Method for manufacturing metal oxide layers

By forming a highly crystalline indium oxide layer in an oxide semiconductor transistor, the problems of low carrier mobility and large leakage current are solved, realizing a transistor with low power consumption, high reliability and fast operation, suitable for semiconductor devices and display devices.

CN123126050APending Publication Date: 2026-11-17SEMICON ENERGY LAB CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202580028109.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-26
Filing Date
2025-04-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the prior art, oxide semiconductor transistors have low carrier mobility and large leakage current, resulting in high power consumption, making it difficult to achieve high integration and miniaturization. In addition, they have large parasitic capacitance, which affects the reliability and operating speed of the transistors.

Method used

A manufacturing method is employed to form an amorphous metal oxide layer on a crystalline portion and to allow it to crystallize and grow through heat treatment. The specific steps include forming a trench on a substrate, covering the trench with a metal oxide layer, and performing heat treatment at a specific temperature and atmosphere to form a highly crystalline indium oxide layer.

Benefits of technology

It improves carrier mobility, reduces leakage current, lowers power consumption, enhances transistor reliability and operating speed, and achieves miniaturization and high integration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123126050A_ABST
    Figure CN123126050A_ABST
Patent Text Reader

Abstract

A metal oxide layer with high carrier mobility and a method for manufacturing the same are provided. The method for manufacturing the metal oxide layer includes the following steps: a first step of forming a crystalline portion; a second step of forming a metal oxide layer with an amorphous structure on the crystalline portion; and a third step of growing the metal oxide layer by heat treatment, using the crystalline portion as a nucleus. The metal oxide layer contains indium. The crystal orientation of the crystalline portion is as follows: <001> The metal oxide layer after heat treatment contains crystals with the following orientation: <111> . crystal grains.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] One aspect of the present invention relates to a metal oxide layer, a semiconductor device, a memory device, a display device, and an electronic device. Furthermore, another aspect of the present invention relates to a method for manufacturing a metal oxide layer and a method for manufacturing a semiconductor device.

[0002] Note that one aspect of the present invention is not limited to the technical fields described above. Examples of technical fields for one aspect of the present invention include semiconductor devices, display devices, light-emitting devices, energy storage devices, memory devices, electronic devices, lighting devices, input devices (e.g., touch sensors), input / output devices (e.g., touch panels), methods for driving them, or methods for manufacturing them.

[0003] In this specification, etc., a semiconductor device refers to a device that utilizes the properties of semiconductors, as well as circuits that include semiconductor elements (transistors, diodes, photodiodes, etc.) and devices that include such circuits. Furthermore, a semiconductor device refers to all devices capable of functioning by utilizing the properties of semiconductors. Examples of semiconductor devices include integrated circuits, chips containing integrated circuits, and electronic components that house chips in packages. In addition, storage devices, display devices, light-emitting devices, lighting devices, and electronic devices are themselves semiconductor devices, and sometimes all include semiconductor devices. Background Technology

[0004] The technique of constructing transistors using semiconductor thin films formed on substrates with insulating surfaces has attracted attention. These transistors are widely used in electronic devices such as integrated circuits (ICs) and display devices. Silicon-based semiconductors are widely known as suitable semiconductor materials for transistors. Among other materials, oxide semiconductors have also garnered interest.

[0005] Furthermore, it is known that transistors using oxide semiconductors have extremely low leakage current in the off state. For example, Patent Document 1 discloses a low-power CPU (Central Processing Unit) that utilizes the low leakage current characteristic of transistors using oxide semiconductors. Additionally, for example, Patent Document 2 discloses a storage device that utilizes the low leakage current characteristic of transistors using oxide semiconductors to achieve long-term retention of stored content.

[0006] Furthermore, examples of oxide semiconductors that can be used as active layers in transistors include indium oxide and indium gallium zinc oxide. Non-Patent Document 1 discloses a thin-film transistor using hydrogenated polycrystalline indium oxide, formed by low-temperature solid-state crystallization, as the active layer.

[0007] [Preliminary Technology Documents]

[0008] [Patent Literature]

[0009] [Patent Document 1] Japanese Patent Application Publication No. 2012-257187

[0010] [Patent Document 2] Japanese Patent Application Publication No. 2011-151383

[0011] [Non-patent literature]

[0012] [Non-Patent Literature 1] Y. Magari et al., “High-mobility hydrogenated polycrystalline In2O3 (In2O3:H) thin-film transistors”, Nature COMMUNICATIONS, 13, 1078 (2022).

[0013] [Non-Patent Literature 2] N. Preissler et al., “Electrical transport, electrothermal transport, and effective electron mass in single-crystalline In2O3 films”, Phys. Rev. B, 88, 085305 (2013).

[0014] [Non-Patent Literature 3] Takashi Koida, “High Mobility Transparent Conductive Film”, National Institute of Advanced Industrial Science and Technology (AIST), Japan, AIST Solar Power Research Results Presentation 2019, website:<URL:https: / / unit.aist.go.jp / rpd-envene / PV / ja / results / 2019 / oral / T13.pdf> Summary of the Invention

[0015] The technical problem that the invention aims to solve

[0016] One objective of this invention is to provide a metal oxide layer with high carrier mobility. Another objective of this invention is to provide a novel metal oxide layer. Finally, one objective of this invention is to provide a transistor, semiconductor device, memory device, or display device using a metal oxide layer.

[0017] One objective of this invention is to provide a transistor with excellent electrical characteristics. Another objective of this invention is to provide a transistor with a large on-state current. Another objective of this invention is to provide a transistor with low parasitic capacitance. Another objective of this invention is to provide a transistor, semiconductor device, memory device, or display device with high reliability. Another objective of this invention is to provide a transistor, semiconductor device, or memory device capable of miniaturization or high integration. Another objective of this invention is to provide a semiconductor device, memory device, or display device with low power consumption. Another objective of this invention is to provide a memory device with high operating speed. Finally, another objective of this invention is to provide a method for manufacturing the aforementioned transistor, semiconductor device, memory device, or display device.

[0018] Note that the description of these objectives does not preclude the existence of other objectives. One aspect of the invention does not necessarily require achieving all of the above objectives. Objectives other than those described above can be extracted from the description, drawings, and claims.

[0019] means of solving technical problems

[0020] One aspect of the present invention is a method for manufacturing a metal oxide layer, the method comprising the following steps: a first step of forming a crystalline portion; a second step of forming a metal oxide layer having an amorphous structure on the crystalline portion; and a third step of causing the metal oxide layer to crystallize and grow using the crystalline portion as a nucleus by heat treatment. The metal oxide layer comprises indium.

[0021] In the above-described method for manufacturing a metal oxide layer, it is preferable that, in the first step, a crystalline portion is formed on the layer having the groove, in the second step, a metal oxide layer is formed in a manner that covers the groove, and in the third step, the metal oxide layer is crystallized and grown along the groove.

[0022] One aspect of the present invention is a method for manufacturing a metal oxide layer, the method comprising the steps of: a first step of forming a crystalline portion; and a second step of forming a single-crystal metal oxide layer on the crystalline portion using the crystalline portion as a seed crystal. The metal oxide layer comprises indium. Furthermore, in the first step, a trench is formed and the crystalline portion is formed on a layer having a curved surface at the upper end of the trench, and in the second step, the metal oxide layer is formed to cover the trench.

[0023] One aspect of the present invention is a method for manufacturing a metal oxide layer, the method comprising the following steps: a first step of forming a crystalline portion; a second step of forming a metal oxide layer having an amorphous structure on the crystalline portion; and a third step of causing the metal oxide layer to crystallize and grow using the crystalline portion as a nucleus by heat treatment. The metal oxide layer comprises indium. Furthermore, in the first step, a trench is formed and the crystalline portion is formed on a layer having a curved surface at the upper end of the trench; in the second step, the metal oxide layer is formed to cover the trench; and in the third step, the metal oxide layer is crystallized and grown along the trench.

[0024] In the above-described method for manufacturing a metal oxide layer, it is preferable to form the metal oxide layer in the second step at a substrate temperature of 100°C or higher and 300°C or lower. In particular, it is preferable to form the metal oxide layer at a substrate temperature of 150°C or higher and 250°C or lower.

[0025] In the above-mentioned method for manufacturing the metal oxide layer, the surface preferably has a portion with a radius of curvature of 1 nm or more and 500 nm or less.

[0026] In the above-described method for manufacturing the metal oxide layer, the curved surface preferably has a portion with a radius of curvature greater than the thickness of the metal oxide layer.

[0027] In the above-described method for manufacturing the metal oxide layer, the layer preferably comprises an insulating material. Alternatively, the layer preferably comprises a conductive material.

[0028] In the above-described method for manufacturing a metal oxide layer, the layer preferably has a curved surface at the bottom of the groove.

[0029] In the above-described method for manufacturing the metal oxide layer, it is preferable to form the metal oxide layer using a sputtering method, with a hydrogen-containing gas used as the sputtering gas.

[0030] In the above-described method for manufacturing the metal oxide layer, it is preferable that a first heat treatment and a second heat treatment are performed sequentially as heat treatments, wherein the temperature of the second heat treatment is higher than the temperature of the first heat treatment.

[0031] In the above-mentioned method for manufacturing the metal oxide layer, it is preferable to perform the first heat treatment in an atmosphere containing hydrogen and nitrogen.

[0032] In the above-described method for manufacturing the metal oxide layer, it is preferable to reduce the hydrogen concentration in the metal oxide layer by performing a second heat treatment.

[0033] In the above-described method for manufacturing a metal oxide layer, the metal oxide layer after heat treatment preferably contains grains in the portion overlapping with the crystalline portion.

[0034] In the above-mentioned method for manufacturing metal oxide layers, the crystal orientation of the grains is preferably... <111> .

[0035] In the above-described method for manufacturing the metal oxide layer, the crystal orientation of the crystalline portion is preferably... <001> .

[0036] In the above-mentioned method for manufacturing metal oxide layers, it is preferable that the crystalline portion contains indium, gallium, and zinc, and the composition of the crystalline portion is In:Ga:Zn=1:1:1 [atomic ratio] or near that, or In:Ga:Zn=1:3:2 [atomic ratio] or near that.

[0037] In the above-mentioned method for manufacturing metal oxide layers, the crystalline portion preferably contains indium oxide.

[0038] One aspect of the present invention is a method for manufacturing a semiconductor device, the method comprising the following steps: a first step of forming a crystalline portion on a first insulating layer; a second step of forming a metal oxide layer having an amorphous structure on the crystalline portion; a third step of growing the metal oxide layer by means of a heat treatment using the crystalline portion as a nucleus; a fourth step of forming a second insulating layer to cover the metal oxide layer; and a fifth step of forming a conductive layer on the second insulating layer. The metal oxide layer comprises indium.

[0039] In the above-described method for manufacturing a semiconductor device, it is preferable that, in the first step, a crystallized portion is formed on an insulating layer having a trench, in the second step, a metal oxide layer is formed to cover the trench, and in the third step, the metal oxide layer is crystallized and grown along the trench.

[0040] In the above-described method for manufacturing a semiconductor device, it is preferable to form a metal oxide layer using a sputtering method, and to use a gas containing hydrogen as the sputtering gas.

[0041] In the above-described method for manufacturing a semiconductor device, it is preferable that a first heating treatment and a second heating treatment are performed sequentially as a heating treatment, wherein the temperature of the second heating treatment is higher than the temperature of the first heating treatment.

[0042] In the above-described method for manufacturing a semiconductor device, it is preferable to perform the first heat treatment in an atmosphere containing hydrogen and nitrogen.

[0043] In the above-described method for manufacturing a semiconductor device, it is preferable to reduce the hydrogen concentration in the metal oxide layer by performing a second heat treatment.

[0044] In the above-described method for manufacturing a semiconductor device, the metal oxide layer after heat treatment preferably contains grains in the portion overlapping with the crystallized portion.

[0045] In the above-described method for manufacturing a semiconductor device, the crystal orientation of the grains is preferably... <111> .

[0046] In the above-described method for manufacturing a semiconductor device, the crystal orientation of the crystallized portion is preferably... <001> .

[0047] In the above-described method for manufacturing a semiconductor device, it is preferable that the crystallized portion comprises indium, gallium, and zinc, and the composition of the crystallized portion is In:Ga:Zn=1:1:1 [atomic ratio] or near thereon, or In:Ga:Zn=1:3:2 [atomic ratio] or near thereon.

[0048] Invention Effects

[0049] According to one aspect of the present invention, a metal oxide layer with high carrier mobility can be provided. According to one aspect of the present invention, a novel metal oxide layer can be provided. According to one aspect of the present invention, a semiconductor device, a memory device, or a display device using a metal oxide layer can be provided.

[0050] According to one aspect of the present invention, a transistor with good electrical characteristics can be provided. According to one aspect of the present invention, a transistor with a large on-state current can be provided. According to one aspect of the present invention, a transistor with small parasitic capacitance can be provided. According to one aspect of the present invention, a transistor, semiconductor device, memory device, or display device with high reliability can be provided. According to one aspect of the present invention, a transistor, semiconductor device, or memory device capable of miniaturization or high integration can be provided. According to one aspect of the present invention, a semiconductor device, memory device, or display device with low power consumption can be provided. According to one aspect of the present invention, a memory device with high operating speed can be provided. According to one aspect of the present invention, a method for manufacturing the above-mentioned transistor, semiconductor device, memory device, or display device can be provided.

[0051] Note that the description of these effects does not preclude the existence of other effects. One aspect of the invention does not necessarily require all of the aforementioned effects. Effects other than those described above can be extracted from the specification, drawings, and claims.

[0052] Brief description of the attached figures

[0053] Figures 1A to 1D This is a three-dimensional schematic diagram showing an example of a semiconductor device.

[0054] Figure 2 This is a graph illustrating the carrier concentration dependence of the indium oxide mobility disclosed in Non-Patent Document 2.

[0055] Figure 3A and Figure 3BThis is a graph illustrating the carrier concentration dependence of Hall mobility. Figure 3C This is a cross-sectional view illustrating the indium oxide film.

[0056] Figures 4A to 4E It is a diagram illustrating the crystal structure of metal oxides.

[0057] Figures 5A to 5D This is a cross-sectional schematic diagram showing an example of a semiconductor device.

[0058] Figure 6A This is a cross-sectional schematic diagram showing an example of a semiconductor device. Figure 6B and Figure 6C This is a three-dimensional schematic diagram showing an example of a semiconductor device.

[0059] Figures 7A to 7D This is a cross-sectional schematic diagram showing an example of a semiconductor device.

[0060] Figure 8A This is a cross-sectional schematic diagram showing an example of a semiconductor device. Figure 8B and Figure 8C This is a three-dimensional schematic diagram showing an example of a semiconductor device.

[0061] Figures 9A to 9C and Figure 9E This is a three-dimensional schematic diagram showing an example of a semiconductor device. Figure 9D and Figure 9F This is a cross-sectional schematic diagram showing an example of a semiconductor device.

[0062] Figure 10A and Figure 10C This is a three-dimensional schematic diagram showing an example of a semiconductor device. Figure 10B This is a cross-sectional schematic diagram showing an example of a semiconductor device.

[0063] Figure 11A , Figure 11C and Figure 11E This is a three-dimensional schematic diagram showing an example of a semiconductor device. Figure 11B , Figure 11D and Figure 11F This is a cross-sectional schematic diagram showing an example of a semiconductor device.

[0064] Figure 12A , Figure 12C and Figure 12E This is a three-dimensional schematic diagram illustrating an example of a semiconductor device manufacturing method. Figure 12B , Figure 12D and Figure 12F This is a cross-sectional schematic diagram illustrating an example of a semiconductor device manufacturing method.

[0065] Figure 13A, Figure 13C and Figure 13E This is a three-dimensional schematic diagram illustrating an example of a semiconductor device manufacturing method. Figure 13B , Figure 13D and Figure 13F This is a cross-sectional schematic diagram illustrating an example of a semiconductor device manufacturing method.

[0066] Figures 14A to 14E This is a three-dimensional schematic diagram showing an example of a semiconductor device.

[0067] Figure 15A , Figure 15B , Figure 15D This is a three-dimensional schematic diagram illustrating an example of a semiconductor device manufacturing method. Figure 15C This is a cross-sectional schematic diagram showing an example of a semiconductor device.

[0068] Figure 16 This is a cross-sectional schematic diagram showing an example of a semiconductor device.

[0069] Figures 17A to 17C This is a three-dimensional schematic diagram showing an example of a semiconductor device.

[0070] Figure 18A This is a plan view showing an example of a semiconductor device. Figures 18B to 18D This is a cross-sectional view showing an example of a semiconductor device.

[0071] Figure 19A This is a plan view showing an example of a semiconductor device. Figure 19B and Figure 19C This is a cross-sectional view showing an example of a semiconductor device.

[0072] Figure 20A This is a plan view showing an example of a semiconductor device. Figure 20B and Figure 20C This is a cross-sectional view showing an example of a semiconductor device.

[0073] Figures 21A to 21D This is a cross-sectional view showing an example of a semiconductor device.

[0074] Figure 22A This is a plan view showing an example of a semiconductor device. Figures 22B to 22D This is a cross-sectional view showing an example of a semiconductor device.

[0075] Figure 23A This is a plan view showing an example of a semiconductor device. Figures 23B to 23D This is a cross-sectional view showing an example of a semiconductor device.

[0076] Figure 24A This is a plan view showing an example of a semiconductor device. Figure 24B and Figure 24C This is a cross-sectional view showing an example of a semiconductor device.

[0077] Figure 25A This is a plan view showing an example of a semiconductor device. Figure 25B and Figure 25C This is a cross-sectional view showing an example of a semiconductor device.

[0078] Figure 26A This is a plan view showing an example of a semiconductor device. Figures 26B to 26D This is a cross-sectional view showing an example of a semiconductor device.

[0079] Figure 27A This is a plan view showing an example of a semiconductor device. Figure 27B and Figure 27C This is a cross-sectional view showing an example of a semiconductor device.

[0080] Figure 28A This is a plan view showing an example of a semiconductor device. Figures 28B to 28D This is a cross-sectional view showing an example of a semiconductor device.

[0081] Figure 29A This is a floor plan showing an example of a storage device. Figure 29B and Figure 29C This is a cross-sectional view showing an example of a storage device.

[0082] Figures 30A to 30C This is a cross-sectional view showing an example of a storage device.

[0083] Figure 31A This is a floor plan showing an example of a storage device. Figure 31B and Figure 31C This is a cross-sectional view showing an example of a storage device.

[0084] Figure 32A and Figure 32B This is a cross-sectional view showing an example of a storage device.

[0085] Figure 33A This is a floor plan showing an example of a storage device. Figure 33B This is a cross-sectional view showing an example of a storage device.

[0086] Figure 34 This is a cross-sectional view showing an example of a storage device.

[0087] Figure 35 This is a cross-sectional view showing an example of a storage device.

[0088] Figure 36This is a block diagram illustrating an example of the structure of a semiconductor device.

[0089] Figures 37A to 37G This is a diagram illustrating an example of the circuit structure of a memory cell.

[0090] Figure 38A and Figure 38B This is a three-dimensional diagram illustrating an example of the structure of a semiconductor device.

[0091] Figure 39 This is a block diagram illustrating the CPU.

[0092] Figure 40A and Figure 40B It is a 3D diagram of a semiconductor device.

[0093] Figure 41A and Figure 41B It is a 3D diagram of a semiconductor device.

[0094] Figure 42 This is a schematic diagram illustrating the hierarchy of storage devices.

[0095] Figure 43A and Figure 43B This is a diagram showing an example of an electronic component.

[0096] Figures 44A to 44C This is a diagram illustrating an example of a large computer. Figure 44D This is a diagram illustrating an example of a space device. Figure 44E This is a diagram illustrating an example of a storage system that can be used in a data center.

[0097] Figures 45A to 45F This is a diagram illustrating an example of an electronic device.

[0098] Figures 46A to 46G This is a diagram illustrating an example of an electronic device.

[0099] Figures 47A to 47F This is a diagram illustrating an example of an electronic device.

[0100] Figure 48 This is a diagram showing a cross-sectional TEM image of a sample according to an embodiment.

[0101] Figure 49A1 and Figure 49B1 This is a STEM image of an indium oxide film. Figure 49A2 and Figure 49B2 This is an EDX mapping image of an indium oxide film.

[0102] Figure 50A and Figure 50B This is a cross-sectional STEM image according to an embodiment.

[0103] Figure 51This is a cross-sectional STEM image according to an embodiment.

[0104] Figure 52 These are the measurement results from EDX analysis.

[0105] Figure 53A and Figure 53B This is a cross-sectional STEM image of an indium zinc oxide film.

[0106] Methods of implementing the invention

[0107] The embodiments will be described in detail with reference to the accompanying drawings. Note that the present invention is not limited to the following description, and those skilled in the art will readily understand that its methods and details can be varied in many ways without departing from the spirit and scope of the invention. Therefore, the present invention should not be construed as being limited only to the contents described in the embodiments shown below.

[0108] Note that in the structure of the invention described below, the same symbols are used in different figures to represent the same parts or parts with the same function, and repeated descriptions are omitted. Furthermore, when representing parts with the same function, the same shading lines are sometimes used without additional symbols.

[0109] Furthermore, for ease of understanding, the positions, sizes, and extents of the constituent elements shown in the accompanying drawings may not represent their actual positions, sizes, and extents. Therefore, the disclosed invention is not necessarily limited to the positions, sizes, and extents disclosed in the accompanying drawings.

[0110] In this specification and the like, ordinal numbers such as "first" and "second" are used for convenience, but these ordinal numbers do not limit the number of constituent elements or the order of the constituent elements (e.g., process sequence or stacking sequence). Furthermore, sometimes the ordinal numbers used for constituent elements in one part of this specification differ from those used for the same constituent element in another part of this specification or in the claims.

[0111] A transistor is a type of semiconductor device that can amplify current or voltage, control switching operations (turning on or off), etc. The transistors discussed in this specification include IGFETs (Insulated Gate Field Effect Transistors) and thin-film transistors (TFTs).

[0112] In this specification and the like, transistors that use oxide semiconductors or metal oxides as semiconductor layers, and transistors that contain oxide semiconductors or metal oxides in the channel formation region, are sometimes referred to as OS (Oxide Semiconductor) transistors. Furthermore, transistors that contain silicon in the channel formation region are sometimes referred to as Si transistors.

[0113] Furthermore, in cases where transistors of different polarities are used or the current direction changes during circuit operation, the functions of the "source" and "drain" are sometimes interchanged. Therefore, in this specification, the "source" and "drain" can be interchanged.

[0114] Note that in this specification, etc., oxynitrides refer to materials in which the oxygen content is greater than the nitrogen content in their composition. Nitrogen oxides refer to materials in which the nitrogen content is greater than the oxygen content in their composition. For example, when described as "silicon oxynitride," it refers to a material in which the oxygen content is greater than the nitrogen content in its composition, while when described as "silicon oxynitride," it refers to a material in which the nitrogen content is greater than the oxygen content in its composition.

[0115] Note that the content percentage in this specification refers to the proportion of the components contained in the film. For example, an oxide semiconductor layer contains metal elements X, Y, and Z, and the number of atoms of each metal element X, Y, and Z contained in the oxide semiconductor layer is A. X A Y A Z When the content of metallic element X is such that it can be expressed as A, the percentage of X in the composition of metal can be expressed as A. X / (A X +A Y +A Z Furthermore, when the ratio of the number of atoms of metal elements X, Y, and Z in the oxide semiconductor layer (atomic number ratio) is expressed as B... X B Y B Z When the content of metallic element X is such that B is used, the percentage of X can be expressed as B. X / (B X +B Y +B Z ).

[0116] Furthermore, depending on the situation or state, the "film" and "layer" can be interchanged. For example, a "conductive layer" can be replaced with a "conductive film." Similarly, an "insulating film" can be replaced with an "insulating layer."

