Coating film formation method, printed wiring board manufacturing method and coating film formation system

By using inkjet printing to repeatedly expose the printed wiring substrate to form a photocurable coating, the problems of gaps between the coating and the substrate and ink seepage are solved, achieving high adhesion and tightness of the coating.

CN123126030APending Publication Date: 2026-11-17KONICA MINOLTA INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202580028669.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-17
Filing Date
2025-03-04
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies often encounter gaps between the coating and the substrate and ink leakage when forming printed wiring substrate coatings with a thickness of 50μm or more, which are particularly difficult to suppress effectively during multiple exposures.

Method used

A photocurable ink is applied to a printed wiring substrate using an inkjet printing method. Multiple exposures are performed, each with a thickness of 6–18 μm, using an exposure dose of 200–700 mJ/cm² and an exposure time of 40 × 10⁻³–119 × 10⁻³ seconds, to form a photocurable coating. The amount of light in each exposure is reduced to suppress coating shrinkage and ink exudation.

Benefits of technology

It effectively suppresses the formation of voids between the coating and the substrate and ink seepage, improves the adhesion and bonding of the coating, and reduces voids and seepage width during coating formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The coating formation method of the present invention is a coating formation method for forming a coating on a printed wiring substrate, comprising: a pre-curing coating formation step, wherein a photocurable ink is applied to a printed wiring substrate having a substrate and a conductor disposed on the substrate with a thickness of 50 μm or more by inkjet printing to form a pre-curing coating by covering the conductor; and a photocurable coating formation step, wherein the pre-curing coating is subjected to multiple exposures, each time for a thickness of 6 to 18 μm, to cure the pre-curing coating and form a photocurable coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a coating film forming method, a printed wiring board manufacturing method, and a coating film forming system. More specifically, it relates to a coating film forming method, a printed wiring board manufacturing method, and a coating film forming system capable of suppressing ink seepage and suppressing the formation of voids between the coating film and the substrate. Background Technology

[0002] Previously, photolithography or screen printing methods were used to form etching resists, solder resists, and markings for printed circuit boards (PCBs). One method for applying inkjet technology to the manufacture of PCBs is, for example, coating a copper-clad laminate for PCBs with inkjet ink containing a photopolymerizable compound (see, for example, Patent Documents 1-3). Furthermore, methods for forming solder resists using inkjet printers have been proposed. Compared to photolithography, which requires photomasks, and screen printing, which requires screen printing plates for resist inks or marking inks, inkjet technology can significantly reduce the number of processes and time required. In addition, inkjet technology can reduce consumables such as developers, various inks, and cleaning solvents, and since it also reduces wastewater, environmental cleanliness is expected.

[0003] Prior art literature

[0004] Patent documents

[0005] Patent Document 1: Japanese Patent Application Publication No. 2015-89540

[0006] Patent Document 2: Japanese Patent Application Publication No. 2022-63284

[0007] Patent Document 3: International Publication No. 2022 / 85183 Summary of the Invention

[0008] The technical problem that the invention aims to solve

[0009] When forming a solder resist film on the wiring of a printed wiring substrate, the thicker the wiring, the thicker the coating (film thickness) needs to be to protect the wiring. When the wiring thickness on the substrate is thin, sequential exposure is performed. Here, sequential exposure means that after partially coating the ink, it is exposed immediately, and the partial coating and exposure of the ink are repeated. However, when the wiring and the coating become thicker, sequential exposure has the problem of creating gaps between the coating and the substrate. Therefore, firstly, ink is applied to cover all or most of the wiring of the printed wiring substrate to form a pre-curing coating (hereinafter also referred to as "pre-curing coating"). Then, the pre-curing coating is exposed multiple times at time intervals to form a coating (hereinafter also referred to as "segmented exposure"). Thus, the generation of the above-mentioned gaps can be suppressed up to a certain wiring thickness, but when the wiring thickness reaches 50 μm or more, it is difficult to suppress the generation of the above-mentioned gaps. In this respect, further improvements are required for the inventions described in Patent Documents 1 to 3. Furthermore, if the illuminance is reduced during the aforementioned segmented exposure, bleed-out may occur. Additionally, while the invention described in Patent Document 2 involves multiple exposures, it also applies multiple layers of ink to create multiple ink layers, aiming to improve the adhesion of the cured film by multiplying the ink.

[0010] The present invention was made in view of the above-mentioned situation. The technical problem to be solved by the present invention is to provide a coating film forming method, a printed wiring board manufacturing method, and a coating film forming system that can suppress the generation of voids between the coating film and the substrate and suppress ink leakage during coating film formation.

[0011] Technical means to solve the problem

[0012] To solve the aforementioned technical problems, the inventors investigated the causes of these problems. As a result, the inventors discovered that by repeatedly exposing the photocurable ink to the light with a specific amount of light and increasing the number of exposures, the formation of voids between the coating and the substrate can be suppressed. Furthermore, the inventors discovered that by forming a coating by repeatedly exposing the photocurable ink to the light with a specific amount of light while avoiding excessively long total exposure time, the exudation of the photocurable ink can be suppressed, thus completing the present invention. In other words, the aforementioned technical problems related to the present invention are solved by the following means.

[0013] 1. A coating forming method for forming a coating film on a printed wiring substrate, comprising a pre-curing coating forming step of forming a pre-curing coating film by applying a photocurable ink to the printed wiring substrate having a substrate and a conductor disposed on the substrate with a thickness of 50 μm or more by inkjet printing, thereby covering the conductor; and a photocurable coating forming step of subjecting the pre-curing coating film to multiple exposures, each time curing to a thickness of 6 to 18 μm, to cure the pre-curing coating film and form a photocurable coating film, wherein the coating forming method comprises the above steps.

[0014] 2. The coating film formation method as described in 1 above, wherein the exposure is an irradiation light intensity of 200–700 mJ / cm. 2 The exposure.

[0015] 3. The coating formation method as described in 1 or 2 above, wherein the exposure time for each exposure is 40 × 10⁻⁶. -3 ~119×10 -3 Second.

[0016] 4. The coating film forming method as described in 1 or 2 above, wherein the photocurable ink contains a photopolymerizable compound with a molecular weight of 200 to 600.

[0017] 5. The coating formation method as described in 1 or 2 above, wherein the thickness of the conductor is 60 to 150 μm.

[0018] 6. The coating film forming method as described in 1 or 2 above, wherein the coefficient of linear expansion of the photocurable ink is 20 to 250 ppm / K.

[0019] 7. The coating film formation method as described in 1 or 2 above, wherein the coating film has a retention rate of 90% or more as determined by the corresponding method of adhesion testing according to JIS K5600.

[0020] 8. The coating film formation method as described in 1 or 2 above, wherein the penetration width from the boundary line between the coating film and the substrate toward the substrate side is less than 20 μm.

[0021] 9. A method for manufacturing a printed wiring board, wherein the printed wiring board is manufactured using the coating formation method described in 1 or 2 above.

[0022] 10. A coating forming system comprising: an inkjet head for coating a printed wiring substrate with the photocurable ink to form the pre-curing coating; and a curing section for curing the pre-curing coating coated on the printed wiring substrate using active energy rays; the coating forming system being used in the coating forming method described in 1 or 2 above.

[0023] Invention Effects

[0024] The coating film forming method of the present invention can suppress the formation of voids between the coating film and the substrate, and can suppress ink leakage during coating film formation. Furthermore, the printed wiring board manufacturing method of the present invention can suppress the formation of voids between the coating film and the substrate, and can suppress ink leakage during coating film formation. Additionally, the coating film forming system of the present invention can be used in the coating film forming method of the present invention, thereby suppressing the formation of voids between the coating film and the substrate during coating film formation, and suppressing ink leakage during coating film formation.

[0025] Although the mechanism of action or effect of the present invention is not clear, it is speculated as follows.

[0026] When a coating is formed on a printed wiring substrate, gaps arise near the wiring on the substrate between the coating and the substrate, which has conductors with a thickness of 50 μm or more. These gaps between the coating and the substrate are sometimes referred to as voids. Since no voids are generated even when the substrate is heated before wiring is applied, it is presumed that bubbles generated on the substrate are not the cause of voids. Furthermore, since voids are generated even when the ink is degassed before coating, it is presumed that bubbles generated by the ink are not the cause of voids. Therefore, it is presumed that the voids are not caused by bubbles generated by the substrate or ink, which are components of the printed wiring substrate. Therefore, it is presumed that a phenomenon hindering the coating from adhering to the substrate surface occurs during coating formation, which is one cause of voids. Specifically, during the curing of the pre-curing coating, the pre-curing coating shrinks while curing to form a coating. It is presumed that due to the shrinkage of this pre-curing coating, the coating peels off from the substrate surface, creating voids. Furthermore, it is presumed that one reason for the pre-curing coating peeling off from the substrate surface is the large shrinkage that occurs in a short period of time. In contrast, the coating formation method of the present invention involves subjecting the coating to multiple exposures, each for a thickness of 6 to 18 μm, before curing. Therefore, the coating formation method of the present invention reduces the exposure amount (also known as "irradiation light amount") during each exposure, thereby reducing shrinkage during each exposure and preventing significant shrinkage in a short period. Therefore, it is presumed that the coating formation method of the present invention can suppress the peeling of the coating from the substrate surface.

