Adhesive tape
By adjusting the shear storage modulus, loss tangent peak temperature, and gel fraction of the adhesive layer, the problems of insufficient high-temperature retention and surface following of the adhesive tape in curved displays were solved, achieving stability and deformation adaptability at high temperatures.
Patent Information
- Application Number
- CN202580027557.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-05-31
- Filing Date
- 2025-05-23
- Publication Date
- 2026-11-17
AI Technical Summary
Existing adhesive tapes have problems with insufficient high-temperature retention and surface following in curved displays, especially the reduction in body strength caused by increased flexibility.
By using an adhesive composition containing a specific (meth)acrylic copolymer, and by adjusting the shear storage modulus, loss tangent peak temperature, and gel fraction of the adhesive layer at 80°C, the gel fraction is ensured to be above 10% and below 45% within the loss tangent peak temperature range of above -20°C and below 0°C.
It achieves an excellent combination of high-temperature retention and surface conformability, ensuring that the adhesive tape maintains its performance at high temperatures and can adapt to surface deformation.
Smart Images

Figure FT_1 
Figure FT_2 
Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to adhesive tape. Background Technology
[0002] Adhesive tapes having an adhesive layer formed using an adhesive composition have been widely used for fixing components in electronic devices, vehicles, homes, and building materials (e.g., Patent Documents 1-3). Specifically, adhesive tapes are used, for example, to bond a cover plate for protecting the surface of a portable electronic device to a touch panel module or a display panel module, or to bond a touch panel module to a display panel module.
[0003] Existing technical documents
[0004] Patent documents
[0005] Patent Document 1: Japanese Patent Application Publication No. 2015-052050
[0006] Patent Document 2: Japanese Patent Application Publication No. 2015-021067
[0007] Patent Document 3: Japanese Patent Application Publication No. 2015-120876 Summary of the Invention
[0008] The problem that the invention aims to solve
[0009] In recent years, flexible and curved displays have received considerable attention due to the need to improve device design. In curved displays, the adhesive tapes used to fix components require high surface conformability (resilience) because a springy force is applied to restore the tape to a flat state. One method to improve the surface conformability of adhesive tapes is to lower the glass transition temperature of the adhesive layer to increase flexibility. However, increasing the flexibility of the adhesive layer sometimes leads to a decrease in the overall strength and a decline in the high-temperature retention of the adhesive tape.
[0010] The purpose of this invention is to provide an adhesive tape with excellent high-temperature retention and surface conformability.
[0011] Methods for solving problems
[0012] This disclosure 1 relates to an adhesive tape having an adhesive layer formed using an adhesive composition containing a (meth)acrylic acid copolymer having structural units derived from alkyl (meth)acrylic acid esters, wherein the adhesive layer has a shear storage modulus of 15000 Pa or more at 80°C as measured by dynamic viscoelasticity determination at a frequency of 1 Hz and a temperature range of -40°C to 200°C, and the peak temperature of the loss tangent of the adhesive layer as measured by dynamic viscoelasticity determination at a frequency of 1 Hz and a temperature range of -40°C to 200°C is in the range of -20°C to 0°C, and the gel fraction of the adhesive layer is 10% by mass or more and 45% by mass or less.
[0013] This disclosure 2 relates to the adhesive tape of this disclosure 1, wherein the alkyl methacrylate comprises an alkyl methacrylate having a glass transition temperature of -60°C or less when the homopolymer is formed, and the structural units derived from the alkyl methacrylate having a glass transition temperature of -60°C or less when the homopolymer is formed are present in the (meth)acrylate copolymer at a content of 50% by mass or more.
[0014] This disclosure 3 relates to the adhesive tape of this disclosure 2, wherein the alkyl (meth)acrylate having a glass transition temperature of -60°C or less when formed into a homopolymer comprises n-hexyl acrylate.
[0015] This disclosure 4 relates to adhesive tapes of disclosures 1, 2 or 3, wherein the aforementioned (meth)acrylic acid copolymers have structural units derived from monomers that do not have crosslinking functional groups and have a glass transition temperature of 0°C or higher when formed into homopolymers.
[0016] This disclosure 5 relates to the adhesive tape of this disclosure 4, wherein the content of the structural units derived from the monomers of the (meth)acrylic acid copolymers, which do not have crosslinking functional groups and have a glass transition temperature of 0°C or higher when made into homopolymers, is 0.1% by mass or more and 70% by mass or less.
[0017] This disclosure 6 relates to adhesive tapes of disclosures 1, 2, 3, 4 or 5, wherein the aforementioned (meth)acrylic acid copolymers have structural units derived from n-heptyl (meth)acrylic acid.
[0018] This disclosure 7 relates to adhesive tapes of disclosures 1, 2, 3, 4 or 5, wherein the aforementioned (meth)acrylic copolymers do not have structural units derived from (meth)acrylic acid n-heptyl acrylate, or the content of the aforementioned structural units derived from (meth)acrylic acid n-heptyl acrylate is less than 90% by mass.
[0019] This disclosure 8 relates to adhesive tapes of disclosures 1, 2, 3, 4, 5, 6 or 7, wherein the aforementioned (meth)acrylic acid copolymers further have structural units derived from monomers having non-crosslinked ether structures, wherein the monomers having non-crosslinked ether structures are selected from at least one of monomers having cyclic ether structures other than epoxy groups and oxobutyl groups, and monomers having non-cyclic ether structures.
[0020] This disclosure 9 relates to the adhesive tape of this disclosure 8, wherein the structural unit derived from the monomer having a non-crosslinked ether structure in the above-mentioned (meth)acrylic copolymer is present in an amount of 0.01% by mass or more and 50% by mass or less.
[0021] This disclosure 10 relates to adhesive tapes of disclosures 1, 2, 3, 4, 5, 6, 7, 8 or 9, wherein the aforementioned (meth)acrylic acid copolymers further have structural units derived from monomers having crosslinking functional groups.
[0022] This disclosure 11 relates to the adhesive tape of this disclosure 10, wherein the monomer having crosslinking functional groups comprises at least one selected from carboxyl-containing monomers and hydroxyl-containing monomers.
[0023] This disclosure 12 relates to the adhesive tape of this disclosure 11, wherein the monomer having crosslinking functional groups comprises the hydroxyl-containing monomer.
[0024] This disclosure 13 relates to adhesive tapes of disclosure 11 or 12, wherein the monomer having crosslinking functional groups comprises the aforementioned carboxyl-containing monomer, and the structural units derived from the aforementioned carboxyl-containing monomers in the (meth)acrylic acid copolymer account for 5% by mass or more.
[0025] This disclosure 14 relates to adhesive tapes of disclosures 10, 11, 12 or 13, wherein the structural units derived from monomers having crosslinking functional groups in the aforementioned (meth)acrylic copolymers are present in an amount of 0.01% by mass or more and less than 20% by mass.
[0026] This disclosure 15 relates to adhesive tapes of disclosures 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13 or 14, wherein the weight average molecular weight of the aforementioned (meth)acrylic acid copolymers is 800,000 or more.
[0027] This disclosure 16 relates to adhesive tapes of disclosures 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14 or 15, wherein the adhesive composition further contains a tackifier.
[0028] This disclosure 17 relates to the adhesive tape of this disclosure 16, wherein the tackifier comprises at least one selected from (meth)acrylic tackifiers, rosin ester tackifiers and terpene tackifiers.
[0029] This disclosure 18 relates to the adhesive tape of this disclosure 17, wherein the tackifier comprises the rosin ester tackifier and the terpene tackifier.
[0030] This disclosure 19 relates to adhesive tapes of disclosures 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17 or 18, wherein the adhesive composition further comprises a crosslinking agent.
[0031] This disclosure 20 relates to the adhesive tape of this disclosure 19, wherein the crosslinking agent comprises at least one selected from isocyanate-based crosslinking agents and epoxy-based crosslinking agents.
[0032] This disclosure 21 relates to the adhesive tape of this disclosure 20, wherein the crosslinking agent comprises the isocyanate-based crosslinking agent and the epoxy-based crosslinking agent.
[0033] This disclosure 22 relates to adhesive tapes of disclosures 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20 or 21, wherein the half-width of the peak of the loss tangent of the adhesive layer, as measured by dynamic viscoelasticity determination at a frequency of 1 Hz and a temperature range of -40°C to 200°C, is 44°C or less.
[0034] This disclosure 23 relates to an adhesive tape of disclosures 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21 or 22, having a substrate layer and having the adhesive layer on at least one side of the substrate layer.
[0035] This disclosure 24 relates to adhesive tapes of disclosures 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22 or 23, used for securing electronic device components or vehicle-mounted components.
[0036] The present invention will now be described in detail.
[0037] Hereinafter, one or more embodiments of the present invention will be referred to as "this embodiment".
[0038] The inventors investigated how, for the adhesive layer in an adhesive tape, based on an adhesive layer made using an adhesive composition containing a specific (meth)acrylic acid copolymer, the temperature of the peak of the shear storage modulus at 80°C and the loss tangent, as measured by dynamic viscoelasticity determination, were adjusted to ensure the gel fraction was within a specific range. The results showed that an adhesive tape with excellent high-temperature retention and surface conformability could be obtained, thus completing the present invention.
[0039] The adhesive tape of this embodiment has an adhesive layer formed using an adhesive composition.
[0040] As a method for forming the adhesive layer using the above-described adhesive composition, examples include: applying the adhesive composition to a release film or the like and then heating and drying the adhesive composition. The adhesive layer may contain uncrosslinked portions of the adhesive composition or crosslinked products of the adhesive composition.
[0041] The lower limit of the shear storage modulus at 80°C (hereinafter also referred to as "the shear storage modulus of the adhesive layer at 80°C") of the adhesive layer, measured by dynamic viscoelasticity measurement at a frequency of 1 Hz and a temperature range of -40°C to 200°C, is 15000 Pa. By making the shear storage modulus of the adhesive layer at 80°C 15000 Pa or higher, the high-temperature retention of the adhesive tape of this embodiment becomes excellent. The preferred lower limit of the shear storage modulus of the adhesive layer at 80°C is 18000 Pa, and the more preferred lower limit is 20000 Pa.
[0042] Furthermore, the preferred upper limit for the shear storage modulus of the adhesive layer at 80°C is not particularly limited, but is 35,000 Pa. By setting the shear storage modulus of the adhesive layer at 80°C to 35,000 Pa or less, the surface following properties of the resulting adhesive tape become more excellent. A more preferred upper limit for the shear storage modulus of the adhesive layer at 80°C is 30,000 Pa.
[0043] The shear storage modulus of the above-mentioned adhesive layer at 80°C can be 15000~35000Pa, 15000~30000Pa, 18000~35000Pa, 18000~30000Pa, 20000~35000Pa, or 20000~30000Pa.
[0044] The shear storage modulus of the adhesive layer at 80°C, as well as the peak temperature and half-peak width of the loss tangent of the adhesive layer described later, can be obtained by the following dynamic viscoelasticity determination.
[0045] First, the adhesive layers are overlapped to create a laminate approximately 1 mm thick, which is then cut into test pieces 6 mm wide and 10 mm long. Next, the test pieces are subjected to dynamic viscoelasticity testing using a dynamic viscoelasticity measuring device in shear mode under a nitrogen atmosphere, at a temperature range of -40°C to 200°C, a heating rate of 5°C / min, a frequency of 1 Hz, and a strain of 0.08%. Examples of such dynamic viscoelasticity measuring devices include the DVA-200 (manufactured by IT Measurement & Control Co., Ltd.).