[0117] In this specification, "parallel" refers to a state where the angle formed by two straight lines is greater than or equal to -10 degrees and less than 10 degrees. Therefore, it also includes states where the angle is greater than or equal to -5 degrees and less than 5 degrees. "Approximately parallel" refers to a state where the angle formed by two straight lines is greater than or equal to -20 degrees and less than 20 degrees. Furthermore, "perpendicular" refers to a state where the angle formed by two straight lines is greater than or equal to 80 degrees and less than 100 degrees. Therefore, it also includes states where the angle is greater than or equal to 85 degrees and less than 95 degrees. "Approximately perpendicular" refers to a state where the angle formed by two straight lines is greater than or equal to 70 degrees and less than 110 degrees.

[0118] Furthermore, in this specification, "electrical connection" includes connections made via "elements that have a certain electrical function." Here, "elements that have a certain electrical function" are not particularly limited as long as they can transmit and receive electrical signals between the connected objects. For example, "elements that have a certain electrical function" include, in addition to electrodes or wiring, switching elements such as transistors, resistors, coils, and other elements with various functions.

[0119] Note that in this specification, the connection between two nodes via insulators such as the dielectric of a capacitor, the gate insulating film of a transistor, or the interlayer insulating film is not included in the "electrical connection" section.

[0120] Note that, in this specification, a tapered shape refers to a shape in which at least a portion of the side surface of a constituent element is inclined relative to the substrate surface or the surface to be formed. For example, it is preferable to have a region where the angle (also called the tapered angle) formed by the inclined side surface and the substrate surface or the surface to be formed is greater than 0 degrees and less than 90 degrees. Here, the side surface of the constituent element, the substrate surface, and the surface to be formed do not necessarily have to be completely flat; they may also be approximately planar with slight curvature or approximately planar with slight irregularities.

[0121] Note that arrows indicating the X, Y, and Z directions are sometimes included in the accompanying drawings and other materials of this specification. Note that in this specification, "X direction" refers to the direction along the X-axis, and unless explicitly stated otherwise, its direction (clockwise or counterclockwise) is not always distinguished. The same applies to "Y direction" and "Z direction." Furthermore, the X, Y, and Z directions are intersecting directions. For example, the X, Y, and Z directions are orthogonal to each other.

[0122] In this specification and other materials, the cubic crystal system is sometimes referred to as cubic crystal, cubic crystal structure, etc. The same applies to other crystal systems (hexagonal, trigonal, tetragonal, orthorhombic, monoclinic, triclinic).

[0123] (Implementation Method 1)

[0124] In this embodiment, refer to Figures 1A to 14EThis invention describes a semiconductor device according to one aspect of the present invention and a method for manufacturing the semiconductor device. One aspect of the semiconductor device includes a transistor having a semiconductor layer.

[0125] <Structure of Semiconductor Devices>

[0126] Figures 1A to 1D This is a three-dimensional schematic diagram of a semiconductor device. Figure 1B It cuts along the YZ plane, including the dotted line. Figure 1A A three-dimensional diagram of a portion of it. Figure 1A and Figure 1B Arrows indicate the X, Y, and Z directions. Note that... Figure 1A and Figure 1B The same symbols for X, Y, and Z are used throughout, but their directions do not necessarily need to be consistent across these figures. In later figures, the X, Y, and Z directions may also differ between figures.

[0127] like Figure 1A and Figure 1B As shown, a semiconductor device according to one aspect of the present invention includes an insulating layer 20, a semiconductor layer 30, an insulating layer 50 on the semiconductor layer 30, and a conductive layer 60 on the insulating layer 50. Furthermore, a semiconductor device according to one aspect of the present invention sometimes includes a layer 29.

[0128] Figure 1C The insulating layer 20 and the semiconductor layer 30, which are components of a semiconductor device, are shown. Figure 1C As shown, the insulating layer 20 has a groove 91. The semiconductor layer 30 is disposed along a portion of the bottom and a portion of the sidewall of the groove 91.

[0129] In this specification and other materials, the groove may be referred to as a slit or a channel. Furthermore, the groove portion may be referred to as a slit portion or a channel portion. Note that the groove portion may also be referred to as a slit or a channel.

[0130] In a transistor according to one embodiment of the invention, a conductive layer 60 is used as a gate electrode, and an insulating layer 50 is used as a gate insulating layer. Furthermore, the semiconductor layer 30 has a channel forming region. At least a portion of the region of the semiconductor layer that overlaps with the conductive layer 60 across the insulating layer 50 is used as the channel forming region.

[0131] According to one aspect of the present invention, a transistor contains a metal oxide (also referred to as an oxide semiconductor) serving as a semiconductor in a semiconductor layer 30 including a channel formation region. That is, the transistor can be described as an OS transistor. Note that in this specification, etc., the semiconductor layer containing the oxide semiconductor can be referred to as an oxide semiconductor layer. Furthermore, since the semiconductor layer 30 contains a metal oxide, the semiconductor layer 30 can be referred to as a metal oxide layer.

[0132] In an OS transistor, when oxygen vacancies (V0) exist in the channel formation region of the oxide semiconductor... O When oxygen vacancies and impurities are present, the electrical properties can easily change, potentially leading to a decrease in reliability. Therefore, in the channel formation region of an oxide semiconductor, it is preferable to minimize oxygen vacancies and impurities. In other words, it is preferable that the carrier concentration in the channel formation region of the oxide semiconductor is reduced and intrinsically or substantially eigentyped.

[0133] Furthermore, when excessive oxygen is supplied to the semiconductor layer 30, electron traps caused by the excess oxygen form in the insulating layer 50. Consequently, in the OS transistor, forward drift degradation is prone to occur during +GBT (Gate Bias-Temperature) stress testing. In other words, the amount of forward drift degradation increases under +GBT stress testing.

[0134] Therefore, in one aspect of the semiconductor device of the present invention, the impurity concentration in the semiconductor layer 30 is preferably low. Furthermore, it is preferable to supply an appropriate amount of oxygen to the semiconductor layer 30. Additionally, it is preferable to reduce the amount of excess oxygen in the semiconductor layer 30.

[0135] Semiconductor layer 30 is preferably made of indium oxide. In this case, semiconductor layer 30 contains indium and oxygen. In metal oxides, the higher the proportion of indium atoms in the total number of atoms of all metal elements, the higher the field-effect mobility of the transistor. Therefore, by using indium oxide in semiconductor layer 30, the transistor can achieve high on-state current and high frequency characteristics.

[0136] Furthermore, the indium oxide film preferably has crystallinity. For example, the indium oxide film preferably contains grains. Examples of films containing grains include monocrystalline films, polycrystalline films, or amorphous films containing grains. Grain boundaries are observed in polycrystalline films.

[0137] The crystallinity of the semiconductor layer 30 can be analyzed, for example, by X-ray diffraction (XRD), transmission electron microscopy (TEM), or electron diffraction (ED). Alternatively, a combination of the above methods can be used for analysis.

[0138] For example, grains can be observed in high-resolution transmission electron microscopy (TEM) images. Furthermore, grain boundaries can sometimes be observed in high-resolution TEM images, for example. That is, grains and grain boundaries can sometimes be observed in high-resolution TEM images of crystalline films. Note that the total magnification when obtaining the TEM image is preferably 2 million times or more, more preferably 4 million times or more.

[0139] Indium oxide films are more preferably single-crystal. Since single crystals lack grain boundaries, carrier scattering at grain boundaries can be suppressed, thereby enabling transistors with high field-effect mobility. Furthermore, transistors with high reliability can be achieved.

[0140] The indium oxide film can also be polycrystalline or amorphous, containing grains. In this case, it is preferable that no grain boundaries are observed or that the grain boundary content is low in the channel formation region. For example, by placing a single grain in the channel formation region, a structure in which no grain boundaries are observed in the channel formation region can be achieved. This structure can also perform the same function as a single-crystal indium oxide film.

[0141] Furthermore, two or more grains can be located in the channel forming region. For example, when the first grain and the second grain are located in the channel forming region, the crystal orientation of the first grain is preferably the same as or substantially the same as the crystal orientation of the second grain. When the crystal orientation of the first grain is the same as or substantially the same as the crystal orientation of the second grain, sometimes no grain boundary is observed at the boundary between the first grain and the second grain. By making the crystal orientation of the first grain the same as or substantially the same as the crystal orientation of the second grain, the formation of grain boundaries between the first grain and the second grain can be suppressed. Therefore, the same effect as the structure where the indium oxide film is a single crystal can be achieved in this structure. For example, sometimes the crystal orientation of the first grain is the same as or substantially the same as the crystal orientation of the second grain can be observed in high-resolution TEM images. Specifically, in high-resolution TEM images, the lattice fringes of the first grain and the second grain are continuously connected at the boundary between the first grain and the second grain.

[0142] Note that in this specification, a grain boundary refers, for example, to the boundary between adjacent grains with different crystal orientations. Therefore, in this specification, the boundary between adjacent grains with the same crystal orientation is not included in the term grain boundary. For example, even if the boundary between two grains is observed in a high-resolution TEM image, it is sometimes not referred to as a grain boundary when the crystal orientations of the two grains are consistent or substantially consistent.

[0143] Furthermore, crystal orientation can be evaluated using diffraction patterns observed by nanobeam electron diffraction (NBED). Alternatively, crystal orientation can also be evaluated using patterns obtained by performing a Fast Fourier Transform (FFT) on a TEM image (also known as FFT patterns). FFT patterns reflect the same reciprocal space information as the diffraction patterns described above.

[0144] For example, in each FFT pattern of the first grain and the second grain, when the angle difference between their FFT patterns is -5 degrees or more and 5 degrees or less, preferably -3 degrees or more and 3 degrees or less, and more preferably -2 degrees or more and 2 degrees or less, it can be said that the crystal orientation of the first grain and the crystal orientation of the second grain are consistent or approximately consistent. Note, for example, the angle of the FFT pattern in the orientation

[111] refers to the acute angle formed by the approximate straight line between the spot originating from the (222) plane and the spot originating from the (-2-2-2) plane and the center spot and the reference line (e.g., a straight line extending in the vertical direction).

[0145] The polycrystalline degree of indium oxide films can be evaluated based on the grain size. The grain size can be calculated, for example, by calculating the grain area, assuming a circle corresponding to that area, and using the diameter of that circle as the grain size. This diameter is sometimes referred to as the equivalent circular area diameter, etc.

[0146] Furthermore, the polycrystalline nature of indium oxide films can be evaluated based on the elongation length of grain boundaries. The elongation length of grain boundaries can be calculated, for example, by extracting a specific area of ​​field of view from a TEM image of the film obtained at a total magnification sufficient to observe the grain boundaries, and using the sum of the lengths of the grain boundaries observed in that field of view as the elongation length. An indium oxide film with an elongation length of 0 nm can be considered a single crystal. This also implies that the longer the elongation length of the grain boundaries, the greater the grain boundary composition.

[0147] The elongation length of grain boundaries in the indium oxide film is preferably 0 nm or more and 1500 nm or less, more preferably 0 nm or more and 1000 nm or less, and even more preferably 0 nm or more and 800 nm or less. By having an indium oxide film with an elongation length of grain boundaries within the aforementioned range in the semiconductor layer 30, a structure in which no grain boundaries are observed or where the grain boundary composition is low can be achieved. Note that, unless otherwise specified in this specification, the field of view used for calculating the elongation length of grain boundaries is 90 nm squared.

[0148] The thickness of the semiconductor layer 30 is preferably 2 nm or more and 50 nm or less, more preferably 2.5 nm or more and 30 nm or less, even more preferably 2.5 nm or more and 20 nm or less, even more preferably 5 nm or more and 20 nm or less, and still more preferably 5 nm or more and 10 nm or less. Furthermore, at least a portion of the semiconductor layer 30 may have the aforementioned thickness. For example, a region in the channel formation region of the semiconductor layer 30 may have the aforementioned thickness. Increasing the thickness of the semiconductor layer 30 can increase the on-state current of the transistor. On the other hand, when the thickness of the semiconductor layer 30 is too thick, the grain boundary elongation length increases, and the on-state current of the transistor may decrease due to the scattering of charge carriers in the grain boundaries. Furthermore, reducing the thickness of the semiconductor layer 30 can suppress the decrease in threshold voltage, thereby enabling normally-off transistors. Furthermore, by setting the thickness of the semiconductor layer 30 within the aforementioned range, the crystallinity of the semiconductor layer 30 can be improved. By improving the crystallinity of the semiconductor layer 30, the semiconductor layer 30 can contain grains.

[0149] Furthermore, when metal oxides contain indium and zinc, they sometimes exhibit a CAAC (c-axis aligned crystalline) structure. CAAC structures have fewer grain boundaries on the ab plane than polycrystalline structures. Examples of metal oxides containing indium and zinc include indium zinc oxide (also known as In-Zn oxide, IZO (registered trademark)) and indium gallium zinc oxide (also known as In-Ga-Zn oxide, IGZO).

[0150] In highly crystalline oxide semiconductor layers, indium oxide (IO) films are, for example, films where hydrogen and oxygen migrate more readily than IGZO films. Therefore, IO films can be considered, for example, films where hydrogen and oxygen are more readily supplied and discharged than IGZO films. Furthermore, IO films can be considered, for example, films with higher permeability to hydrogen and oxygen than IGZO films. In other words, IO films can be considered, for example, films with lower barrier properties to hydrogen and oxygen than IGZO films.

[0151] The indium oxide film preferably has the following properties: in a heat treatment at a heating temperature of 400°C and a treatment time of 8 hours, for example, 1×10 20 atoms / cm 3 Above and 2×10 21 atoms / cm 3 Oxygen permeability within the following range is preferably 2×10 20 atoms / cm 3 Above and 1×10 21 atoms / cm 3Oxygen permeability within the following range. Furthermore, the indium oxide film preferably possesses the following properties: [e.g., 1×10⁻⁶] [This refers to a specific heat treatment process, e.g., heat treatment at 400°C for 8 hours, resulting in a film with a permeability of 1×10⁻⁶]. 20 atoms / cm 3 Above and 2×10 21 atoms / cm 3 The following is preferred: 2×10 20 atoms / cm 3 Above and 1×10 21 atoms / cm 3 Oxygen diffuses within the grains within the following range.

[0152] By allowing oxygen in the indium oxide film to diffuse through grains and grain boundaries, the amount of V present in grains or grain boundaries can be reduced. O Therefore, the electrical characteristics and reliability of transistors can be improved.

[0153] Furthermore, the permeability of the membrane to oxygen and hydrogen can be evaluated, for example, using calculations based on the NEB (Nudged elastic band) method. Specifically, this can be evaluated by calculating the migration barriers of oxygen and hydrogen atoms using the NEB method. In other words, the smaller the migration barrier value, the easier it is for the atom to migrate (the easier it is to permeate).

[0154] Table 1 shows an example of the calculation results. The In₂O₃ shown in Table 1 is the crystal model of indium oxide, and the IGZO shown is the crystal model of In-Ga-Zn oxide. Note that the excess oxygen shown in Table 1 refers to oxygen not located at lattice positions or oxygen located between lattice points.

[0155] [Table 1]

[0156]

[0157] Table 1 shows that the migration barriers for oxygen, hydrogen, and excess oxygen are large in the In-Ga-Zn oxide crystal model but small in the indium oxide crystal model. This indicates that oxygen and hydrogen migrate more easily (permeate more readily) in indium oxide compared to In-Ga-Zn oxide. Furthermore, the permeability of the indium oxide film to oxygen and hydrogen atoms is higher than that of the In-Ga-Zn oxide film. Therefore, it can be inferred that the indium oxide film is a film where hydrogen and oxygen are easily supplied and expelled. Additionally, it is expected that oxygen can be used to fill the V generated during the +GBT test. O Based on its function, it can be inferred that it can achieve highly reliable transistors.

[0158] Thus, as Figure 3C As shown, diffusion occurs into the indium oxide film (referred to as InO). XOxygen (O) permeates through the indium oxide membrane and is released as oxygen molecules (O2). Additionally, it is sometimes released as water molecules (H2O) by reacting with hydrogen contained in the membrane. Furthermore, when oxygen vacancies (V) are present in the membrane... O When oxygen diffuses, it fills the oxygen vacancies. Because oxygen diffuses easily, indium oxide films can fill oxygen vacancies more readily than IGZO films. Therefore, indium oxide films are more likely to reduce oxygen vacancies compared to IGZO films. Thus, by using indium oxide films in transistors, transistors with extremely high reliability can be realized.

[0159] In addition, such as Figure 3C As shown, hydrogen diffuses through the indium oxide membrane. Hydrogen diffuses from the outside into the indium oxide membrane and is released as hydrogen molecules (H2) through the membrane. Alternatively, as described above, the hydrogen reacts with oxygen contained in the membrane and is released as water molecules.

[0160] The content of the first element in the semiconductor layer 30 is preferably low. Furthermore, the concentration of the first element in the semiconductor layer 30 is preferably low. In particular, the concentration of the first element in the channel forming region is preferably low. Here, the first element is at least one selected from boron, carbon, aluminum, silicon, zinc, and gallium. That is, in the semiconductor layer 30, it is preferable that the concentration of any one of boron, carbon, aluminum, silicon, zinc, and gallium is low; more preferably, the concentration of two selected from boron, carbon, aluminum, silicon, zinc, and gallium is low; and even more preferably, the concentrations of each of boron, carbon, aluminum, silicon, zinc, and gallium are low. The concentration of the first element in the semiconductor layer 30 is preferably, for example, 1 atomic% or less, more preferably 0.1 atomic% or less, and even more preferably 0.01 atomic% (100 ppm) or less. Furthermore, the preferred concentration of the first element in the semiconductor layer 30 can also be considered the preferred concentration of the first element in the channel forming region.

[0161] Furthermore, as described below, by using a precursor that has undergone more than one distillation, the concentration of the first element in the semiconductor layer 30 can be set to 0.01 atomic% (100 ppm) or less, 0.0001% (1 ppm) or less, 0.00001% (0.1 ppm or 100 ppb) or less, or 0.0000001% (0.001 ppm or 1 ppb) or less. In other words, the content (purity) of indium other than oxygen in the semiconductor layer 30 can be set to 99.99 atomic% or more (4N), 99.9999 atomic% or more (6N), 99.99999 atomic% or more (7N), or 99.9999999 atomic% or more (9N), making it possible to form a semiconductor layer 30 with a purity equivalent to that of silicon used in the semiconductor layer (10N).

[0162] The crystallinity of semiconductor layer 30 can be improved by reducing the concentration of boron, carbon, aluminum and silicon in semiconductor layer 30.

[0163] When the semiconductor layer 30 contains gallium atoms, these gallium atoms bond with excess oxygen atoms to form a Ga-O structure. The Ga-O structure acts as an acceptor for trapped electrons. Therefore, in transistors including a semiconductor layer 30 containing both gallium atoms and excess oxygen atoms, the threshold voltage variation in the PBTS (Positive Bias Temperature Stress) test increases. Therefore, by reducing the gallium concentration in the semiconductor layer 30, the threshold voltage variation in the PBTS test can be reduced. Thus, a transistor with high reliability when applying a positive bias voltage can be realized. Furthermore, when the semiconductor layer 30 contains zinc atoms, the same situation may occur as when it contains gallium atoms.

[0164] Furthermore, aluminum, gallium, and zinc atoms have stronger bonding forces with oxygen atoms compared to indium atoms. Therefore, by reducing the concentration of aluminum, gallium, and zinc in the indium oxide film, the decrease in oxygen permeability can be suppressed.

[0165] Furthermore, impurities such as the first element contained in the indium oxide film can act as crystal nuclei. By minimizing impurities in the indium oxide film, the number of crystal nuclei can be reduced, which can promote larger crystal sizes as described below.

[0166] Furthermore, when the indium oxide film is a polycrystalline film, the first element segregates at the grain boundaries, forming an oxide containing the first element. Because this oxide has insulating properties, it can potentially cause a decrease in the transistor's on-state current or field-effect mobility. By minimizing the amount of the first element in the indium oxide film, the transistor's on-state current or field-effect mobility can be improved.

[0167] Furthermore, by reducing impurities in the indium oxide film, impurity scattering can be suppressed. This allows for the realization of transistors with high field-effect mobility. For example, by setting the concentration of the first element in the semiconductor layer 30 within the aforementioned preferred range, the field-effect mobility of the transistor can be set to 100 cm⁻¹. 2 / (V·s) or more, preferably 150cm 2 / (V·s) or more, more preferably 200cm 2 / (V·s) or more, further preferably 250cm 2 / (V·s) above.

[0168] Furthermore, Non-Patent Literature 2 reports the fact that, assuming the primary cause of scattering in indium oxide is ionized impurities and polar optical phonons, the Hall mobility is calculated to have an upper limit of 270 cm⁻¹. 2 / (V·s)(reference) Figure 2 ).

[0169] Here, the carrier concentration dependence of Hall mobility for indium oxide, silicon, and IGZO is explained. Figure 3A It concerns silicon (Si) and indium oxide (InO). X A schematic diagram illustrating the carrier concentration dependence of Hall mobility. Figure 3B This is a schematic diagram showing the carrier concentration dependence of Hall mobility in IGZO.

[0170] First, such as Figure 3B As indicated by the arrows, IGZO tends to exhibit higher Hall mobility with higher carrier concentrations. On the other hand, as... Figure 3A As indicated by the arrows, indium oxide (INO) tends to exhibit higher Hall mobility with lower carrier concentrations (see Non-Patent Literature 3). This tendency is similar to that of silicon; the lower the concentration of dopants (impurities) in the material, the less impurity scattering occurs, and the higher the Hall mobility. In other words, in INO, higher purity and more intrinsic properties result in higher Hall mobility. From this result, it can be concluded that, unlike IGZO, INO possesses properties close to those of silicon. Note that... Figure 3A The properties of indium oxide shown are those assuming a single crystal. Therefore, when indium oxide is not a single crystal (e.g., polycrystalline), its properties may differ. Figure 3A The characteristics shown are different.

[0171] exist Figure 3B In this context, the range R1, characterized by low carrier concentration, corresponds to a range with extremely high Hall mobility. Therefore, it can be considered, for example, a suitable range of carrier concentrations for use in the channel formation region of a transistor. For instance, in indium oxide, the range R1 includes carrier concentrations of 1 × 10⁻⁶. 15 cm -3 The range, for example, is 1×10 14 cm -3 Above and 1×10 18 cm -3 The following range. By sufficiently reducing the carrier concentration, it is expected that the Hall mobility value can be increased to 270 cm⁻¹. 2 / (V) (s) around.

[0172] Furthermore, in indium oxide, the region with a carrier concentration in the range R1 can contain elements that reduce the carrier concentration. Examples of elements that reduce carrier concentration include magnesium, calcium, cadmium, and copper. Replacing indium with these elements reduces the carrier concentration. Other examples of elements that reduce carrier concentration include nitrogen, phosphorus, arsenic, and antimony. For example, replacing oxygen with nitrogen, phosphorus, arsenic, or antimony reduces the carrier concentration.

[0173] On the other hand, the range of high carrier concentration R2 is the range of low resistance; for example, it can be said to be the range of carrier concentrations suitable for use in the source and drain regions of transistors, resistive bodies, or transparent conductive films. The range R2 includes carrier concentrations of 1 × 10⁻⁶. 20 cm -3 The range, for example, is 1×10 19 cm -3 Above and 1×10 22 cm -3 The following range. By significantly increasing the carrier concentration, it is expected that the resistivity can be reduced to 1 × 10⁻⁶. -4 Ω Less than cm.

[0174] Furthermore, in indium oxide, the region with a carrier concentration in the range R2 can contain elements that increase the carrier concentration. For example, it is preferable to include the same elements as the source and drain electrodes of the transistor. Examples of elements that increase the carrier concentration include titanium, tantalum, tungsten, molybdenum, tin, silicon, germanium, zirconium, hafnium, and boron. In particular, it is more preferable to use elements whose oxides have conductive or semiconductor properties.

[0175] Thus, in indium oxide, regions with low carrier concentration are used for the channel formation region of the transistor, while regions with high carrier concentration are used for the source and drain regions. In other words, indium oxide can also be considered an oxide capable of controlling valence electrons. Note that valence electron control in silicon transistors is generally known. On the other hand, valence electron control in indium oxide transistors is a novel technical concept that is not usually considered. Based on this technical concept, transistors with high mobility, low off-state current, and the ability to be normally off can be realized.