[0027] Furthermore, in order to form a coating film by repeatedly exposing the pre-curing coating to cure it, the exposure amount per exposure needs to be reduced. If the exposure amount per exposure is reduced and the pre-curing coating film is exposed multiple times over a longer period, ink seepage occurs around the coating film. It is presumed that this seepage is caused by photopolymerizable compounds (monomers) or the like that seeping outwards during the curing of the pre-curing coating film. In contrast, the coating film forming method of the present invention exposes the pre-curing coating film multiple times, each time curing a thickness of 6 to 18 μm. Therefore, it is possible to cure the pre-curing coating film while avoiding excessively long curing times. As a result, it is presumed that the polymerization of photopolymerizable compounds or the like (curing of the pre-curing coating film) can be promoted while suppressing the generation of seepage. That is, the coating film forming method of the present invention can promote the polymerization of photopolymerizable compounds (curing of the pre-curing coating film) at a certain or higher rate. As a result, it is presumed that the seepage of photopolymerizable compounds or the like can be prevented, and seepage is suppressed. Attached Figure Description

[0028] Figure 1 It is a plan view schematically representing a portion of the state of a coating film formed on a printed wiring substrate before curing.

[0029] Figure 2 yes Figure 1 A-A sectional view.

[0030] Figure 3 This is a flowchart illustrating an example of a coating formation method according to this embodiment.

[0031] Figure 4A This is a schematic diagram illustrating the process of forming a coating using the coating forming system of this embodiment.

[0032] Figure 4B This is a schematic diagram illustrating the process of forming a coating using the coating forming system of this embodiment. Detailed Implementation

[0033] One embodiment of the coating formation method of the present invention is characterized as follows: A photocurable ink is applied to a printed wiring substrate by inkjet printing to form a pre-curing coating film covering the conductor. The pre-curing coating film is then subjected to multiple exposures, each time curing to a thickness of 6 to 18 μm. This process cures the pre-curing coating film to form a photocurable coating film. The printed wiring substrate has a substrate and a conductor disposed on the substrate with a thickness of 50 μm or more. Furthermore, "photocurable ink" is sometimes simply referred to as "ink." This feature is a common or corresponding technical feature of the embodiments described below.

[0034] In this embodiment, the preferred method for forming a coating film is to use an exposure (light irradiation) of 200–700 mJ / cm² per exposure. 2This allows for multiple exposures, each curing a thickness of 6–18 μm, suppressing the formation of voids and ink seepage.

[0035] In this embodiment, the preferred exposure time for the coating formation method is 40 × 10 seconds. -3 ~119×10 -3 Seconds. This allows for multiple exposures, each curing a thickness of 6–18 μm, suppressing the formation of voids and ink seepage.

[0036] The coating film formation method of this embodiment preferably uses a photopolymerizable ink containing a photopolymerizable compound with a molecular weight of 200 to 600, and more preferably contains a photopolymerizable compound with a molecular weight of 200 to 350. Therefore, the photopolymerizable ink exhibits excellent ejection stability when ejected from the inkjet head.

[0037] In this embodiment, the coating film formation method preferably uses a conductor thickness of 60–150 μm. This coating film formation method, even for printed wiring substrates with thick conductors, can suppress the formation of voids between the coating film and the substrate, and can suppress ink leakage during coating film formation.

[0038] The coating film formation method of this embodiment preferably uses a photocurable ink with a coefficient of linear expansion of 20 to 250 ppm / K. This reduces the shrinkage during the curing process of the pre-cured coating film. Therefore, it is possible to suppress the formation of voids during coating film formation. Here, the coefficient of linear expansion of the photocurable ink refers to the coefficient of linear expansion of the pre-cured coating film and the cured photocurable coating film.

[0039] The coating film formation method of this embodiment preferably achieves a coating film retention rate of 90% or higher after multiple exposures in the adhesion test. The adhesion test is conducted according to the corresponding method of adhesion testing in JIS K5600. This demonstrates that the formation of voids is suppressed during coating film formation. The adhesion test is conducted according to "JIS K5600-5-6 Part 5-Section 6: Adhesion (Cross-cut Test)".

[0040] The coating film formation method of this embodiment preferably has an ink penetration width of 20 μm or less. This penetration width is the penetration width from the boundary line between the coating film and the substrate towards the substrate side after multiple exposures. Therefore, it can be seen that ink penetration is suppressed during coating film formation.

[0041] One embodiment of the printed wiring board manufacturing method of the present invention is characterized by using the coating film forming method of the present invention to manufacture the printed wiring board. This suppresses the formation of voids between the coating film and the substrate, and also suppresses ink leakage during coating film formation. Furthermore, in this specification, a distinction is made between a "substrate with conductors disposed on" without a coating film and a "substrate with conductors disposed on" with a coating film. Specifically, the "substrate with conductors disposed on" without a coating film is referred to as a printed wiring board, and the "substrate with conductors disposed on" with a coating film is referred to as a printed wiring board.

[0042] One embodiment of the coating formation system of the present invention includes an inkjet head that coats a photocurable ink onto a printed wiring substrate to form a pre-curing coating. Furthermore, the coating formation system of this embodiment includes a curing section that uses active energy rays to cure the pre-curing coating coated on the printed wiring substrate. This coating formation system is used in the coating formation method of this embodiment. Therefore, the generation of voids between the coating and the substrate can be suppressed. Furthermore, ink leakage during coating formation can be suppressed.

[0043] Hereinafter, the present invention, its constituent elements, and the forms and methods for carrying out the present invention will be described in detail with reference to the accompanying drawings. In this application, "~" is used to include the numerical values ​​described before and after it as lower and upper limits.

[0044] 1. Coating film formation method

[0045] An embodiment of the coating film formation method of the present invention will be described. For example... Figure 3 As shown, the coating film forming method of this embodiment includes a pre-curing coating film forming step S01 and a photocuring coating film forming step S02. The coating film forming method of this embodiment may also include a thermocuring coating film forming step S03.

[0046] like Figures 1-3 As shown, in this embodiment, the coating formation method applies a photocurable ink to a printed wiring substrate 3 to form a pre-curing coating 4 covering the conductor. This is the pre-curing coating formation step S01. Next, the pre-curing coating 4 is subjected to multiple exposures, each time curing a thickness of 6-18 μm, to cure the pre-curing coating 4 and form a photocurable coating. This is the photocurable coating formation step S02. Furthermore, the printed wiring substrate 3 is a printed wiring substrate 3 having a substrate 1 and a conductor 2 with a thickness of 50 μm or more disposed on the substrate 1. Additionally, when applying the photocurable ink to the printed wiring substrate 3, the photocurable ink is applied by inkjet printing. The coating formation method of this embodiment can also further thermally cure the photocurable coating to form a thermally curable coating. This is the thermally curable coating formation step S03.

[0047] As described above, the coating formation method of this embodiment exposes the pre-curing coating 4 multiple times, each time curing a thickness of 6 to 18 μm. Therefore, according to the coating formation method of this embodiment, the generation of voids between the coating and the substrate can be suppressed. Furthermore, according to the coating formation method of this embodiment, ink seepage during coating formation can be suppressed. Here, "curing a thickness of 6 to 18 μm each time" means that the pre-curing coating is cured to a thickness of only 6 to 18 μm along the thickness direction. In addition, "curing the pre-curing coating" means that the pre-curing coating, after exposure, reaches a state where color transfer on the white paper cannot be visually confirmed after pressing and wiping with white paper.

[0048] The coating formed by the coating formation method of this embodiment is preferably a solder resist film. In this specification, "coating" refers to the film ultimately formed on the printed circuit board. When the final film is a photocurable coating obtained by photocuring a pre-cured coating, this photocurable coating is formed by the coating formation method of this embodiment. Furthermore, when the final film is a thermocurable coating obtained by further thermally curing a photocurable coating, this thermocurable coating is formed by the coating formation method of this embodiment.

[0049] 1-1. Coating film formation process before curing

[0050] The pre-curing coating formation process involves applying a photocurable ink to a printed wiring substrate to cover the conductors and form a pre-curing coating. Furthermore, when applying the photocurable ink to the printed wiring substrate, the ink is applied using an inkjet printing method.

[0051] 1-1-1. Inkjet method

[0052] (Ejection method)

[0053] In this embodiment, the inkjet method involves ejecting ink from an inkjet head and applying the ink to the surface of a printed wiring substrate. Furthermore, the coating formation method of this embodiment preferably uses the inkjet method to apply a photocurable ink, such as solder resist inkjet ink, to a pattern on the printed wiring substrate. The ejection method from the inkjet head can be either on-demand or continuous. On-demand inkjet heads can be any of electromechanical conversion or electrothermal conversion methods. Examples of electromechanical conversion methods include single-cavity, dual-cavity, bent-plate, piston, shear-mode, and shared-wall types. Examples of electrothermal conversion methods include thermal inkjet and bubble inkjet ("bubble inkjet" is a registered trademark of Canon Corporation).

[0054] (Ejection volume)

[0055] From the viewpoint of improving the pattern forming speed and forming a finer pattern, the amount of ink droplets ejected is preferably 3.0 pL or more and 9.0 pL or less.

[0056] (Ejection temperature)

[0057] From the viewpoint of further improving the ejection performance of the inkjet head, it is preferable to set the ink temperature when the ink is filled into the inkjet head to 40°C or higher and 100°C or lower. More preferably, the temperature is set to 40°C or higher and 90°C or lower. In particular, when the ink contains a gelling agent, the ink droplets are ejected from the inkjet head in a state of gelation due to heating. Therefore, it is preferable to set the ink temperature when the ink is filled into the inkjet head to be 10°C or higher than the gelation temperature of the ink and 30°C or lower. When the temperature of the photocurable ink in the inkjet head is 10°C or higher than the gelation temperature, the reduction in ejection performance due to gelation of the ink in the inkjet head or on the nozzle surface is less likely to occur. On the other hand, when the temperature of the ink in the inkjet head is 30°C or lower than the gelation temperature, the degradation of components due to high temperature is less likely to occur.