[0046] The peak temperature of the loss tangent (hereinafter also referred to as "the loss tangent of the adhesive layer") of the adhesive layer, measured by dynamic viscoelasticity measurement at a frequency of 1 Hz and a temperature range of -40°C to 200°C, is in the range of -20°C to 0°C. By ensuring that the peak temperature of the loss tangent of the adhesive layer is within this range, the surface following performance of the adhesive tape of this embodiment becomes excellent.
[0047] It should be noted that when there are multiple peaks of the loss tangent of the adhesive layer, it is acceptable as long as the peak temperature of at least one of the peaks is in the range of -20°C to 0°C. The preferred lower limit of the peak temperature of the loss tangent of the adhesive layer is -17°C, the preferred upper limit is -3°C, the more preferred lower limit is -15°C, and the more preferred upper limit is -5°C.
[0048] The peak temperature of the loss tangent of the aforementioned adhesive layer can be in the range of -20°C to -3°C, or in the range of -20°C to -5°C, or in the range of -17°C to 0°C, or in the range of -17°C to -3°C, or in the range of -17°C to -5°C, or in the range of -15°C to 0°C, or in the range of -15°C to -3°C, or in the range of -15°C to -5°C.
[0049] Regarding the aforementioned adhesive layer, the preferred upper limit of the half-width at half-maximum (WHM) of the loss tangent peak of the adhesive layer is 44°C. By setting the WHM of the loss tangent peak of the adhesive layer to 44°C or less, the loss tangent near room temperature of the adhesive layer becomes smaller, thus reducing stress dispersion. Consequently, the resulting adhesive tape exhibits excellent high-speed peelability. A more preferred upper limit of the WHM of the loss tangent peak of the adhesive layer is 42°C, a further preferred upper limit is 40°C, and an even more preferred upper limit is 38°C.
[0050] Furthermore, the preferred lower limit of the half-peak width of the loss tangent of the adhesive layer is 20°C. By making the half-peak width of the loss tangent of the adhesive layer 20°C or higher, the resulting adhesive tape exhibits superior resistance to drop impact. A more preferred lower limit of the half-peak width of the loss tangent of the adhesive layer is 23°C, a further preferred lower limit is 25°C, and an even more preferred lower limit is 26°C.
[0051] The half-peak width of the loss tangent peak of the aforementioned adhesive layer can be 20℃~44℃, 23℃~44℃, 25℃~44℃, 26℃~44℃, 20℃~42℃, 23℃~42℃, 25℃~42℃, 26℃~42℃, 20℃~40℃, 23℃~40℃, 25℃~40℃, 26℃~40℃, 20℃~38℃, 23℃~38℃, 25℃~38℃, or 26℃~38℃.
[0052] It should be noted that when there are multiple peaks of the loss tangent of the adhesive layer, the "half-peak width of the adhesive layer peak" refers to the half-peak width of the peak at the lowest temperature among the peaks of the loss tangent of the adhesive layer within a temperature range of -25°C to 50°C. Furthermore, in this specification, the "half-peak width" refers to the full half-peak width.
[0053] The lower limit of the gel fraction of the adhesive layer is 10% by mass, and the upper limit is 45% by mass. By making the gel fraction of the adhesive layer within this range, the surface following performance of the adhesive tape in this embodiment becomes excellent. A more preferred lower limit of the gel fraction of the adhesive layer is 15% by mass, a more preferred upper limit is 35% by mass, and a further preferred lower limit is 20% by mass.
[0054] The gel fraction of the above adhesive layer can be 10-35% by mass, 15-45% by mass, 15-35% by mass, 20-45% by mass, or 20-35% by mass.
[0055] It should be noted that the gel fraction of the above adhesive layer was determined by the following method.
[0056] Specifically, firstly, a test piece is prepared by cutting the adhesive tape with the aforementioned adhesive layer into a flat rectangular shape with a width of 20 mm and a length of 40 mm. The test piece is then immersed in ethyl acetate at 23°C for 24 hours, removed from the ethyl acetate, and dried at 110°C for 1 hour. The mass of the dried test piece is measured, and the gel fraction is calculated using the following formula (I). It should be noted that no release film for protecting the aforementioned adhesive layer is laminated on the test piece. Furthermore, if the adhesive tape is an unsupported tape without a substrate, the measurement is performed using a test piece obtained by applying the aforementioned adhesive layer to a substrate and then cutting it; alternatively, the substrate is not used, and W0 in the following formula (I) is set to 0 for calculation.
[0057] Gel fraction (mass%) = 100 × (W2 - W0) / (W1 - W0) (I)
[0058] (W0: quality of the substrate, W1: quality of the test piece before impregnation, W2: quality of the test piece after impregnation and drying)
[0059] The shear storage modulus of the adhesive layer at 80°C, the peak temperature of the loss tangent of the adhesive layer, and the gel fraction of the adhesive layer can be adjusted to the values described above by adjusting the types and contents of the components constituting the adhesive composition.
[0060] The above adhesive composition contains (meth)acrylic copolymers.
[0061] The above-mentioned (meth)acrylic acid copolymers have structural units derived from alkyl (meth)acrylic acid esters.
[0062] It should be noted that in this specification, "(meth)acrylic acid" refers to acrylic acid or methacrylic acid, and "(meth)acrylate" refers to acrylate or methacrylate.
[0063] The aforementioned alkyl methacrylate preferably comprises an alkyl methacrylate having a glass transition temperature of -60°C or lower when forming a homopolymer. That is, the aforementioned methacrylic copolymer preferably has structural units derived from the aforementioned alkyl methacrylate having a glass transition temperature of -60°C or lower when forming a homopolymer. By having the aforementioned methacrylic copolymer have structural units derived from the aforementioned alkyl methacrylate having a glass transition temperature of -60°C or lower when forming a homopolymer, it is easier to adjust the peak temperature of the loss tangent of the aforementioned adhesive layer to the aforementioned range. The preferred upper limit for the glass transition temperature of the aforementioned alkyl methacrylate having a glass transition temperature of -60°C or lower when forming a homopolymer is -62°C, and more preferably -65°C.
[0064] Furthermore, the preferred lower limit of the glass transition temperature of the alkyl methacrylate (meth)acrylate, which has a glass transition temperature of -60°C or less when forming a homopolymer, is not particularly limited, but the practical lower limit is -70°C.
[0065] The glass transition temperature of the alkyl methacrylate (meth)acrylate, which is below -60°C when it is made into a homopolymer, can be -70°C to -60°C, -70°C to -62°C, or -70°C to -65°C.
[0066] It should be noted that the "glass transition temperature when preparing homopolymers" in this specification refers to the glass transition temperature measured by differential scanning calorimetry (DSC) when preparing homopolymers with a weight-average molecular weight of 100,000 or more and 2,000,000 or less. The glass transition temperature when preparing homopolymers can be measured, for example, under a nitrogen atmosphere (nitrogen flow rate 50 mL / min) using a differential scanning calorimeter, according to the method of JIS K 6240:2011, at a measurement temperature of -100°C to 200°C and a heating rate of 10°C / min. For example, a 220C (manufactured by Seiko Instruments) can be used as the differential scanning calorimeter.
[0067] Examples of alkyl (meth)acrylates having a glass transition temperature of -60°C or lower when forming homopolymers include: n-hexyl acrylate (glass transition temperature of -65°C when forming homopolymers), 2-ethylhexyl acrylate (glass transition temperature of -70°C when forming homopolymers), and n-heptyl acrylate (glass transition temperature of -68°C when forming homopolymers). Preferably, the alkyl (meth)acrylate having a glass transition temperature of -60°C or lower when forming homopolymers includes n-hexyl acrylate.
[0068] The preferred lower limit for the content of structural units derived from alkyl methacrylates with a glass transition temperature of -60°C or lower during the preparation of the homopolymer in the above-mentioned (meth)acrylate copolymer is 50% by mass. By ensuring that the content of structural units derived from alkyl methacrylates with a glass transition temperature of -60°C or lower during the preparation of the homopolymer is 50% by mass or more, it is easier to adjust the peak temperature of the loss tangent of the above-mentioned adhesive layer to the above-mentioned range. The more preferred lower limit for the content of structural units derived from alkyl methacrylates with a glass transition temperature of -60°C or lower during the preparation of the homopolymer is 75% by mass.
[0069] Furthermore, the preferred upper limit for the content of structural units derived from alkyl (meth)acrylates with a glass transition temperature of -60°C or below when the homopolymer is formed is 99.99% by mass, and from the viewpoint of the cohesive strength of the adhesive layer body, an even more preferred upper limit is 99% by mass.
[0070] The content of structural units derived from alkyl (meth)acrylates with a glass transition temperature below -60°C during the preparation of the homopolymer can be 50–99.99% by mass, 50–99% by mass, 75–99.99% by mass, or 75–99% by mass.
[0071] The above-mentioned (meth)acrylic copolymers may, without hindering the purpose of the present invention, have structural units derived from other (meth)acrylic alkyl esters, other than those derived from (meth)acrylic alkyl esters with a glass transition temperature of -60°C or below when the homopolymer is made, as the above-mentioned structural units derived from (meth)acrylic alkyl esters.
[0072] Other examples of the aforementioned alkyl methacrylates include: n-butyl acrylate (with a glass transition temperature of -55°C when forming a homopolymer), 1-methylheptyl acrylate (with a glass transition temperature of -45°C when forming a homopolymer), n-hexyl methacrylate (with a glass transition temperature of 0°C when forming a homopolymer), tert-butyl acrylate (with a glass transition temperature of 14°C when forming a homopolymer), and tert-butyl methacrylate (with a glass transition temperature of 107°C when forming a homopolymer).
[0073] Furthermore, the aforementioned (meth)acrylic acid copolymers preferably have structural units derived from monomers that do not have crosslinking functional groups and have a glass transition temperature of 0°C or higher when made into homopolymers. By having structural units derived from monomers that do not have crosslinking functional groups and have a glass transition temperature of 0°C or higher when made into homopolymers, the resulting adhesive tape exhibits superior high-temperature retention.
[0074] It should be noted that the monomers that do not have crosslinking functional groups and have a glass transition temperature of 0°C or higher when forming homopolymers can be monomers contained in the other alkyl methacrylates mentioned above, or monomers other than the alkyl methacrylates mentioned above. Furthermore, the monomers that do not have crosslinking functional groups and have a glass transition temperature of 0°C or higher when forming homopolymers can also be included in the monomers with non-crosslinking ether structures described later.
[0075] Examples of cross-linking functional groups include carboxyl, hydroxyl, glycidyl, amide, and nitrile groups.