[0176] Furthermore, the concentration of the first element can be evaluated using methods such as inductively coupled plasma mass spectrometry (ICP-MS), X-ray photoelectron spectroscopy (XPS), secondary ion mass spectrometry (SIMS), time-of-flight secondary ion mass spectrometry (ToF-SIMS), Auger electron spectroscopy (AES), energy dispersive X-ray spectroscopy (EDX), or inductively coupled plasma atomic emission spectrometry (ICP-AES).

[0177] Hydrogen contained in oxide semiconductors reacts with oxygen bonded to metal atoms to form water, sometimes creating oxygen vacancies. This can cause electrical properties to fluctuate, leading to decreased reliability. On the other hand, hydrogen present at grain boundaries can sometimes terminate dangling bonds at grain boundaries, improving the electrical properties and reliability of transistors. Therefore, while it is preferable to reduce the hydrogen concentration in the indium oxide film, the hydrogen concentration can sometimes be higher than the concentration of the first element.

[0178] Indium oxide has a band gap of 2.5 eV or higher and 3.7 eV or lower. By using indium oxide, which has a larger band gap than silicon, in semiconductor layer 30, the off-state current of transistors can be reduced, thus significantly reducing the power consumption of semiconductor devices.

[0179] OS transistors are accumulation transistors where electrons are the majority carriers. In other words, the carriers in an OS transistor are electrons. Assuming a constant relaxation time for the carriers, the smaller the effective mass of the electrons (carriers), the higher the electron mobility (carrier mobility). That is, by using metal oxides with small effective electron mass in the semiconductor layer of the transistor, the on-state current or field-effect mobility of the transistor can be improved.

[0180] Table 2 shows the effective masses of single-crystal indium oxide (In₂O₃ in this case) and single-crystal silicon (Si). The effective masses of electrons and holes shown in Table 2 are values ​​calculated using first-principles electronic state calculations.

[0181] [Table 2]

[0182]

[0183] As shown in Table 2, indium oxide (IO) has a low effective electron mass. Therefore, by using IO, which has a low effective electron mass, in semiconductor layer 30, transistors with high on-state current, high field-effect mobility, and high frequency characteristics (also known as f-characteristics) can be realized. Furthermore, IO has the characteristic that the effective electron mass is almost independent of crystal orientation. Moreover, the effective electron mass of IO is, for example, smaller than that of silicon. Therefore, from the viewpoint of effective electron mass, transistors using IO in the channel formation region exhibit higher f-characteristics than Si transistors.

[0184] As shown in Table 2, indium oxide (IO) has a large effective hole mass. Therefore, by using IO with a large effective hole mass in semiconductor layer 30, transistors with extremely low off-state current can be realized. Furthermore, the effective hole mass of IO is, for example, greater than that of silicon. Therefore, from the viewpoint of effective hole mass, the off-state current of transistors using IO in the channel formation region is significantly smaller than that of Si transistors.

[0185] In a transistor using indium oxide as the semiconductor layer 30, the off-state current value per channel width of 1 μm at room temperature (25 °C) can be set to 1 × 10⁻⁶. -17 Below A / μm, preferably 1×10 -18 A / μm or less, more preferably 1×10 -19 Below A / μm. Furthermore, the off-state current value per channel width of 1μm at 85°C can be set to 1×10⁻⁶. -16 Below A / μm, preferably 1×10 -17 A / μm or less, more preferably 1×10 -18 Below A / μm.

[0186] Furthermore, miniaturizing the OS transistor can improve its high-frequency characteristics. For example, the transistor's cutoff frequency (fT) can be increased. Specifically, at room temperature (25°C), the transistor's cutoff frequency can be 50 GHz or higher, preferably 100 GHz or higher, and more preferably 150 GHz or higher.

[0187] Indium oxide films can contain one or more of the periodic elements with high period numbers in the periodic table, within a range that exhibits crystallinity. There is a tendency for greater overlap of the orbitals of metal elements in metal oxides to result in greater carrier conductivity. Therefore, by including periodic elements with high period numbers in the periodic table, the field-effect mobility of transistors can sometimes be improved. Examples of periodic elements with high period numbers in the periodic table include elements belonging to period 5 and period 6. Specifically, examples of such elements include yttrium, zirconium, silver, cadmium, tin, antimony, barium, lead, bismuth, and light rare earth elements (lanthanum, cerium, praseodymium, neodymium, promethium, samarium, and europium).

[0188] Figure 1B An example of a single-layer structure for semiconductor layer 30 is shown. Furthermore, semiconductor layer 30 can have a stacked structure of two or more layers. For example, in the case where semiconductor layer 30 has a two-layer structure of a first semiconductor layer and a second semiconductor layer on the first semiconductor layer, it is preferable to use a metal oxide (typically indium oxide) suitable for the aforementioned semiconductor layer 30 as the first semiconductor layer, and a metal oxide whose conduction band bottom is closer to the vacuum level than that of the first semiconductor layer as the second semiconductor layer. In this case, the first semiconductor layer can be primarily used as a current path (channel). That is, the surface of the first semiconductor layer on the side of the second semiconductor layer and its vicinity have a channel forming region.

[0189] By employing the above structure, the number of carriers trapped at and near the interface of the first semiconductor layer can be reduced. Furthermore, by positioning the channel away from the surface of the insulating layer 50, the effects of surface scattering can be reduced. This, in turn, improves the electric field mobility of the transistor.

[0190] As metal oxides that can be used for the second semiconductor layer, examples include indium gallium oxide (In-Ga oxide), In-Zn oxide, indium tin oxide (In-Sn oxide, also denoted as ITO), indium titanium oxide (In-Ti oxide), indium aluminum zinc oxide (In-Al-Zn oxide, also denoted as IAZO), In-Ga-Zn oxide, indium tin zinc oxide (also denoted as In-Sn-Zn oxide), indium titanium zinc oxide (In-Ti-Zn oxide), and indium tin oxide containing silicon oxide (also denoted as ITSO). Alternatively, zinc oxide, aluminum zinc oxide (Al-Zn oxide, also denoted as AZO), and aluminum tin oxide (Al-Sn oxide) can be used.

[0191] Specifically, the In-Zn oxide used for the second semiconductor layer can have an In:Zn ratio of 1:1 or similar, an In:Zn ratio of 2:1 or similar, or an In:Zn ratio of 4:1 or similar. Similarly, the IGZO used for the second semiconductor layer can have an In:Ga:Zn ratio of 1:1:1 or similar, an In:Ga:Zn ratio of 1:3:2 or similar, or an In:Ga:Zn ratio of 1:3:4 or similar.

[0192] There are no particular restrictions on the crystallinity of the metal oxide contained in the second semiconductor layer. For example, the second semiconductor layer may sometimes contain one or more of the following: amorphous semiconductor (semiconductor with an amorphous structure), single-crystal semiconductor (semiconductor with a single-crystal structure), and semiconductor with crystallinity other than single crystal (microcrystalline semiconductor, polycrystalline semiconductor, or a portion thereof having a crystalline region).

[0193] Figure 1D The insulating layer 20 and layer 29 are shown as components of a semiconductor device. Figure 1D As shown, the island-shaped layer 29 is arranged in contact with the insulating layer 20. Figure 1D In the middle, layer 29 is disposed in contact with the top surface of insulating layer 20 on the outside of trench 91. Semiconductor layer 30 is disposed as a cover layer 29.

[0194] Layer 29 contains crystals. When a process is performed to improve the crystallinity of semiconductor layer 30, layer 29 is used as a seed or nucleus. In other words, layer 29 is used as a seed or nucleus during the crystal growth of semiconductor layer 30. In this specification, layer 29 or the crystals contained in layer 29 may be referred to as seed crystals or nuclei. Furthermore, since layer 29 contains crystals, layer 29 may be referred to as a crystalline portion.

[0195] Indium oxide has a cubic crystal structure (manganese permanganate type). When indium oxide is used in semiconductor layer 30, layer 29 preferably contains, for example, hexagonal or trigonal crystals. In this case, by making layer 29 contain crystals with a crystal orientation relative to the surface of layer 29 or the surface to which it is formed... <001> The crystallization can form crystals with a crystal orientation of <111> The crystalline semiconductor layer 30. The crystal orientation of the crystals contained in layer 29 relative to the surface of layer 29 or the surface in which they are formed is... <001> At this time, the c-axis of the crystal is perpendicular or substantially perpendicular to the surface of layer 29 or the surface on which it is formed. Note that hexagonal or trigonal crystals can sometimes be referred to as crystals with layered structures, so the above structure can be considered as a structure in which a semiconductor layer 30 containing cubic crystals is formed on a layer 29 containing crystals with layered structures. In other words, it can also be considered as a stacked structure manufactured using heteroepitaxial growth technology or a technique such as heteroepitaxial growth.

[0196] In this specification, space groups are represented using shortnotation of the International Notation (or Hermann-Mauguin notation). Furthermore, Miller indices are used to represent crystal faces and crystal orientations. In crystallography, a superscript is added to numbers to indicate space groups, crystal faces, and crystal orientations. However, in this specification, due to the notation limitations in the patent application, a - (negative number symbol) is sometimes added before numbers to indicate space groups, crystal faces, and crystal orientations instead of a superscript. Additionally, "[ ]" indicates the individual orientation within a crystal, "< >" indicates the collective orientation of all equivalent orientations, "()" indicates the individual face of a crystal face, and "{}" indicates a collective face with equivalent symmetry.

[0197] In this specification and the like, the crystal orientation of a crystal refers to its orientation relative to the surface of the film containing the crystal or the surface on which it is formed. Therefore, for example, the crystal orientation is... <100> The crystallization can be described as the (100) plane being parallel to the surface of the film containing the crystal or the surface to which the crystal is formed.

[0198] Specifically, zinc oxide, In-Ga oxide, gallium zinc oxide (Ga-Zn oxide, also denoted as GZO), aluminum zinc oxide (Al-Zn oxide, also denoted as AZO), In-Al-Zn oxide, In-Ga-Zn oxide, or In-Sn-Zn oxide can be used as layer 29. In-Ga-Zn oxide is preferred as layer 29. In this case, layer 29 contains indium, gallium, zinc, and oxygen. Furthermore, its composition is preferably In:Ga:Zn = 1:1:1 [atomic ratio] or close to it, or In:Ga:Zn = 1:3:2 [atomic ratio] or close to it. Since the metal oxides with the above compositions readily form layered structures, they are suitable for use as layer 29. Note that the nearby composition includes a range of ±30% of the desired atomic ratio.

[0199] In-Ga-Zn oxides and In-Sn-Zn oxides readily possess a CAAC structure. When an oxide with a CAAC structure is used as layer 29, the c-axis of the crystals contained in layer 29 is perpendicular or substantially perpendicular to the surface of layer 29 or the plane to which it is formed. In other words, the crystal orientation of the crystals contained in layer 29 relative to the surface of layer 29 or the plane to which it is formed is... <001> Therefore, by using oxides that readily possess a CAAC structure for layer 29, the controllability of the crystal orientation of the crystals contained in layer 29 can be improved.

[0200] Here, Figures 4A to 4E The crystal structure of the metal oxide is shown. Figure 4A This is a diagram of the crystal structure of an In-Ga-Zn oxide with an In:Ga:Zn ratio of 1:1:1 [atomic number ratio], viewed from a direction perpendicular to the c-axis. Figure 4B Viewed from the c-axis direction Figure 4A The diagram shows the surface indicated by the dashed lines. Figure 4C Viewed from the c-axis direction Figure 4A The dotted lines in the diagram represent the surface, and Figure 4D Viewed from the c-axis direction Figure 4A The diagram shows the surface indicated by the double-dotted line. Figure 4A , Figure 4C and Figure 4D In this context, Mx represents either a Ga atom or a Zn atom. Note that in... Figure 4A In Chinese, the surfaces shown by dashed lines, dotted lines, and double-dotted lines are sometimes collectively referred to as surface c. Furthermore, Figure 4E This is a diagram of the crystal structure of indium oxide viewed from the direction perpendicular to the (111) plane.

[0201] The interatomic spacing of the metal on the c-plane ( Figures 4B to 4D The arrows shown are considered to be 0.330 nm. Furthermore, the In-In distance in the (111) plane ( Figure 4EThe arrows shown are considered to be 0.334 nm and 0.385 nm. In other words, the c-plane of the CAAC structure is similar to the metal atom configuration of the (111) plane of indium oxide. Therefore, oxides that readily have a CAAC structure can be used as layer 29.

[0202] When an oxide that readily possesses a CAAC structure is used for layer 29, a structure containing crystal orientations can be formed. <111> The crystalline semiconductor layer 30. Note that when layer 29 is disposed in a region of insulating layer 20 that does not overlap with trench 91, the crystal orientation of the grains of semiconductor layer 30 located in the region of insulating layer 20 that does not overlap with trench 91 can be set as follows: <111> .

[0203] Figure 5A and Figure 5B A cross-sectional view of the upper end of the groove 91 and the insulating layer 20 and semiconductor layer 30 in its vicinity is shown. Figure 5A and Figure 5B In the diagram, layer 29, insulating layer 50, and conductive layer 60 are omitted. Parallel to semiconductor layer 30... <111> The crystal growth rate in the orientation direction is higher than that perpendicular to the direction. <111> When the crystal growth rate is fast in the orientation direction, such as Figure 5A As shown, the semiconductor layer 30 contains grains of... <111> The orientation is readily perpendicular or approximately perpendicular to the substrate surface (not shown). Furthermore, depending on the crystal orientation and configuration of the seed layer 29, such as... Figure 5B As shown, the grains <111> The orientation is sometimes parallel to the substrate surface. For example, such as... Figure 5C As shown, when layer 29 is provided on the upper part of insulating layer 20, the grains... <111> Orientation is easily perpendicular to the substrate surface. On the other hand, such as Figure 5D As shown, when layer 29 is provided along the side of insulating layer 20, the grains... <111> The orientation is easily parallel to the substrate surface.

[0204] Here, the anisotropy of the effective mass of electrons in indium oxide is small. For example, in indium oxide, the effective mass of electrons in the

[100] orientation,

[110] orientation, and

[111] orientation are approximately the same, ranging from 0.17 to 0.19. Therefore, high field-effect mobility can be obtained regardless of the crystal orientation of the grains located in the channel-forming region.

[0205] Layer 29 can also be an oxide with a cubic crystal structure. By making layer 29 have the same crystal structure as semiconductor layer 30, semiconductor layer 30 can be epitaxially grown using layer 29 as a seed or nucleus, thereby improving the crystallinity of semiconductor layer 30. The crystal structure of oxides containing elements of Group 3 in the periodic table is prone to be cubic. Furthermore, the Group 3 elements in this crystal mainly exist as trivalent cations. Therefore, layer 29 preferably contains at least one element that can be a trivalent cation. The element that can be a trivalent cation contained in layer 29 is preferably scandium, yttrium, cerium, gadolinium, erbium, or ytterbium.

[0206] As layer 29, for example, oxides containing one or both of yttrium and zirconium, erbium oxide, etc., can be used. Examples of oxides containing one or both of yttrium and zirconium include yttrium oxide, zirconium oxide, and yttrium zirconium oxide.

[0207] Furthermore, the difference between the lattice constant or the length of a unit lattice vector of the crystal nucleus and the lattice constant or the length of a unit lattice vector of the crystal contained in the semiconductor layer 30 (also known as lattice mismatch) is preferably small. By using an oxide with small lattice mismatch in layer 29, the crystallinity of the semiconductor layer 30 can be improved.

[0208] One method for evaluating the degree of lattice mismatch is to use the value of the lattice mismatch degree shown below. The lattice mismatch degree Δa[%] of the crystals contained in the formed film (here, the indium oxide film) relative to the crystals contained in the film being formed is calculated according to the following formula (1). Hereinafter, the lattice mismatch degree Δa of the crystals contained in the formed film relative to the crystals contained in the film being formed is sometimes simply referred to as the lattice mismatch degree Δa of the formed film relative to the film being formed.

[0209] [Equation 1]

[0210]

[0211] In formula (1), L1 represents the lattice constant or the length of the unit lattice vector of the crystal contained in the above-formed film, and L2 represents the lattice constant or the length of the unit lattice vector of the crystal contained in the above-formed film.

[0212] The lattice mismatch Δa of the grains contained in the semiconductor layer 30 relative to the crystal nucleus is preferably -10% or more and 10% or less, more preferably -5% or more and 5% or less, and even more preferably -3% or more and 3% or less. By using a material with a small lattice mismatch relative to the semiconductor layer 30 in layer 29, the crystallinity of the semiconductor layer 30 can be improved.

[0213] For example, the lattice constant of indium oxide crystal (argentite type) is considered to be 1.01194 nm. Furthermore, the lattice constant of yttrium oxide crystal (argentite type) is considered to be 1.05976 nm. Therefore, the lattice mismatch of indium oxide crystal relative to yttrium oxide crystal is -4.5%. Therefore, when indium oxide is used in semiconductor layer 30, yttrium oxide can be used in layer 29.

[0214] For example, the lattice constant of erbium oxide crystal (argentite type) is considered to be 1.0582 nm. Therefore, the lattice mismatch of indium oxide crystal relative to erbium oxide crystal is -4.4%. In the case of using indium oxide as semiconductor layer 30, erbium oxide can be used as layer 29.

[0215] For example, Zr, as an example of yttrium zirconium oxide 0.9 Y 0.1 O 1.95 The lattice constant of the crystal (fluorite type) is 0.51481 nm (refer to ICSD coll.code.248790). Therefore, the lattice constant of indium oxide crystal relative to Zr... 0.9 Y 0.1 O 1.95 The crystal has a lattice mismatch of -1.7%. Therefore, when indium oxide is used for semiconductor layer 30, yttrium zirconium oxide can be used for layer 29. Note that yttrium zirconium oxide contains yttrium, zirconium, and oxygen.

[0216] By adding yttrium or yttrium oxide to yttrium oxide, specifically setting the yttrium content in yttrium zirconium oxide to be greater than 0 atomic%, the crystal structure of yttrium oxide can be stabilized. Note that as this content increases, the crystal structure of yttrium zirconium oxide sometimes changes from a cubic crystal system to other crystal systems; therefore, this content is preferably not too high. Thus, for example, the yttrium content contained in yttrium zirconium oxide is preferably 2 atomic% or more and 15 atomic% or less, more preferably 5 atomic% or more and 10 atomic% or less.

[0217] In addition, indium oxide can also be used as layer 29. By using indium oxide as layer 29, the semiconductor layer 30 can be homoepitaxially grown using layer 29 as a seed or nucleus, thereby improving the crystallinity of the semiconductor layer 30.

[0218] There are no particular restrictions on the materials that can be used for layer 29. Layer 29 can be made of insulating, semiconductor, or conductive materials. When a semiconductor material is used for layer 29, layer 29 can also be considered as part of semiconductor layer 30.

[0219] Figure 6A A cross-sectional view is shown when the upper end of the insulating layer 20 in the groove 91 has a curved surface. Furthermore, Figure 6B yes Figure 6A 3D image, Figure 6C This is a perspective view showing the insulating layer 20 and layer 29. The upper end of the insulating layer 20 has a curved surface, and the top surface of the insulating layer 20 is smoothly continuous with the side surface of the trench 91. Therefore, when the semiconductor layer 30 is crystallized, distortion is less likely to occur at the upper end of the insulating layer 20, thus resulting in a semiconductor layer 30 with fewer crystal defects. This allows for the realization of a transistor with high reliability.

[0220] The radius of curvature R1 of the upper end of the insulating layer 20 in the trench portion 91 can be 1 nm or more and 500 nm or less, preferably 1 nm or more and 300 nm or less, more preferably 1 nm or more and 200 nm or less, and even more preferably 1 nm or more and 100 nm or less. The radius of curvature R1 is preferably greater than the thickness of the semiconductor layer 30. Note that the radius of curvature R1 is preferably at least less than the thickness of the insulating layer 20.

[0221] Furthermore, by making the bottom of the trench 91 also have a curved shape, a semiconductor layer 30 with fewer crystal defects can be obtained as described above. Although Figure 6A An example is shown where a portion of the insulating layer 20 at the bottom of the trench 91 has a curved shape, but this is not limited to the insulating layer 20; other insulating or conductive layers may also have curved shapes. The radius of curvature R2 of the surface of the layer at the bottom of the trench 91 (here, the insulating layer 20) can be 1 nm or more and 500 nm or less, preferably 1 nm or more and 300 nm or less, more preferably 1 nm or more and 200 nm or less, and even more preferably 1 nm or more and 100 nm or less. The radius of curvature R1 is preferably greater than the thickness of the semiconductor layer 30. Note that the radius of curvature R1 is preferably at least less than half the width of the trench 91.

[0222] Figure 7A and Figure 7B A cross-sectional view of the vicinity of the upper end of the insulating layer 20 is shown when the upper end has a curved surface. Figure 7A and 7B Corresponding to Figure 5A and 5B .like Figure 7A and Figure 7B As shown, the upper end of the insulating layer 20 has a curved surface, thus allowing crystal growth to proceed smoothly regardless of the crystal structure, thereby forming a semiconductor layer 30 with good crystallinity throughout. Furthermore, Figure 7C and Figure 7D Corresponding to Figure 5C and Figure 5D This shows an example of setting layer 29.

[0223] Figures 8A to 8CAn example is shown where a pair of layers 40 are included on the upper portion of the insulating layer 20. The layers 40 are separated by a groove 91. Furthermore, the layers 40 have a curved surface at the upper end of the groove 91. Additionally, in Figures 8A to 8C In this structure, layer 70 is included at the bottom of the trench 91. Layer 70 has a curved surface at the bottom of the trench 91. Thus, the layer on which the semiconductor layer 30 is formed can be a layer other than the insulating layer 20, and in this case, the layer on which the semiconductor layer 30 is formed preferably has a curved surface. Layers 40 and 70 can be made of conductive materials, semiconductor materials, or insulating materials. For example, if conductive materials are used for layers 40 and 70, layer 40 can be used as one of the source electrode and drain electrode, and layer 70 can be used as the other of the source electrode and drain electrode.

[0224] Figure 1D An example is shown where layer 29 appears circular when viewed from a plane. Note that the invention is not limited to this. The shape of layer 29 when viewed from a plane can be, for example, a circle or an ellipse, or an approximate circle; a triangle, a quadrilateral (including rectangles, rhombuses, and squares), a pentagon, or a star-shaped polygon; or a shape where the corners of these polygons are rounded. Furthermore, when sputtered particles are used as layer 29, layer 29 may sometimes appear triangular or hexagonal when viewed from a plane.

[0225] In addition, such as Figure 9A As shown, layer 29 can also be conical. For example, the angle formed between the top surface of the insulating layer 20 on the outer side of the trench 91 and the side surface of layer 29 can be less than 90°, preferably 30° or more and less than 90°. By making layer 29 conical, the coverage of semiconductor layer 30 can be improved, thereby reducing defects such as voids. In addition, the crystal growth of semiconductor layer 30 can be promoted.

[0226] Figure 1D An example with island-shaped layers 29 is shown. Note that the invention is not limited thereto. For example, as... Figure 9B As shown, layer 29 can also have a region extending in a direction perpendicular to the Z direction. Or, for example, as... Figure 9C and Figure 9D As shown, layer 29 can also be provided on the outside of groove 91 in a manner that covers the top surface of insulating layer 20.

[0227] Alternatively, a layer can be provided between the insulating layer 20 and the layer 29. Figure 9E and Figure 9F This illustrates a structure in which a layer 40 is disposed between insulating layer 20 and layer 29. That is, Figure 9E and Figure 9F The structure shown can be said to be in Figure 9C and Figure 9DThe structure shown includes a layer 40. Furthermore, layer 40 can be a conductive material, a semiconductor material, an insulating material, or a stack of two or more of these materials. For example, when a conductive material is used as layer 40, layer 40 is in contact with the semiconductor layer 30 (not shown) at least on the side of the trench 91, and therefore can be used as a source electrode or a drain electrode.