[0058] There are no particular limitations on the method of heating the ink. For example, at least one of the ink supply system, such as the ink tank that makes up the head bracket, the supply pipe and the ink tank in front of the head, the piping with a filter, and the piezoelectric head, can be heated by a panel heater, a strip heater, or insulating water.

[0059] 1-1-2. Printed Wiring Substrate

[0060] The printed wiring substrate has a substrate and a conductor with a thickness of 50 μm or more disposed on the substrate. Furthermore, in this specification, as described above, a substrate without a coating is referred to as a "printed wiring substrate," while a substrate with a coating is referred to as a "printed wiring board."

[0061] 1-1-2(1). substrate

[0062] In the coating formation method of this embodiment, the printed wiring substrate to which ink is applied is a substrate with conductors disposed on its surface. As the conductor, a conductive film such as copper foil is preferably disposed on the substrate. The substrate includes rigid substrates and flexible substrates. Examples of rigid substrates include paper phenolic substrates, paper epoxy boards, glass epoxy boards, glass polyimide substrates, Teflon (registered trademark) substrates, PPO substrates, and composite substrate epoxy boards. Examples of materials for flexible substrates include PET films and polyimide films.

[0063] There are no particular limitations on the thickness and size of the substrate.

[0064] 1-1-2(2). Conductor

[0065] In the coating formation method of this embodiment, the conductor thickness is 50 μm or more. The coating formation method of this embodiment exhibits better performance when the conductor thickness is 60–150 μm. Here, "performance" refers to the effect of "suppressing the generation of voids and leakage." When the conductor thickness is less than 50 μm, the generation of voids or leakage during coating formation on the printed wiring substrate is not significant. Therefore, even without using the coating formation method of this embodiment, a coating can be formed while reducing the generation of voids or leakage. In contrast, when the conductor thickness reaches 50 μm or more, the generation of voids or leakage during coating formation becomes significant. At this time, the "effect of suppressing the generation of voids and leakage" of the coating formation method of this embodiment is significantly achieved. Furthermore, when the conductor thickness reaches 60 μm or more, the generation of voids or leakage during coating formation becomes even more significant. Even with such thick conductors, the "effect of suppressing the generation of voids and leakage" of the coating formation method of this embodiment is significantly achieved.

[0066] The printed wiring substrate preferably forms wiring on the substrate surface through the conductor, and a circuit pattern is formed on the substrate surface through the wiring through the conductor. Furthermore, the conductor is preferably made of copper foil, and the wiring formed by the conductor is copper wiring. The width of the wiring formed by the conductor is not particularly limited and is determined according to the characteristics of the printed wiring board, etc. The width of the wiring is preferably in the range of 30 to 100 μm, more preferably in the range of 50 to 70 μm. When the width of the wiring is within this range, the effect of "suppressing the generation of voids and exudation" of the coating formation method of this embodiment is significantly achieved.

[0067] 1-1-3. Photocurable inks

[0068] In the coating formation method of this embodiment, a photocurable ink is applied to the surface of a printed wiring substrate to form a pre-curing coating film by covering the conductor. Furthermore, the photocurable ink used to form the pre-curing coating film is exposed to specific light multiple times to form a photocurable coating film.

[0069] 1-1-3(1) Photopolymerizable compounds

[0070] Photopolymerizable inks preferably contain photopolymerizable compounds. These compounds are polymerized and cross-linked by irradiation with active energy rays. Alternatively, the photopolymerizable compound may be a compound that further polymerizes and cross-links after being heated following irradiation with active energy rays. Photopolymerizable inks may contain only one type of photopolymerizable compound, or they may contain two or more types.

[0071] The molecular weight of the photopolymerizable compound is preferably 200 to 600. By having a molecular weight of 200 or higher, the liquid component of the photocurable ink is less prone to volatiles. This further suppresses the drying of the photocurable ink adhering to the nozzle of the inkjet head and the fixation of non-volatile components such as pigments contained in the photocurable ink onto the nozzle, thus preventing a decrease in ejection stability. By having a molecular weight of 600 or lower, excessively high viscosity of the photocurable ink can be prevented, thus suppressing a decrease in ejection stability. From this perspective, the molecular weight is more preferably 250 to 500.

[0072] Polymerizable compounds can be either cationic or radical polymerizable, but are preferably radical polymerizable. Radical polymerizable compounds are compounds with olefinic unsaturated bonds that can polymerize on free radicals.

[0073] As photopolymerizable compounds, specifically, unsaturated carboxylic acid esters can be cited. Preferably, (meth)acrylate compounds (hereinafter also simply referred to as (meth)acrylates) are unsaturated carboxylic acid esters. Furthermore, in this specification, "(meth)acrylate" refers to acrylates or methacrylates.

[0074] Examples of (meth)acrylates include: isopentyl (meth)acrylate, stearyl (meth)acrylate, lauryl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, isomyrmyryl (meth)acrylate, isostearyl (meth)acrylate, 2-ethylhexyl-diethylene (meth)acrylate, butoxyethyl (meth)acrylate, ethoxydiethylene (meth)acrylate, methoxydiethylene (meth)acrylate, methoxy... Monofunctional acrylates such as polyethylene glycol (meth)acrylate, methoxypropylene glycol (meth)acrylate, phenoxyethyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, isobornyl (meth)acrylate, and t-butylcyclohexyl (meth)acrylate; as well as triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, and polypropylene glycol di(meth)acrylate. Dimethacrylates of alcohols, 1,4-butanediol dimethacrylate, 1,6-hexanediol dimethacrylate, 1,9-nonanediol dimethacrylate, neopentyl glycol dimethacrylate, dimethyl tricyclodecane dimethacrylate, PO adduct of bisphenol A dimethacrylate, neopentyl glycol dimethacrylate of hydroxypentanoic acid, polytetramethylene glycol dimethacrylate, polyethylene glycol diacrylate, tripropylene glycol dipropylene Difunctional acrylates include esters such as tricyclodecanediethanol diacrylate and propoxylated (3)neopentyl glycol diacrylate; and polyfunctional acrylates with three or more functions such as trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, glycerol propoxy tri(meth)acrylate, and pentaerythritol ethoxy tetra(meth)acrylate. Examples of (meth)acrylates also include o-phenylphenol EO acrylate.

[0075] From the viewpoint of photosensitivity, stearyl methacrylate, lauryl methacrylate, isostearyl methacrylate, ethoxydiethylene methacrylate, isobornyl methacrylate, tetraethylene glycol dimethacrylate, and glyceryl propoxytrimethacrylate are preferred. Methacrylates can also be modified. Examples of modified methacrylates include: ethylene oxide-modified methacrylates containing ethylene oxide-modified trimethylolpropane trimethacrylate, ethylene oxide-modified pentaerythritol tetraacrylate, and 4EO-modified hexanediol diacrylate; caprolactone-modified methacrylates containing caprolactone-modified trimethylolpropane trimethacrylate; and caprolactam-modified methacrylates containing caprolactam-modified dipentaerythritol hexamethacrylate and nonylphenol 2PO-modified acrylate.

[0076] (Meth)acrylates can also be polymerizable oligomers. Examples of (meth)acrylates that are polymerizable oligomers include epoxy (meth)acrylate oligomers, aliphatic urethane (meth)acrylate oligomers, aromatic urethane (meth)acrylate oligomers, polyester (meth)acrylate oligomers, and linear (meth)acrylate oligomers.

[0077] 1-1-3(2) Photopolymerization initiator

[0078] In the coating film formation method of this embodiment, the photocurable ink preferably contains a photopolymerization initiator. The photopolymerization initiator is a compound that initiates the polymerization and crosslinking of the photopolymerizable compound by irradiation with active energy rays.

[0079] The photocurable ink can be cured by free radical polymerization. In the coating formation method of this embodiment, a free radical polymerization initiator is preferably used as the photopolymerization initiator when curing the photocurable ink. Hereinafter, "free radical polymerization initiator" will sometimes be simply referred to as "initiator". The photocurable ink may contain only one photopolymerization initiator or may contain two or more photopolymerization initiators.

[0080] Examples of free radical polymerization initiators include α-cleavage type free radical polymerization initiators and hydrogen abstraction type free radical polymerization initiators. α-cleavage type free radical polymerization initiators are also known as Norrish type I polymerization initiators. Hydrogen abstraction type free radical polymerization initiators are also known as Norrish type II polymerization initiators.

[0081] The content of the α-pyrolysis type free radical polymerization initiator is preferably in the range of 0.3% to 6% by mass relative to the total mass of the photocurable ink. Furthermore, the content of the hydrogen abstraction type free radical polymerization initiator is preferably in the range of 0.5% to 10% by mass relative to the total mass of the photocurable ink.

[0082] α-Cleavage radical polymerization initiators are initiators that cleave after photoinitiation, directly releasing initiating radicals. Conversely, hydrogen-abstracting radical polymerization initiators are photopolymerization initiators activated by active energy rays (e.g., ultraviolet light) and generate radicals by abstracting hydrogen from a second compound. In this case, the second compound becomes the actual initiating radical. This second compound is referred to as a polymerization synergist or co-initiator. In the coating formation method of this embodiment, both the α-cleavage radical polymerization initiator and the hydrogen-abstracting radical polymerization initiator can be used alone or in combination.

