characterized in that, The haze of the adhesive layer is less than 1.2%.
11. The adhesive film according to claim 7, characterized in that, The energy storage modulus of the adhesive layer at a temperature of -20°C is 10. 5 Below Pa.
Citation Information
Patent Citations
Scalable system on a chip
KR1020240055141A