[0228] Figure 1D An example is shown where layer 29 is disposed in contact with the top surface of the insulating layer 20 on the outer side of the groove 91. Note that the invention is not limited thereto. For example, such as Figure 10A and Figure 10B As shown, layer 29 can also be provided in a manner that is embedded in an opening provided in the insulating layer 20. This allows the top surface of the insulating layer 20 outside the groove 91 to be flattened, improving the crystallinity of the semiconductor layer 30. Furthermore, layer 29 embedded in the aforementioned recess can also have an extended region (see reference). Figure 10C ).

[0229] Figure 9C and Figure 9D An example is shown where layer 29 is disposed on the outer side of groove 91. Note that the invention is not limited thereto. For example, as... Figure 11A and Figure 11B As shown, a portion of layer 29 may also be disposed at the bottom of groove 91. Alternatively, for example, as... Figure 11C and Figure 11D or Figure 11E and Figure 11F As shown, layer 29 can also be provided in contact with at least a portion of the sidewall of groove 91.

[0230] By providing layer 29 in contact with at least a portion of the sidewall of groove 91, a structure containing... <111> Semiconductor layer 30 with grains oriented in a direction consistent with or substantially consistent with the direction perpendicular to the sidewall of the trench 91. Furthermore, in semiconductor layer 30, when perpendicular to... <111> Crystal growth rate in the orientation direction is higher than that parallel to the direction. <111> When the crystal growth rate is fast in the orientation direction, such as Figure 5D As shown, the semiconductor layer 30 contains grains of... <111> The orientation is easily parallel or approximately parallel to the substrate surface (not shown).

[0231] The thickness of layer 29 is preferably thin. For example, the thickness of layer 29 is preferably smaller than the thickness of semiconductor layer 30. Specifically, layer 29 preferably has a region with a thickness of 0.1 nm or more and less than 2 nm, and more preferably has a region with a thickness of 0.5 nm or more and less than 2 nm. By reducing the thickness of layer 29, the step between layer 29 and insulating layer 20 is reduced. Therefore, the coverage of semiconductor layer 30 is improved, and defects such as voids can be reduced. In addition, the crystal growth of semiconductor layer 30 can be promoted. Note that layer 29 can be layered or granular.

[0232] The insulating layer 50 preferably has the function of supplying oxygen to the semiconductor layer 30. The insulating layer 50 preferably has, for example, regions containing oxygen that has been released by heating (hereinafter sometimes referred to as excess oxygen). By contacting the semiconductor layer 30 with the insulating layer having regions containing excess oxygen, oxygen can be supplied to the semiconductor layer 30. The oxygen supplied to the semiconductor layer 30 repairs oxygen vacancies, thereby reducing the amount of oxygen vacancies in the semiconductor layer 30. Examples of insulating materials that readily form regions containing excess oxygen include silicon oxide, silicon oxynitride, or porous silicon oxide.

[0233] Furthermore, the insulating layer 50 preferably has the function of trapping or fixing (also known as gettering) oxygen. As mentioned above, indium oxide film is a film in which oxygen readily migrates. Therefore, when the insulating layer 50 has the function of trapping or fixing oxygen, excess oxygen in the semiconductor layer 30 diffuses to the insulating layer 50, and this oxygen can be trapped or fixed. Therefore, the OS transistor can suppress the positive drift degradation caused by excess oxygen in the +GBT stress test. Examples of insulating materials with the function of trapping or fixing oxygen include alumina, hafnium oxide, hafnium zirconium oxide, and oxides containing hafnium and silicon (hafnium silicate).

[0234] Note that aluminum oxide, hafnium oxide, hafnium zirconium oxide, and hafnium silicate have the function of capturing or fixing hydrogen. As mentioned above, indium oxide film is a film in which hydrogen easily migrates. Therefore, when the insulating layer 50 has the function of capturing or fixing hydrogen, hydrogen diffuses from the semiconductor layer 30 to the insulating layer 50, and the hydrogen can be captured or fixed. As a result, the hydrogen concentration in the semiconductor layer 30 (especially the hydrogen concentration in the channel formation region) can be reduced.

[0235] Figure 1B An example of a single-layer structure for the insulating layer 50 is shown. Note that the insulating layer 50 may have a stacked structure of two or more layers. When the insulating layer 50 has a stacked structure of two or more layers, the insulating material (typically alumina) that can be used in the insulating layer 50 is preferably the layer that contacts the semiconductor layer 30 among the two or more layers included in the insulating layer 50. By adopting this structure, oxygen can be supplied to the semiconductor layer 30 and the amount of oxygen vacancies can be reduced. In addition, excess oxygen in the semiconductor layer 30 can be discharged to the insulating layer 50. Furthermore, hydrogen in the semiconductor layer 30 can be trapped or fixed.

[0236] The insulating layer 20 preferably has the function of supplying oxygen to the semiconductor layer 30. For example, the insulating layer 20 preferably has a region containing excess oxygen. Furthermore, the insulating layer 50 preferably has the function of trapping or fixing oxygen. By employing this structure, oxygen can be forced into the semiconductor layer 30 from the insulating layer 20 side to reduce the amount of oxygen vacancies in the semiconductor layer 30, and excess oxygen in the semiconductor layer 30 can be pulled out from the insulating layer 50 side to reduce excess oxygen in the semiconductor layer 30. Thus, a semiconductor device with high reliability can be provided.

[0237] Furthermore, the insulating layer 20 preferably uses a material with a smaller coefficient of thermal expansion than the metal oxide used for the semiconductor layer 30. For example, the insulating layer 20 can use a material with a smaller coefficient of thermal expansion than indium oxide. Specifically, the coefficient of thermal expansion of the insulating layer 20 is preferably 0.01 × 10⁻⁶. -6 K -1 Above and 5.5×10 -6 K -1 Hereinafter, 0.01×10 is more preferred. -6 K -1 Above and 5.0×10 -6 K -1 Hereinafter, 0.01×10 is further preferred. -6 K -1 Above and 3.0×10 -6 K -1 The following is a further preferred value of 0.01×10 -6 K -1 Above and 1.0×10 -6 K -1 The following describes how, through this structure, by placing the semiconductor layer 30 containing indium oxide in contact with or near an insulating layer 20 with a low coefficient of thermal expansion, tensile stress is applied to the indium oxide upon cooling, making it energy-unstable. As a result, the indium oxide becomes a more energy-stable cubic crystal. Furthermore, crystal growth can be promoted to form large-grained cubic crystals. Since silicon oxide has a lower coefficient of thermal expansion than indium oxide, it is suitable for use in the insulating layer 20.

[0238] Table 3 shows the coefficients of thermal expansion for oxide semiconductors and insulators. In Table 3, the coefficients of thermal expansion for IGZO and indium oxide (In2O3) are shown as oxide semiconductors, and the coefficients of thermal expansion for silicon oxide (SiO2), silicon nitride (Si3N4), and yttrium-stabilized zirconium oxide (YSZ) are shown as insulators.

[0239] [Table 3]

[0240]

[0241] Figure 1B An example of a single-layer structure for the insulating layer 20 is shown. Alternatively, the insulating layer 20 may have a stacked structure of two or more layers. When the insulating layer 20 has a stacked structure of two or more layers, the layer in contact with the semiconductor layer 30 among the two or more layers included in the insulating layer 20 is preferably an insulating material suitable for the aforementioned insulating layer 20 (typically silicon oxide). By employing this structure, the crystallinity of the semiconductor layer 30 can be improved.

[0242] As the conductive layer 60, a material with high conductivity, such as tungsten, is preferably used. Furthermore, as the conductive layer 60, a conductive material that is not easily oxidized or a conductive material that has the function of inhibiting oxygen diffusion is preferably used. Examples of such conductive materials include nitrogen-containing conductive materials (e.g., titanium nitride or tantalum nitride) and oxygen-containing conductive materials (e.g., ruthenium oxide). This helps to suppress the decrease in conductivity of the conductive layer 60.

[0243] Furthermore, the conductive layer 60 preferably uses a conductive material containing the metal element and oxygen contained in the metal oxide forming the channel. For example, one or more selected from ITO, indium oxide containing tungsten oxide, indium zinc oxide containing tungsten oxide, indium oxide containing titanium oxide, indium tin oxide containing titanium oxide, In-Zn oxide, and ITSO can also be used. In addition, indium gallium zinc oxide containing nitrogen can also be used. By using the above materials, hydrogen contained in the metal oxide forming the channel can sometimes be trapped. Alternatively, hydrogen mixed in from the insulating layer or the like outside the transistor can sometimes be trapped.

[0244] In this embodiment, an example is shown where the groove 91 extends in the X direction. Note that the invention is not limited thereto. The shape of the groove 91 when viewed in a plane can be, for example, a circle or an ellipse, or an approximate circle; a triangle, a quadrilateral (including rectangles, rhombuses, and squares), a pentagon, or a star-shaped polygon; or the corners of these polygons are rounded. Note that the circle is not limited to a perfect circle. The polygon can also be a concave polygon (a polygon with at least one interior angle exceeding 180 degrees) or a convex polygon (a polygon with all interior angles less than 180 degrees).

[0245] <Examples of Semiconductor Device Manufacturing Methods>

[0246] The following describes an example of a method for manufacturing a semiconductor device according to one aspect of the present invention. One example of the method for manufacturing a semiconductor device described herein includes a method for manufacturing a semiconductor layer.

[0247] Figure 12A , Figure 12C , Figure 12E , Figure 13A , Figure 13C and Figure 13EThis is a three-dimensional schematic diagram of a semiconductor device. Figure 12B , Figure 12D , Figure 12F , Figure 13B , Figure 13D and Figure 13F This is a cross-sectional view of a semiconductor device viewed from the X direction.

[0248] The layers constituting the semiconductor device (insulating layer 20, layer 29, semiconductor layer 30, insulating layer 50, and conductive layer 60, etc.) can be formed using sputtering, chemical vapor deposition (CVD), vacuum evaporation, molecular beam epitaxy (MBE), pulsed laser deposition (PLD), or atomic layer deposition (ALD). In particular, the semiconductor layer 30 and the insulating layer 50 are preferably formed using ALD.

[0249] Unlike deposition methods that deposit particles released from a target or similar material, ALD (Alternating Layer Deposition) is a deposition method that forms a film through a reaction on the surface of the workpiece. Therefore, ALD is a deposition method with good step coverage, less affected by the shape of the workpiece. In particular, ALD exhibits excellent step coverage and thickness uniformity, making it suitable for covering surfaces with high aspect ratios, such as openings or grooves.

[0250] The precursors used in ALD (Alternating Discharge) methods sometimes contain elements such as carbon or chlorine. Therefore, films formed using ALD methods sometimes contain more carbon or chlorine than films formed using other deposition methods. Furthermore, the quantification of these elements can be performed using XPS or SIMS. Note that by employing one or both of the following methods during ALD, the amount of carbon and chlorine contained in the film can sometimes be reduced compared to using ALD without employing these methods: high substrate temperature during deposition and impurity removal processes.

[0251] Examples of ALD methods include thermal ALD (thermal ALD) which uses only thermal energy to react precursors and reactants, and plasma ALD (PEALD) which uses reactants excited by plasma.

[0252] In a deposition apparatus utilizing the ALD method, a first source gas (sometimes referred to as a precursor, precursor, or metal precursor) and a second source gas (sometimes referred to as a reactant, reactant, oxidant, or nonmetal precursor) are alternately introduced into the chamber, and this introduction of source gases is repeated to achieve deposition. Note that, for example, the introduced source gas can be switched by switching various on / off valves (sometimes referred to as high-speed valves). Furthermore, inert gases such as nitrogen (N2), argon (Ar), or helium (He) can be used as carrier gases when introducing the source gas, and they are introduced into the chamber along with the source gas. By using a carrier gas, even if the source gas has low volatility or vapor pressure, adsorption of the source gas into the pipes and valves can be suppressed, thereby allowing the source gas to be introduced into the chamber. Furthermore, the uniformity of the formed film is improved, making this method preferred.

[0253] When using the ALD method, films of arbitrary composition can be deposited by simultaneously introducing multiple different precursors. Alternatively, by controlling the number of cycles for each precursor when introducing multiple different precursors, films of arbitrary composition can be deposited.

[0254] First, such as Figure 12A and Figure 12B As shown, an insulating layer 20 is formed on a substrate (not shown). The top surface of the insulating layer 20 is preferably flat. By making the top surface of the insulating layer 20 flat, the crystallinity of the semiconductor layer 30 formed subsequently can be improved. For example, lateral growth of the crystals contained in the semiconductor layer 30 during the first heat treatment described later can be promoted.

[0255] The insulating layer 20 can be formed, for example, by sputtering in an oxygen-containing atmosphere. By using a sputtering method that does not require the use of hydrogen-containing molecules as a deposition gas, the hydrogen concentration in the insulating layer 20 can be reduced. Furthermore, by forming the insulating layer 20 using a sputtering method in an oxygen-containing atmosphere, oxygen can be added to the insulating layer 20. Since the heat applied after the formation of the semiconductor layer 30 can supply oxygen from the insulating layer 20 to the semiconductor layer 30, defects such as oxygen vacancies and hydrogen ingress into oxygen vacancies (hereinafter sometimes referred to as V) can be reduced. O H).

[0256] Before forming layer 29, it is preferable to perform a heat treatment. As a heat treatment, for example, it can be performed at a temperature of 250°C or higher and 650°C or lower, preferably 300°C or higher and 500°C or lower, and more preferably 320°C or higher and 450°C or lower.

[0257] The heat treatment is performed in an atmosphere of nitrogen or an inert gas, or in an atmosphere containing 10 ppm (0.001%) or more, 1% or more, or 10% or more of an oxidizing gas. For example, when the heat treatment is performed in a mixed atmosphere of nitrogen and oxygen gas, the ratio of oxygen gas is preferably set to about 20%. The heat treatment can also be performed under reduced pressure. Alternatively, the heat treatment can be performed in a nitrogen or inert gas atmosphere, and then, in order to replenish the detached oxygen, the heat treatment is performed in an atmosphere containing 10 ppm or more, 1% or more, or 10% or more of an oxidizing gas. By performing the above-described heat treatment, impurities such as hydrogen or water contained in the insulating layer 20, etc., can be reduced before the deposition of the semiconductor layer 30.

[0258] Furthermore, the gas used in the above-described heat treatment is preferably of high purity. For example, the water content in the gas used in the above-described heat treatment is preferably 1 ppb (1 × 10⁻⁶). -3 ppm or less, more preferably 0.1 ppb (1×10⁻⁶ ppm). -4 ppm or less, more preferably 0.05 ppb (5 × 10⁻⁶ ppm), -5 (ppm) or less. By using a highly purified gas for heating treatment, it is possible to minimize the absorption of moisture and other substances by the insulating layer 20.

[0259] There are no particular restrictions on the heating device used for heat treatment; devices that utilize heat conduction or thermal radiation generated by heating elements such as resistance heating elements can also be used to heat the workpiece. For example, electric furnaces or RTA (Rapid Thermal Annealing) devices such as LRTA (Lamp Rapid Thermal Annealing) devices and GRTA (Gas Rapid Thermal Annealing) devices can be used. LRTA devices heat the workpiece using radiation of light (electromagnetic waves) emitted from lamps such as halogen lamps, metal halide lamps, xenon arc lamps, carbon arc lamps, high-pressure sodium lamps, or high-pressure mercury lamps. GRTA devices use high-temperature gases for heat treatment.

[0260] Furthermore, it is preferable to perform the oxygen supply process before forming layer 29. Oxygen is thus supplied to insulating layer 20, and oxygen can be supplied from insulating layer 20 to semiconductor layer 30 by applying heat or the like after forming semiconductor layer 30.

[0261] Examples of oxygen supply methods include heating in an oxygen-containing atmosphere or plasma treatment (including microwave plasma treatment) in an oxygen-containing atmosphere. Alternatively, oxygen can be supplied to the insulating layer 20 by depositing an oxide film (preferably a metal oxide film) in an oxygen-containing atmosphere using sputtering. The deposited oxide film can be removed immediately or left as a residue. When the deposited oxide film remains, it can be used as part of the semiconductor layer 30. Furthermore, the oxygen-containing atmosphere includes, in addition to oxygen gas (O2), atmospheres containing oxygen-containing compounds such as ozone (O3) or nitrous oxide (N2O). Additionally, the substrate temperature in the plasma treatment is above room temperature (25°C) and below 450°C.

[0262] Next, layer 29 is formed on insulating layer 20. Figure 12A and Figure 12B Layer 29 is used as a seed or nucleus for the crystal growth of semiconductor layer 30. Therefore, layer 29 can be referred to as a seed layer, seed crystal, etc.

[0263] There are no particular limitations on the method of forming layer 29. For example, insulating layer 29 can be formed by forming and processing the film that will become layer 29. The film can be formed by sputtering, CVD, vacuum evaporation, MBE, PLD or ALD, etc.

[0264] Layer 29 can also be formed using sputtering. By forming layer 29 using sputtering, the crystallinity of layer 29 can be improved. Furthermore, by forming insulating layer 29 using sputtering in an oxygen-containing atmosphere, oxygen can be added to insulating layer 20.

[0265] When a sputtering target has multiple grains with a layered structure and easily cleavable interfaces within the grains, ions can collide with the sputtering target, sometimes causing the grains to cleave and resulting in plate-shaped or granular sputtered particles. The plate-shaped or granular sputtered particles deposited on the insulating layer 20 can also be used as layer 29. For example, when the grains contain indium, gallium, zinc, and oxygen, and their crystal structure is hexagonal or trigonal, the grains are easily cleaved at the {001} plane. Therefore, the plate-shaped or granular sputtered particles are deposited on the insulating layer 20 with their {001} planes parallel to the surface of the insulating layer 20. Thus, by using plate-shaped or granular sputtered particles as layer 29, a structure containing crystals with a specific orientation can be formed. <111> The crystalline semiconductor layer 30.

[0266] Next, as Figure 12A and Figure 12BAs shown, the insulating layer 20 is processed to form a groove 91. The groove 91 extends in the X direction. When forming the groove 91, a portion of the insulating layer 20 can be processed using an etching process. In particular, dry etching is suitable for micro-machining and is therefore preferred.

[0267] Furthermore, by forming the groove 91 without processing the film that will become layer 29, it is possible to form... Figure 9C and Figure 9D Layer 29 is shown. Therefore, compared to processing this film, the number of manufacturing steps in a semiconductor device can be reduced.

[0268] Furthermore, by sequentially forming films that will become layers 40 and 29 on the insulating layer 20 and forming grooves 91, it is possible to manufacture... Figure 9E and Figure 9F The structure shown.

[0269] Alternatively, an opening can be formed in the insulating layer 20, allowing the film that will become layer 29 to be embedded in the opening. The film can then be polished using CMP or similar methods until the surface of the insulating layer 20 is exposed, thereby forming... Figure 10A and Figure 10B Layer 29 or shown Figure 10C Layer 29 is shown. This allows the top surface of the insulating layer 20 on the outer side of the groove 91 to be flat.

[0270] Alternatively, by forming the film that will become layer 29 using sputtering after forming the groove 91, it is possible to form... Figure 11A and Figure 11B Layer 29 is shown. Therefore, compared to processing this film, the number of manufacturing steps for the semiconductor device can be reduced. Alternatively, it can be removed by anisotropic etching such as dry etching. Figure 11A and Figure 11B A portion of layer 29 shown can be formed Figure 11C and Figure 11D Layer 29 is shown.

[0271] Alternatively, after forming the trench 91, a film that will become layer 29 can be formed using a deposition method with good coverage, such as ALD. A portion of this film can then be removed by anisotropic etching, such as dry etching, thereby forming... Figure 11E and Figure 11F Layer 29 is shown.

[0272] As described above, by forming layer 29 before forming semiconductor layer 30, the effect of heat on semiconductor layer 30 can be reduced, thereby suppressing the miniaturization of crystals contained in semiconductor layer 30 and the increase of grain boundaries.

[0273] Next, as Figure 12C and Figure 12DAs shown, a semiconductor layer 30 is formed with a capping layer 29 and a trench 91. The semiconductor layer 30 is preferably formed using a sputtering method. As the sputtering gas, a rare gas (typically argon), a single gas of oxygen, or a mixture of a rare gas and oxygen can be used. The proportion of the rare gas (typically argon) in the total sputtering gas is, for example, 50% or more and 100% or less, preferably 70% or more and 100% or less, more preferably 90% or more and 100% or less. By increasing the proportion of the rare gas (typically argon) in the total sputtering gas, a semiconductor layer 30 with low crystallinity can be formed. Furthermore, a semiconductor layer 30 with many dangling bonds can be formed. Therefore, the etching rate of the semiconductor layer 30 can be increased. Thus, the processing of the semiconductor layer 30 becomes easier, and the productivity of semiconductor devices can be improved. Note that the semiconductor layer 30 with low crystallinity has, for example, an amorphous structure.

[0274] Note that the sputtering gas may also contain hydrogen (H2). By introducing hydrogen during the formation of the semiconductor layer 30 using sputtering, a semiconductor layer 30 with low crystallinity can be formed. Furthermore, during the formation of the semiconductor layer 30, the generation of crystal nuclei can be suppressed or the elimination of crystal nuclei can be promoted. Moreover, when there are many crystal nuclei, the growing crystals collide with each other, thereby suppressing large-size crystals. In other words, small-size crystals are formed. However, by further reducing the number of crystal nuclei by eliminating some of the crystal nuclei in the film while suppressing the generation of crystal nuclei, and performing the first heat treatment described later, crystal growth can be promoted with fewer crystal nuclei, thereby increasing the grain size in the semiconductor layer 30.

[0275] The semiconductor layer 30 can also be formed by sputtering in an oxygen-containing atmosphere. In this case, by using a sputtering method that does not require the use of hydrogen-containing molecules as the deposition gas, the hydrogen concentration in the semiconductor layer 30 can be reduced. For example, oxygen or a mixture of oxygen and rare gases can be used as the sputtering gas.

[0276] Furthermore, the semiconductor layer 30 can also be formed using the ALD method. When forming the semiconductor layer 30, a first precursor and a first oxidant can be used. The first precursor preferably contains indium. At this time, an indium oxide film is formed as the semiconductor layer 30. In other words, an oxide film containing a single element other than oxygen is deposited. Note that when the first precursor contains indium, the ALD method can be a thermal ALD method.

[0277] As precursors containing indium, for example, trimethylindium, triethylindium, ethyl dimethylindium, tris(1-methylethyl)indium, tris(2,2,6,6-tetramethyl-3,5-heptanoic acid)indium, cyclopentadienylindium, iridium(III) acetylacetonate, 3-(dimethylamino)propyl)dimethylindium, (diethylphosphine)dimethylindium, dimethylchloroindium, dimethylbromoindium, dimethyl(2-propanol)indium, etc.

[0278] In addition, inorganic precursors that do not contain hydrocarbons can also be used as indium-containing precursors. Halogenated indium compounds such as indium trifluoride (indium(III) fluoride), indium trichloride (indium(III) chloride), indium tribromide (indium(III) bromide), and indium triiodide (indium(III) iodide) can be used as indium-containing inorganic precursors. The decomposition temperature of indium trichloride is approximately 500°C to 700°C. Therefore, by using indium trichloride, deposition can be performed using the ALD method while heating the substrate to approximately 400°C to 600°C, for example, 500°C.

[0279] In the method for forming the semiconductor layer 30, it is preferable to use a precursor with low impurity concentration, i.e., high purity. For example, by using a precursor with a purity of 3N (99.9%) or higher, preferably 4N (99.99%) or higher, more preferably 5N (99.999%) or higher, and even more preferably 6N (99.9999%) or higher, impurities in the semiconductor layer 30 can be reduced.

[0280] The gallium and aluminum content of the indium-containing precursor is preferably 1000 ppm or less, more preferably 500 ppm or less, even more preferably 100 ppm or less, further preferably 50 ppm or less, even more preferably 10 ppm or less, and even more preferably 1 ppm or less. By using a precursor with low gallium content, the gallium concentration in the semiconductor layer 30 can be reduced, thereby improving the reliability of the transistor. By using a precursor with low aluminum content, the aluminum concentration in the semiconductor layer 30 can be reduced, thereby improving the crystallinity of the semiconductor layer 30.