[0083] Examples of α-cleavage free radical polymerization initiators include acetophenone initiators, benzoin initiators, acylphosphine oxide initiators, biphenyl ester and methyl phenyl acetal ester.

[0084] Examples of acetophenone-based initiators include diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropane-1-one, biphenyl dimethyl ketal, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropane-1-one, 4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)one, 1-hydroxycyclohexylphenylone, 2-methyl-2-morpholino(4-thiomethylphenyl)propane-1-one, and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone.

[0085] Examples of benzoin-based initiators include benzoin, benzoin methyl ether, and benzoin isopropyl ether.

[0086] Examples of acylphosphine oxide initiators include 2,4,6-trimethylbenzoin diphenylphosphine oxide and phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide.

[0087] Examples of hydrogen-abstracting free radical initiators include benzophenone-based initiators, thioxanthone-based initiators, aminobenzophenone-based initiators, 10-butyl-2-chloroacridone, 2-ethylanthraquinone, 9,10-phenanthrenequinone, and camphorquinone.

[0088] Examples of benzophenone-based initiators include benzophenone, methyl o-benzoylbenzoate-4-phenylbenzophenone, 4,4'-dichlorobenzophenone, hydroxybenzophenone, 4-benzoyl-4'-methyl diphenyl sulfide, acrylated benzophenone, 3,3',4,4'-tetra(t-butylperoxycarbonyl)benzophenone, and 3,3'-dimethyl-4-methoxybenzophenone.

[0089] Examples of thioxanthone-based initiators include 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, and 2,4-dichlorothioxanthone.

[0090] Examples of aminobenzophenone-based initiators include milchone and 4,4'-diethylaminobenzophenone.

[0091] 1-1-3 (4) Other components

[0092] [A. Polymerization inhibitor]

[0093] The photocurable ink preferably further contains a polymerization inhibitor. By containing a polymerization inhibitor, the adhesion between the multiple curable compounds can be reduced. In this specification, the term "polymerization inhibitor" includes all compounds added to inhibit polymerization reactions during the preparation of the ink containing polymerizable compounds or during storage after preparation.

[0094] In the photocurable ink of the coating formation method of this embodiment, various conventionally known polymerization inhibitors can be used. From the viewpoint of performance, at least one of the following is preferred as a polymerization inhibitor: an N-oxygen-based polymerization inhibitor, a phenolic polymerization inhibitor containing 0.1-butyl, and a polymerization inhibitor having two or more aromatic rings. Furthermore, from the viewpoint of adhesion to the printed wiring board, an N-oxygen-based polymerization inhibitor is even more preferred.

[0095] The content of the polymerization inhibitor is preferably in the range of 0.05 to 0.5% by mass relative to the total mass of the ink.

[0096] [A-1. N-oxygen-based polymerization inhibitor]

[0097] Examples of N-oxygen-based polymerization inhibitors include 4-hydroxy-2,2,6,6-tetramethylpiperidine-N-oxy (TEMPO), 4-hydroxy-2,2,6,6-tetramethylpiperidine-N-oxy, 4-oxo-2,2,6,6-tetramethylpiperidine-N-oxy, 4-methoxy-2,2,6,6-tetramethylpiperidine-N-oxy, 4-acetoxy-2,2,6,6-tetramethylpiperidine-N-oxy, and Irgastab (registered trademark) UV10 (manufactured by BASF).

[0098] [A-2. Phenolic polymerization inhibitor]

[0099] Examples of phenolic polymerization inhibitors include 2,6-di-tert-butylphenol, 2,4-di-tert-butylphenol, 2-tert-butyl-4,6-dimethylphenol, 2,6-di-tert-butyl-4-methylphenol, 2,4,6-tri-tert-butylphenol, 2,6-di-t-butyl-p-cresol (butylated hydroxytoluene: BHT), 4-methoxyphenol, and 2-methoxy-4-methylphenol.

[0100] [A-3. Quinone polymerization inhibitor]

[0101] Examples of quinone-based polymerization inhibitors include hydroquinone, methoxyhydroquinone, benzoquinone, 1,4-naphthoquinone, and p-tert-butylcatechol.

[0102] [A-4. Amine polymerization inhibitor]

[0103] Examples of amine polymerization inhibitors include alkylated diphenylamine, N,N'-diphenyl-p-phenylenediamine, and phenothiazine.

[0104] [A-5. Other polymerization inhibitors]

[0105] Examples of other polymerization inhibitors include copper dithiocarbamate-based inhibitors such as copper dimethyl dithiocarbamate, copper diethyl dithiocarbamate, and copper dibutyl dithiocarbamate.

[0106] These may contain only one type or two or more. Among them, N-oxygen-based and quinone-based polymerization inhibitors are preferred, such as 4-hydroxy-2,2,6,6-tetramethylpiperidin-N-oxy (TEMPO), 2,6-di-t-butyl-p-cresol (butylated hydroxytoluene: BHT), and 2,4-di-tert-butylphenol. As polymerization inhibitors having two or more aromatic rings, naphthoquinone is preferred.

[0107] [B. Gelling agent]

[0108] The photocurable ink preferably contains a gelling agent. By containing a gelling agent, the ink on the recording medium can be temporarily fixed in a gel state, thus inhibiting the wetting and diffusion of the ink.

[0109] The gelling agent preferably crystallizes at a temperature below the gelation temperature of the ink. The "gelation temperature" refers to the temperature at which the gelling agent undergoes a phase transition from sol to gel, and the viscosity of the composition changes drastically, when the heated and sol- or liquefied composition is cooled. Specifically, the gelation temperature of the composition can be determined by cooling the sol- or liquefied composition while measuring its viscosity using a viscoelasticity measuring device, and the temperature at which the viscosity rises sharply can be taken as the gelation temperature of the composition. An example of a viscoelasticity measuring device is the MCR300 (manufactured by Anton Paar).

[0110] When the gelling agent crystallizes in the ink, a so-called house of cards structure is formed. The house of cards structure is a structure in which a photopolymeric compound is encapsulated within a three-dimensional space formed by a plate-like crystallized gelling agent. For this house of cards structure to form, it is preferable that the photopolymeric compound dissolved in the ink is compatible with the gelling agent.

[0111] Examples of gelling agents suitable for forming the structure of a house of cards include aliphatic ketones, aliphatic esters, petroleum-based waxes, plant-based waxes, animal-based waxes, mineral-based waxes, cured castor oil, modified waxes, higher fatty acids, higher alcohols, hydroxystearic acid, fatty acid amides including N-substituted aliphatic acid amides and special aliphatic acid amides, higher amines, esters of sucrose fatty acids, synthetic waxes, dibenzylidene sorbitol, dimer acids, and dimer glycols.

[0112] From the perspective of improving adhesion, aliphatic ketones, aliphatic esters, higher fatty acids, and higher alcohols with hydrocarbon groups having 9 to 25 carbon atoms are preferred. The gelling agent may contain only one type or two or more.

[0113] [B-1. Aliphatic ketones]

[0114] Examples of aliphatic ketones include ditetracosyl ketone, dibenzyl ketone, distearyl ketone, dieicosyl ketone, dipalmityl ketone, dilauryl ketone, dimyristyl ketone, myristylpalmityl ketone, and palmitylstearyl ketone.

[0115] [B-2. Aliphatic esters]

[0116] Examples of aliphatic esters include fatty acid esters of monohydric alcohols such as behenyl behenate, eicosyl eicosanoate, and palmitic acid oleyl ester; and fatty acid esters of polyhydric alcohols such as glycerol fatty acid esters, sorbitan fatty acid esters, propylene glycol fatty acid esters, ethylene glycol fatty acid esters, and polyoxyethylene fatty acid esters.

[0117] Examples of commercially available aliphatic esters include the EMLEX (registered trademark) series manufactured by Nippon Emulsion Co., Ltd., the Likamar (registered trademark) series manufactured by Riken Vitamin Co., Ltd., and the Boehm (registered trademark) series.

[0118] [B-3, higher fatty acids]

[0119] Examples of higher fatty acids include behenic acid, arachidic acid, stearic acid, palmitic acid, myristic acid, lauric acid, oleic acid, and erucic acid.

[0120] [B-4. Higher alcohols]

[0121] Examples of higher alcohols include stearyl alcohol and behenol.

[0122] [B-5. Suitable gelling agent]

[0123] In the coating film forming method of this embodiment, the gelling agent is particularly preferably an aliphatic ketone represented by the following general formula (G1) or an aliphatic ester represented by the following general formula (G2).

[0124] General formula (G1): R1-CO-R2

[0125] In the above general formula (G1), R1 and R2 independently represent alkyl groups with 12 to 26 carbon atoms, including straight-chain portions and possibly branched portions. R1 and R2 may be the same or different.

[0126] General formula (G2): R3-COO-R4

[0127] In the above general formula (G2), R3 and R4 independently represent alkyl groups with 12 to 26 carbon atoms, including straight-chain portions and possibly branched alkyl groups. R3 and R4 may be the same or different.

[0128] In general formulas (G1) and (G2), by making the number of carbon atoms in the straight-chain or branched hydrocarbon groups 12 or more, the crystallinity of the aliphatic ketone represented by general formula (G1) or the aliphatic ester represented by general formula (G2) is further improved, and more sufficient space is generated in the card house structure. Therefore, photopolymerizable compounds are easily and sufficiently encapsulated within the space, and the ink's adhesion is improved.