[0076] Examples of monomers that do not possess crosslinking functional groups and have a glass transition temperature of 0°C or higher when forming homopolymers include: methyl acrylate (glass transition temperature of 8°C when forming homopolymers), methyl methacrylate (glass transition temperature of 105°C when forming homopolymers), ethyl methacrylate (glass transition temperature of 65°C when forming homopolymers), n-butyl methacrylate (glass transition temperature of 20°C when forming homopolymers), n-hexyl methacrylate (glass transition temperature of 0°C when forming homopolymers), tert-butyl acrylate (glass transition temperature of 14°C when forming homopolymers), and tert-butyl methacrylate (glass transition temperature of 0°C when forming homopolymers). The glass transition temperature of the polymer is 107℃, cyclohexyl acrylate (glass transition temperature of 15℃ when made into homopolymer), cyclohexyl methacrylate (glass transition temperature of 66℃ when made into homopolymer), 3,3,5-trimethylcyclohexyl acrylate (glass transition temperature of 52℃ when made into homopolymer), benzyl acrylate (glass transition temperature of 6℃ when made into homopolymer), benzyl methacrylate (glass transition temperature of 54℃ when made into homopolymer), isobornyl acrylate (glass transition temperature of 97℃ when made into homopolymer), and isobornyl methacrylate (glass transition temperature of 180℃ when made into homopolymer), etc.
[0077] The preferred lower limit for the content of structural units derived from monomers that do not have crosslinking functional groups and have a glass transition temperature of 0°C or higher when made into homopolymers in the aforementioned (meth)acrylic acid copolymers is 0.1% by mass, and the preferred upper limit is 70% by mass. By setting the content of structural units derived from monomers that do not have crosslinking functional groups and have a glass transition temperature of 0°C or higher when made into homopolymers within this range, the high-temperature retention of the resulting adhesive tape becomes more excellent. The more preferred lower limit for the content of structural units derived from monomers that do not have crosslinking functional groups and have a glass transition temperature of 0°C or higher when made into homopolymers is 10% by mass, and the more preferred upper limit is 50% by mass.
[0078] The content of the above-mentioned structural units derived from monomers that do not have cross-linking functional groups and whose glass transition temperature is above 0°C when made into homopolymers can be 0.1 to 70% by mass, 0.1 to 50% by mass, 10 to 70% by mass, or 10 to 50% by mass.
[0079] It should be noted that the content ratio of the structural units derived from monomers that do not have crosslinking functional groups and whose glass transition temperature is above 0°C when forming homopolymers can be calculated as follows: The determination of the above (meth)acrylic acid copolymers based on mass spectrometry and / or nuclear magnetic resonance spectroscopy (…) 1 H-NMR measurement, 13The results are calculated based on the integral intensity ratio of hydrogen peaks originating from monomers that do not have cross-linking functional groups and whose glass transition temperature is above 0°C when they are made into homopolymers.
[0080] From the viewpoint that it can exert excellent adhesion to both smooth and rough surfaces, the above-mentioned (meth)acrylic copolymers preferably have structural units derived from n-heptyl (meth)acrylate.
[0081] On the other hand, from the viewpoint of making the obtained adhesive tape have better high-temperature retention and better adhesion to the adhered objects, the above-mentioned (meth)acrylic copolymer preferably does not have the above-mentioned structural units derived from (meth)acrylic acid n-heptyl ester, or the content of the above-mentioned structural units derived from (meth)acrylic acid n-heptyl ester is less than 90% by mass.
[0082] The aforementioned (meth)acrylic acid copolymer preferably also has structural units derived from monomers having non-crosslinked ether structures, wherein the monomers having non-crosslinked ether structures are selected from at least one of monomers having cyclic ether structures other than epoxy and oxetyl groups, and monomers having non-cyclic ether structures. By incorporating the aforementioned (meth)acrylic acid copolymer with structural units derived from monomers having non-crosslinked ether structures, the surface energy of the resulting adhesive composition is reduced, thereby enabling superior adhesion to the adhered substrate.
[0083] In addition, the monomers having the above-mentioned non-crosslinked ether structure preferably have (meth)acryloyl groups.
[0084] It should be noted that in this specification, "(meth)acryloyl" refers to acryloyl or methacryloyl.
[0085] Examples of monomers having cyclic ether structures other than epoxy and oxobutyl groups include tetrahydrofurfuryl (meth)acrylate and methyl acrylate (2-methyl-2-ethyl-1,3-dioxolane-4-yl)acrylate.
[0086] Examples of monomers having a noncyclic ether structure include: 2-methoxyethyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, ethyl carbitol (meth)acrylate, and 2-(2-(2-methoxyethoxy)ethoxy)ethyl (meth)acrylate.
[0087] The preferred lower limit for the content of the structural units derived from monomers having a non-crosslinked ether structure in the aforementioned (meth)acrylic copolymer is 0.01% by mass, and the preferred upper limit is 50% by mass. By setting the content of the structural units derived from monomers having a non-crosslinked ether structure within this range, the resulting adhesive tape exhibits superior adhesion to the adhered object. A more preferred lower limit for the content of the structural units derived from monomers having a non-crosslinked ether structure is 10% by mass, and a more preferred upper limit is 30% by mass.
[0088] The content of the above-mentioned structural units derived from monomers with non-crosslinked ether structures can be 0.01–50% by mass, 0.01–30% by mass, 10–50% by mass, or 10–30% by mass.
[0089] It should be noted that the content ratio of the structural units derived from monomers with non-crosslinked ether structures can be calculated as follows: This is based on the determination of the above (meth)acrylic acid copolymers using mass spectrometry and / or nuclear magnetic resonance spectroscopy. 1 H-NMR measurement, 13 (e.g., C-NMR determination), calculated based on the integral intensity ratio of hydrogen peaks originating from the aforementioned monomers with non-crosslinked ether structures.
[0090] It should be noted that the above-mentioned (meth)acrylic acid copolymers may not have the structural units derived from monomers with non-crosslinked ether structures, that is, the content of the structural units derived from monomers with non-crosslinked ether structures can be 0 by mass.
[0091] The aforementioned (meth)acrylic acid copolymers preferably also have structural units derived from monomers having crosslinking functional groups.
[0092] By giving the above-mentioned (meth)acrylic acid copolymer the structural units derived from monomers with crosslinking functional groups, the cohesive force of the adhesive layer is improved, and the resulting adhesive tape exhibits better adhesion to the adhered objects.
[0093] It should be noted that the glass transition temperature of the monomers with cross-linking functional groups mentioned above can be above 0°C when they are made into homopolymers.
[0094] Examples of monomers having crosslinking functional groups include, for instance, monomers containing carboxyl groups, monomers containing hydroxyl groups, monomers containing glycidyl groups, monomers containing amide groups, and monomers containing nitrile groups. From the perspective of easily adjusting the gel fraction of the adhesive layer described later, the monomers having crosslinking functional groups preferably include at least one selected from the aforementioned monomers containing carboxyl groups and the aforementioned monomers containing hydroxyl groups, and more preferably include the aforementioned monomers containing hydroxyl groups.
[0095] Furthermore, the monomers with cross-linking functional groups mentioned above preferably have (meth)acryloyl groups.
[0096] Examples of the aforementioned carboxyl-containing monomers include (meth)acrylic acid.
[0097] Examples of hydroxyl-containing monomers include: 2-hydroxyethyl methacrylate, 3-hydroxypropyl methacrylate, 3-hydroxybutyl methacrylate, 1-methyl-3-hydroxypropyl methacrylate, 1-methyl-2-hydroxyethyl methacrylate, 4-hydroxybutyl methacrylate, 1-methyl-2-hydroxypropyl methacrylate, 2-hydroxypropyl methacrylate, 2-hydroxybutyl methacrylate, 1-ethyl-2-hydroxyethyl methacrylate, 6-hydroxyhexyl methacrylate, 5-hydroxypentyl methacrylate, 7-hydroxyheptyl methacrylate, 8-hydroxyoctyl methacrylate, and 9-hydroxynonyl methacrylate.
[0098] Examples of monomers containing glycidyl groups include glycidyl (meth)acrylate.
[0099] Examples of monomers containing amide groups include isopropyl (meth)acrylamide and dimethylaminopropyl (meth)acrylamide.
[0100] Examples of the aforementioned nitrile-containing monomers include (meth)acrylonitrile.
[0101] The preferred lower limit for the content of structural units derived from the carboxyl-containing monomers in the above-mentioned (meth)acrylic acid copolymers is 0.1% by mass, and the preferred upper limit is 15% by mass. By keeping the content of structural units derived from the carboxyl-containing monomers within this range, the resulting adhesive tape exhibits superior adhesion to the adhered object. A more preferred lower limit for the content of structural units derived from the carboxyl-containing monomers is 1% by mass, a more preferred upper limit is 10% by mass, a further preferred lower limit is 3.0% by mass, a further preferred upper limit is 8.0% by mass, and an even more preferred lower limit is 5.0% by mass.
[0102] The proportion of structural units derived from the aforementioned carboxyl-containing monomers can be 0.1–15% by mass, 0.1–10% by mass, 0.1–8.0% by mass, 1.0–15% by mass, 1.0–10% by mass, 1.0–8.0% by mass, 3.0–15% by mass, 3.0–10% by mass, 3.0–8.0% by mass, 5.0–15% by mass, 5.0–10% by mass, and 5.0–8.0% by mass.
[0103] It should be noted that the proportion of structural units derived from the aforementioned carboxyl-containing monomers in the above-mentioned (meth)acrylic acid copolymers can be calculated as follows: This is determined by mass spectrometry and / or nuclear magnetic resonance spectroscopy of the above-mentioned (meth)acrylic acid copolymers. 1 H-NMR, 13 (e.g., C-NMR), calculated based on the integral intensity ratio of hydrogen peaks originating from the aforementioned carboxyl-containing monomers.
[0104] The preferred lower limit for the content of structural units derived from the hydroxyl-containing monomers in the above-mentioned (meth)acrylic acid copolymers is 0.01% by mass, and the preferred upper limit is 2.0% by mass. By keeping the content of structural units derived from the hydroxyl-containing monomers within this range, the resulting adhesive tape exhibits superior adhesion to the adhered object. A more preferred lower limit for the content of structural units derived from the hydroxyl-containing monomers is 0.05% by mass, a more preferred upper limit is 1.0% by mass, and a further preferred lower limit is 0.1% by mass.
[0105] The proportion of structural units derived from the above-mentioned hydroxyl-containing monomers can be 0.01–2.0% by mass, 0.01–1.0% by mass, 0.05–2.0% by mass, 0.05–1.0% by mass, 0.1–2.0% by mass, or 0.1–1.0% by mass.
[0106] It should be noted that the proportion of structural units derived from the hydroxyl-containing monomers in the above-mentioned (meth)acrylic acid copolymers can be calculated as follows: This is determined by mass spectrometry and / or nuclear magnetic resonance spectroscopy of the above-mentioned (meth)acrylic acid copolymers. 1 H-NMR, 13 (e.g., C-NMR), calculated based on the integral intensity ratio of hydrogen peaks originating from the aforementioned hydroxyl-containing monomers.
[0107] The preferred lower limit for the content of the structural units derived from monomers having crosslinking functional groups in the aforementioned (meth)acrylic copolymer is 0.01% by mass, and the preferred upper limit is 20% by mass. By setting the content of the structural units derived from monomers having crosslinking functional groups within this range, the resulting adhesive tape exhibits superior adhesion to the adhered object. A more preferred lower limit for the content of the structural units derived from monomers having crosslinking functional groups is 0.1% by mass, a more preferred upper limit is 10% by mass, and a further preferred lower limit is 1% by mass.
[0108] The content of the above-mentioned structural units derived from monomers with cross-linking functional groups can be 0.01–20% by mass, 0.01–10% by mass, 0.1–20% by mass, 0.1–10% by mass, 1–20% by mass, or 1–10% by mass.