[0281] Furthermore, as the precursor used in this embodiment, it is preferable to use a precursor purified by performing two or more distillations (also known as rectification or precision distillation). Using the aforementioned precursor allows for the easy deposition of metal oxides with few impurities, which is therefore preferred. Multiple distillations further suppress the residue of impurities from the starting materials used in the precursor's production, which is also preferred. Note that the present invention is not limited to the above structure; a precursor purified by single distillation (i.e., one distillation) can also be used. Using single distillation reduces manufacturing costs, which is therefore preferred.

[0282] By performing one or more distillations, the aluminum content of the indium-containing precursor can be set to below 100 ppm, below 1 ppm, or below 1 ppb (0.001 ppm). Using this indium-containing precursor, it may be possible to form an indium oxide film with a purity equivalent to that of silicon (10N) used for semiconductor layers.

[0283] As the first oxidant, ozone (O3), oxygen (O2), water (H2O), hydrogen peroxide (H2O2), etc., can be used. The first oxidant preferably includes at least one of ozone and oxygen. By using ozone, oxygen, etc., which do not contain hydrogen, as the first oxidant, the amount of hydrogen mixed into the insulating layer 20 can be reduced. Furthermore, the first oxidant can include at least one of water and hydrogen peroxide. Thus, a semiconductor layer 30 with low crystallinity can be formed.

[0284] In this specification and the like, unless otherwise specified, when ozone, oxygen, and water are used as oxidants, they also include plasma states, free radical states, and ionic states, and are not limited to gaseous states or molecular states.

[0285] The pulse duration for introducing the first oxidant is preferably 0.1 seconds or more and 30 seconds or less, more preferably 0.3 seconds or more and 15 seconds or less, and even more preferably 0.3 seconds or more and 10 seconds or less. By shortening the pulse duration for introducing the first oxidant, the amount of the first oxidant introduced is reduced, and most of the hydrogen contained in the first precursor remains in the membrane. By allowing more hydrogen to remain in the membrane, the formation of crystal nuclei can be suppressed while eliminating some of the crystal nuclei in the membrane, thereby reducing the number of crystal nuclei in the membrane.

[0286] Here, the substrate heating temperature when the first precursor is introduced into the reaction chamber is preferably a temperature corresponding to the decomposition temperature of the first precursor. In the thermal ALD method using triethylindium as the indium-containing precursor, the substrate heating temperature can be, for example, 100°C or higher and 350°C or lower, preferably 150°C or higher and 300°C or lower. When layer 29 is provided, the substrate heating temperature can be room temperature (25°C) or higher and 300°C or lower, preferably room temperature or higher and 200°C or lower, more preferably room temperature or higher and 150°C or lower. By lowering the substrate heating temperature, the crystallinity of the semiconductor layer 30 during deposition can be reduced.

[0287] When the semiconductor layer 30 has a stacked structure, it can be formed using methods such as sputtering and ALD (Alternating Deposition). For example, when the semiconductor layer 30 has a two-layer structure consisting of a first semiconductor layer and a second semiconductor layer on the first semiconductor layer, the first semiconductor layer can be deposited using ALD and the second semiconductor layer can be deposited using sputtering. Because the coverage of the ALD method is superior to that of the sputtering method, the coverage of the semiconductor layer 30 can be improved by depositing the first semiconductor layer using ALD. Therefore, oxide semiconductor layers can be used to effectively cover steps and openings with high aspect ratios. Furthermore, productivity can be improved by depositing the second semiconductor layer using sputtering.

[0288] Alternatively, a first semiconductor layer can be deposited using sputtering, and a second semiconductor layer can be deposited using ALD. Even if pinholes or breaks are formed in the first semiconductor layer deposited using sputtering, the overlapping portions with the aforementioned pinholes or breaks can be filled using a second semiconductor layer deposited using the well-covering ALD method.

[0289] Next, the semiconductor layer 30 is processed into the desired shape. Figure 12E and Figure 12F In this process, the semiconductor layer 30 is processed into an island shape to form multiple semiconductor layers 30. Specifically, the semiconductor layers 30 are processed in a manner in which the multiple semiconductor layers 30 are separated in the X direction.

[0290] Furthermore, it is preferable to supply the second element (or add or implant the second element) to the semiconductor layer 30 before processing the semiconductor layer 30. This supplies the second element to the semiconductor layer 30. By supplying the second element to the semiconductor layer 30, the crystallinity of the semiconductor layer 30 can be reduced. Therefore, the processing of the semiconductor layer 30 becomes easier, and the productivity of the semiconductor device can be improved.

[0291] As the second element, one or more of hydrogen and rare gases (helium, neon, argon, krypton, xenon, etc.) are preferred.

[0292] Plasma processing can be applied when supplying the second element. When using plasma processing, the second element can be supplied by generating plasma in a gas atmosphere containing the supplied second element. As an apparatus for generating the plasma, a dry etching apparatus, an ashing apparatus, a plasma CVD apparatus, or a high-density plasma CVD apparatus can be used. By accelerating the supply of the second element, the collision energy during the supply of the second element to the semiconductor layer 30 increases, which can more effectively reduce the crystallinity of the semiconductor layer 30, and is therefore preferred.

[0293] Note that the supply of the second element is not limited to the methods described above; for example, ion implantation can also be used. Ion implantation can precisely control the concentration distribution in the depth direction based on the ion acceleration energy and dosage. Furthermore, by using ion implantation to mass-separate the ions by ionizing the source gas, a specific mass of ions can be supplied, and the purity of the supplied second element can be improved. Alternatively, by using ion implantation to supply ions without mass separation, productivity can be improved. In this specification, unless otherwise specified, the presence or absence of mass separation is not limited. Note that sometimes the method of supplying ions by mass separation is called ion implantation, and the method of supplying ions without mass separation is called ion doping.

[0294] As the source gas, a gas containing the second element can be used. When argon is used as the second element, argon gas can be used as the source gas. Furthermore, when argon and hydrogen are used as the second element, a mixture of argon and hydrogen gas can be used as the source gas. Alternatively, a mixture of a gas containing the second element and other gases can also be used. Note that the raw material used to supply the second element is not limited to a gas; it can also be a solid or liquid that has been heated to vaporize it.

[0295] Next, a first heat treatment is performed. The first heat treatment is preferably performed, for example, in an atmosphere containing at least one of hydrogen (H2) and nitrogen (N2), more preferably in an atmosphere containing both hydrogen (H2) and nitrogen (N2). At this time, the hydrogen flow rate ratio is preferably 3% or more and 15% or less, more preferably 5% or more and 10% or less. Note that the hydrogen flow rate ratio refers to the proportion of hydrogen gas flow rate to the total gas flow rate. Furthermore, the temperature of the first heat treatment is preferably 120°C or more and 300°C or less, more preferably 120°C or more and 250°C or less, and even more preferably 120°C or more and 200°C or less. Furthermore, the duration of the first heat treatment is preferably 1 hour or more and 8 hours or less.

[0296] By performing a first heat treatment, using layer 29 as a seed or nucleus, the epitaxial growth and lateral grain growth of semiconductor layer 30 can be advanced, thereby improving the crystallinity of semiconductor layer 30. In particular, using a material with a low coefficient of thermal expansion in insulating layer 20 can promote crystal growth. For example, grains formed in the portion of semiconductor layer 30 overlapping with layer 29 undergo lateral growth, thereby allowing semiconductor layer 30 to crystallize along trench 91. That is, as... Figure 13A and Figure 13B As shown, using layer 29 as the seed or nucleus, crystallization proceeds laterally, causing region 31c to expand. Region 31c is a region with higher crystallinity than region 31a. With the passage of processing time, region 31c further expands along the formed surface ( Figure 13C and Figure 13D Then, at the end of the first heat treatment, region 31c diffuses into the entire semiconductor layer 30. Figure 13E and Figure 13F This improves the crystallinity of semiconductor layer 30. Thus, indium oxide that improves crystallinity by growing crystals laterally from the crystal nucleus is called Lateral Growth Indium Oxide (LGIO).

[0297] Furthermore, by using silicon oxide, which has a low coefficient of thermal expansion, in insulating layer 20 and applying tensile stress to indium oxide from the bottom and sidewalls of trench 91 during cooling, the crystal growth of semiconductor layer 30 can be promoted.

[0298] Next, a second heat treatment is performed. The second heat treatment is preferably performed in an atmosphere containing nitrogen and oxygen (typically, a nitrogen:oxygen volume ratio of 4:1). The temperature of the second heat treatment is preferably higher than that of the first heat treatment. For example, it is preferably 300°C or higher and 400°C or lower, more preferably 300°C or higher and 350°C or lower. Furthermore, the duration of the second heat treatment is preferably 1 hour or more and 4 hours or less.

[0299] The gas used for the second heating treatment is preferably highly purified. By using a highly purified gas for heating treatment, the absorption of moisture and other substances by the semiconductor layer 30 can be minimized.

[0300] There are no particular restrictions on the heating treatment used for the second heating treatment; for example, an electric furnace or an RTA device can be used.

[0301] By performing the first heat treatment at a temperature lower than that of the second heat treatment, the generation of crystal nuclei can be suppressed, and the crystals can be made larger in size. Furthermore, since the first heat treatment is performed in a reducing atmosphere, the amount of oxygen vacancies contained in the semiconductor layer 30 increases. Therefore, by performing the second heat treatment, oxygen can be supplied to the semiconductor layer 30, and the supplied oxygen can fill the oxygen vacancies (making them null). Furthermore, by performing the first heat treatment at a temperature lower than that of the second heat treatment, impurities sometimes remain in the semiconductor layer 30. Therefore, by performing the second heat treatment at a temperature higher than that of the first heat treatment, the impurity concentration in the semiconductor layer 30 can be reduced. Furthermore, the hydrogen concentration in the semiconductor layer 30 can be reduced. Moreover, by performing the second heat treatment, the grains in the semiconductor layer 30 can be made larger.

[0302] As described above, by sequentially performing the first heating treatment and the second heating treatment, the amount of oxygen vacancies and impurities in the semiconductor layer 30 can be reduced while the semiconductor layer 30 is crystallizing and growing.

[0303] Alternatively, microwave plasma treatment can be performed after depositing the semiconductor layer 30. This microwave plasma treatment can reduce the concentration of impurities such as hydrogen or water contained in the semiconductor layer 30. Furthermore, sometimes crystalline regions of the semiconductor layer 30 are grown.

[0304] In this specification and the like, microwaves refer to electromagnetic waves with frequencies of 300 MHz or higher and 300 GHz or lower. Microwave plasma treatment, for example, refers to a process using a device that includes a power source for generating high-density plasma using microwaves. Microwave plasma treatment may also be referred to as microwave-excited high-density plasma treatment.

[0305] By performing microwave plasma treatment in an oxygen-containing atmosphere, the impurity concentration in the semiconductor layer 30 can be reduced. Carbon is an example of an impurity. Note that the above describes a structure in which the semiconductor layer 30 is subjected to microwave plasma treatment in an oxygen-containing atmosphere, but the method is not limited thereto. For example, an insulating film disposed near the semiconductor layer 30, more specifically, a silicon oxide film, can also be subjected to microwave plasma treatment in an oxygen-containing atmosphere. Furthermore, due to the heat generated during microwave plasma treatment, the crystallinity of the semiconductor layer 30 is sometimes improved.

[0306] Microwave plasma treatment is preferably carried out under reduced pressure, preferably 10 Pa or more and 1000 Pa or less, more preferably 50 Pa or more and 700 Pa or less, and even more preferably 100 Pa or more and 400 Pa or less. Furthermore, the treatment temperature is preferably room temperature (25°C) or more and 750°C or less, more preferably 300°C or more and 500°C or less, and can be 400°C or more and 450°C or less.

[0307] During microwave plasma treatment, the substrate can also be heated. The heating temperature of the substrate is preferably above room temperature (e.g., 25°C), above 100°C, above 200°C, above 300°C, or above 400°C and below 500°C, or below 450°C. For example, the heating temperature of the substrate is preferably above room temperature and below 500°C, more preferably above 100°C and below 450°C, even more preferably above 200°C and below 450°C, even more preferably above 300°C and below 450°C, and still even more preferably above 400°C and below 450°C.

[0308] For example, oxygen and argon gases can be used for microwave plasma treatment. However, when the oxygen flow ratio (O2 / (O2+Ar)) in microwave plasma treatment is too high, stable discharge is difficult to achieve. Therefore, for example, the oxygen flow ratio (O2 / (O2+Ar)) is preferably greater than 0% and less than 50%, more preferably greater than 0% and less than 40%, and even more preferably greater than 0% and less than 30%.

[0309] In microwave plasma treatment using oxygen and argon gases, the main oxygen free radicals can be triplet oxygen (O( 3 P j Singlet oxygen (O( 1 D2) and oxygen ions (O2) +The three states of the oxide film are as follows. Furthermore, oxygen ions play an effective role in reducing the hydrogen concentration in the oxide film through microwave plasma treatment. Moreover, the amount of oxygen free radicals in each state varies depending on the oxygen flow rate ratio or pressure during microwave plasma treatment. For example, under conditions of low oxygen flow rate ratio and low pressure, there is a tendency for the amount of oxygen ions to increase. On the other hand, when the oxygen flow rate ratio or pressure is too low, there are concerns such as: unstable control of the oxygen flow rate makes it difficult to stabilize the discharge; and etching of the oxide film, etc. Therefore, for example, the oxygen flow rate ratio (O2 / (O2+Ar)) during microwave plasma treatment is preferably greater than 0% and less than 10%, more preferably more than 0.5% and less than 5%, further preferably more than 0.5% and less than 3%, and typically preferably 1%.

[0310] The shorter the processing time of microwave plasma treatment, the higher the productivity. Therefore, for example, the processing time of microwave plasma treatment is preferably more than 1 minute and less than 60 minutes, more preferably more than 1 minute and less than 30 minutes, and even more preferably more than 1 minute and less than 10 minutes.

[0311] By performing microwave plasma treatment in an oxygen-containing atmosphere, oxygen gas can be plasmaized using microwaves or RF (radio frequency) to generate oxygen free radicals that act on the oxide semiconductor layer. Due to the effects of plasma, microwaves, and oxygen free radicals, the Vo in the oxide semiconductor layer can be deionized. O H is divided into oxygen vacancies and hydrogen, and hydrogen is removed from the oxide semiconductor layer. This reduces V in the oxide semiconductor layer. O H. At this time, carbon bonded to oxygen or hydrogen can sometimes also be removed. Thus, impurities can be reduced by performing microwave plasma treatment. Furthermore, by supplying the aforementioned oxygen radicals to the oxygen vacancies formed in the oxide semiconductor layer, oxygen vacancies in the oxide semiconductor layer can be further reduced.

[0312] Furthermore, when some oxygen in the oxide semiconductor present before microwave plasma treatment reacts with hydrogen in the oxide semiconductor, i.e., when the reaction "2H + O → H₂O↑" occurs, this hydrogen can be removed as H₂O (also known as dehydration or dehydrogenation). Since H₂O is one of the main factors hindering the improvement of crystallinity, it is preferable to remove H₂O from the oxide semiconductor. Removing hydrogen from the oxide semiconductor as H₂O reduces the hydrogen concentration in the oxide semiconductor, thereby promoting improved crystallinity. Furthermore, by increasing the temperature in the microwave plasma treatment, the hydrogen concentration in the oxide semiconductor can be further reduced.

[0313] Alternatively, the heating process can be performed continuously after microwave plasma treatment without exposure to the atmosphere. The heating temperature is preferably 100°C or higher and 750°C or lower, more preferably 300°C or higher and 500°C or lower, and even more preferably 400°C or higher and 450°C or lower. By keeping the temperature within the above range, even when performing this heating treatment, substrate deformation (strain or warping) can be minimized.

[0314] Note that plasma treatment containing oxygen gas can also be used instead of microwave plasma treatment to improve crystallinity.

[0315] The oxygen supplied to the oxide semiconductor layer can take various forms, such as oxygen atoms, oxygen molecules, oxygen ions (charged oxygen atoms or oxygen molecules), and oxygen free radicals (oxygen atoms, oxygen molecules, or oxygen ions containing unpaired electrons). Furthermore, the oxygen implanted into the oxide semiconductor layer is preferably one or more of the aforementioned forms, and particularly preferably oxygen free radicals.

[0316] Alternatively, a hydrogen supply process (also known as hydrogenation) can be performed on the semiconductor layer 30 before the insulating layer 50 is formed. By supplying hydrogen to the semiconductor layer 30, dangling bonds present at grain boundaries or the like can sometimes be terminated, thereby improving the electrical characteristics and reliability of the transistor. Other examples of hydrogen supply processes include heating in a hydrogen-containing atmosphere or plasma treatment.

[0317] Next, an insulating layer 50 is formed to cover the semiconductor layer 30. The insulating layer 50 is preferably formed by an ALD (Alternating Deposition) method. When forming the insulating layer 50, a second precursor and a second oxidant can be used. The second precursor preferably contains one of aluminum and hafnium. At this time, an aluminum oxide film or a hafnium oxide film is formed as the insulating layer 50. In other words, an oxide film containing a single element other than oxygen is deposited. Note that when the second precursor contains one of aluminum and hafnium, a thermal ALD method can be used as the ALD method.

[0318] As aluminum-containing precursors, aluminum chloride or trimethylaluminum can be used, for example. As hafnium-containing precursors, hafnium tetrachloride, tetra(ethylmethylamide)hafnium (TEMAHf) can be used, for example.

[0319] The second oxidizing agent can be any of the materials described above that can be used with the first oxidizing agent. The first and second oxidizing agents can be the same or different oxidizing agents.

[0320] In the ALD process, a precursor is introduced into the chamber and adsorbed onto the substrate surface. Here, because the precursor adheres to the substrate surface, the self-limiting mechanism of the surface chemical reaction is activated, preventing further adhesion of the precursor to the substrate's precursor layer. Note that the appropriate range of substrate temperature that enables the self-stopping mechanism of the surface chemical reaction is called the ALD window. The ALD window is determined based on the temperature characteristics, vapor pressure, and decomposition temperature of the precursor. In other words, the ALD window varies depending on the precursor. Therefore, when depositing oxide films containing multiple elements besides oxygen, the ALD window of each precursor must be considered to adjust the deposition conditions. On the other hand, when depositing oxide films such as indium oxide or alumina films containing only a single element besides oxygen, the ALD window of only one precursor can be considered to adjust the deposition conditions, making it easier to adjust the deposition conditions and thus depositing high-quality oxide films.

[0321] Preferably, microwave plasma treatment is performed after the deposition of the insulating layer 50. This microwave plasma treatment can reduce the concentration of impurities such as hydrogen or water contained in the semiconductor layer 30. Details of the microwave plasma treatment can be found in the above description.

[0322] Next, a conductive layer 60 is formed on the insulating layer 50 in such a way as to embed at least a portion of the groove 91. As described above, it is possible to manufacture... Figures 1A to 1D The semiconductor device shown.

[0323] In addition, Figures 1A to 1D In this process, layer 29 and the semiconductor layer 30 near layer 29 remain intact. This reduces the number of manufacturing steps in the semiconductor device. Note that the invention is not limited to this. For example, layer 29 and the semiconductor layer 30 near layer 29 can also be removed. This allows for the manufacture of… Figures 14A to 14C The semiconductor device shown.

[0324] In addition, by using Figure 9E and Figure 9F The structure shown can be manufactured Figure 14D and Figure 14E The semiconductor device shown. Specifically, through... Figure 9E and Figure 9F A semiconductor layer 30 is formed on the structure shown. The semiconductor layers 30, 29, and 40 are processed into desired shapes, and a first heat treatment and a second heat treatment are performed sequentially. An insulating layer 50 and a conductive layer 60 are then formed sequentially, enabling the manufacture of... Figure 14D and Figure 14E The semiconductor device shown.

[0325] In addition, such as Figure 10A , Figure 10B or Figure 10C As shown, by employing a structure in which layer 29 is embedded in insulating layer 20, layer 29 does not need to be removed, which can reduce the number of manufacturing steps in a semiconductor device.

[0326] In addition, in use Figure 6B and Figure 6C In the case where the insulating layer 20 has a curved surface at the upper end of the trench 91, a layer 29 serving as a crystallization portion is formed on the insulating layer 20 with the curved surface at the upper end. Then, a semiconductor layer 30 containing a metal oxide is formed to cover the trench, and a heat treatment is performed to allow the semiconductor layer 30 to crystallize and grow, thereby manufacturing a semiconductor device. In this case, the curved surface at the upper end of the insulating layer 20 preferably has a portion with a radius of curvature of 1 nm or more and 500 nm or less. Furthermore, this curved surface preferably has a portion with a radius of curvature greater than the thickness of the semiconductor layer 30.

[0327] Note that when forming the semiconductor layer 30 using the ALD method, it is sometimes possible to form a highly crystalline semiconductor layer 30 using layer 29 as a seed or nucleus during the formation of the semiconductor layer 30. For example, by setting the substrate heating temperature during ALD deposition within a range of 150°C to 300°C, a highly crystalline semiconductor layer 30 can be formed during deposition. In this case, the heating treatment for crystal growth of the semiconductor layer 30 may not be performed. Note that if the substrate heating temperature is too high, crystal nuclei may form, hindering large grain formation. On the other hand, if the substrate heating temperature is too low, crystal growth may not occur during the formation of the semiconductor layer 30.

[0328] Furthermore, when a highly crystalline semiconductor layer 30 can be formed during the formation of the semiconductor layer 30, at least one of the above-mentioned first heat treatment, second heat treatment, microwave plasma treatment, and hydrogenation treatment can be performed. This can sometimes further improve the crystallinity of the semiconductor layer 30.

[0329] Furthermore, if a highly crystalline semiconductor layer 30 can be formed during the formation of the semiconductor layer 30, the semiconductor layer 30 can also be processed into a desired shape after the layer is formed on the semiconductor layer 30.

[0330] [Application Examples]

[0331] By using a method for forming a metal oxide layer according to one aspect of the present invention, a large-area semiconductor layer 30 can be formed. Therefore, transistors using the semiconductor layer 30 and semiconductor chips using the transistors can be mass-produced with high yield. Reference is made below. Figures 15A to 15D This describes the manufacturing method of semiconductor chip 81.

[0332] Figure 15AA three-dimensional schematic diagram of substrate 80 is shown. (e.g.) Figure 15A As shown, a layer 29 is formed near the outer periphery of the substrate 80, and then a semiconductor layer 30 is formed over the entire surface of the substrate 80 as a capping layer 29. Thus, as... Figure 15B As shown, layer 29 can be used as a seed crystal for crystal growth to form a single-crystal or polycrystalline semiconductor layer 30 with a uniform crystal orientation across the entire surface of the substrate 80. More specifically, the crystal orientation of layer 29 is... <001> In this case, crystal orientation can be formed. <111> A crystalline semiconductor layer 30 is perpendicular to the top surface of the substrate 80. Figure 15B In the diagram, the dividing line 85 is shown as a dashed line. Layer 29 is preferably positioned at a location overlapping the dividing line 85.

[0333] Silicon wafers can typically be used as the substrate 80. In addition, insulating substrates such as glass substrates, quartz substrates, sapphire substrates, and yttrium-stabilized zirconia substrates (yttrium-stabilized zirconia substrates), as well as semiconductor substrates such as germanium substrates, silicon carbide substrates, silicon-germanium substrates, gallium arsenide substrates, indium phosphide substrates, zinc oxide substrates, and gallium oxide substrates can be used. The substrate 80 can, for example, be a substrate with a diameter of 3 inches, 5 inches, 8 inches, or 12 inches. In particular, even when using a large substrate such as a 12-inch substrate, a semiconductor layer 30 with good crystallinity can be obtained, thereby improving productivity.

[0334] Then, by forming transistors having a semiconductor layer 30, wiring, electrodes, etc., multiple semiconductor chips 81 can be formed. Next, as... Figure 15D As shown, multiple semiconductor chips 81 can be separated by dividing the substrate 80, on which semiconductor chips 81 are formed, along the dividing line 85. At this time, by placing the layer 29 at a position overlapping with the dividing line 85, a structure in which the layer 29 is not left inside the semiconductor chip 81 can be achieved.