[0129] In addition, by making the number of carbon atoms in the straight-chain or branched hydrocarbon groups less than 26, the melting point of the aliphatic ketone represented by general formula (G1) or the aliphatic ester represented by general formula (G2) will not rise excessively, that is, it can be a temperature that is easy to handle when melting, so that the ink does not need to be overheated when the ink is sprayed.

[0130] Examples of aliphatic ketones represented by the general formula (G1) include diteicosethinyl ketone (carbon number: 23, 24), dibenzyl ketone (carbon number: 21, 22), distearyl ketone (carbon number: 17, 18), dieicosethinyl ketone (carbon number: 19, 20), dipalmityl ketone (carbon number: 15, 16), dimyristyl ketone (carbon number: 13, 14), dilauryl ketone (carbon number: 11, 12), and lauryl nutmeg. Myristyl palmityl ketone (carbon numbers: 11, 14), lauryl palmityl ketone (carbon numbers: 11, 16), myristyl palmityl ketone (carbon numbers: 13, 16), myristyl stearyl ketone (carbon numbers: 13, 18), myristyl behenyl ketone (carbon numbers: 13, 22), palmyl stearyl ketone (carbon numbers: 15, 18), palmyl behenyl ketone (carbon numbers: 15, 22), and stearyl behenyl ketone (carbon numbers: 17, 22). Furthermore, the carbon number in parentheses indicates the number of carbon atoms in each of the two hydrocarbon groups separated by the carbonyl group.

[0131] Examples of commercially available aliphatic ketones represented by the general formula (G1) include 18-Pentatriacontanon and Hentriacontan-16-one manufactured by Alfa Aesar, and Caudalie T-1 manufactured by Kao Corporation.

[0132] Examples of aliphatic esters represented by the general formula (G2) include behenyl behenate (carbon number: 21, 22), eicosyl eicosanoate (carbon number: 19, 20), stearyl stearate (carbon number: 17, 18), palmityl stearate (carbon number: 16, 17), lauryl stearate (carbon number: 12, 17), hexadecyl palmitate (carbon number: 16, 15), and stearyl palmitate (carbon number: 15, 18). The following are listed: myristyl myristate (carbon numbers: 13, 14), hexadecyl myristate (carbon numbers: 13, 16), octyl dodecyl myristate (carbon numbers: 13, 20), stearyl oleate (carbon numbers: 17, 18), stearyl erucate (carbon numbers: 18, 21), stearyl linoleate (carbon numbers: 17, 18), behenyl oleate (carbon numbers: 18, 22), and arachidic linoleate (carbon numbers: 17, 20). Furthermore, the carbon number in parentheses indicates the number of carbon atoms in each of the two hydrocarbon groups separated by the ester group.

[0133] Examples of commercially available aliphatic esters represented by the general formula (G2) include Nippon Oil Co., Ltd.’s M-2222SL and Spam acetate, Kao Corporation’s SS and MY-M excipients, Nippon Emulsion Co., Ltd.’s EMLEX CC-18 and CC-10, and Advanced Alcohols Industries Ltd.’s Amulex PC.

[0134] The content of the gelling agent is preferably in the range of 1 to 10% by mass relative to the total mass of the photocurable ink.

[0135] [C. Other ingredients]

[0136] [C-1. Surfactant]

[0137] In the coating film formation method of this embodiment, the photocurable ink may further contain surfactants as needed. Examples of surfactants include anionic surfactants such as dialkyl sulfosuccinates, alkyl naphthalene sulfonates, and fatty acid salts; nonionic surfactants such as polyoxyethylene alkyl ethers, polyoxyethylene alkyl allyl ethers, acetylene glycols, and polyoxyethylene-polyoxypropylene block copolymers; cationic surfactants such as alkylamine salts and quaternary ammonium salts; and silicone-based or fluorinated surfactants.

[0138] [C-2. Colorant]

[0139] In the coating film forming method of this embodiment, the photocurable ink may further contain a colorant as needed. The colorant may be a pigment or a dye, but from the viewpoint of having good dispersibility with the ink's constituent components and excellent weather resistance, a pigment is preferred. There are no particular limitations on the pigment, and examples include organic or inorganic pigments listed in the color index.

[0140] In the coating film formation method of this embodiment, the colorant may contain only one type, or two or more types, and may be tinted to a desired color. The content of the colorant relative to the total mass of the photocurable ink is preferably in the range of 0.1% to 20% by mass, and more preferably in the range of 0.2% to 10% by mass.

[0141] (pigment)

[0142] <Red or magenta pigment>

[0143] Examples of red or magenta pigments include those selected from Pigment Red 3, 5, 19, 22, 31, 38, 43, 48:1, 48:2, 48:3, 48:4, 48:5, 49:1, 53:1, 57:1, 57:2, 58:4, 63:1, 81, 81:1, 81:2, 81:3, 81:4, 88, 104, 108, 112, 122, 123, 144, 146, 149, 166, 168, 169, 170, 177, 178, 179, 184, 185, 208, 216, 226, 257, Pigment Violet 3, 19, 23, 29, 30, 37, 50, 88, and Pigment Orange. Pigments of 13, 16, 20, 36 or mixtures thereof.

[0144] <Blue or Cyan pigment>

[0145] Examples of blue or cyan pigments include pigments or mixtures thereof selected from Pigment Blue 1, 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 17:1, 22, 27, 28, 29, 36, 60.

[0146] <Green Pigment>

[0147] Examples of green pigments include pigments selected from Pigment Green 7, 26, 36, 50, or mixtures thereof.

[0148] <Yellow Pigment>

[0149] Examples of yellow pigments include pigments or mixtures thereof selected from Pigment Yellow 1, 3, 12, 13, 14, 17, 34, 35, 37, 55, 74, 81, 83, 93, 94, 95, 97, 108, 109, 110, 137, 138, 139, 153, 154, 155, 157, 166, 167, 168, 180, 185, and 193.

[0150] <Black Pigment>

[0151] Examples of black pigments include pigments or mixtures thereof selected from Pigment Black 7, 28, 26.

[0152] <Examples of commercially available pigments>

[0153] Examples of commercially available pigments include: Black Pigment (manufactured by Mikuni), Chromofine Yellow 2080, 5900, 5930, AF-1300, 2700L, Chromofine Orange 3700L, 6730, Chromofine Scarlet 6750, Chromofine Magenta 6880, 6886, 6891N, 6790, 6887, Chromofine Violet RE, Chromofine Red 6820, 6830, and Chromofine Blue. HS-3, 5187, 5108, 5197, 5085N, SR-5020, 5026, 5050, 4920, 4927, 4937, 4824, 4933GN-EP, 4940, 4973, 5205, 5208, 5214, 5221, 5000P, Chromofine Green 2GN, 2GO, 2G-550D, 310, 5370, 6830, Chromofine Black A-1103, SEIKAFAST YELLOW 10GH, A-3, 2035, 2054, 2200, 2270, 2300, 2400(B), 2500, 2600, ZAY-260, 2700(B), 2770, Seika FastRed 8040, C405(F), CA120, LR-116, 1531B, 8060R, 1547, ZAW-262, 1537B, GY, 4R-4016, 3820, 3891, ZA-215, Seika FastCarmine 6B1476T-7, 1483LT, 3840, 3870, Seika Fast Bordeaux 10B-430, Seika LightRose R40, Seika Light Violet B800, 7805, Seika Fast Maroon 460N, Seika FastOrange 900, 2900, Seika Light Blue C718, A612, Cyanine Blue 4933M, 4933GN-EP, 4940, 4973 (all manufactured by Daihatsu Seika Kogyo Co., Ltd.)In addition, "Chromofine" is a registered trademark of the company; KETYellow 401, 402, 403, 404, 405, 406, 416, 424, KET Orange 501, KET Red 301, 302, 303, 304, 305, 306, 307, 308, 309, 310, 336, 337, 338, 346, KET Blue 101, 102, 103, 104, 105, 106, 111, 118, 124, KET Green 201 (all manufactured by DIC); Colortex Yellow 301, 314, 315, 316, P-624, 314, U10GN, U3GN, UNN, UA-414, U263, Finecol Yellow T-13, T-05, Pigment Yellow1705, Colortex Orange 202, Colortex Red 101, 103, 115, 116, D3B, P-625, 102, H-1024, 105C, UFN, UCN, UBN, U3BN, URN, UGN, UG276, U456, U457, 105C, USN, Colortex Maroon 601, Colortex Brown B610N, Colortex Violet 600, Pigment Red 122, Colortex Blue 516, 517, 518, 519, A818, P-908, 510, Colortex Green 402, 403, Colortex Black 702, U905 (all manufactured by Sanyo Pigment Co., Ltd. "Colortex" and "Finecol" are registered trademarks of this company); LionolYellow 1405G, Lionol Blue FG7330, FG7350, FG7400G, FG7405G, ES, ESP-S (all manufactured by Toyo Ink Co., Ltd. "Lionol" is a registered trademark of the company); Toner Magenta E02, Permanent Rubin F6B, Toner Yellow HG, Permanent Yellow GG-02, Hostapeam Blue B2G (all manufactured by Hearst Industries); Novoperm P-HG, Hostapeam Pink E, Hostapeam Blue B2G (all manufactured by Clariant).In addition, "Novoperm" and "Hostaperm" are registered trademarks of the company; Carbon Black #2600, #2400, #2350, #2200, #1000, #990, #980, #970, #960, #950, #850, MCF88, #750, #650, MA600, MA7, MA8, MA11, MA100, MA100R, MA77, #52, #50, #47, #45, #45L, #40, #33, #32, #30, #25, #20, #10, #5, #44, CF9 (all manufactured by Mitsubishi Chemical), etc.