[0109] It should be noted that the proportion of structural units derived from monomers with crosslinking functional groups in the above-mentioned (meth)acrylic acid copolymers can be calculated as follows: This is determined by mass spectrometry and / or nuclear magnetic resonance spectroscopy of the above-mentioned (meth)acrylic acid copolymers. 1 H-NMR measurement, 13 (e.g., C-NMR measurements), calculated based on the integral intensity ratio of hydrogen peaks originating from the aforementioned monomers with cross-linking functional groups.
[0110] Furthermore, the aforementioned (meth)acrylic acid copolymers may, without hindering the purpose of the present invention, have structural units derived from alkyl methacrylic acids, structural units derived from monomers that do not have crosslinking functional groups and have a glass transition temperature of 0°C or higher when forming homopolymers, structural units derived from monomers having non-crosslinking ether structures, and structural units derived from other monomers besides the structural units derived from monomers having crosslinking functional groups.
[0111] Other monomers mentioned above can be, for example, vinyl acetate, styrene, and other monomers commonly used as raw materials for (meth)acrylic acid copolymers.
[0112] The weight-average molecular weight of the above-mentioned (meth)acrylic acid copolymers is not particularly limited, and can be, for example, in the range of about 30,000 to 2 million.
[0113] Furthermore, the preferred lower limit for the weight-average molecular weight of the aforementioned (meth)acrylic acid copolymer is 800,000. By making the weight-average molecular weight of the aforementioned (meth)acrylic acid copolymer 800,000 or more, the resulting adhesive tape exhibits superior adhesion to the adhered object and better high-temperature retention. A more preferred lower limit for the weight-average molecular weight of the aforementioned (meth)acrylic acid copolymer is 900,000, and a further preferred lower limit is 1,000,000.
[0114] Furthermore, considering that the adhesive layer has moderate softness and the resulting adhesive tape has better surface conformability, the preferred upper limit for the weight-average molecular weight of the (meth)acrylic acid copolymer is 1.5 million, and a more preferred upper limit is 1.2 million.
[0115] The weight-average molecular weight of the above-mentioned (meth)acrylic acid copolymers can be 30,000 to 2,000,000, 30,000 to 1,500,000, 30,000 to 1,200,000, 800,000 to 2,000,000, 800,000 to 1,500,000, 800,000 to 1,200,000, 900,000 to 2,000,000, 900,000 to 1,500,000, 900,000 to 1,200,000, 1,000,000 to 2,000,000, 1,000,000 to 1,500,000, or 1,000,000 to 1,200,000.
[0116] It should be noted that, in this specification, the weight-average molecular weight mentioned above is the weight-average molecular weight converted from standard polystyrene based on GPC (Gel Permeation Chromatography). Specifically, the (meth)acrylic acid copolymer is diluted 50 times with tetrahydrofuran (THF), and the resulting diluted solution is filtered through a filter (material: polytetrafluoroethylene, pore size: 0.2 μm) to prepare the test sample. Next, the test sample is fed into a gel permeation chromatograph, and GPC determination is performed at a sample flow rate of 1 mL / min and a column temperature of 40°C. The polystyrene-converted molecular weight of the (meth)acrylic acid copolymer is determined, and this value is taken as the weight-average molecular weight of the (meth)acrylic acid copolymer. Examples of gel permeation chromatographs include the 2690 Separations Module (manufactured by Waters Corporation).
[0117] Methods for adjusting the weight-average molecular weight of the above-mentioned (meth)acrylic acid copolymers include, for example, changing the type, amount, and monomer concentration of the polymerization initiator during the polymerization reaction; adding a small amount of chain transfer agent such as dodecyl mercaptan; changing the type of polymerization solvent to control chain transfer to the solvent; changing the reaction temperature; etc.
[0118] The above-mentioned (meth)acrylic acid copolymers can be obtained by polymerizing a mixture of monomers used as raw materials through a free radical reaction in the presence of a polymerization initiator.
[0119] Examples of free radical reactions include living radical polymerization and free radical polymerization. Compared with free radical polymerization, living radical polymerization can produce copolymers with more uniform molecular weight and composition, suppress the formation of low molecular weight components, and thus improve the cohesiveness of the resulting adhesive layer, resulting in a better adhesion of the adhesive tape to the adhered objects.
[0120] As the method for polymerizing the above monomer mixture, conventionally known methods can be used, and examples thereof include solution polymerization (boiling point polymerization or constant temperature polymerization), UV polymerization, emulsion polymerization, suspension polymerization, bulk polymerization and the like. Among these, from the viewpoint that the obtained adhesive tape has more excellent conformability to an adherend, solution polymerization and UV polymerization are preferred.
[0121] In the case of using solution polymerization as the method for polymerizing the above monomer mixture, examples of the reaction solvent include ethyl acetate, toluene, methyl ethyl ketone, dimethyl sulfoxide, ethanol, acetone, diethyl ether and the like.
[0122] Examples of the above polymerization initiator include organic peroxides, azo compounds and the like.
[0123] Examples of the above organic peroxides include 1,1-bis(tert-hexylperoxy)-3,3,5-trimethylcyclohexane, tert-hexyl peroxypivalate, tert-butyl peroxypivalate, 2,5-dimethyl-2,5-bis(2-ethylhexanoylperoxy)hexane, tert-hexyl peroxy-2-ethylhexanoate, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxyisobutyrate, tert-butyl peroxy-3,5,5-trimethylhexanoate, tert-butyl peroxylaurate and the like.
[0124] Examples of the above azo compounds include azobisisobutyronitrile, azobiscyclohexanecarbonitrile and the like.
[0125] In addition, when the mode of the above radical reaction is the above living radical polymerization, examples of the above polymerization initiator include organic tellurium polymerization initiators. The above organic tellurium polymerization initiator is not particularly limited as long as it is an organic tellurium polymerization initiator generally used in living radical polymerization, and examples thereof include organic tellurium compounds, organic telluride compounds and the like. It should be noted that in the above living radical polymerization, in addition to the above organic tellurium polymerization initiator, an azo compound may also be used as the above polymerization initiator for the purpose of accelerating the polymerization rate.
[0126] The preferred lower limit of the content ratio of the above (meth)acrylic copolymer in the above adhesive composition is 50% by mass, and the preferred upper limit is 99.5% by mass. By setting the content ratio of the above (meth)acrylic copolymer within this range, the obtained adhesive tape has more excellent conformability to an adherend. The more preferred lower limit of the content ratio of the above (meth)acrylic copolymer is 55% by mass, the more preferred upper limit is 95% by mass, the further preferred lower limit is 65% by mass, the further preferred upper limit is 90% by mass, the particularly preferred lower limit is 70% by mass, and the particularly preferred upper limit is 80% by mass.
[0127] The content of the above-mentioned (meth)acrylic acid copolymer can be 50-99.5% by mass, 50-95% by mass, 50-90% by mass, 50-80% by mass, 55-99.5% by mass, 55-95% by mass, 55-90% by mass, 55-80% by mass, 65-99.5% by mass, 65-95% by mass, 65-90% by mass, 65-80% by mass, 70-99.5% by mass, 70-95% by mass, 70-90% by mass, and 70-80% by mass.
[0128] The adhesive composition described above preferably contains a tackifier. By containing the aforementioned tackifier, the adhesive tape of this embodiment exhibits superior adhesion to the adhered objects.
[0129] Examples of such tackifiers include: (meth)acrylic acid tackifiers, rosin-based resins, rosin ester tackifiers, terpene-based tackifiers, coumarone-indene tackifiers, alicyclic saturated hydrocarbon tackifiers, C5-based petroleum tackifiers, C9-based petroleum tackifiers, and C5-C9 copolymer petroleum tackifiers. These tackifiers can be used alone or in combination of two or more. Preferably, at least one selected from (meth)acrylic acid tackifiers, rosin ester tackifiers, and terpene-based tackifiers is included. By including at least one selected from the above-mentioned (meth)acrylic acid tackifiers, rosin ester tackifiers, and terpene-based tackifiers as the tackifier, the resulting adhesive tape exhibits superior adhesion to the adhered objects. More preferably, the tackifier includes at least one selected from the above-mentioned rosin ester tackifiers and terpene-based tackifiers; even more preferably, it includes both the above-mentioned rosin ester tackifiers and the above-mentioned terpene-based tackifiers.
[0130] It should be noted that the aforementioned rosin ester-based tackifiers refer to tackifiers containing rosin ester-based resins, and the aforementioned terpene-based tackifiers refer to tackifiers containing terpene-based resins. Furthermore, the aforementioned terpene-based resins include terpene resins and terpene phenol resins.
[0131] Examples of rosin-based tackifiers include rosin resins and rosin polyol resins.
[0132] Examples of rosin ester-based tackifiers include rosin ester resins, polymerized rosin ester resins, and hydrogenated rosin ester resins. Specifically, examples include Pensel D-135, Pine Crystal KE-359, Ester Gum AA-V, and Ester Gum H (all manufactured by Arakawa Chemical Industry Co., Ltd.).
[0133] Examples of terpene-based tackifiers include terpene resins and terpene phenol resins, specifically YS RESIN PX1250 (manufactured by YASUHARA CHEMICAL) and YS POLYSTER G150 (manufactured by YASUHARA CHEMICAL).
[0134] The aforementioned rosin ester-based tackifying resin and the aforementioned terpene-based tackifying resin are preferably derived from biological sources. Examples of biologically derived rosin ester-based tackifying resins include rosin ester-based tackifying resins derived from natural resins such as pine resin. Examples of biologically derived terpene-based tackifying resins include terpene-based tackifying resins derived from plant essential oils, etc.
[0135] The aforementioned (meth)acrylic acid-based tackifiers contain (meth)acrylic acid compounds with a weight-average molecular weight of less than 30,000.
[0136] Examples of (meth)acrylic acid compounds with a weight average molecular weight of less than 30,000 include acrylic oligomers and acrylic monomers with a weight average molecular weight of less than 30,000. Among these, acrylic oligomers with a weight average molecular weight of less than 30,000 are preferred.
[0137] The weight-average molecular weight of the aforementioned acrylic oligomers with a weight-average molecular weight of less than 30,000 is preferably 1,000 or more and less than 30,000. By ensuring that the weight-average molecular weight of the aforementioned acrylic oligomers with a weight-average molecular weight of less than 30,000 is within this range, the adhesive strength of the resulting adhesive composition is further improved. More preferably, the weight-average molecular weight of the aforementioned acrylic oligomers with a weight-average molecular weight of less than 30,000 is 1,500 or more and less than 20,000, and even more preferably, 2,000 or more and less than 10,000.
[0138] It should be noted that the weight-average molecular weight of the above-mentioned acrylic oligomers with a weight-average molecular weight of less than 30,000 can be determined by the same method as the method for determining the weight-average molecular weight of the above-mentioned (meth)acrylic copolymers.
[0139] The preferred lower limit of the glass transition temperature for the aforementioned acrylic oligomers with a weight average molecular weight of less than 30,000 is 0°C, and the preferred upper limit is 300°C. By setting the glass transition temperature of the aforementioned acrylic oligomers with a weight average molecular weight of less than 30,000 within this range, the adhesive strength of the resulting adhesive composition is further improved. A more preferred lower limit of the glass transition temperature for the aforementioned acrylic oligomers with a weight average molecular weight of less than 30,000 is 20°C, and a further preferred lower limit is 40°C.