[0335] Furthermore, layer 29 can also be located outside the dividing line 85. Moreover, layer 29 is not limited to one; two or more layers can be provided. For example, multiple layers 29 can be provided at equal intervals and configured to overlap with the dividing line 85 respectively.

[0336] Figure 15C Show Figure 15B This is a cross-sectional schematic diagram showing the stages of forming the semiconductor layer 30. A layer 29 is disposed at a position overlapping the dividing line 85, and the semiconductor layer 30 is formed as a cover layer 29. The semiconductor layer 30 is formed along the side and bottom surfaces of the trench 91 provided in the insulating layer 20. Furthermore, the semiconductor layer 30 also covers the structure 83 formed on the insulating layer 20. Thus, even if the semiconductor layer 30 is disposed in a manner that covers the uneven shape on the substrate 80, a single-crystal or polycrystalline film with consistent crystal orientation as described above can be formed.

[0337] Examples of structures 83 include wiring, electrodes, or protrusions in the insulating layer 20. Furthermore, structure 83 can also be a component of a transistor having a structure different from that of the transistor disposed in the slot 91. The structure of a transistor that can be used with structure 83 will be described below.

[0338] Figure 16 A schematic cross-sectional view of transistor 400 is shown. Transistor 400 is a transistor (OS transistor) containing metal-oxide in the channel formation region. Transistor 400 includes a pair of gates such that the semiconductor forming the channel is sandwiched between them.

[0339] Transistor 400 is disposed on insulating layer 412. Insulating layer 412 corresponds to the aforementioned insulating layer 20.

[0340] Insulating layers 414, 416, 420, 422, 440, 444, 441, 442, 446, and 448 are stacked on insulating layer 412. Insulating layers 412, 416, 440, 441, 446, and 448 are used as interlayer insulating films. Furthermore, insulating layers 414, 420, 422, 444, and 442 are preferably barrier insulating films capable of preventing the diffusion of hydrogen, impurities, etc.

[0341] The transistor 400 includes a conductive layer 405 disposed in insulating layers 414 and 416, insulating layers 420 and 422 on insulating layers 416 and conductive layers 405, an insulating layer 424 on insulating layer 422, a semiconductor layer 401 on insulating layer 424, a pair of conductive layers 404 disposed on semiconductor layer 401, an insulating layer 440 located on conductive layer 404 and having a trench reaching semiconductor layer 401, and an insulating layer 403 and conductive layer 402 disposed in insulating layer 440.

[0342] The semiconductor layer 30 described above can be used as semiconductor layer 401.

[0343] One of the pair of conductive layers 404 is used as the source electrode, and the other is used as the drain electrode. Conductive layer 402 is used as the first gate electrode, and insulating layer 403 is used as the first gate insulating layer. Conductive layer 405 is used as the second gate electrode, and insulating layers 420, 422, and 424 are used as the second gate insulating layers.

[0344] As insulating layers 424 and 403 in contact with semiconductor layer 401, oxides or oxynitrides such as silicon oxide, silicon oxynitride, aluminum oxide, and hafnium oxide are preferably used. Alternatively, nitrogen-containing compounds such as silicon nitride, silicon oxynitride, and aluminum nitride can also be used. Furthermore, single layers or stacks of insulators containing materials with high relative permittivity (high-k), such as aluminum oxide, hafnium oxide, tantalum oxide, and zirconium oxide, are preferred. When miniaturizing and highly integrating transistors, problems such as leakage current sometimes occur due to the thinning of the gate insulating film. Therefore, by using a high-k material as the insulator for the gate insulating film, the gate potential during transistor operation can be reduced while maintaining the physical thickness.

[0345] As the insulating layer 403, a laminated film consisting of multiple insulating films is preferably used. For example, a laminated film consisting of two, three, or four or more layers of the above-mentioned insulating material is preferred.

[0346] The insulating layer 434 is provided to cover the conductive layer 404 and has the function of suppressing the oxidation of the conductive layer 404. At this time, the insulating layer 434 is provided to cover the side surface of the semiconductor layer 401 and the side surface of the insulating layer 424 and to contact the insulating layer 422. As the insulating layer 434, it is preferable to use an insulating film with barrier properties that can prevent the diffusion of hydrogen, impurities, etc.

[0347] Additionally, a conductive layer 454 for wiring may be included on the insulating layer 446. The conductive layer 454 and the conductive layer 404 are connected via conductive layers 436 and 438. Conductive layers 436 and 438 serve as a connector. The conductive layer 436 is preferably made of a conductive material with low oxygen permeability. In particular, the conductive layer 436 is preferably made of a conductive material that is not easily oxidized or that retains conductivity even if oxidized. Furthermore, the conductive layer 438 is preferably made of a conductive material with low resistance.

[0348] This embodiment can be appropriately combined with other embodiments. Furthermore, in this specification, where multiple structural examples are shown in one embodiment, these structural examples can be appropriately combined.

[0349] (Implementation Method 2)

[0350] In this embodiment, a semiconductor device using the structure described in Embodiment 1 will be described.

[0351] <Example 1 of semiconductor device structure>

[0352] Reference Figures 17A to 28D An example of the structure of a semiconductor device according to one aspect of the present invention is provided.

[0353] Figures 17A to 17CThis is a three-dimensional schematic diagram of a semiconductor device including transistor 200A. Figure 17B It is a cutoff Figure 17A A partial 3D view. Furthermore, in Figure 17A and Figure 17B In the diagram, some components (such as interlayer insulation) are shown only by dashed lines, indicating their outlines. Furthermore, Figure 17C Show along Figure 17A The three-dimensional diagram is shown by the dotted line.

[0354] Figure 18A This is a plan view of a semiconductor device including transistor 200A. Figure 18B It is along Figure 18A The cross-sectional view of the dotted line A1-A2 shown. Figure 18C It is along Figure 18A The cross-sectional view shown is the dotted-dash line A3-A4. Figure 18D It is along Figure 18B The cross-sectional view shown is along the dashed-dot line A5-A6. Note that, for clarity, in... Figure 18A Some constituent elements are omitted in the plan view. Sometimes, some constituent elements are also omitted in subsequent plan views.

[0355] Figures 18A to 18D The semiconductor device shown includes an insulating layer 210 on a substrate (not shown), a transistor 200A on the insulating layer 210, and an insulating layer 280 on the insulating layer 210. It also includes an insulating layer 283 on the transistor 200A and an insulating layer 285 on the insulating layer 283. Furthermore, it includes conductive layers 243a, 243b, and 246.

[0356] [Transistor 200A]

[0357] Transistor 200A includes a conductive layer 220, conductive layers 240a and 240b on an insulating layer 280, layer 229a on conductive layer 240a, layer 229b on conductive layer 240b, a semiconductor layer 230 on layers 229a and 229b, an insulating layer 250 on semiconductor layer 230, and a conductive layer 260 on insulating layer 250. The insulating layer 280 is located on the conductive layer 220.

[0358] The semiconductor layer 230, insulating layer 280, insulating layer 250, and conductive layer 260 included in transistor 200A correspond to the oxide semiconductor layer 30, insulating layer 20, insulating layer 50, and conductive layer 60 described in Embodiment 1, respectively. Therefore, the structure (material, thickness, etc.) and formation method of semiconductor layer 230, insulating layer 280, insulating layer 250, and conductive layer 260 can refer to the structure and formation method of oxide semiconductor layer 30, insulating layer 20, insulating layer 50, and conductive layer 60 described in Embodiment 1. Furthermore, layers 229a and 229b correspond to layer 29 described in Embodiment 1. Therefore, the structure (material, thickness, etc.) and formation method of layers 229a and 229b can refer to the structure and formation method of layer 29 described in Embodiment 1.

[0359] like Figures 18A to 18D As shown, a trench 291 extending to the conductive layer 220 is provided in the insulating layer 280. The trench 291 extends in the X direction. The semiconductor layer 230, the insulating layer 250, and the conductive layer 260 are all arranged such that at least a portion of each is located within the trench 291. The trench 291 corresponds to the trench 91 described in Embodiment 1. Therefore, the structure and forming method of the trench 291 can be referred to the structure and forming method of the trench 91 described in Embodiment 1.

[0360] Figures 18A to 18D The semiconductor device shown is Figure 14D and Figure 14E A detailed structural example of a semiconductor device is shown.

[0361] The semiconductor layer 230 is configured as an island. The semiconductor layer 230 is disposed along a portion of the bottom and a portion of the sidewall of the trench 291. The semiconductor layer 230 has a portion that contacts the side surface of the trench 291 side of the conductive layer 240a, a portion that contacts the side surface of the trench 291 side of the conductive layer 240b, and a portion that contacts the bottom and side surfaces of the recess of the conductive layer 220 in the trench 291.

[0362] The insulating layer 250 is provided in a manner that covers the semiconductor layer 230. In addition, the insulating layer 250 is provided on the insulating layer 280 in a manner that covers the top and side surfaces of the semiconductor layer 230 and the side surfaces of the conductive layer 240.

[0363] The conductive layer 260 is provided in such a way that it is embedded in at least a portion of the groove 291. Therefore, the conductive layer 260 is provided extending in the direction in which the groove 291 extends.

[0364] Conductive layer 220 is used as one of the source and drain electrodes of transistor 200A, and conductive layers 240a and 240b are used as the other. In addition, conductive layer 260 has a region used as gate wiring.

[0365] Semiconductor layer 230 has a region overlapping conductive layer 260 with insulating layer 250 as a gap. At least a portion of this region is used as a channel formation region for transistor 200A. One of the regions near conductive layer 220 and conductive layer 240b of semiconductor layer 230 is used as a source region, and the other is used as a drain region. That is, the channel formation region is sandwiched between the source region and the drain region.

[0366] Semiconductor layer 230 is disposed inside the trench portion 291. Furthermore, in transistor 200A, one of the source and drain electrodes (here, conductive layer 220) is located below, and the other of the source and drain electrodes (here, conductive layers 240a and 240b) is located above, so current flows in the vertical direction. That is, a channel is formed along the side of the trench portion 291. Therefore, compared to planar transistors where the channel forming region, source region, and drain region are respectively provided on the XY plane, transistor 200A can reduce the occupied area. This allows for high integration of the semiconductor device. Furthermore, when the semiconductor device of one aspect of the present invention is used in a memory device, the storage capacity per unit area can be increased. Moreover, transistor 200A can be said to have a vertical component along the length of the channel; therefore, this transistor can also be referred to as VFET (Vertical Field Effect Transistor), vertical transistor, vertical channel transistor, vertical channel type transistor, etc.

[0367] like Figure 18B As shown, the conductive layer 220 has a recess that overlaps with the trench 291. Specifically, this recess is provided in the conductive layer 220 at the position where it overlaps with the trench 291. By having this recess in the conductive layer 220, compared to the case where it does not have this recess, the height of the bottom surface of the insulating layer 250 and the bottom surface of the conductive layer 260 within the trench 291 can be lower than the height of the top surface of the conductive layer 220 that contacts the insulating layer 280. Here, the height of each surface can be determined with reference to the surface on which the transistor is formed. Here, the top surface of the insulating layer 210 is used as the reference. The surface used for the reference is not limited to the surface on which the transistor is formed. For example, the top surface of the substrate on which the transistor or semiconductor device is disposed can also be used as the reference.

[0368] Furthermore, the bottom and side surfaces of the recesses in the semiconductor layer 230 and the conductive layer 220 are in contact. By making the conductive layer 220 have recesses, the contact area between the semiconductor layer 230 and the conductive layer 220 can be increased. Therefore, the contact resistance between the semiconductor layer 230 and the conductive layer 220 can be reduced.

[0369] like Figure 18BAs shown, the recess included in the conductive layer 220 may have a curved portion. When the recess has a curved portion, portions of the semiconductor layer 230, insulating layer 250, etc., disposed on the recess may also have a curved portion near the recess. In other words, this portion may sometimes have a curved or concave surface when viewed in cross-section. Furthermore, this portion may sometimes lack corners (right angles or acute angles) when viewed in cross-section. This can mitigate the electric field concentration on the insulating layer 250 near the recess, improve the insulation withstand voltage of the transistor 200A, and thus suppress electrostatic breakdown of the transistor 200A. Therefore, the reliability of the semiconductor device can be improved.

[0370] Figure 18B The diagram shows a structure in which the end of the conductive layer 240 on the outer side of the groove 291 is aligned or substantially aligned with the end of the semiconductor layer 230. The conductive layer 240 and the semiconductor layer 230 can be manufactured using the same mask. Therefore, the number of masks required for manufacturing the semiconductor device can be reduced, which is preferable. Note that the invention is not limited thereto. For example, in the X or Y direction, either the end of the semiconductor layer 230 or the end of the conductive layer 240 may be located on the other inner or outer side.

[0371] The width D1 of the groove 291 sometimes varies in the depth direction. Here, the shortest distance between conductive layers 240a and 240b when viewed in cross-section is used as the width D1. Alternatively, the shortest distance between the top surfaces of conductive layers 240a and 240b, the shortest distance between the bottom surfaces of conductive layers 240a and 240b, or the average of these two shortest distances can also be used as the width D1. Here, an example is shown where the width D1 of the groove 291 is determined using the shortest distance between conductive layers 240a and 240b, but there are no particular limitations on the method for determining the width D1. For example, the shortest distance between the two sides of one side of the groove 291 on the insulating layer 280 can be used as the width D1. Furthermore, the width of the groove 291 at its highest position in the insulating layer 280, the width of the groove 291 at its lowest position, the width of the groove 291 at these intermediate points, or the average of these three widths can also be used as the width D1.

[0372] The width D1 of the trench 291 is set according to the thickness of the semiconductor layer 230, the insulating layer 250, and the conductive layer 260 in the trench 291. The width D1 of the trench 291 is preferably 5 nm or more and 100 nm or less, more preferably 10 nm or more and 60 nm or less, even more preferably 20 nm or more and 50 nm or less, even more preferably 20 nm or more and 40 nm or less, and even more preferably 20 nm or more and 30 nm or less.

[0373] When viewed from a planar perspective, the side surface of the conductive layer 260 disposed in the trench 291 has a portion that faces the side surface of the semiconductor layer 230 across the insulating layer 250. Therefore, the channel width of the transistor 200A depends on the width D2 of the semiconductor layer 230 (refer to...). Figure 18D The channel width of transistor 200A can be calculated as "2×D2".

[0374] By increasing the width D2 of the semiconductor layer 230, the channel width per unit area can be increased, thereby increasing the on-state current. On the other hand, the occupied area of ​​the transistor 200A, for example, the area of ​​the transistor 200A when viewed from a planar surface, is approximately determined by the width D1 of the trench portion 291 and the width D2 of the semiconductor layer 230. By decreasing the width D1 of the trench portion 291 and the width D2 of the semiconductor layer 230, the occupied area of ​​the transistor 200A can be reduced, thereby achieving high integration of the semiconductor device.

[0375] The channel length of transistor 200A is the distance between the source region and the drain region. In other words, the channel length of transistor 200A can be said to be determined by the thickness of insulating layer 280 on conductive layer 220. Therefore, the channel length of transistor 200A does not affect the area occupied by transistor 200A, such as the area of ​​transistor 200A when viewed from a planar perspective. When viewed in cross-section, the channel length can be considered as the distance between the end of the region where semiconductor layer 230 and conductive layer 220 contact each other and the end of the region where semiconductor layer 230 and conductive layer 240a or conductive layer 240b contact each other. In this case, the channel length is equivalent to the length of the side of the trench portion 291 of insulating layer 280 when viewed in cross-section.

[0376] The channel length of transistor 200A can be set to, for example, 500nm or less, 300nm or less, 100nm or less, 60nm or less, 50nm or less, 40nm or less, 30nm or less, 20nm or less, or 10nm or less and 0.1nm or more, 1nm or more, or 5nm or more. Typically, it can be set to 1nm or more and 300nm or less, preferably 5nm or more and 100nm or less. This improves productivity and yield during the formation of insulating layer 280 and the formation of trench 291 in insulating layer 280. Consequently, the on-state current of transistor 200A increases, thereby improving frequency characteristics.

[0377] Figure 18B Examples of residual layers 229a and 229b are shown. Note that the invention is not limited thereto. For example, such as Figures 19A to 19C As shown, the layer used as the core (equivalent to layer 29 in embodiment 1) can also be removed. Figure 19A This is a plan view of a semiconductor device including transistor 200A. Figure 19B It is along Figure 19AThe cross-sectional view of the dotted line A1-A2 shown. Figure 19C It is along Figure 19A The cross-sectional view shown is along the dashed-dot line A3-A4. Note that along... Figure 19B The cross-sectional view of the dotted lines A5-A6 shown can be referenced. Figure 18D .

[0378] For example, a layer serving as a core (equivalent to layer 29 in Embodiment 1) is formed on the conductive film that will become conductive layers 240a and 240b. A trench 291 is formed in this layer, the conductive film, and the insulating layer 280. A semiconductor layer 230 is formed to cover this layer. The first and second heat treatments described in Embodiment 1 are performed to improve the crystallinity of the semiconductor layer 230. Then, the regions overlapping with this layer and the aforementioned conductive film and semiconductor layer 230 near them are removed, thereby manufacturing... Figures 19A to 19C The semiconductor device shown. By employing this structure, the contact area between the semiconductor layer 230 and the conductive layer 240a or 240b can be increased. Therefore, the contact resistance between the semiconductor layer 230 and the conductive layer 240a or 240b can be reduced.

[0379] Figures 19A to 19C The diagram illustrates a structure in which conductive layers 240a and 240b are disposed between semiconductor layer 230 and insulating layer 280. Note that the invention is not limited thereto. For example, such as... Figures 20A to 20C As shown, the semiconductor layer 230 can also contact the top surface of the insulating layer 280 on the outside of the trench 291. Figure 20A This is a plan view of a semiconductor device including transistor 200A. Figure 20B It is along Figure 20A The cross-sectional view of the dotted line A1-A2 shown. Figure 20C It is along Figure 20A The cross-sectional view shown is along the dashed-dot line A3-A4. Note that along... Figure 20B The cross-sectional view of the dotted lines A5-A6 shown can be referenced. Figure 18D .

[0380] like Figures 20A to 20C As shown, the crystallinity of the semiconductor layer 230 can be further improved by forming a semiconductor layer 230 on an insulating layer 280 with a flat top surface and made of a material with a small coefficient of thermal expansion.

[0381] An opening is provided in insulating layer 285, insulating layer 283, insulating layer 250, and semiconductor layer 230 to reach conductive layer 240a, and conductive layer 243a is disposed within the opening. An opening is also provided in insulating layer 285, insulating layer 283, insulating layer 250, and semiconductor layer 230 to reach conductive layer 240b, and conductive layer 243b is disposed within the opening. Conductive layer 243a is in contact with conductive layer 240a, and conductive layer 243b is in contact with conductive layer 240b.

[0382] Conductive layers 243a and 243b may use conductive materials described in the section on [Conductive Layers], which will be explained later. For example, conductive layers 243a and 243b are preferably made of conductive materials with tungsten, copper, or aluminum as their main components. Furthermore, conductive layers 243a and 243b may also have a laminated structure.

[0383] For example, both conductive layers 243a and 243b can have a two-layer structure: a first conductive layer formed along the opening and a second conductive layer formed inside the first conductive layer. As the first conductive layer, a conductive material with the function of reducing hydrogen diffusion can be used. This can suppress the mixing of impurities such as water and hydrogen into the semiconductor layer 230 through the second conductive layer. Furthermore, as the second conductive layer, the conductive material described above that can be used in conductive layers 243a and 243b can be used.

[0384] A conductive layer 246 is disposed on the insulating layer 285. The conductive layer 246 is connected to the conductive layer 240a via a conductive layer 243a, and to the conductive layer 240b via a conductive layer 243b. The conductive layer 246 is used as another component in both source and drain wiring. The conductive layer 246 extends in the Y direction. That is, the direction in which the conductive layer 246 extends intersects the direction in which the groove 291 extends. Figure 18A As shown, transistor 200A is disposed at the intersection of conductive layer 260 extending in the X direction and conductive layer 246 extending in the Y direction.

[0385] In transistor 200A, conductive layers 240a and 240b, which serve as the source and drain electrodes respectively, are connected by conductive layer 246. Therefore, the width of conductive layers 240a and 240b in the X direction can be reduced, and miniaturization of the semiconductor device can be achieved. For example, the width of conductive layers 240a and 240b in the X direction can be smaller than the width D1 of the trench portion 291 (see reference). Figure 18D ).

[0386] exist Figures 18A to 18CIn the transistor 200A shown, the height of the top surface of the conductive layer 260 is lower than the height of the top surface of the insulating layer 250. By employing this structure, the area of ​​the conductive layer 260 relative to the conductive layer 240a or 240b can be reduced, thereby reducing the parasitic capacitance generated between the conductive layer 260 and the conductive layer 240a or 240b. Furthermore, by employing the above structure, the physical distance between the conductive layer 260 and the conductive layer 246 can be increased, further reducing the parasitic capacitance generated between the conductive layer 260 and the conductive layer 246. Therefore, the frequency characteristics of the circuit using this transistor can be improved.

[0387] Figure 18B Examples of semiconductor layer 230 having a single-layer structure are shown. Furthermore, semiconductor layer 230 may have a stacked structure of two or more layers. For example, semiconductor layer 230 may have a two-layer structure consisting of a first semiconductor layer and a second semiconductor layer on the first semiconductor layer. The first semiconductor layer and the second semiconductor layer correspond to the first semiconductor layer and the second semiconductor layer described in Embodiment 1, respectively. Therefore, the structure (material, thickness, etc.) and formation method of the first semiconductor layer and the second semiconductor layer can refer to the structure and formation method of the first semiconductor layer and the second semiconductor layer described in Embodiment 1.

[0388] Insulating layer 210 is used as an interlayer film, and therefore a material with a low relative permittivity is preferred. By using a material with a low relative permittivity as the interlayer film, parasitic capacitance generated between wirings can be reduced.

[0389] The insulating layer 210 preferably has hydrogen-blocking properties. By having hydrogen-blocking properties, the insulating layer 210 disposed below the semiconductor layer 230 can suppress the diffusion of hydrogen from below the transistor 200A into the semiconductor layer 230.

[0390] Furthermore, the insulating layer 210 preferably has the function of trapping or fixing hydrogen. By making the insulating layer 210 have the function of trapping or fixing hydrogen, hydrogen in the semiconductor layer 230 diffuses through the conductive layer 220 to the insulating layer 210, and the hydrogen can be trapped or fixed. Therefore, the hydrogen concentration in the semiconductor layer 230 can be reduced.

[0391] Furthermore, the concentration of impurities such as hydrogen or water in the insulating layer 210 is preferably reduced. This helps to suppress the mixing of impurities such as hydrogen or water into the channel formation region of the semiconductor layer 230.

[0392] Figure 18BAn example of a single-layer structure for insulating layer 210 is shown. However, insulating layer 210 can also have a stacked structure of two or more layers. For example, insulating layer 210 can have a two-layer structure with a first insulating layer and a second insulating layer on the first insulating layer. In this case, for example, it is preferable that the first insulating layer has hydrogen-blocking properties and the second insulating layer has the function of trapping or fixing hydrogen. Specifically, it is preferable that silicon nitride is used as the first insulating layer and aluminum oxide, hafnium oxide, hafnium zirconium oxide, or hafnium silicate is used as the second insulating layer.

[0393] Figure 18B An example of a single-layer structure for insulating layer 250 is shown. Note that insulating layer 250 may have a stacked structure of two or more layers. In this case, insulating layer 250 is preferably formed from two or more films. By using two or more films as insulating layer 250, insulating layer 250 can have multiple functions. Examples of functions of insulating layer 250 include the function of extracting excess oxygen from semiconductor layer 230, the function of extracting hydrogen from semiconductor layer 230, and the function of inhibiting hydrogen diffusion into semiconductor layer 230.