[0154] <Dispersion of Pigments>

[0155] Pigments can be dispersed using, for example, ball mills, sand mills, grinding mills, roller mills, mixers, Henschel mixers, colloid mills, ultrasonic homogenizers, bead mills, wet jet mills, and paint vibrators.

[0156] The pigment is preferably dispersed with a volume average particle size of 0.08 to 0.5 μm. Furthermore, the pigment is preferably dispersed with a maximum particle size of 0.3 to 10 μm, more preferably 0.3 to 3 μm. The dispersion of the pigment is adjusted according to the selection of the pigment dispersant and dispersion medium, dispersion conditions, and filtration conditions.

[0157] <Dispersant>

[0158] To improve pigment dispersibility, photocurable inks may further contain dispersants. Examples of dispersants include hydroxyl-containing carboxylic acid esters, salts of long-chain polyaminoamides and high molecular weight acid esters, salts of high molecular weight polycarboxylic acids, salts of long-chain polyaminoamides and polar acid esters, high molecular weight unsaturated acid esters, polymer copolymers, modified polyurethanes, modified polyacrylates, polyether ester-type anionic surfactants, naphthalenesulfonic acid formaldehyde condensate salts, aromatic sulfonic acid formaldehyde condensate salts, polyoxyethylene alkyl phosphates, polyoxyethylene nonylphenyl ethers, and stearamine acetate. Commercially available examples of dispersants include the Solsperse (registered trademark) series manufactured by Avecia Corporation and the PB series manufactured by Ajinomoto Fine Chemicals Co., Ltd.

[0159] <Dispersing Agents>

[0160] UV-curable inks may contain further dispersing agents as needed. The dispersing agents can be selected based on the pigment. The total content of dispersants and dispersing aids is preferably in the range of 1 to 50% by mass relative to the total mass of the pigment.

[0161] <Dispersion Medium>

[0162] Photocurable inks may further contain a dispersion medium for dispersing pigments, as needed. Solvents may be included in photocurable inks as a dispersion medium, but to suppress solvent residue in the resulting image, it is preferable to use the aforementioned photopolymerizable compounds (especially low-viscosity photopolymerizable compounds) as the dispersion medium.

[0163] [C-3. Other Additives]

[0164] Photocurable inks can be further enriched with coupling agents, solvents, etc., as needed.

[0165] (Coupled agent)

[0166] Photocurable inks can be further formulated with various coupling agents as needed. The presence of coupling agents improves adhesion to printed wiring boards. Examples of various coupling agents include silane-based, titanium-based, and aluminum-based coupling agents.

[0167] (solvent)

[0168] From the perspective of rapid curing and spraying stability, solvent-free is preferred for photocurable inks, but solvents can be added to adjust the ink viscosity.

[0169] 1-1-4. Formation of the coating film before curing

[0170] The coating formation method of this embodiment involves coating a photocurable ink onto the surface of a printed wiring substrate to form a pre-cured coating by covering the conductor.

[0171] 1-1-4 (1) Coating of UV-curable inks

[0172] The method for applying photocurable ink to the surface of a printed wiring substrate is inkjet printing. Preferably, the photocurable ink is applied along the wiring pattern of the printed wiring substrate in a manner that covers the wiring. That is, the photocurable ink is applied to the conductors constituting the wiring, forming a pre-curing coating film by covering the conductors. Forming a pre-curing coating film by covering the conductors means that the photocurable ink is applied to the conductors in a manner that overflows from the conductor surface, with its outer edge contacting the substrate surface, thus forming a pre-curing coating film. In other words, the pre-curing coating film is formed on the surface of the conductor (wiring pattern) and overflows from the conductor surface, with its outer edge contacting the substrate surface. Therefore, the conductors are not exposed on the surface, and insulation is maintained.

[0173] 1-1-4 (2) Coating before curing

[0174] The pre-curing coating is a coating formed by applying photocurable ink to the surface of a printed wiring substrate to cover the conductor. Furthermore, the pre-curing coating is a coating formed by photocurable ink before it is photocured.

[0175] The thickness of the coating before curing is preferably 40–200 μm, more preferably 50–180 μm, and particularly preferably 60–160 μm. By keeping the thickness of the coating before curing within this range, a coating with high insulation is formed when a printed wiring board is manufactured by forming a coating on a printed wiring substrate. If the thickness of the coating before curing is less than 40 μm, the insulation of the formed coating may sometimes decrease. If the thickness of the coating before curing is more than 200 μm, the resulting coating becomes too thick, and voids may sometimes be generated.

[0176] The pre-curing coating is applied to the conductor forming the wiring pattern, arranged along the shape of the conductor, with the outer edge of the pre-curing coating overflowing from the outer edge of the conductor and contacting the substrate surface. This results in a coating with high insulation properties. The width of the pre-curing coating overflowing from the outer edge of the conductor is preferably 2 to 5 μm. By setting the width (the overflow length) to such a value, sufficient insulation can be maintained.

[0177] 1-2. Photocurable coating formation process

[0178] The photocurable coating formation process involves subjecting a pre-curable coating to multiple exposures, each for a thickness of 6–18 μm, to curing, thereby forming a photocurable coating. Here, "exposures for each thickness of 6–18 μm" are sometimes referred to as "specific condition exposures." Thus, in the photocurable coating formation method of this embodiment, the pre-curable coating is subjected to multiple exposures under specific conditions during the photocurable coating formation process, thereby curing the pre-curable coating. Therefore, the coating formation method of this embodiment can suppress the formation of voids between the coating and the substrate, and can suppress ink leakage during coating formation.

[0179] 1-2-1. Exposure Method

[0180] In the photocurable coating process, an exposure method called "multiple exposures under specific conditions" is used. During the "specific condition exposure" of the coating before curing, the light intensity in each exposure is 200–700 mJ / cm². 2 The exposure time is 40 × 10⁻⁶. Therefore, shrinkage of the coating before curing during each exposure can be reduced, and the formation of voids between the coating and the substrate can be suppressed. Furthermore, the exposure time for each exposure is preferably 40 × 10⁻⁶. -3 ~119×10 -3 Seconds. The curing rate during each exposure can be measured by the light illuminance (W / cm²). 2 This is adjusted by adjusting the exposure time. To set the exposure time within the specified range each time, exposure needs to be performed at a specific low illumination. The preferred illumination is 4.0–6.0 W / cm². 2 More preferably, it is 4.5–5.5 W / cm². 2 The optimal value is 5.0 W / cm.2 The pre-curing coating shrinks during exposure to light, becoming a photocurable coating. If significant shrinkage occurs within a short period, voids are likely to form between the formed coating and the substrate. The coating formation method of this embodiment cures the pre-curing coating by repeatedly performing small shrinkage cycles, forming a photocurable coating. Therefore, the coating formation method of this embodiment prevents significant shrinkage within a short period, suppressing the formation of voids between the formed coating and the substrate. In this specification, the term "illuminance" refers to "irradiance (W / cm²)". 2 In addition, the illuminance is the illuminance of the coating surface before curing.

[0181] As described above, the coating formation method of this embodiment performs "specific condition exposure" on the pre-curing coating. Therefore, it is possible to suppress the seepage of ink (photocurable ink) during coating formation. When exposing the pre-curing coating, if low-illuminance light is used and the amount of light irradiated each time is excessively reduced, ink seepage occurs around the formed coating. If the illuminance of the light in each exposure is reduced, the curing time becomes longer. Consequently, it is believed that uncured photopolymerizable compounds cannot remain within the coating and flow out to the periphery. In contrast, the coating formation method of this embodiment performs multiple "exposures on the pre-curing coating, each time curing a thickness of 6 to 18 μm". Furthermore, it is preferable to avoid excessively long exposure times. Therefore, the exposure and curing of the pre-curing coating can be advanced at a speed that prevents photopolymerizable compounds from seeping out. Furthermore, this prevents the seepage of photopolymerizable compounds and suppresses seepage during coating formation. As described above, if the curing of the pre-curing coating is advanced too quickly, seepage does not occur, but gaps are created between the coating and the substrate. Furthermore, if the curing of the pre-curing coating is advanced too slowly, gaps between the coating and the substrate will not be created, but exudation will occur. To balance these opposing characteristics, the inventors discovered an exposure method that involves "exposing the pre-curing coating multiple times, each time curing a thickness of 6 to 18 μm." The thickness of the pre-curing coating cured in each exposure is obtained by measuring the thickness of the photocurable coating after the pre-curing coating has been cured as a whole, and dividing the thickness by the number of exposures.

[0182] In the coating formation method of this embodiment, if the thickness of each exposure is less than 6 μm, the number of exposures increases, making the total curing (exposure) time of the coating before curing too long, resulting in exudation, which is undesirable. Hereinafter, the thickness of each exposure is sometimes referred to as "exposure thickness". If the exposure thickness exceeds 18 μm, in order to avoid exudation, the illuminance is increased, and the coating before curing is exposed and cured for a specified time, resulting in a large shrinkage amount per exposure, creating gaps between the coating and the substrate, which is also undesirable. In addition, if the illuminance is reduced to avoid creating gaps between the coating and the substrate, and the coating before curing is exposed and cured, the curing time is too long, resulting in exudation, which is also undesirable. Furthermore, if the exposure time is less than 40 × 10 -3 If the exposure time is longer than 119 × 10 seconds, then to cure the specified thickness of the pre-curing coating, the illuminance needs to be increased for exposure. Therefore, gaps are created between the coating and the substrate, which is undesirable. Furthermore, if the exposure time is longer than 119 × 10 seconds... -3 If the light exposure is too short, then in order to cure the specified thickness of the pre-curing coating, the light intensity needs to be reduced. Therefore, this will cause exudation, which is not preferable.