[0140] The glass transition temperature of the above-mentioned acrylic oligomers with a weight average molecular weight of less than 30,000 can be 0℃~300℃, 20℃~300℃, or 40℃~300℃.
[0141] It should be noted that the glass transition temperature of the aforementioned acrylic oligomers with a weight average molecular weight of less than 30,000 can be determined, for example, by differential scanning calorimetry under a nitrogen atmosphere (nitrogen flow rate 50 mL / min) according to JIS K 6240:2011, at a measurement temperature of -100℃ to 200℃ and a heating rate of 10℃ / min.
[0142] Examples of acrylic monomers constituting the aforementioned acrylic oligomers with a weight average molecular weight of less than 30,000, and examples of acrylic monomers with a weight average molecular weight of less than 30,000, include: monomers that are the same as the structural units derived from alkyl methacrylates that form the aforementioned (meth)acrylic copolymers, the structural units derived from monomers having crosslinking functional groups, and the structural units derived from other monomers.
[0143] As constituent monomers of the aforementioned acrylic oligomers with a weight average molecular weight of less than 30,000, the aforementioned acrylic monomers with a weight average molecular weight of less than 30,000 specifically include, for example: methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, butyl methacrylate, isobutyl methacrylate, sec-butyl methacrylate, tert-butyl methacrylate, amyl methacrylate, isoamyl methacrylate, hexyl methacrylate, 2-ethylhexyl methacrylate, heptyl methacrylate, octyl methacrylate, and propyl methacrylate. Alkyl methacrylates such as isooctyl methacrylate, nonyl methacrylate, isononyl methacrylate, decyl methacrylate, isodecyl methacrylate, undecyl methacrylate, and dodecyl methacrylate; esters of methacrylic acid and alicyclic alcohols such as cyclohexyl methacrylate, isobornyl methacrylate, and dicyclopentyl methacrylate (methacrylic esters containing alicyclic hydrocarbon groups); aryl methacrylic esters such as phenyl methacrylate and benzyl methacrylate; and methacrylic esters derived from terpene compound derivative alcohols.
[0144] As for the aforementioned acrylic oligomers with a weight-average molecular weight of less than 30,000, from the viewpoint of further improving the adhesion of the adhesive layer, it is preferable to include acrylic monomers with a large volume structure, such as alkyl methacrylates with branched alkyl chains, such as isobutyl methacrylate and tert-butyl methacrylate; esters of methacrylate and alicyclic alcohols, such as cyclohexyl methacrylate, isobornyl methacrylate, and dicyclopentyl methacrylate (meth acrylates containing alicyclic hydrocarbon groups); and aryl methacrylates with cyclic structures, such as phenyl methacrylate and benzyl methacrylate.
[0145] In addition to the monomers mentioned above, monomers containing functional groups can also be used as constituent monomers of acrylic oligomers with a weight average molecular weight of less than 30,000. Examples of such monomers containing functional groups include: monomers with nitrogen-containing rings (typically nitrogen-containing heterocycles) such as N-vinyl-2-pyrrolidone and N-acryloylmorpholine; monomers containing amino groups such as N,N-dimethylaminoethyl methacrylate; monomers containing amide groups such as N,N-diethyl(meth)acrylamide; monomers containing carboxyl groups such as acrylic acid and methacrylic acid; and monomers containing hydroxyl groups such as 2-hydroxyethyl methacrylate. These monomers containing functional groups can be used alone or in combination of two or more. Among them, monomers containing carboxyl groups are preferred, and acrylic acid is particularly preferred. By using monomers containing carboxyl groups as the aforementioned monomers containing functional groups, the adhesive strength to highly polar substrates can be improved.
[0146] Furthermore, by using structural units derived from monomers with cross-linking functional groups as constituent monomers of the acrylic oligomers with a weight average molecular weight of less than 30,000, the adhesive strength of the obtained adhesive composition can be further improved.
[0147] The aforementioned tackifier preferably includes a tackifier with a softening temperature of 80°C or higher. By including the aforementioned tackifier with a softening temperature of 80°C or higher, the adhesive layer does not become too soft, and the reduction in the adhesive strength of the resulting adhesive tape can be suppressed. The softening temperature of the aforementioned tackifier with a softening temperature of 80°C or higher is preferably 90°C or higher, more preferably 100°C or higher.
[0148] Furthermore, from the viewpoint of improving the wettability of the interface of the adhesive layer, the softening temperature of the tackifier with a softening temperature of 80°C or higher is preferably 170°C or lower, more preferably 160°C or lower, and even more preferably 150°C or lower.
[0149] The softening temperature of the aforementioned tackifier with a softening temperature of 80℃ or above can be 80℃~170℃, 80℃~160℃, 80℃~150℃, 90℃~170℃, 90℃~160℃, 90℃~150℃, 100℃~170℃, 100℃~160℃, or 100℃~150℃.
[0150] It should be noted that, in this specification, the "softening temperature" refers to the softening temperature determined by means of the method according to JIS K 2207 (ring and ball method).
[0151] In the above adhesive composition, the preferred lower limit of the content of the tackifier relative to 100 parts by weight of the above (meth)acrylic copolymer is 10 parts by weight, and the preferred upper limit is 50 parts by weight. By setting the content of the tackifier within this range, the resulting adhesive tape exhibits superior adhesion to the adhered object and better high-temperature retention. A more preferred lower limit of the content of the tackifier is 15 parts by weight, a more preferred upper limit is 40 parts by weight, and a further preferred lower limit is 20 parts by weight.
[0152] The content of the above-mentioned thickener can be 10-50 parts by weight, 10-40 parts by weight, 20-50 parts by weight, or 20-40 parts by weight.
[0153] The adhesive composition described above preferably further contains a crosslinking agent.
[0154] Examples of crosslinking agents include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, aziridine-based crosslinking agents, and metal chelate-type crosslinking agents. From the perspective of improving the adhesion of the resulting adhesive tape to the adhered object, the crosslinking agent preferably includes at least one selected from isocyanate-based and epoxy-based crosslinking agents, more preferably including the aforementioned isocyanate-based crosslinking agent, and even more preferably including both the aforementioned isocyanate-based and epoxy-based crosslinking agents. It should be noted that the aforementioned crosslinking agents can be used alone or in combination of two or more. Furthermore, when using two or more crosslinking agents, two or more crosslinking agents of the same system can be used (e.g., using two or more isocyanate-based crosslinking agents), or crosslinking agents of different systems can be used in combination (e.g., using one or more isocyanate-based and epoxy-based crosslinking agents respectively).
[0155] In the above adhesive composition, the preferred lower limit of the crosslinking agent content relative to 100 parts by weight of the above (meth)acrylic copolymer is 0.1 parts by weight, and the preferred upper limit is 10 parts by weight. By setting the content of the crosslinking agent within this range, the resulting adhesive tape exhibits superior adhesion and transparency to the adhered object. A more preferred lower limit of the crosslinking agent content is 0.2 parts by weight, and a more preferred upper limit is 5 parts by weight.
[0156] The content of the crosslinking agent can be 0.1 to 10 parts by mass, 0.1 to 5 parts by mass, 0.2 to 10 parts by mass, or 0.2 to 5 parts by mass.
[0157] It should be noted that in this specification, the "content of crosslinking agent" refers to the content of the solid component of the crosslinking agent.
[0158] The adhesive composition described above may further contain a crosslinking catalyst for promoting crosslinking based on the crosslinking agent described above.
[0159] Examples of crosslinking catalysts, such as dibutyltin dilaurate, dibutyltin diacetate, and dioctyltin dilaurate, can be used as crosslinking catalysts for the aforementioned isocyanate-based crosslinking agents.
[0160] The above-mentioned adhesive composition preferably also contains pigments.
[0161] By containing the aforementioned pigments, the resulting adhesive tape exhibits excellent light-blocking properties, making it suitable for fixing components used in devices requiring protection against light leakage.
[0162] Examples of pigments mentioned above include coloring pigments such as black fillers.
[0163] Examples of black fillers mentioned above include, for instance, carbon black and titanium black.
[0164] The preferred lower limit for the average particle size of the aforementioned black filler is 0.01 μm, and the preferred upper limit is 1.0 μm. By keeping the average particle size of the aforementioned black filler within this range, the light-shielding properties of the resulting adhesive tape become more excellent. A more preferred lower limit for the average particle size of the aforementioned black filler is 0.1 μm, and a more preferred upper limit is 0.8 μm.
[0165] The average particle size of the aforementioned black filler can be 0.01–1.0 μm, 0.01–0.8 μm, 0.1–1.0 μm, or 0.1–0.8 μm.
[0166] It should be noted that the average particle size of the aforementioned black filler is determined, for example, by observing any 50 black fillers with an electron microscope or an optical microscope and calculating the average particle size of each black filler; or by performing laser diffraction particle size distribution measurement.
[0167] In the above adhesive composition, the preferred lower limit of the pigment content relative to 100 parts by weight of the above (meth)acrylic copolymer is 0.1 parts by weight, and the preferred upper limit is 5.0 parts by weight. By setting the pigment content within this range, the light-blocking properties of the resulting adhesive tape become more excellent. A more preferred lower limit of the pigment content is 0.5 parts by weight, and a more preferred upper limit is 3.0 parts by weight.
[0168] The content of the above-mentioned pigment can be 0.1 to 5.0 parts by weight, 0.1 to 3.0 parts by weight, 0.5 to 5.0 parts by weight, or 0.5 to 3.0 parts by weight.
[0169] The above-mentioned adhesive composition may contain additives such as silane coupling agents, plasticizers, softeners, fillers, and dyes as needed, without hindering the purpose of the present invention.
[0170] The preferred lower limit for the bio-derived carbon content in the aforementioned adhesive layer is 10%. From the viewpoint of conserving petroleum resources and reducing carbon dioxide emissions, the adhesive tape of this embodiment is excellent and can reduce environmental impact by ensuring that the bio-derived carbon content in the aforementioned adhesive layer is 10% or more. A more preferred lower limit is 40%, and a further preferred lower limit is 60%.
[0171] Furthermore, there is no specific upper limit to the above-mentioned carbon content derived from biological sources, which can be 100%. In addition, the above-mentioned carbon content derived from biological sources can be 95% or less, or 90% or less.
[0172] The bio-derived carbon content in the aforementioned adhesive layer can be 10-100%, 40-100%, 60-100%, 10-95%, 40-95%, 60-95%, 10-90%, 40-90%, or 60-90%.
[0173] It should be noted that bio-derived carbon contains a certain proportion of the radioactive isotope (C-14), while petroleum-derived carbon contains almost no C-14. Therefore, the bio-derived carbon content can be calculated by measuring the C-14 concentration in the adhesive layer. Specifically, this can be done according to ASTM D6866-22, a standard used in many bioplastics industries.
[0174] The preferred lower limit for the thickness of the adhesive layer in the adhesive tape of this embodiment is 3 μm, and the preferred upper limit is 300 μm. By making the thickness of the adhesive layer within this range, the resulting adhesive tape exhibits superior adhesion to the adhered object. A more preferred lower limit for the thickness of the adhesive layer is 5 μm, and a more preferred upper limit is 200 μm.
[0175] The thickness of the adhesive layer can be 3–300 μm, 3–200 μm, 5–300 μm, or 5–200 μm.