[0394] Figures 21A to 21D An enlarged view of the insulating layer 250 and its vicinity is shown. Figures 21A to 21D Too Figure 18B The enlarged view of region P, surrounded by a dotted line, is shown.

[0395] Figure 21A An example is shown where the insulating layer 250 has a three-layer structure consisting of insulating layer 250_1, insulating layer 250_2 on insulating layer 250_1, and insulating layer 250_3 on insulating layer 250_2. In this case, insulating layer 250_1 is in contact with semiconductor layer 230.

[0396] As insulating layer 250_1, the materials described above that can be used for insulating layer 50 can be used. For example, by including an insulating layer with the function of trapping or fixing oxygen in insulating layer 250_1, excessive oxygen in semiconductor layer 230 can be reduced. Furthermore, insulating layers with the function of trapping or fixing oxygen sometimes also have the function of trapping or fixing hydrogen, thus sometimes reducing the hydrogen concentration in semiconductor layer 230. Therefore, a highly reliable transistor can be realized.

[0397] Furthermore, the insulating layer 250_1 can be made of a high-k material. As an example of a high-k material, there are oxides containing one or both of aluminum and hafnium. When a high-k material is used as the insulating layer 250_1, the gate potential applied during transistor operation can be reduced while maintaining the physical thickness of the gate insulator. Furthermore, the equivalent oxide thickness (EOT) of the insulator used as the gate insulator can be reduced.

[0398] Therefore, as the insulating layer 250_1, an oxide containing one or both of aluminum and hafnium is preferred, and an oxide having an amorphous structure and containing one or both of aluminum and hafnium is more preferred. Since alumina can be easily deposited into an amorphous film using the ALD method, alumina with an amorphous structure is preferred. Alumina has the function of trapping or fixing oxygen and hydrogen, so it is suitable for use in the insulating layer 250_1. Alternatively, hafnium oxide has a strong function of trapping or fixing oxygen and hydrogen, so it is suitable for use in the insulating layer 250_1.

[0399] For example, the insulating layer 250_2 is preferably made of a material with a low relative permittivity. For example, the insulating layer 250_2 preferably includes a silicon oxide film or a silicon oxynitride film.

[0400] Furthermore, silicon oxide or silicon nitride are insulating materials with high dielectric strength. This reduces the leakage current of transistors. Additionally, silicon oxide or silicon oxynitride films are also highly hydrogen permeable. Therefore, as... Figure 21B As shown, the insulating layer 250 can also have a three-layer structure consisting of insulating layer 250_2, insulating layer 250_1 on insulating layer 250_2, and insulating layer 250_3 on insulating layer 250_1. By employing this structure, hydrogen in the semiconductor layer 230 diffuses through insulating layer 250_2 to insulating layer 250_1, whereby the hydrogen can be trapped or fixed. Therefore, the hydrogen concentration in the semiconductor layer 230 can be reduced.

[0401] The insulating layer 250_3 preferably has hydrogen-blocking properties. By employing this structure, hydrogen diffusion into the semiconductor layer 230 can be suppressed. Furthermore, the insulating layer 250_3 preferably has oxygen-blocking properties. The insulating layer 250_3 is disposed between the channel formation region of the semiconductor layer 230 and the conductive layer 260. By employing this structure, oxygen diffusion from the channel formation region of the semiconductor layer 230 into the conductive layer 260, thus preventing the formation of oxygen vacancies in the channel formation region of the semiconductor layer 230, can be suppressed. Furthermore, oxygen diffusion from the semiconductor layer 230 into the conductive layer 260, preventing oxidation of the conductive layer 260, can be suppressed. The insulating layer 250_3 is preferably at least less permeable to oxygen than the insulating layer 250_2. Furthermore, the insulating layer 250_3 preferably has the function of suppressing hydrogen diffusion. Thus, impurities such as hydrogen in the conductive layer 260 can be prevented from diffusing into the semiconductor layer 230. For example, silicon nitride is preferably used as the insulating layer 250_3.

[0402] In addition, such as Figure 21CAs shown, a structure in which an insulating layer 250_4 is provided on the insulating layer 250_2 can also be adopted. The insulating material that can be used for the insulating layer 250_1 can be used as the insulating layer 250_4. For example, by providing an insulating layer 250_4 with the function of trapping or fixing hydrogen between the insulating layer 250_3 and the insulating layer 250_2, hydrogen in the insulating layer 250_2, etc., can be trapped or fixed.

[0403] Specifically, the insulating layer 250 preferably has a four-layer structure in which an aluminum oxide film, a silicon oxide film, a hafnium oxide film, and a silicon nitride film are sequentially stacked from one side of the semiconductor layer 230. By adopting this structure, hydrogen diffuses from the semiconductor layer 230 to the insulating layer 250_1 or the insulating layer 250_4, whereby the hydrogen can be captured or fixed. Therefore, the hydrogen concentration in the semiconductor layer 230 can be reduced.

[0404] The insulating layer 250 is preferably a thin film. For example, by setting the thickness of the insulating layer 250 to be 1 nm or more and 20 nm or less, preferably 3 nm or more and 10 nm or less, the subthreshold swing value (also known as the S-value) can be reduced. The S-value refers to the change in gate voltage when the drain current changes by a single digit at a constant drain voltage in the subthreshold region.

[0405] Furthermore, the thickness of each layer constituting the insulating layer 250 is preferably 0.1 nm or more and 20 nm or less, more preferably 0.1 nm or more and 10 nm or less, even more preferably 0.1 nm or more and 5.0 nm or less, further preferably 0.5 nm or more and 5.0 nm or less, even more preferably 1.0 nm or more and less than 5.0 nm, and even more preferably 1.0 nm or more and 3.0 nm or less. At least a portion of each layer constituting the insulating layer 250 may include a region having the aforementioned thickness.

[0406] Alternatively, insulation layer 250_3 in the four-layer insulation layer 250 structure can be omitted (see reference). Figure 21D For example, insulating layer 250_1 can be an insulating layer with the function of capturing or fixing oxygen, insulating layer 250_2 can be an insulating layer containing a material with a relatively low permittivity, and insulating layer 250_4 can be an insulating layer with the function of capturing or fixing hydrogen. Specifically, insulating layer 250 can have a three-layer structure in which an aluminum oxide film, a silicon oxide film, and a hafnium oxide film are sequentially stacked from the semiconductor layer 230 side.

[0407] Furthermore, the insulating layer 250 can have a three-layer structure in which a hafnium oxide film, a silicon oxide film, and a silicon nitride film are sequentially stacked from the semiconductor layer 230 side. The thicknesses of the hafnium oxide film, silicon oxide film, and silicon nitride film are 2 nm, 2 nm, and 1 nm, respectively. By employing this structure, excess oxygen in the semiconductor layer 230 can be discharged to the insulating layer 250, thereby reducing the amount of oxygen in the semiconductor layer 230. Furthermore, hydrogen in the semiconductor layer 230 can be trapped or immobilized. Therefore, the electrical characteristics and reliability of the transistor 200A can be improved.

[0408] In order to reduce the thickness of insulating layers 250_1 to 250_4 as described above, it is preferable to use the ALD method for deposition. Furthermore, in order to form insulating layers 250_1 to 250_4 with high coverage within the opening 290, it is preferable to use the ALD method for deposition.

[0409] Furthermore, in the formation of the insulating layer 250 with a multilayer insulating film structure, it is preferable to perform the ALD process twice or more. For example, two or more of the multiple insulating films included in the insulating layer 250 are preferably formed by the ALD process. By forming at least two or more insulating films using the ALD process, the coverage and thickness uniformity of the insulating layer 250 can be improved. In addition, for example, by continuously forming two or more insulating films using the ALD process, productivity can be improved.

[0410] Note that the above description indicates that the insulating layer 250 has a three-layer or four-layer structure, but the present invention is not limited thereto. The insulating layer 250 may have a structure including at least one of insulating layers 250_1 to 250_4. By having the insulating layer 250 consist of one, two, or three of insulating layers 250_1 to 250_4, the manufacturing process of semiconductor devices can be simplified, thereby improving productivity.

[0411] The insulating layer 280 is used as an interlayer film, and therefore a material with a low relative permittivity is preferably used. By using a material with a low relative permittivity as the interlayer film, the parasitic capacitance generated between the wirings can be reduced. Silicon oxide or silicon oxynitride can be used, for example, as the insulating layer 280.

[0412] As described above, by using silicon oxide with a small coefficient of thermal expansion as the insulating layer 280 provided before the formation of the semiconductor layer 230, the crystal growth of the semiconductor layer 30 formed inside the trench 291 of the insulating layer 280 can be promoted.

[0413] Figure 18B An example of insulating layer 280 having a single-layer structure is shown. Note that insulating layer 280 may have a stacked structure of two or more layers. Figures 22A to 22D Other structural examples of semiconductor devices including transistor 200A are shown. Figure 22AThis is a plan view of a semiconductor device including transistor 200A. Figure 22B It is along Figure 22A The cross-sectional view of the dotted line A1-A2 shown. Figure 22C It is along Figure 22A The cross-sectional view shown is the dotted-dash line A3-A4. Figure 22D It is along Figure 22B The cross-sectional view shown is the dotted-dash line A5-A6.

[0414] like Figure 22B As shown, the insulating layer 280 may have a three-layer structure consisting of insulating layer 280_1, insulating layer 280_2 on insulating layer 280_1, and insulating layer 280_3 on insulating layer 280_2. Preferably, the insulating layer 280_2 uses a material with a relatively low permittivity, and the insulating layers 280_1 and 280_3 use oxygen-barrier insulating layers. This suppresses oxidation of conductive layers 220, 240a, and 240b, and also suppresses high resistivity. Furthermore, by forming the trench 291, at least a portion of the top surface of the conductive layer 220 can be exposed, while preventing a portion of the insulating layer 210 from being exposed and removed. This provides a highly reliable semiconductor device. Moreover, since the manufacturing yield of the semiconductor device can be improved, a semiconductor device that can be manufactured at low cost can be provided.

[0415] For example, preferably, silicon nitride film or aluminum oxide film is used as insulating layer 280_1 and insulating layer 280_3, and silicon oxide film is used as insulating layer 280_2. In addition, insulating layer 280_1 and insulating layer 280_3 may each have a stacked structure of two or more layers.

[0416] Since conductive layers 220, 240a, and 240b are all in contact with semiconductor layer 230, it is preferable to use conductive materials that are not easily oxidized, conductive materials that maintain low resistance even when oxidized, conductive metal oxides (also known as oxide conductors), or conductive materials that suppress oxygen diffusion. Examples of such conductive materials include nitrogen-containing conductive materials and oxygen-containing conductive materials. This helps to suppress the decrease in conductivity of conductive layers 220, 240a, and 240b.

[0417] By using oxygen-containing conductive materials as conductive layers 220, 240a, and 240b, conductivity can be maintained even if conductive layers 220, 240a, and 240b absorb oxygen. Furthermore, conductive layer 220 can maintain conductivity even when using an oxygen-containing insulator such as hafnium oxide as insulating layer 210, which is therefore preferred. For example, ITO, ITSO, and In-Zn oxides are preferably used as conductive layers 220, 240a, and 240b.

[0418] Figure 18B An example is shown where conductive layers 220, 240a, and 240b each have a single-layer structure. Note that conductive layers 220, 240a, and 240b can each have a stacked structure of two or more layers. When conductive layers 220, 240a, and 240b all have a stacked structure, by using an oxygen-containing conductive material as the layer with the largest contact area with the semiconductor layer 230 in this stacked structure, the contact resistance between conductive layer 220 and semiconductor layer 230, and between conductive layer 240a or conductive layer 240b and semiconductor layer 230, can be reduced.

[0419] Figure 22B An example is shown where the conductive layer 220 has a three-layer structure: conductive layer 220_1, conductive layer 220_2 on conductive layer 220_1, and conductive layer 220_3 on conductive layer 220_2. In this case, it is preferable, for example, to use a conductive material that is not easily oxidized or a conductive material that has the function of inhibiting oxygen diffusion as conductive layer 220_1, to use a material with high conductivity as conductive layer 220_2, and to use an oxygen-containing conductive material (more preferably an oxide conductor) as conductive layer 220_3. Specifically, it is preferable to use titanium nitride as conductive layer 220_1, tungsten as conductive layer 220_2, and an oxide conductor (e.g., ITO, ITSO, or In-Zn oxide) as conductive layer 220_3. In this case, the titanium nitride film is in contact with the insulating layer 210, and the oxide conductive film is in contact with the semiconductor layer 230. Furthermore, the oxide conductor is used in the layer closest to the channel formation region of the semiconductor layer 230. Compared to tungsten, the oxide conductor has a lower contact resistance with the semiconductor layer 230, thus shortening the current path between the source and drain, thereby increasing the on-state current of the transistor 200A. With this structure, conductivity can be maintained even when the conductive layer 220 is in contact with the semiconductor layer 230. Furthermore, using an oxide insulating layer as the insulating layer 210 can prevent excessive oxidation of the conductive layer 220 due to the insulating layer 210. Moreover, by using a metal material (in this case, tungsten) with higher conductivity than the oxide conductor and titanium nitride as the conductive layer 220_2, the conductivity of the conductive layer 220 can be improved.

[0420] Figure 22BAn example is shown where both conductive layer 240a and conductive layer 240b have a two-layer structure, each having a first conductive layer and a second conductive layer on the first conductive layer. In this case, for example, it is preferable to use an oxygen-containing conductive material as the second conductive layer and a material with higher conductivity than the second conductive layer as the first conductive layer. Specifically, it is preferable to use an oxide conductor (e.g., ITO, ITSO, or In-Zn oxide) as the second conductive layer and tungsten as the first conductive layer. Alternatively, ruthenium, titanium nitride, or tantalum nitride can also be used as the first conductive layer. By using an oxide conductor as the second conductive layer, which is primarily in contact with the semiconductor layer 230, the contact resistance with the semiconductor layer 230 can be reduced. Furthermore, by using a material with higher conductivity than the oxide conductor as the layer constituting conductive layers 240a and 240b, the conductivity of conductive layers 240a and 240b can be improved.

[0421] Furthermore, an oxygen-containing conductive material can be used as the first conductive layer, and a material with higher conductivity than the first conductive layer can be used as the second conductive layer. In this case, an oxide conductor is used in each of the conductive layers 240a and 240b, the layer closest to the channel formation region of the semiconductor layer 230. Therefore, the current path between the source and drain can be shortened, and the on-state current of the transistor 200A can be increased.

[0422] Figure 18B An example of a single-layer structure is shown for the conductive layer 260. Alternatively, the conductive layer 260 may have a stacked structure of two or more layers. Figure 22B The conductive layer 260 shown has a two-layer structure: a conductive layer 260_1 and a conductive layer 260_2 on the conductive layer 260_1. For example, titanium nitride is preferably used as the conductive layer 260_1, and tungsten is preferably used as the conductive layer 260_2. Alternatively, it is preferable to use tantalum nitride as the conductive layer 260_1 and copper as the conductive layer 260_2. By adopting this structure, the conductivity of the conductive layer 260 can be improved.

[0423] Furthermore, the conductive layer 260 may also have a stacked structure of three or more layers. For example, the conductive layer 260 may also have a three-layer structure of a tantalum nitride film, a titanium nitride film on the tantalum nitride film, and a tungsten film on the titanium nitride film.

[0424] like Figure 18B As shown, an insulating layer 283 can also be provided on transistor 200A. Specifically, an insulating layer 283 can also be provided on conductive layer 260 and insulating layer 250.

[0425] As the insulating layer 283, a hydrogen-blocking insulating layer is preferably used. By adopting this structure, hydrogen diffusion from above the transistor 200A to the semiconductor layer 230 can be suppressed.

[0426] Within the trench 291, the side surface of the conductive layer 240a or 240b is preferably aligned or substantially aligned with the side surface of the insulating layer 280. By employing this structure, the trench 291 can be formed in both the conductive layer 240a or 240b and the insulating layer 280 in a single step. Furthermore, the thickness of the semiconductor layer 230 and the like disposed within the trench 291 can be made uniform. Additionally, separation of the semiconductor layer 230 and the like due to steps or the like between the conductive layer 240a or 240b and the insulating layer 280 can be prevented.

[0427] Note that the present invention is not limited to the structure described above. For example, the side surface of the conductive layer 240a or 240b within the groove 291 may be discontinuous with the side surface of the insulating layer 280. Furthermore, the inclination of the side surface of the conductive layer 240a or 240b within the groove 291 may differ from the inclination of the side surface of the insulating layer 280. In this case, a portion of the sidewall of the groove 291 becomes tapered.

[0428] exist Figures 18A to 18D The example shown illustrates a structure where the extending direction of the trench 291 coincides with the extending direction of the conductive layer 260 used as a gate wiring, but the present invention is not limited thereto. For example, the extending direction of the trench 291 may also intersect with the extending direction of the gate wiring.

[0429] The following is for reference Figures 23A to 25C This section illustrates a transistor structure that differs from that of transistor 200A. Note that descriptions that are repeated above are omitted here; only the differences are explained in detail. Furthermore, even if components differ in location or shape, they will be given the same symbol and their descriptions will be omitted if their functions are the same.

[0430] [Transistor 200B]

[0431] Figure 23A It is a plan view of a semiconductor device including transistor 200B. Figure 23B It is along Figure 23A The cross-sectional view of the dotted line A1-A2 shown. Figure 23C It is along Figure 23A The cross-sectional view shown is the dotted-dash line A3-A4. Figure 23D It is along Figure 23B The cross-sectional view shown is the dotted-dash line A5-A6.

[0432] Figures 23A to 23D The semiconductor device shown is mainly similar to the one shown in that it includes a conductive layer 265 but does not include an insulating layer 283, conductive layer 243a, conductive layer 243b, and conductive layer 246. Figures 18A to 18D The semiconductor device shown is different. Furthermore, it differs from the example in that the conductive layer 260 is configured as an island and the conductive layers 240a and 240b are extended. Figures 18A to 18D The semiconductor devices shown are different.

[0433] A conductive layer 265 is disposed on the insulating layer 285 and is in contact with the conductive layer 260. The conductive layer 265 extends in the Y direction. Conductive layers 240a and 240b extend in the X direction.

[0434] The conductive layer 260 is configured in an island shape. When viewed from a planar perspective, the outer periphery of the conductive layer 260 is located inside the outer periphery of the semiconductor layer 230. Furthermore, when viewed from a planar perspective, the outer periphery of the conductive layer 260 may overlap with a portion of the outer periphery of the semiconductor layer 230, or it may be located outside a portion of the outer periphery of the semiconductor layer 230.

[0435] In the YZ plane including the semiconductor layer 230, the end outside the trench 291 of the semiconductor layer 230 is located inside the end outside the trench 291 of the conductive layer 240 (refer to...). Figure 23B Furthermore, in the YZ plane including the semiconductor layer 230, the end outside the trench 291 of the semiconductor layer 230 may be aligned or substantially aligned with the end outside the trench 291 of the conductive layer 240, or it may be located outside the end outside the trench 291 of the conductive layer 240.

[0436] An insulating layer 285 is disposed on the insulating layer 250. Furthermore, the insulating layer 285 is disposed in such a way that it is embedded in the portion of the groove 291 where the conductive layer 260 is not disposed.

[0437] By adopting Figures 23A to 23D The structure shown increases the physical distance between conductive layer 260 and conductive layer 240a or 240b, thereby reducing the parasitic capacitance generated between them. Furthermore, increasing the physical distance between conductive layer 265 and conductive layer 240a or 240b further reduces the parasitic capacitance between them. Therefore, the frequency characteristics of circuits using this transistor can be improved.

[0438] exist Figures 23A to 23D The example illustrates a structure where the conductive layer 260 has a region facing the side of the conductive layer 240a across the semiconductor layer 230 and a region facing the side of the conductive layer 240b across the semiconductor layer 230; however, the present invention is not limited thereto. For example, a first conductive layer facing the side of the conductive layer 240a across the semiconductor layer 230 and a second conductive layer facing the side of the conductive layer 240b across the semiconductor layer 230 may also be provided.

[0439] [Transistor 200Ca and Transistor 200Cb]

[0440] Figure 24A It is a plan view of a semiconductor device including transistors 200Ca and 200Cb. Figure 24B It is along Figure 24A The cross-sectional view of the dotted line A1-A2 shown. Figure 24C It is along Figure 24B The cross-sectional view shown is the dotted-dash line A5-A6.

[0441] Figures 24A to 24C The semiconductor device shown is similar in that the conductive layer 220, semiconductor layer 230, insulating layer 250, and conductive layer 260 are all separated in and around the trench 291. Figures 23A to 23C The semiconductor devices shown are different.

[0442] Transistor 200Ca includes a conductive layer 220a, a conductive layer 240a on an insulating layer 280, a semiconductor layer 230a, an insulating layer 250a on the semiconductor layer 230a, and a conductive layer 260a on the insulating layer 250a. Transistor 200Cb includes a conductive layer 220b, a conductive layer 240b on an insulating layer 280, a semiconductor layer 230b, an insulating layer 250b on the semiconductor layer 230b, and a conductive layer 260b on the insulating layer 250b.

[0443] In transistor 200Ca, semiconductor layer 230a is used as the semiconductor layer, conductive layer 260a is used as the gate electrode, insulating layer 250a is used as the gate insulating layer, conductive layer 220a is used as one of the source and drain electrodes, and conductive layer 240a is used as the other of the source and drain electrodes. In transistor 200Cb, semiconductor layer 230b is used as the semiconductor layer, conductive layer 260b is used as the gate electrode, insulating layer 250b is used as the gate insulating layer, conductive layer 220b is used as one of the source and drain electrodes, and conductive layer 240b is used as the other of the source and drain electrodes.

[0444] By placing transistor 200Ca in contact with one sidewall of the trench 291 and transistor 200Cb in contact with the other sidewall of the trench 291, miniaturization and high integration of semiconductor devices can be advanced.

[0445] exist Figures 24A to 24C The example illustrates a structure in which the insulating layer 250 is divided into an insulating layer 250a and an insulating layer 250b, but the present invention is not limited thereto.

[0446] Reference Figures 25A to 25C Reference Figures 24A to 24C The illustration shows two variations of transistors. Figure 25A It is a plan view of a semiconductor device that includes two transistors. Figure 25B It is along Figure 25AThe cross-sectional view of the dotted line A1-A2 shown. Figure 25C It is along Figure 25A The cross-sectional view shown is the dotted-dash line A5-A6.

[0447] Figures 25A to 25C The semiconductor device shown is similar to the one in that the insulating layer 250 covers both semiconductor layers 230a and 230b. Figures 24A to 24C The semiconductor device shown is different. By covering semiconductor layers 230a and 230b with insulating layer 250, the side surface of the trench portion 291 of semiconductor layer 230a and the side surface of the trench portion 291 of semiconductor layer 230b can be covered. Therefore, hydrogen diffusion into semiconductor layers 230a and 230b can be suppressed. Therefore, a highly reliable transistor can be realized.

[0448] In transistors 200A to 200Cb, at least a portion of the transistor's constituent elements are disposed in the extended groove 291, but the present invention is not limited thereto. At least a portion of the transistor's constituent elements may be disposed in an opening that is circular when viewed from a plan view.

[0449] [Transistor 200D]

[0450] Figure 26A It is a plan view of a semiconductor device including transistor 200D. Figure 26B It is along Figure 26A The cross-sectional view of the dotted line A1-A2 shown. Figure 26C It is along Figure 26A The cross-sectional view shown is the dotted-dash line A3-A4. Figure 26D It is along Figure 26B The cross-sectional view shown is the dotted-dash line A5-A6.

[0451] Figures 26A to 26D The semiconductor device shown is Figures 18A to 18D The difference in the semiconductor device shown is that: Figures 26A to 26D The semiconductor device shown does not include conductive layer 243a, conductive layer 243b and conductive layer 246. Figures 26A to 26D The transistor 200D shown is Figures 18A to 18D The difference in the transistor 200A shown is that: Figures 26A to 26D In the transistor 200D shown, a portion of the transistor's constituent elements are disposed in the opening 290 instead of in the slot 291. Furthermore, Figures 26A to 26D The transistor 200D shown is Figures 18A to 18D The difference in the transistor 200A shown is that: Figures 26A to 26D The transistor 200D shown includes a conductive layer 240 having a region extending in the Y direction instead of conductive layers 240a and 240b.