[0183] Exposure of a pre-curing coating disposed on the surface of a printed wiring substrate is performed by curing the pre-curing coating by irradiating it with active energy rays. The active energy rays can be selected from, for example, electron beams, ultraviolet light, alpha rays, gamma rays, X-rays, etc., but are preferably ultraviolet light or electron beams. The ultraviolet light is preferably light with a peak wavelength between 360 nm and 410 nm. Furthermore, the ultraviolet light is preferably irradiated from an LED light source. Since LEDs radiate less heat than conventional light sources (such as metal halide lamps), the ink is less likely to melt during irradiation with active energy rays, and uneven gloss is less likely to occur.

[0184] 1-2-2. Coating

[0185] The coating thickness formed by the coating formation method of this embodiment is preferably 40 to 200 μm, more preferably 50 to 180 μm, and particularly preferably 60 to 160 μm. The coating thickness is the height perpendicular to the substrate surface. By keeping the coating thickness within this range, insulation can be improved in printed wiring boards with thick conductors. If it is thinner than 40 μm, it is sometimes difficult to maintain insulation. If it is thicker than 200 μm, voids can easily form. Furthermore, the coating thickness is preferably 20 to 50 μm thicker than the conductor thickness, more preferably 25 to 45 μm, and particularly preferably 30 to 40 μm thicker. By keeping the coating thickness within this range, insulation can be improved in printed wiring boards with thick conductors. If it is thinner than 20 μm, it is sometimes difficult to maintain insulation. If it is thicker than 50 μm, voids can easily form.

[0186] 1-3. Heating Coating Formation Process

[0187] The coating formation method of this embodiment can include a heating coating formation step after the photocurable coating formation step. The heating coating formation step is a step of further heating the photocurable coating to form a heated coating. By further heating the photocurable coating, the photocurable coating can be further cured. The heated coating improves the curability of the photocurable coating by further curing it. Furthermore, as described above, when the photocurable coating is the final coating, it is the coating formed by the coating formation method of this embodiment. Similarly, when the heated coating is the final coating, it is the coating formed by the coating formation method of this embodiment. This improves the adhesion of the coating to the conductor and substrate, and further enhances the heat resistance of the coating.

[0188] 1-3-1. Heating Method

[0189] There are no particular restrictions on the method of heating the UV-curable coating; for example, an oven can be used. The heating temperature of the UV-curable coating is not particularly limited as long as the coating can be thermally cured, but it is preferably between 140°C and 180°C. Furthermore, the heating time of the UV-curable coating is preferably between 30 minutes and 120 minutes, more preferably between 30 minutes and 60 minutes.

[0190] 2. Printed Wiring Board Manufacturing Method

[0191] The printed wiring board manufacturing method of the present invention is a method for manufacturing a printed wiring board using the coating formation method of the present invention. The resulting printed wiring board has a structure comprising a substrate, a printed wiring substrate having a thickness of 50 μm or more disposed on the substrate, and a coating film disposed to cover the conductor.

[0192] An embodiment of the printed wiring board manufacturing method involves fabricating a printed wiring board using the aforementioned coating formation method. Therefore, the resulting printed wiring board suppresses the formation of voids between the coating and the substrate, and also suppresses ink leakage.

[0193] 3. Coating Formation System

[0194] Reference Figure 4A , Figure 4B The coating forming system of this embodiment will be described. Figure 4A and Figure 4B This is a schematic diagram illustrating the process of forming a coating (photocurable coating 13) using the coating forming system of this embodiment. Figure 4A This is a schematic diagram illustrating the state in which photocurable ink is applied to the printed wiring substrate 3 via the inkjet head 11. Figure 4BThis is a schematic diagram illustrating the state in which the curing unit 12 cures the pre-cured coating to form a photocurable coating 13. The coating forming system of this embodiment includes an inkjet head 11 and a curing unit 12, and is used in the coating forming method of this embodiment. The coating forming system is divided into... Figure 4A and Figure 4B As shown. The inkjet head 11 is a component that applies photocurable ink to the printed wiring substrate 3 to form a pre-curing coating 4. The curing section 12 is a component that uses active energy rays (light) to cure the pre-curing coating 4 applied to the printed wiring substrate 3, forming a photocurable coating 13. That is, the active energy rays used for curing irradiate the pre-curing coating from the curing section 12.

[0195] There are no particular limitations on the inkjet head 11, but a piezoelectric inkjet head is preferred. An example of a piezoelectric inkjet head is the KM1800iSHC-C (600 dpi resolution) manufactured by Konica Minolta. Furthermore, it is preferable to arrange the independent drive heads of two of the aforementioned piezoelectric inkjet heads in a manner where the nozzles are staggered, forming a nozzle array with a resolution of 1200 dpi. Preferably, the inkjet head is filled with UV-curable ink from an ink tank containing UV-curable ink via an ink flow path.

[0196] As described above, the curing section 12 is a component that uses active energy rays (light) to cure the pre-curing coating applied to the printed wiring substrate. The curing section 12 irradiated with active energy rays preferably includes an LED light source, a metal halide lamp, etc., but more preferably an LED light source. The LED light source is preferably a component that irradiates ultraviolet light.

[0197] Example

[0198] The following examples illustrate the invention in detail, but the invention is not limited thereto. Furthermore, in the examples described below, unless otherwise specified, the operation is performed at room temperature (25°C). Additionally, unless otherwise specified, "%" and "parts" refer to "mass %" and "parts by mass," respectively.

[0199] <Preparation of Pigment Dispersion A>

[0200] Pigment dispersion A is a cyan pigment dispersion. Dispersant 1 and dispersant 2, along with the dispersion medium, are placed in a stainless steel beaker and heated and stirred on a hot plate at 65°C for 1 hour to dissolve. After cooling to room temperature, the pigment is added, and 200g of 0.5mm diameter zirconia beads are placed in a glass bottle and sealed. The mixture is dispersed to the desired particle size using a paint shaker, and then the zirconia beads are removed. Furthermore, in this specification, "pigment dispersion" refers to the entire dispersion of pigment and dispersant in the dispersion medium.

[0201] Dispersant (PX4701 (manufactured by BASF)): 7.0 parts by weight

[0202] Dispersion medium (dipropylene glycol diacrylate (containing 0.2% UV-10)): 70 parts by weight

[0203] Pigment Blue 15:4 (manufactured by Daihatsu Seika, CFB6332JC (Chromofine (registered trademark) Blue 6332JC)): 23 parts by weight

[0204] <Preparation of Pigment Dispersion B>

[0205] Pigment dispersion B is a yellow pigment dispersion. It is prepared in the same manner as pigment dispersion A, except that the dispersant, dispersion medium, and pigment are changed as described below.

[0206] Dispersant 1 (PX4701 (manufactured by BASF)): 6.0 parts by weight

[0207] Dispersant 2 (Solsperse 22000 (manufactured by Lubrizol Corporation, Japan)): 0.3 parts by weight

[0208] Dispersion medium (dipropylene glycol diacrylate (containing 0.2% UV-10)): 61.5 parts by weight

[0209] Pigment (Pigment Yellow 147 (manufactured by BASF, Orracet Y 140)): 10.2 parts by weight

[0210] The photopolymerizable compounds and photopolymerization initiators used in the formulation of the following photocurable inks are as follows.

[0211] <Photopolymerizable compounds>

[0212] Photopolymerizable compound A: dipropylene glycol di(meth)acrylate, product name (manufacturer) = M222 (manufactured by Miwon), molecular weight 242

[0213] Photopolymerizable compound B: Tricyclodecanedimethylethanol diacrylate, Product name (manufacturer) = M262 (manufactured by Miwon), Molecular weight 304

[0214] Photopolymerizable compound C: Isoborneol (meth)acrylate, Product name (manufacturer) = IBXA (manufactured by Miwon), Molecular weight 208

[0215] Photopolymerization initiator

[0216] Photopolymerization initiator A: Product name (manufacturer) = Omnirad 379 EG (manufactured by IGM).

[0217] Photopolymerization initiator B: Product name (manufacturer) = Omnirad TPO H (manufactured by IGM Corporation)

[0218] Photopolymerization initiator C: 2-Isopropylthioxanthone, Product Name (Manufacturer) = ITX (Manufactured by Sartomer Company)

[0219] <Preparation of UV-curable inks>

[0220] The following components were mixed and filtered through a 3μm Teflon membrane filter (registered trademark) manufactured by ADVATEC to prepare a photocurable ink. The resulting photocurable ink was evaluated for its ejection stability using the following methods. The composition of the photocurable ink and the results of the ejection stability evaluation are shown in Table I.