[0176] The adhesive tape of this embodiment can be a non-supporting type tape without a substrate layer, or a supporting type tape having the aforementioned substrate layer and having the aforementioned adhesive layer on at least one side of the aforementioned substrate layer. In the case where the adhesive tape of this embodiment is a supporting type tape, it can be a double-sided adhesive tape having the aforementioned adhesive layer on both sides of the aforementioned substrate layer.
[0177] Examples of substrates constituting the aforementioned substrate layer include films and nonwoven fabrics.
[0178] Furthermore, from the viewpoint of increasing the carbon content derived from biological sources in the adhesive tape as a whole, a substrate made of biologically derived materials is preferred as the aforementioned substrate.
[0179] Examples of biologically derived materials include: polyethylene terephthalate (PET), polyethylene furanate (PEF), polylactic acid (PLA), polypropylene terephthalate (PTT), polybutylene terephthalate (PBT), polybutylene succinate (PBS), and other plant-derived materials such as polyester (PE), polyethylene (PE), polypropylene (PP), polyurethane (PU), triacetyl cellulose (TAC), cellulose, and polyamide (PA).
[0180] From the viewpoint of substrate strength, the aforementioned substrate is preferably a film containing PES or a film containing PA. Furthermore, from the viewpoint of heat resistance and oil resistance, a film containing PA is preferred.
[0181] Examples of PAs mentioned above include: Nylon 11, Nylon 1010, Nylon 610, Nylon 510, Nylon 410, etc., which are made from castor oil, and Nylon 56, which is made from cellulose.
[0182] Furthermore, from the perspective of reducing environmental impact by decreasing the use of new petroleum resources and suppressing carbon dioxide emissions, substrates using recycled resources can also be employed. Examples of resource recycling methods include: recycling waste from packaging containers, household appliances, automobiles, building materials, food, and other manufacturing processes, and then reusing the extracted materials as raw materials through cleaning, decontamination, or decomposition via heating or fermentation. Examples of substrates using the aforementioned recycled resources include films and nonwoven fabrics containing PET, PBT, PE, PP, PA, etc., obtained by re-resinizing recycled plastics. Additionally, the recycled waste can be incinerated to utilize the heat energy related to the manufacture of the substrate and its raw materials; or the oils contained in the recycled waste can be mixed with petroleum, and the fractionated and refined material can be used as a raw material.
[0183] From the perspective of improving compression properties, the above-mentioned substrate can be a foam substrate.
[0184] As the aforementioned foam substrate, a foam substrate comprising at least one selected from PE, PP, and PU is preferred. From the viewpoint of balancing flexibility and strength to a high degree, a foam substrate comprising PE is more preferred. Examples of components of the aforementioned foam substrate comprising PE include PE made from sugarcane.
[0185] As a method for manufacturing the above-mentioned foamed material, the preferred method is, for example, the following: preparing a foamable resin composition containing PE resin and a foaming agent, wherein the PE resin comprises PE made from sugarcane, foaming the foaming agent when the foamable resin composition is extruded into a sheet using an extruder, and crosslinking the obtained polyolefin foam as needed.
[0186] The preferred lower limit for the thickness of the aforementioned foam substrate is 50 μm, and the preferred upper limit is 5000 μm. By keeping the thickness of the aforementioned foam substrate within this range, high impact resistance and high flexibility that allows it to conform closely to the shape of the adhered object can be achieved. A more preferred upper limit for the thickness of the aforementioned foam substrate is 1000 μm, and a further preferred upper limit is 300 μm.
[0187] The thickness of the aforementioned foamed substrate can be 50–5000 μm, 50–1000 μm, or 50–300 μm.
[0188] Regarding the adhesive tape of this embodiment, the preferred lower limit for the total thickness of the adhesive tape (the sum of the thicknesses of the substrate layer and the adhesive layer) is 3 μm, and the preferred upper limit is 6000 μm. By setting the total thickness of the adhesive tape within this range, the adhesive strength becomes higher. A more preferred upper limit for the total thickness of the adhesive tape is 1200 μm, and a further preferred upper limit is 500 μm.
[0189] The total thickness of the adhesive tape can be 3–6000 μm, 3–1200 μm, or 3–500 μm.
[0190] The manufacturing method of the adhesive tape in this embodiment is not particularly limited, and it can be manufactured by conventionally known manufacturing methods. For example, in the case of double-sided adhesive tape, the following methods can be cited.
[0191] First, an adhesive composition A is prepared by adding a solvent to a (meth)acrylic copolymer and, as needed, tackifiers, crosslinking agents, etc. The resulting adhesive composition A is applied to the surface of a substrate, and the solvent in the composition is completely dried and removed by heating to form an adhesive layer A. Next, a release film is overlapped onto the formed adhesive layer A with its release-treated surface facing the adhesive layer A.
[0192] Next, another release film other than the aforementioned release film is prepared. Adhesive composition B, prepared using the same method as adhesive composition A, is applied to the release treatment surface of this release film. The solvent in the composition is completely dried and removed, thereby creating a laminated film with adhesive layer B formed on the surface of the release film. The resulting laminated film is overlapped onto the back side of the substrate with adhesive layer B facing each other, to create a laminate. Then, by applying pressure to the laminated film using a rubber roller or the like, a double-sided adhesive tape is obtained, in which adhesive layers are present on both sides of the substrate and the surfaces of these adhesive layers are covered by the release film.
[0193] Alternatively, two sets of laminated films can be made using the same method. These laminated films are then overlapped on both sides of the substrate with the adhesive layer of the laminated film facing the substrate, respectively, to create a laminate. The laminate is then pressed using a rubber roller or the like, thereby obtaining a double-sided adhesive tape with adhesive layers on both sides of the substrate and the surface of the adhesive layers being covered by a release film.
[0194] Regarding the adhesive tape of this embodiment, for a laminate obtained by bonding an aluminum plate with a width of 25 mm, a length of 150 mm, and a thickness of 0.3 mm to a polycarbonate resin plate with a width of 25 mm, a length of 200 mm, and a thickness of 1 mm using the adhesive tape with a width of 25 mm and a length of 150 mm disposed at the center of the polycarbonate resin plate in the longitudinal direction, after applying bending stress to the laminate and deforming it into an arc shape with the two ends of the polycarbonate resin plate spaced 180 mm apart in the longitudinal direction, and then performing a resilience test at 60°C and 90%RH for 72 hours, the preferred upper limit of the float height between the aluminum plate and the polycarbonate resin plate (hereinafter also referred to as "float height after the resilience test") is 5 mm. By making the float height after the resilience test 5 mm or less, the adhesive tape of this embodiment is more suitable for applications requiring surface conformability. A more preferred upper limit of the float height after the resilience test is 2 mm. The optimal float height after the above resilience test is 0 mm, that is, no float occurs after the above resilience test.
[0195] The floating height after the above resilience test can be 0-5mm or 0-2mm.
[0196] Specifically, the above-mentioned resilience test can be performed using the following methods. Figure 1 This is a schematic diagram illustrating the method for testing the resilience of adhesive tape.
[0197] First, adhesive tape 1 is cut into a flat rectangular shape with a width of 25mm and a length of 150mm. Using adhesive tape 1, an aluminum plate 2 with a width of 25mm, a length of 150mm, and a thickness of 0.3mm is bonded to a polycarbonate resin plate 3 with a width of 25mm, a length of 200mm, and a thickness of 1mm. At this point, the adhesive tape 1 is positioned at the center of the polycarbonate resin plate 3 along its length. A 2kg rubber roller is then used to reciprocate once on the polycarbonate resin plate 3 at a speed of 300mm / minute, integrating the polycarbonate resin plate 3 and the aluminum plate 2 via adhesive tape 1. The mixture is then left to stand at 23°C for 24 hours to create a laminate 4. Figure 1 As shown, the laminate 4 is mounted on the fixture 5, and bending stress is applied along the length of the laminate 4, thereby deforming the laminate 4 into an arc shape with the distance between its two ends along the length of the polycarbonate resin plate 3 becoming 180 mm. In this state, the laminate 4 is placed in a constant temperature and humidity oven at 60°C and 90%RH and left to stand for 72 hours. The laminate 4 is then removed from the oven in its warped arc shape, and the floating height H (mm) between the aluminum plate 2 and the polycarbonate resin plate 3 is measured using a vernier caliper.
[0198] The application of the adhesive tape in this embodiment is not particularly limited, but it is preferably used for fixing electronic device components or vehicle-mounted components. Specifically, the adhesive tape in this embodiment can be preferably used for bonding and fixing electronic device components in large portable electronic devices with curved surfaces, and for bonding and fixing vehicle-mounted components with curved surfaces (such as vehicle-mounted panels).
[0199] Invention Effects
[0200] According to the present invention, an adhesive tape with excellent high-temperature retention and surface conformability can be provided. Attached Figure Description
[0201] Figure 1 This is a schematic diagram illustrating the method for testing the resilience of adhesive tape.
[0202] Figure 2 This is a schematic diagram illustrating the method of high-temperature holding test. Detailed Implementation
[0203] The present invention will be described in more detail below with examples, but the present invention is not limited to these examples.
[0204] The materials used in the examples and comparative examples are as follows.
[0205] <Hexyl acrylate containing carbon derived from biological sources>
[0206] After converting linoleic acid derived from castor oil to linoleic acid hydroperoxide via lipoxygenase, a mixture containing hexanal was obtained via isomerase. Distillation of the resulting mixture yielded hexanal containing biologically derived carbon. Further, hydrogenation of the obtained hexanal containing biologically derived carbon yielded hexanol containing biologically derived carbon. Esterification of the obtained hexanol containing biologically derived carbon with acrylic acid (manufactured by Nippon Shokubai Co., Ltd.) prepared hexyl acrylate containing biologically derived carbon (glass transition temperature of -65°C when forming a homopolymer).
[0207] <Heptyl acrylate containing carbon derived from biological sources>
[0208] Castor oil-derived ricinoleic acid was cleaved to obtain a mixture containing undecenoic acid and n-heptanol. Next, undecenoic acid was separated from the resulting mixture by distillation, thereby obtaining n-heptanol containing bio-derived carbon. The obtained n-heptanol containing bio-derived carbon was esterified with acrylic acid (manufactured by Nippon Shokubai Co., Ltd.) to prepare n-heptyl acrylate containing bio-derived carbon (glass transition temperature of -68°C when forming a homopolymer).
[0209] <1-Methylheptaacrylate containing carbon derived from biological sources>
[0210] Ricinoleic acid, derived from castor oil, was subjected to alkali fusion to obtain a mixture containing sebacic acid and 1-methylheptanol. Sebacic acid was then separated from the resulting mixture by distillation, yielding 1-methylheptanol containing bio-derived carbon. This bio-derived carbon-containing 1-methylheptanol was then esterified with acrylic acid (manufactured by Nippon Shokubai Co., Ltd.) to prepare 1-methylheptan acrylate containing bio-derived carbon (glass transition temperature of the homopolymer was -45°C).
[0211] <2-Hydroxyethyl acrylate containing carbon derived from biological sources>
[0212] Ethanol containing bio-derived carbon was obtained by fermenting the sugar contained in sugarcane. The ethanol containing bio-derived carbon was dehydrated to obtain ethylene, which was then oxidized. Water was added to the resulting ethylene oxide to obtain ethylene glycol containing bio-derived carbon. 2-hydroxyethyl acrylate (a hydroxyl-containing monomer) containing bio-derived carbon was prepared by esterifying the obtained ethylene glycol containing bio-derived carbon with acrylic acid (manufactured by Nippon Shokubai Co., Ltd.).
[0213] <Monomers without biologically derived carbon>
[0214] • n-Butyl acrylate (manufactured by Tokyo Chemical Industry Co., Ltd., with a glass transition temperature of -55°C when made into homopolymer)
[0215] • 2-Ethylhexyl acrylate (manufactured by Nippon Shokubai Co., Ltd., with a glass transition temperature of -70°C when made into homopolymer)
[0216] • Acrylic acid (manufactured by Nippon Shokubai Co., Ltd., a monomer containing carboxyl groups)
[0217] • Methyl acrylate (manufactured by Tokyo Chemical Industry Co., Ltd., with a glass transition temperature of 8°C when it is made into a homopolymer)
[0218] • 2-Methoxyethyl acrylate (manufactured by Tokyo Chemical Industry Co., Ltd., with a glass transition temperature of -55°C when made into homopolymer, a monomer with a non-cyclic ether structure)
[0219] <Tackifier>
[0220] • Tackifier A: Terpene-based tackifier (terpene phenol resin, manufactured by YASUHARA CHEMICAL, "YSPOLYSTER G150", softening temperature: 145℃~155℃)
[0221] • Tackifier B: Rosin ester tackifier (manufactured by Arakawa Chemical Industry Co., Ltd., "Pine Crystal KE-359", softening temperature: 94℃~104℃)
[0222] • Tackifier C: Rosin ester tackifier (softening temperature: 150℃, hydroxyl value: 35mgKOH / g)
[0223] <Cross-linking agent>
[0224] • Isocyanate-based crosslinking agent (Covestro, “Desmodur L-75”)
[0225] • Epoxy crosslinking agent (manufactured by MITSUBISHI GAS CHEMICAL, "TETRAD X")
[0226] <Pigment>
[0227] • Carbon black (manufactured by TOYO COLOR, "Multilac (Japanese: マルチラック) A903 Black")
[0228] (Example 1)
[0229] (1) Manufacturing of acrylic copolymers
[0230] Ethyl acetate, used as the polymerization solvent, was added to the reaction vessel. After bubbling with nitrogen, the reaction vessel was heated to induce reflux while nitrogen was flowing in. Next, a polymerization initiator solution obtained by diluting 0.1 parts by mass of azobisisobutyronitrile (azobisisobutyronitrile) as a polymerization initiator by ethyl acetate was added to the reaction vessel. Over 2 hours, 89.9 parts by mass of 2-ethylhexyl acrylate, 0.1 parts by mass of 2-hydroxyethyl acrylate containing bio-derived carbon, and 10.0 parts by mass of acrylic acid were added dropwise. After the addition was complete, the polymerization initiator solution obtained by diluting 0.1 parts by mass of azobisisobutyronitrile (azobisisobutyronitrile) as a polymerization initiator by ethyl acetate was added back to the reaction vessel, and the polymerization reaction was carried out for 4 hours, yielding a solution containing an acrylic copolymer.
[0231] The obtained acrylic copolymer was diluted 50-fold with tetrahydrofuran (THF), and the diluted solution was filtered through a filter (material: polytetrafluoroethylene, pore size: 0.2 μm) to prepare the test sample. This test sample was fed into a gel permeation chromatograph (Waters, “2690 Separations Module”) and GPC was performed at a sample flow rate of 1 mL / min and a column temperature of 40 °C to determine the polystyrene-converted molecular weight of the acrylic copolymer and calculate the weight-average molecular weight. The results are shown in Table 1.
[0232] (2) Manufacturing of adhesive tape
[0233] In a solution containing acrylic copolymers, 30.0 parts by weight of a terpene-based tackifier were added relative to 100 parts by weight of the acrylic copolymers in the solution, and the isocyanate-based crosslinking agent was added such that the solid component of the isocyanate-based crosslinking agent was 2.5 parts by weight, to prepare an adhesive composition. The obtained adhesive composition was applied to the release surface of a 75 μm thick release PET film with a dried adhesive layer thickness of 50 μm, and then dried at 110°C for 5 minutes to obtain an adhesive layer. The obtained adhesive layer was then overlapped onto the release surface of the 75 μm thick release PET film and cured at 40°C for 48 hours to obtain an adhesive tape (non-supported type).
[0234] (3) Determination of gel fraction of adhesive layer
[0235] The release PET film on one side of the obtained adhesive tape was peeled off and adhered to a 23 μm thick substrate PET film (manufactured by FUTAMURA CHEMICAL, "FE2002"), and cut into a planar rectangular shape with a width of 20 mm and a length of 40 mm. Further, the release PET film on the other side of the adhesive tape was peeled off to prepare a test piece, and its mass was measured. The test piece was immersed in ethyl acetate at 23°C for 24 hours, then removed from the ethyl acetate and dried at 110°C for 1 hour. The mass of the dried test piece was measured, and the gel fraction was calculated using the following formula (I). The results are shown in Table 1.
[0236] Gel fraction (mass%) = 100 × (W2 - W0) / (W1 - W0) (I)
[0237] (W0: quality of the substrate, W1: quality of the test piece before impregnation, W2: quality of the test piece after impregnation and drying)
[0238] (4) Determination of the shear storage modulus of the adhesive layer at 80℃ and the peak temperature of the loss tangent of the adhesive layer.
[0239] The release film of the obtained adhesive tape was peeled off, and the adhesive layers were overlapped to create a laminate with a thickness of approximately 1 mm. This laminate was then cut into pieces 6 mm wide and 10 mm long to obtain test pieces. Next, dynamic viscoelasticity was measured on the obtained test pieces using a dynamic viscoelasticity measuring device in shear mode under a nitrogen atmosphere, at a temperature range of -40℃ to 200℃, a heating rate of 5℃ / min, a frequency of 1 Hz, and a strain of 0.08%. The shear storage modulus of the adhesive layer at 80℃ and the peak temperature of the loss tangent of the adhesive layer were derived. The dynamic viscoelasticity measuring device used was a DVA-200 (manufactured by IT Measurement & Control Co., Ltd.). The results are shown in Table 1.
[0240] (Examples 2-32, 35-47, Comparative Examples 1-8)
[0241] Except that the types and amounts of monomers constituting the acrylic copolymer and the types and amounts of each component contained in the adhesive composition were set as shown in Tables 1-4, the adhesive tape was obtained by operating in the same manner as in Example 1. It should be noted that for Examples 28-30, the types and amounts of each component in the adhesive composition were changed as shown in Table 2, and further, the amount of polymerization initiator was appropriately changed, etc., but otherwise, the adhesive tape was obtained by operating in the same manner as in Example 1. In addition, the weight-average molecular weight of the acrylic copolymer, the gel fraction of the adhesive layer, the shear storage modulus of the adhesive layer at 80°C, and the peak temperature of the loss tangent of the adhesive layer were measured by operating in the same manner as in Example 1. The results are shown in Tables 1-4.
[0242] (Example 33)
[0243] Except that the types and amounts of each component in the adhesive composition were as shown in Table 3, the adhesive composition was prepared in the same manner as in Example 1. The obtained adhesive composition was applied to the release treatment surface of a 75 μm thick release PET film with a dried adhesive layer thickness of 19 μm, and then dried at 110°C for 5 minutes to obtain an adhesive layer. The obtained adhesive layer was then bonded to one side of a 12 μm thick substrate PET film (manufactured by Toyobo Co., Ltd., "FE2002"). Furthermore, an adhesive layer with the same composition and thickness was prepared on the release treatment surface of another 75 μm thick release PET film, bonded to the other side of the substrate PET film, and cured at 40°C for 48 hours to obtain an adhesive tape (support type, total thickness excluding the release PET film 50 μm) with adhesive layers and release PET film on both sides of the substrate. In addition, the weight-average molecular weight of the acrylic copolymer and the gel fraction of the adhesive layer were measured in the same manner as in Example 1. The gel fraction of the adhesive layer was determined using test pieces obtained by peeling off release PET films from both sides after cutting the adhesive tape into planar rectangular shapes with a width of 20 mm and a length of 40 mm. Furthermore, the shear storage modulus of the adhesive layer at 80°C and the peak temperature of the loss tangent of the adhesive layer were measured for the adhesive layer before it was bonded to the substrate PET film. The results are shown in Table 3.
[0244] (Example 34)
[0245] Except that the types and amounts of each component in the adhesive composition were set as shown in Table 3, the same procedure as in Example 1 was followed to obtain the adhesive composition. The obtained adhesive composition was applied to the release treatment surface of a 75 μm thick release PET film with a dried adhesive layer thickness of 50 μm, and then dried at 110°C for 5 minutes to obtain an adhesive layer. The obtained adhesive layer was then bonded to one side of a 150 μm thick substrate PE foam (manufactured by Sekisui Chemicals Co., Ltd., "WL02"). Furthermore, an adhesive layer with the same composition and thickness was prepared on the release treatment surface of another 75 μm thick release PET film, bonded to the other side of the substrate PE foam, and cured at 40°C for 48 hours to obtain an adhesive tape (support type, total thickness excluding the release PET film 250 μm) having an adhesive layer and a release PET film on both sides of the substrate. Additionally, the weight-average molecular weight of the acrylic copolymer and the gel fraction of the adhesive layer were measured, following the same procedure as in Example 1. The gel fraction of the adhesive layer was determined using test pieces obtained by peeling off the release PET film from both sides after cutting the adhesive tape into planar rectangular shapes with a width of 20 mm and a length of 40 mm. Additionally, the shear storage modulus of the adhesive layer at 80°C and the peak temperature of the loss tangent of the adhesive layer were measured on the adhesive layer before it was bonded to the substrate PE foam. The results are shown in Table 3.
[0246] <Evaluation>
[0247] The adhesive tapes obtained in the examples and comparative examples were evaluated using the following methods. The results are shown in Tables 1 to 4.
[0248] (High-temperature performance)
[0249] High temperature holding test was conducted according to JIS Z 0237:2009. Figure 2 This is a schematic diagram illustrating the method of high-temperature holding test.
[0250] Specifically, firstly, a test piece was prepared by backing one side (the side not being measured) of the adhesive tape 1 with a 23 μm thick PET film 6 (manufactured by FUTAMURA CHEMICAL, "FE2002") and cutting it into pieces 25 mm wide and 75 mm long. The test piece was then placed with its adhesive layer (the side being measured) facing a 2 mm thick, 50 mm wide, and 80 mm long SUS304 board 7 (a SUS304 board that had been cleaned with ethanol and then dry-rubbed). A 2 kg rubber roller was then applied to the test piece by reciprocating once at a speed of 300 mm / min. The test piece was then cured at 23°C and 50% RH for 20 minutes to prepare a test sample. The obtained test sample was then placed in an environment of 80°C and 50% RH and allowed to stand for 15 minutes. Under this environment, a 1.0 kg weight 8 was then applied to the PET film 6 of the test sample in a shear direction, according to JIS Z 0237:2009. Twenty-four hours after the installation of the heavy load (24 hours after the start of the test), the amount of offset of the adhesive layer from the position where it is bonded to the SUS304 board 7 in the shear direction is measured. The high-temperature retention of the adhesive tape is evaluated according to the following criteria.