[0221] (Photopolymerizable compounds)

[0222] Photopolymerizable compound A: 36.7 parts by weight

[0223] Photopolymerizable compound B: 21.0 parts by weight

[0224] Photopolymerizable compound C: 33.0 parts by weight

[0225] (Pigment dispersion)

[0226] Pigment dispersion A: 0.2 parts by weight

[0227] Pigment dispersion B: 0.4 parts by weight

[0228] (Photopolymerization initiator)

[0229] Photopolymerization initiator A: 3.6 parts by weight

[0230] Photopolymerization initiator B: 4.8 parts by weight

[0231] Photopolymerization initiator C: 0.3 parts by weight

[0232] (Example 1)

[0233] <Forming a coating using inkjet technology>

[0234] (Coating formation process before curing)

[0235] A modified photocurable ink is mounted into an inkjet recording apparatus having an inkjet head with piezoelectric inkjet nozzles. Using this apparatus, the photocurable ink is applied to a printed wiring substrate by inkjet printing to form a pre-curing coating covering the conductors. The printed wiring substrate is a substrate comprising a substrate and conductors disposed on the substrate. Furthermore, the conductors in the printed wiring substrate are copper foils arranged on the substrate in a linear pattern. The conductor thickness is 70 μm. The printed wiring substrate is 1.6 mm thick and 150 mm × 95 mm in size.

[0236] The UV-curable ink supply system consists of an ink tank, an ink flow path, a secondary ink tank directly in front of the inkjet head, piping with a metal filter, and a piezoelectric head. The ink is heated to 80°C from the ink tank to the head. The piezoelectric head also has a built-in heater to heat the ink inside the head to 80°C. The piezoelectric head has a nozzle diameter of 22 μm and a nozzle resolution of 360 dpi, arranged in a 1 / 2-hole configuration to form a 720 dpi nozzle array. Using this inkjet device, voltage is applied to coat the UV-curable ink at a droplet volume of 6.0 pL.

[0237] (Photocurable coating formation process)

[0238] The pre-curing coating was subjected to six exposures using active energy rays, each curing a thickness of 10.0 μm, to solidify the pre-curing coating and form a photocurable coating. The irradiation intensity of the active energy rays in each exposure was 300 mJ / cm². 2 The total light intensity is 1800 mJ / cm². 2 Additionally, the irradiance of the active energy rays is 5.0 W / cm². 2 Irradiation with active energy rays was performed using an LED lamp (Fire Jet FJ100, manufactured by Phoseon Technology, wavelength 395nm).

[0239] The apparatus for curing a pre-curing coating applied to the wiring substrate by means of active energy rays is the curing section of the coating forming system of the present invention. Furthermore, the curing section includes the LED lamp that irradiates the active energy rays. The apparatus having the inkjet head and the curing section is the coating forming system of the present invention.

[0240] (Thermosetting coating (coating) formation process)

[0241] After forming a photocurable coating, the photocurable coating is heated to form a thermocurable coating. Specifically, the printed wiring substrate with the photocurable coating is placed in an oven set to 150°C for 60 minutes to obtain a printed wiring board. The coating thickness is 60 μm. In this embodiment, the thermocurable coating is obtained by the coating formation method of this embodiment. The coating thickness is measured using a contact thickness gauge (MH-15M).

[0242] For the printed wiring substrate, the amount of leakage was measured using the method shown below. The results are shown in Table II. In Tables II to IV, "Embodiment" indicates "Example", for example, "Embodiment 1" indicates "Example 1". In addition, "Comparison" indicates "Comparative Example", for example, "Comparison 1" indicates "Comparative Example 1".

[0243] In addition, in Example 1, a printed wiring board was fabricated in the same manner as in Example 1, except that the pre-curing coating was applied to the entire printed wiring substrate. This printed wiring board is also referred to as a "solid pattern". An adhesion test was conducted on this sample, which was used as a sample of Example 1. The results are shown in Table II.

[0244] (Examples 2-11, Comparative Examples 1-4)

[0245] In Example 1, a printed wiring board was fabricated in the same manner as in Example 1, except that the compounding components and photocuring conditions were changed as shown in Tables II to IV.

[0246] [evaluate]

[0247] <Ejection Stability>

[0248] A piezoelectric head is used to continuously eject (drive) photocurable ink. The conditions for continuous ejection (driving) are: droplet volume 3.5 pL, droplet velocity 7 m / s, ejection frequency 40 kHz, and print rate 100%. Furthermore, the number of nozzles that failed to eject (missing nozzles) is counted after 1 minute, 5 minutes, and 10 minutes from the start of continuous ejection (driving). The evaluation criteria for this test are as follows: in categories A through C, A and B are acceptable, and C is unacceptable.

[0249] A: In any count after 1 minute, 5 minutes, or 10 minutes, the number of missing nozzles is less than 5.

[0250] B: In any count after 1 minute, 5 minutes, or 10 minutes, the number of missing nozzles is more than 5 but less than 20.

[0251] C: In any count after 1 minute, 5 minutes, or 10 minutes, the number of missing nozzles is 20 or more.

[0252] <Coefficient of linear expansion>

[0253] The coefficient of linear expansion was determined using a thermomechanical analysis apparatus via the compression loading method. The test samples were obtained by cutting the coating film using a cutting machine. The test samples were set with longitudinal length, transverse length, and thickness of 5 mm, 10 mm, and 10 mm. The thermomechanical analysis apparatus used was a TMA 4000SE (manufactured by NETZSCH Japan). The test conditions were: nitrogen atmosphere, compression loading mode, temperature range from room temperature to 180 °C, heating rate of 5 °C / min, and load of 5 gf.

[0254] <Exudate>

[0255] The obtained printed wiring board was observed using a microscope (KEYENCE VHX-5000) at 500x magnification. The amount of monomer components of the photopolymerizable compound without pigment content (hereinafter also referred to as "leakage") leached from the outer edge of the coating was measured. The evaluation criteria for this test are as follows: A to C are acceptable, and D is unacceptable.

[0256] A: Exudation rate is below 20μm

[0257] B: Exudation volume exceeding 20μm but below 30μm

[0258] C: Exudation volume exceeding 30μm but below 40μm

[0259] D: Exudation rate exceeds 40μm

[0260] <Seamless>

[0261] For solid patterns, an adhesion test was conducted according to JIS K5600 (JIS K5600-5-6 Part 5-Section 6: Adhesion (Cross-cut Test)). Specifically, checkerboard-shaped cuts were made into the coating, adhesive tape was applied, and the peeling state of the coating was observed. The adhesion residue rate was determined using the following method and evaluated according to the following criteria. Here, the adhesion residue rate is calculated with the number of cuts as the denominator and the number of cuts remaining on the printed wiring board after tape peeling as the numerator. A to C are acceptable, and D is unacceptable.

[0262] (Benchmark)

[0263] A: Adhesion residue rate 100%

[0264] B: Adhesion residue rate ≥80% but <100%

[0265] C: Adhesion residue rate ≥ 60% and < 80%

[0266] D: Adhesion residue rate is less than 60%.

[0267]

[0268]

[0269]

[0270]

[0271] As can be seen from the above results, the coating obtained by the coating film forming method of the embodiment has less exudation and higher adhesion compared with the coating film obtained by the coating film forming method of the comparative example.

[0272] Industrial availability

[0273] A coating forming method, a printed wiring board manufacturing method, and a coating forming system are provided that can suppress ink seepage and suppress the formation of gaps between the coating and the substrate.

[0274] Symbol Explanation

[0275] 1: Substrate

[0276] 2: Conductor

[0277] 3: Printed wiring substrate

[0278] 4: Coating before curing

[0279] 11: Inkjet head

[0280] 12: Curing Department

[0281] 13: UV-cured coating

[0282] S01: Coating formation process before curing

[0283] S02: Photocurable coating formation process

[0284] S03: Thermosetting coating formation process

Claims

1. A coating film forming method, comprising forming a coating film on a printed wiring substrate, including: In the pre-curing coating formation process, a photocurable ink is applied to the printed wiring substrate having a substrate and a conductor with a thickness of 50 μm or more disposed on the substrate by inkjet printing, so as to cover the conductor and form a pre-curing coating. as well as In the photocurable coating formation process, the pre-curable coating is exposed multiple times, each time to a thickness of 6-18 μm, to cure the pre-curable coating and form a photocurable coating.

2. The coating film forming method as described in claim 1, wherein, The exposure is an irradiation intensity of 200–700 mJ / cm². 2 The exposure.

3. The coating film forming method as described in claim 1 or 2, wherein, The duration of each exposure is 40 × 10. -3 ~119×10 -3 Second.

4. The coating film forming method as described in claim 1 or 2, wherein, The photocurable ink contains a photopolymerizable compound with a molecular weight of 200 to 600.

5. The coating film forming method as described in claim 1 or 2, wherein, The thickness of the conductor is 60–150 μm.

6. The coating film forming method as described in claim 1 or 2, wherein, The coefficient of linear expansion of the photocurable ink is 20 to 250 ppm / K.

7. The coating film forming method as described in claim 1 or 2, wherein, The coating, when tested according to the adhesion test method of JIS K5600, showed a retention rate of over 90%.

8. The coating film forming method as described in claim 1 or 2, wherein, The penetration width from the boundary line between the coating and the substrate toward the substrate side is less than 20 μm.

9. A method for manufacturing a printed wiring board, wherein, Printed wiring boards are manufactured using the coating formation method described in claim 1 or 2.

10. A coating film forming system for use in the coating film forming method of claim 1 or 2, comprising: An inkjet head applies the photocurable ink to the printed wiring substrate to form the pre-cured coating; and... The curing section uses active energy rays to cure the pre-curing coating applied to the printed wiring substrate.

Citation Information

Patent Citations

  • Method of manufacturing cured film, method of manufacturing electronic component, and the electronic component

    JP2015089540A

  • Inkjet ink for resist, resist film, and method for forming resist film

    JP2022063284A

  • Recording method and method for manufacturing printed article

    WO2022085183A1