[0251] ○: Cases where the offset is less than 0.5mm
[0252] △: Cases where the offset exceeds 0.5mm, but the test piece has not fallen after 24 hours from the start of the test.
[0253] ×: The condition of the test piece falling 24 hours after the start of the experiment.
[0254] (Surface following performance (planar springback test))
[0255] Cut the obtained adhesive tape into a flat rectangular shape with a width of 25mm and a length of 150mm. Use the adhesive tape to bond an aluminum plate with a width of 25mm, a length of 150mm, and a thickness of 0.3mm to a polycarbonate resin plate with a width of 25mm, a length of 200mm, and a thickness of 1mm. At this point, adjust the adhesive tape so that it is centered along the length of the polycarbonate resin plate. Use a 2kg rubber roller to reciprocate once on the polycarbonate resin plate at a speed of 300mm / min, integrating the polycarbonate resin plate and the aluminum plate via the adhesive tape. Let it stand at 23°C for 24 hours to create a laminate. The resulting laminate is then... Figure 1As shown, the laminate is mounted in a fixture, and bending stress is applied along its length, causing the laminate to warp into an arc shape with the distance between its two ends along the length of the polycarbonate resin plate becoming 180 mm. In this state, the laminate is placed in a constant temperature and humidity oven at 60°C and 90%RH for 72 hours. The laminate is then removed from the oven in its warped arc shape, and the floating height H (mm) between the aluminum plate and the polycarbonate resin plate is measured using a vernier caliper.
[0256] Surface following performance is evaluated according to the following benchmarks.
[0257] ○: Cases where the buoyancy height H is less than 2mm
[0258] △: Cases where the buoyancy height H exceeds 2mm but is less than 5mm
[0259] ×: Cases where the buoyancy height H exceeds 5mm
[0260] (Adhesion to the adhered material)
[0261] The obtained adhesive tape was cut into 25mm wide strips. The release film on one side was peeled off, and a 2kg rubber roller was used to apply the tape to the SUS board by reciprocating once at a speed of 300mm / min. Next, the strips were left to stand for 20 minutes at 23°C and 50%RH to obtain test pieces. Tensile tests were performed on the obtained test pieces using a tensile testing machine (A&D, “RTI-1310”) according to JIS Z 0237:2009, at 80°C, a peel speed of 300mm / min, and a peel angle of 180°. The 180° peel adhesion was measured. The adhesion to the substrate was evaluated according to the following criteria.
[0262] ○: Cases where the 180° peel adhesion is 10N / 25mm or higher.
[0263] △: Cases where the 180° peel adhesion is greater than 5N / 25mm but less than 10N / 25mm
[0264] ×: Cases where the 180° peel adhesion is less than 5N / 25mm.
[0265] (High-speed and easy-to-peel properties)
[0266] (1) Determination of 180° peel force of SUS when peeling adhesive tape at a peeling speed of 1500 mm / min
[0267] After cutting the obtained adhesive tape into pieces 25mm wide and 100mm long, the release PET film on one side (the side not being measured) was peeled off. A 50μm thick PET film (manufactured by Toyobo Co., Ltd., "E5200#50") was used as a backing to expose the adhesive layer, thus creating a test piece. The release PET film on the other side of the test piece (the side being measured) was peeled off, and a 2kg rubber roller was pressed against it once at a speed of 10mm / s at 23°C. This pressed the sample against an SUS plate (an SUS304 plate that had been cleaned with alcohol and then dry-rubbed), and allowed to stand at 23°C for 5 minutes to prepare the test sample. For the obtained test samples, according to JIS Z 0237:2009, a peel test was conducted using a tensile testing machine (Shimadzu Corporation, "Autograph AGS-X") at 23°C and a peel speed of 1500 mm / min, in which the adhesive tape was peeled from the SUS board in a 180° direction. The 180° peel force F1 (N / 25 mm) on the SUS when the adhesive tape was peeled at a peel speed of 1500 mm / min was measured.
[0268] (2) Determination of 180° peel force of SUS when peeling adhesive tape at a peeling speed of 300 mm / min
[0269] In the peel test, the adhesive tape was peeled from the SUS board at a speed of 300 mm / min. Otherwise, the 180° peel force F2 (N / 25 mm) on the SUS when the adhesive tape was peeled at a peel speed of 300 mm / min was measured by the same method as described above in "(1) Determination of 180° peel force on SUS when the adhesive tape was peeled at a peel speed of 1500 mm / min".
[0270] (3) Calculation of the rate of increase in adhesive force during high-speed peeling
[0271] Based on F1 and F2 obtained by the above method, the rate of increase in adhesive force during high-speed peeling is calculated using the following formula (II).
[0272] The rate of increase in adhesive force during high-speed peeling (%) = {(F1-F2) / F2} × 100 (II)
[0273] (4) Evaluation of high-speed peelability
[0274] Based on the calculated rate of increase in adhesive force during high-speed peeling, the high-speed peelability of the adhesive tape to the adhered object is evaluated according to the following criteria.
[0275] ◎: When the rate of increase in adhesive force during high-speed peeling is less than 10%.
[0276] ○: When the rate of increase in adhesive force during high-speed peeling exceeds 10% but is less than 20%.
[0277] △: When the rate of increase in adhesive force during high-speed peeling exceeds 20% but is less than 30%.
[0278] ×: Cases where the adhesive strength increase rate exceeds 30% during high-speed peeling.
[0279] [Table 1]
[0280]
[0281] [Table 2]
[0282]
[0283] [Table 3]
[0284]
[0285] [Table 4]
[0286]
[0287] Industrial availability
[0288] According to the present invention, an adhesive tape with excellent high-temperature retention and surface conformability can be provided.
[0289] Explanation of reference numerals in the attached figures
[0290] 1. Adhesive tape
[0291] 2 Aluminum Plate
[0292] 3. Polycarbonate resin board
[0293] 4-layered body
[0294] 5. Fixtures
[0295] 6 PET film
[0296] 7 SUS304 board
[0297] 8. Weight (1.0kg)
Claims
1. An adhesive tape, characterized in that, It has an adhesive layer formed using an adhesive composition. The adhesive composition contains a (meth)acrylic acid copolymer. The (meth)acrylic copolymer has structural units derived from alkyl (meth)acrylic esters. The adhesive layer, measured by dynamic viscoelasticity testing at a frequency of 1 Hz and a temperature range of -40°C to 200°C, has a shear storage modulus of over 15000 Pa at 80°C. The peak temperature of the loss tangent of the adhesive layer, measured by dynamic viscoelasticity testing at a frequency of 1 Hz and a temperature range of -40°C to 200°C, is within the range of -20°C to 0°C. The gel content of the adhesive layer is 10% by mass or more and 45% by mass or less.
2. The adhesive tape according to claim 1, wherein, The alkyl (meth)acrylate comprises alkyl (meth)acrylates having a glass transition temperature below -60°C when used to form homopolymers. The (meth)acrylic copolymer contains at least 50% by mass structural units derived from alkyl (meth)acrylic acid esters with a glass transition temperature below -60°C when the homopolymer is formed.
3. The adhesive tape according to claim 2, wherein, The alkyl (meth)acrylates with a glass transition temperature below -60°C when forming homopolymers include n-hexyl acrylate.
4. The adhesive tape according to claim 1, 2 or 3, wherein, The (meth)acrylic acid copolymer has structural units derived from monomers that do not have crosslinking functional groups and have a glass transition temperature of 0°C or higher when made into homopolymers.
5. The adhesive tape according to claim 4, wherein, In the (meth)acrylic acid copolymer, the structural units derived from monomers that do not have crosslinking functional groups and have a glass transition temperature of 0°C or higher when made into homopolymers are present in a proportion of 0.1% by mass or more and 70% by mass or less.
6. The adhesive tape according to claim 1, 2, 3, 4 or 5, wherein, The (meth)acrylic copolymer has structural units derived from n-heptyl (meth)acrylic acid.
7. The adhesive tape according to claim 1, 2, 3, 4 or 5, wherein, The (meth)acrylic copolymer does not have structural units derived from n-heptyl (meth)acrylate, or the content of the structural units derived from n-heptyl (meth)acrylate is less than 90% by mass.
8. The adhesive tape according to claim 1, 2, 3, 4, 5, 6 or 7, wherein, The (meth)acrylic acid copolymer also has structural units derived from monomers having non-crosslinked ether structures, wherein the monomers having non-crosslinked ether structures are selected from at least one of monomers having cyclic ether structures other than epoxy and oxetyl groups, and monomers having non-cyclic ether structures.
9. The adhesive tape according to claim 8, wherein, In the (meth)acrylic acid copolymer, the structural units derived from monomers having a non-crosslinked ether structure are present in an amount of 0.01% by mass or more and 50% by mass or less.
10. The adhesive tape according to claim 1, 2, 3, 4, 5, 6, 7, 8 or 9, wherein, The (meth)acrylic acid copolymers also have structural units derived from monomers with crosslinking functional groups.
11. The adhesive tape according to claim 10, wherein, The monomer having crosslinking functional groups comprises at least one selected from monomers containing carboxyl groups and monomers containing hydroxyl groups.
12. The adhesive tape according to claim 11, wherein, The monomer having cross-linking functional groups includes the hydroxyl-containing monomer.
13. The adhesive tape according to claim 11 or 12, wherein, The monomer having crosslinking functional groups includes the carboxyl-containing monomer, and the structural units derived from the carboxyl-containing monomer in the (meth)acrylic copolymer account for more than 5% by mass.
14. The adhesive tape according to claim 10, 11, 12 or 13, wherein, In the (meth)acrylic acid copolymer, the structural unit derived from the monomer having crosslinking functional groups is present in an amount of 0.01% by mass or more and less than 20% by mass.
15. The adhesive tape according to claim 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13 or 14, wherein, The weight-average molecular weight of the (meth)acrylic acid copolymer is above 800,000.
16. The adhesive tape according to claim 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14 or 15, wherein, The adhesive composition also contains a tackifier.
17. The adhesive tape according to claim 16, wherein, The tackifier comprises at least one selected from (meth)acrylic tackifiers, rosin ester tackifiers, and terpene tackifiers.
18. The adhesive tape according to claim 17, wherein, The tackifier comprises the rosin ester-based tackifier and the terpene-based tackifier.
19. The adhesive tape according to claim 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17 or 18, wherein, The adhesive composition also contains a crosslinking agent.
20. The adhesive tape according to claim 19, wherein, The crosslinking agent comprises at least one selected from isocyanate-based crosslinking agents and epoxy-based crosslinking agents.
21. The adhesive tape according to claim 20, wherein, The crosslinking agent comprises the isocyanate-based crosslinking agent and the epoxy-based crosslinking agent.
22. The adhesive tape according to claim 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20 or 21, wherein, The half-width of the peak of the loss tangent of the adhesive layer, measured by dynamic viscoelasticity determination at a frequency of 1 Hz and a temperature range of -40°C to 200°C, is below 44°C.
23. The adhesive tape according to claim 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21 or 22, having a substrate layer and having the adhesive layer on at least one side of the substrate layer.
24. The adhesive tape according to any one of claims 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22 or 23, used for securing electronic device components or vehicle-mounted components.
Citation Information
Patent Citations
Thermally conductive adhesive tape, article and image display device
JP2015021067A
Base material for heat-resistant adhesive tape and heat-resistant adhesive tape composed of the same
JP2015052050A
Double-sided adhesive sheet
JP2015120876A