[0452] The conductive layer 220 is used as one of the source and drain electrodes of the transistor 200D, and the conductive layer 240 is used as the other of the source and drain electrodes of the transistor 200D.

[0453] like Figure 26B and Figure 26C As shown, the insulating layer 280 and the conductive layer 240 are provided with an opening 290 that reaches the conductive layer 220.

[0454] The opening 290 includes the opening in the insulating layer 280 and the opening in the conductive layer 240. Furthermore, the shape and size of the openings 290 in each layer can differ when viewed from a planar perspective. Additionally, when the top surface of the opening 290 is circular, the openings in each layer can be concentric or non-concentric.

[0455] The semiconductor layer 230, the insulating layer 250, and the conductive layer 260 are all arranged such that at least a portion of each is located within the opening 290. Furthermore, the portions of the semiconductor layer 230, the insulating layer 250, and the conductive layer 260 arranged within the opening 290 reflect the shape of the opening 290.

[0456] The semiconductor layer 230 is disposed such that it covers the bottom and sidewalls of the opening 290. Furthermore, the semiconductor layer 230 has a recess that reflects the shape of the opening 290. The semiconductor layer 230 includes a portion that contacts the top surface of the conductive layer 240 and a portion that contacts the top surface of the conductive layer 220 within the opening 290.

[0457] The insulating layer 250 is provided to cover the semiconductor layer 230. Furthermore, the insulating layer 250 is provided on the insulating layer 280 to cover the top and side surfaces of the semiconductor layer 230 and the side surfaces of the conductive layer 240. Additionally, the insulating layer 250 has recesses that reflect the shape of the recesses in the semiconductor layer 230.

[0458] The conductive layer 260 is provided in such a way that at least a portion of the recess in the insulating layer 250 is embedded.

[0459] Furthermore, the conductive layer 260 has a region in the opening 290 that overlaps with the semiconductor layer 230 through the insulating layer 250.

[0460] like Figure 26DAs shown, the semiconductor layer 230, insulating layer 250, and conductive layer 260 are arranged concentrically by forming the opening 290 in a circular shape when viewed from the plane. Therefore, the side of the conductive layer 260, located at the center of the opening 290, faces the side of the semiconductor layer 230 across the insulating layer 250. In other words, the entire outer periphery of the semiconductor layer 230 forms a channel formation region when viewed from the plane. At this time, for example, the channel width of the transistor 200D is determined by the length of the outer periphery of the semiconductor layer 230. That is to say, the channel width of the transistor 200D is determined by the width of the opening 290 (the diameter if the opening 290 is circular when viewed from the plane).

[0461] Furthermore, by setting the semiconductor layer 230, the insulating layer 250, and the conductive layer 260 in a concentric circle, the distance between the conductive layer 260 and the semiconductor layer 230 is approximately uniform, so a gate electric field can be applied to the semiconductor layer 230 approximately uniformly.

[0462] Furthermore, in this embodiment, an example is shown where the opening 290 is circular when viewed from a plane. By using a circle, the processing accuracy when forming the opening can be improved, and openings of minute size can be formed. Note that the present invention is not limited thereto. The shape of the opening 290 when viewed from a plane can be, for example, a circle, an ellipse or other approximate circle, a triangle, a quadrilateral (including rectangles, rhombuses, and squares), a pentagon, a star-shaped polygon, or other polygons with rounded corners.

[0463] [Transistor 200E]

[0464] Figure 27A This is a plan view of a semiconductor device including transistor 200E. Figure 27B It is along Figure 27A The cross-sectional view of the dotted line A1-A2 shown. Figure 27C It is along Figure 27A The cross-sectional view shown is along the dashed-dot line A3-A4. Note that along... Figure 27B The cross-sectional view of the dotted lines A5-A6 shown can be referenced. Figure 26D .

[0465] Figures 27A to 27C The semiconductor device shown is similar in that it includes conductive layer 265, insulating layer 284, and insulating layer 285. Figures 26A to 26D The semiconductor devices shown are different.

[0466] In transistor 200E, the stacked structure from conductive layer 220 to insulating layer 250 is the same as that of transistor 200D described above, so detailed description is omitted.

[0467] like Figure 27B and Figure 27CAs shown, the insulating layer 284 is disposed on the insulating layer 250. Furthermore, the insulating layer 284 has an opening 270 that reaches the insulating layer 250 at a position overlapping with the opening 290.

[0468] The conductive layer 260 is disposed in a manner that embeds into the openings 290 and 270. The conductive layer 260 is disposed on the insulating layer 250 and contacts the insulating layer 250 in the opening 270. The conductive layer 260 includes a portion in the opening 290 that is opposite to the semiconductor layer 230 across the insulating layer 250 and a portion located in the opening 270.

[0469] Figure 27B and Figure 27C An example is shown where both conductive layers 260_1 and 260_2 are provided in the opening 290. Note that when the widths of the opening 290 and 270 are small, sometimes only conductive layer 260_1 is provided in the opening 290, and both conductive layers 260_1 and 260_2 are provided in the opening 270. Furthermore, sometimes only conductive layer 260_1 is provided in the opening 270.

[0470] A conductive layer 265 is disposed on the conductive layer 260 and is in contact with the top surface of the conductive layer 260. The conductive layer 260 and the conductive layer 265 can also be considered to be connected to each other. Furthermore, the conductive layer 265 can be considered as a component of the transistor 200E. The height of the top surface of the conductive layer 260 is the same as or approximately the same as the height of the top surface of the insulating layer 285.

[0471] Conductive layer 265 is used as gate wiring. As conductive layer 265, materials suitable for conductive layer 260 can be used. For example, high-melting-point materials such as tungsten or molybdenum, which combine heat resistance and conductivity, can be used as conductive layer 265. Alternatively, low-resistance conductive materials such as aluminum or copper can be used. Using low-resistance conductive materials reduces wiring resistance.

[0472] The portion of conductive layer 265 that does not overlap with opening 290 is primarily located on insulating layer 285. Therefore, conductive layer 265 mainly overlaps with conductive layer 240 through insulating layer 284 and insulating layer 285. This increases the physical distance between conductive layer 265 and conductive layer 240, reducing parasitic capacitance between them. Furthermore, conductive layer 240 and conductive layer 265 may also have portions that do not overlap through insulating layer 285.

[0473] Transistor 200E has a structure that reduces the parasitic capacitance between the source and drain electrodes and the gate wiring. Therefore, the frequency characteristics of circuits using this transistor can be improved.

[0474] Note that this embodiment shows an example where the opening 270 is circular when viewed from a plane, but the invention is not limited thereto. The shape that can be used for the opening 270 is the same as the shape that can be used for the opening 290 described above.

[0475] The width of the opening 270 sometimes varies in the depth direction. Here, in particular, the maximum value of the width of the opening 270 provided in the insulating layer 284 when viewed from the cross-section is used as the width of the opening 270.

[0476] The insulating layer 284 preferably has the function of trapping or fixing hydrogen. By adopting this structure, the diffusion of hydrogen from above the insulating layer 284 to the semiconductor layer 230 can be suppressed, and the hydrogen contained in the semiconductor layer 230 can be trapped or fixed. Therefore, the hydrogen concentration in the semiconductor layer 230 can be reduced. As the insulating layer 284, alumina, hafnium oxide, hafnium zirconium oxide, or hafnium silicate, etc., can be used.

[0477] Furthermore, a hydrogen barrier insulating layer can be used as the insulating layer 284. This suppresses hydrogen diffusion from above the insulating layer 284 to the semiconductor layer 230. Silicon nitride and silicon oxynitride both have the characteristic of not allowing oxygen and hydrogen to permeate easily, making them suitable for use in the insulating layer 284.

[0478] When the insulating layer 284 comprises a silicon nitride film, the silicon nitride film is preferably deposited by sputtering. Because sputtering does not require the use of hydrogen-containing molecules in the deposition gas, the hydrogen concentration of the insulating layer 284 can be reduced. By depositing the insulating layer 284 by sputtering, a high-density silicon nitride film can be formed.

[0479] Furthermore, the insulating layer 284 can also be a laminated structure of an insulating layer with the function of trapping or fixing hydrogen and a hydrogen barrier insulating layer. For example, the insulating layer 284 can also include a laminated film of an aluminum oxide film and a silicon nitride film on the aluminum oxide film.

[0480] The insulating layer 285 is used as an interlayer film, and therefore a material with a relatively low permittivity as described above is preferred. For example, the insulating layer 285 preferably comprises a silicon oxide film.

[0481] [Transistor 200F]

[0482] Figure 28A It is a plan view of a semiconductor device including transistor 200F. Figure 28B It is along Figure 28A The cross-sectional view of the dotted line A1-A2 shown. Figure 28C It is along Figure 28A The cross-sectional view shown is the dotted-dash line A3-A4. Figure 28D It is along Figure 28B The cross-sectional view shown is the dotted-dash line A5-A6.

[0483] Figures 28A to 28D The semiconductor device shown is mainly similar to the one comprising insulating layer 225, conductive layer 255, and insulating layer 281. Figures 26A to 26D The semiconductor devices shown are different.

[0484] like Figure 28B As shown, conductive layer 255 is located on insulating layer 280, and insulating layer 281 is located on both conductive layer 255 and insulating layer 280. Furthermore, conductive layer 240 is located on insulating layer 281. Openings 290 leading to conductive layer 220 are provided in insulating layer 280, conductive layer 255, insulating layer 281, and conductive layer 240. Insulating layer 225 is located between insulating layer 280 and semiconductor layer 230.

[0485] like Figure 28B As shown, the conductive layer 220 includes a first recess and a second recess located outside the first recess. The depth of the first recess is greater than that of the second recess. In other words, the bottom surface of the first recess is located below the bottom surface of the second recess (on the side of the insulating layer 210). Furthermore, the side surface of the second recess is aligned or substantially aligned with the side surface of the insulating layer 280 in the opening 290, and the side surface of the first recess is aligned or substantially aligned with the side surface of the semiconductor layer 230 of the insulating layer 225. Hereinafter, the first recess and the second recess will sometimes be collectively referred to as recesses.

[0486] exist Figure 28B In the above configuration, insulating layer 225 contacts the bottom and side surfaces of the second recess included in conductive layer 220, and contacts the side surfaces of insulating layer 280 and conductive layer 240 in opening 290. Semiconductor layer 230 contacts the bottom and side surfaces of the first recess included in conductive layer 220, insulating layer 225, and top surfaces of conductive layer 240. Insulating layer 250 is located inside semiconductor layer 230 in opening 290, and conductive layer 260 is located inside insulating layer 250 in opening 290.

[0487] Transistor 200F can also be structured such that the insulating layer 225 does not cover at least a portion of the side surface of the conductive layer 240. In this case, the side of the conductive layer 240 not covered by the insulating layer 225 is in contact with the semiconductor layer 230. Therefore, the contact resistance between the semiconductor layer 230 and the conductive layer 240 can be reduced.

[0488] Figure 28A An example of a single-layer structure for insulating layer 225 is shown. However, insulating layer 225 can also have a stacked structure of two or more layers. For example, insulating layer 225 can have a two-layer structure with a first insulating layer and a second insulating layer. The first insulating layer contacts the side of the insulating layer 280 in the opening 290, and the second insulating layer is located between the first insulating layer and the semiconductor layer 230.

[0489] The insulating material described in the section on [Insulating Layers], which will be explained later, can be used as the first insulating layer, and the material described above that can be used for insulating layer 20 can be used as the second insulating layer. For example, a hydrogen-barrier insulating layer can be used as the first insulating layer, and an insulating layer having regions containing excess oxygen can be used as the second insulating layer. By adopting this structure, one or both of the oxygen vacancies and hydrogen in the semiconductor layer 230 can be reduced. Therefore, the electrical characteristics of the transistor can be improved, thereby increasing the reliability of the transistor. For example, it is preferable to use silicon nitride as the first insulating layer and silicon oxide or silicon oxynitride as the second insulating layer.

[0490] Semiconductor layer 230 has a region that overlaps with conductive layer 255 across insulating layer 225 and with conductive layer 260 across insulating layer 250. At least a portion of this region is used as a channel formation region for transistor 200F.

[0491] In transistor 200F, conductive layer 260 is used as the first gate electrode, insulating layer 250 is used as the first gate insulating layer, conductive layer 255 is used as the second gate electrode, and insulating layer 225 is used as the second gate insulating layer.

[0492] Furthermore, in transistor 200F, one of conductive layer 255 and conductive layer 260 may be used as the gate electrode, and the other as the back gate electrode. Transistor 200F is sometimes particularly preferably configured such that conductive layer 260 is used as the gate electrode and conductive layer 255 is used as the back gate electrode. By using conductive layer 260, which has a larger region opposite semiconductor layer 230 than conductive layer 255, as the gate electrode, the gate electric field is applied to semiconductor layer 230 more effectively, thus sometimes improving the electrical characteristics of the transistor. Note that when conductive layer 260 is used as the gate electrode and conductive layer 255 is used as the back gate electrode, insulating layer 250 is used as the gate insulating layer, and insulating layer 225 is used as the back gate insulating layer.

[0493] Because transistor 200F includes a conductive layer that serves as a back gate electrode, the threshold voltage of transistor 200F can be controlled according to the potential supplied to this conductive layer. Therefore, by controlling the threshold voltage, a normally off transistor can be easily implemented.

[0494] The conductive layer 255 can use a conductive material that can be used in the conductive layer 260.

[0495] Insulating layer 281 is used as an interlayer membrane. Insulating layer 281 can use an insulating material that can be used for insulating layer 280.

[0496] Figure 28BAn example of a single-layer structure for insulating layer 281 is shown. However, insulating layer 281 can also have a stacked structure of two or more layers. For example, insulating layer 281 can have a three-layer structure consisting of a first insulating layer, a second insulating layer on the first insulating layer, and a third insulating layer on the second insulating layer. In this case, it is preferable to use a material with a low relative permittivity as the second insulating layer, and to use oxygen-barrier insulating layers as the first and third insulating layers. This suppresses oxidation of conductive layers 255 and 240 and prevents high resistivity.

[0497] Materials Constituting Semiconductor Devices

[0498] The following describes the materials that can be used in the semiconductor device of this embodiment. Note that each layer constituting the semiconductor device of this embodiment may have a single-layer structure or a stacked structure.

[0499] [Oxide semiconductor layer]

[0500] Regarding the oxide semiconductor layer of the transistor that can be used as one aspect of the present invention, refer to the description in <Structure of Semiconductor Device>.

[0501] The carrier concentration in the channel formation region is preferably below 1×10⁻⁶. 19 cm -3 Below, less than 1×10 18 cm -3 Below, less than 5×10 17 cm -3 Less than 1×10 17 cm -3 Less than 1×10 16 cm -3 Less than 1×10 15 cm -3 Less than 1×10 14 cm -3 Less than 1×10 13 cm -3 Less than 1×10 12 cm -3 Less than 1×10 11 cm -3 Or less than 1×10 10 cm -3 Note that there is no specific limit to the lower limit of carrier concentration in the channel formation region; for example, it can be 1 × 10⁻⁶. -7 cm -3 .

[0502] As described above, in an OS transistor, when oxygen vacancies (V0) exist in the channel formation region of the oxide semiconductor... OWhen impurities are present, the electrical characteristics can easily change, leading to a decrease in reliability. Therefore, reducing the impurity concentration in the oxide semiconductor is effective in stabilizing the electrical characteristics of the OS transistor. To further reduce the impurity concentration in the oxide semiconductor, it is preferable to also reduce the impurity concentration in the nearby film. Examples of impurities include hydrogen, carbon, and nitrogen.

[0503] When nitrogen is present in oxide semiconductors, trapped states sometimes form. As a result, the electrical characteristics of the transistor can sometimes be unstable. Therefore, the nitrogen concentration in the channel formation region of the oxide semiconductor, as measured by SIMS, is set to 1 × 10⁻⁶. 20 atoms / cm 3 The following is preferred: 5×10 19 atoms / cm 3 Hereinafter, 1×10 is more preferred. 19 atoms / cm 3 The following is more preferably 5×10 18 atoms / cm 3 Hereinafter, 1×10 is more preferred. 18 atoms / cm 3 The following is a further preferred option: 5×10 17 atoms / cm 3 the following.

[0504] Furthermore, when oxide semiconductors contain alkali metals or alkaline earth metals, defect states sometimes form, making the electrical characteristics of the transistor unstable. Therefore, the concentration of alkali metals or alkaline earth metals in the channel formation region of the oxide semiconductor, measured using SIMS, is set to 1 × 10⁻⁶. 18 atoms / cm 3 The following is preferred: 2×10 16 atoms / cm 3 the following.

[0505] By using oxide semiconductors with sufficiently reduced impurities in the channel formation region of a transistor, the transistor can have stable electrical characteristics.

[0506] [Insulating layer]

[0507] Inorganic insulating films are preferably used for the insulating layers (insulating layer 210, insulating layer 225, insulating layer 250, insulating layer 280, insulating layer 283, insulating layer 284, insulating layer 285, etc.) included in the semiconductor device. Examples of inorganic insulating films include oxide insulating films, nitride insulating films, oxynitride insulating films, and oxynitride insulating films. Examples of oxide insulating films include silicon oxide films, aluminum oxide films, magnesium oxide films, gallium oxide films, germanium oxide films, yttrium oxide films, zirconium oxide films, lanthanum oxide films, neodymium oxide films, hafnium oxide films, tantalum oxide films, cerium oxide films, gallium zinc oxide films, and hafnium aluminum oxide films. Examples of nitride insulating films include silicon nitride films and aluminum nitride films. Examples of oxynitride insulating films include silicon oxynitride films, aluminum oxynitride films, gallium oxynitride films, yttrium oxynitride films, and hafnium oxynitride films. Examples of oxynitride insulating films include silicon oxynitride films and aluminum oxynitride films. Furthermore, organic insulating films can also be used as insulating layers included in semiconductor devices.

[0508] For example, when miniaturizing and highly integrating transistors, problems such as leakage current sometimes occur due to the thinning of the gate insulating layer. By using a high-k material as the gate insulating layer, low voltage can be achieved during transistor operation while maintaining the physical thickness. Furthermore, the equivalent oxide thickness (EOT) of the gate insulating layer can be thinned. On the other hand, by using a material with a low relative permittivity as the insulating layer used as an interlayer film, parasitic capacitance generated between wirings can be reduced. Therefore, it is preferable to select the material based on the function of the insulating layer. Moreover, materials with a low relative permittivity are also materials with high dielectric strength.

[0509] Materials with relatively high permittivity include, for example, aluminum oxide, gallium oxide, hafnium oxide, tantalum oxide, zirconium oxide, hafnium zirconium oxide, oxides containing aluminum and hafnium, oxynitrides containing aluminum and hafnium, oxides containing silicon and hafnium, oxynitrides containing silicon and hafnium, and nitrides containing silicon and hafnium.

[0510] Examples of materials with low relative permittivity include inorganic insulating materials such as silicon oxide, silicon oxynitride, and silicon oxynitride, as well as resins such as polyesters, polyolefins, polyamides (nylon and aramids, etc.), polyimides, polycarbonates, and acrylic resins. Furthermore, examples of inorganic insulating materials with low relative permittivity other than those mentioned above include fluorine-containing silicon oxide, carbon-containing silicon oxide, and silicon oxide containing both carbon and nitrogen. Additionally, porous silicon oxide can be used as an example. Moreover, these silicon oxides may contain nitrogen.

[0511] Furthermore, ferroelectric materials can be used as the insulating layer included in the semiconductor device. As a ferroelectric material, an oxide containing one or both of hafnium and zirconium is preferred. Examples of such oxides include metal oxides such as hafnium oxide, zirconium oxide, and hafnium-zirconium oxide. Furthermore, as a ferroelectric material, a material in which element J1 (here, element J1 is selected from one or more of the other of hafnium and zirconium, silicon, aluminum, gadolinium, yttrium, lanthanum, and strontium) is added to a metal oxide containing one of hafnium and zirconium can be used.

[0512] Furthermore, by adding a Group 3 element from the periodic table to an oxide containing one or both of hafnium and zirconium, the oxygen vacancy concentration in the oxide is increased, thereby facilitating the formation of crystals with an orthorhombic crystal structure. This increases the proportion of crystals with an orthorhombic crystal structure, enhancing remanent polarization, which is therefore preferable. On the other hand, excessive addition of a Group 3 element may reduce the crystallinity of the oxide, making it less likely to exhibit ferroelectricity. Therefore, the content of a Group 3 element in the oxide containing one or both of hafnium and zirconium is preferably 0.1 atomic% or more and 10 atomic% or less, more preferably 0.1 atomic% or more and 5 atomic% or less, and even more preferably 0.1 atomic% or more and 3 atomic% or less. Here, the content of a Group 3 element refers to the percentage of Group 3 element atoms in the sum of the atomic numbers of all metal elements contained in the layer. The Group 3 element is preferably selected from one or more of scandium, lanthanum, and yttrium, more preferably from one or both of lanthanum and yttrium.

[0513] Furthermore, as materials capable of exhibiting ferroelectric properties, examples include metal nitrides comprising at least one of elements M1 and M2 and nitrogen. Here, element M1 is selected from one or more of aluminum, gallium, and indium. Furthermore, element M2 is selected from one or more of boron, scandium, yttrium, lanthanum, cerium, neodymium, europium, titanium, zirconium, hafnium, vanadium, niobium, tantalum, and chromium. Furthermore, as materials capable of exhibiting ferroelectric properties, examples include materials incorporating element M3 into the aforementioned metal nitrides. Furthermore, element M3 is selected from one or more of magnesium, calcium, strontium, zinc, and cadmium.

[0514] Furthermore, perovskite-type oxynitrides such as SrTaO2N and BaTaO2N, as well as κ-type alumina such as GaFeO3, can be cited as materials that can exhibit ferroelectric properties. Additionally, lead titanate (PbTiO2) can also be used as a material that can exhibit ferroelectric properties. X Piezoelectric ceramics with perovskite structure, such as barium strontium titanate (BST), strontium titanate, lead zirconate titanate (PZT), strontium bismuth tantalate (SBT), bismuth ferrite (BFO), or barium titanate.

[0515] Note that while examples of metal oxides and metal nitrides are shown in the above description, the invention is not limited to these. For example, metal oxynitrides with nitrogen added to the aforementioned metal oxides or metal oxynitrides with oxygen added to the aforementioned metal nitrides may also be used.

[0516] Furthermore, as a material that can be ferroelectric, for example, a mixture or compound composed of multiple materials selected from the above-mentioned materials can be used. Additionally, the insulating layer 130 described in Embodiment 3 can have a laminated structure composed of multiple materials selected from the above-mentioned materials. Note that the crystal structure (properties) of the materials listed above may vary not only depending on the deposition conditions but also depending on various processes, etc. Therefore, in this specification, materials exhibiting ferroelectricity are referred not only to ferroelectric materials but also to materials that can be ferroelectric.

[0517] In this specification and the like, a ferroelectric material formed in a layered manner is sometimes referred to as a ferroelectric layer, a metal oxide film, or a metal nitride film. Furthermore, in this specification and the like, a device comprising a ferroelectric layer, a metal oxide film, or a metal nitride film is sometimes referred to as a ferroelectric device.

[0518] The ferroelectric layer preferably has a crystal with an orthorhombic crystal structure, thereby exhibiting ferroelectricity. The crystal structure of the crystal contained in the ferroelectric layer can be one or more selected from the tetragonal, orthorhombic, monoclinic, and hexagonal crystal systems. Alternatively, the ferroelectric layer can also have an amorphous structure. In this case, the ferroelectric layer can also have a composite structure of amorphous and crystalline structures.

[0519] Metal oxides containing one or both of hafnium and zirconium are also insulating materials with the function of trapping or fixing hydrogen. Therefore, by using a metal oxide containing one or both of hafnium and zirconium for at least a portion of the gate insulating layer, hydrogen contained in the oxide semiconductor layer can be trapped or fixed, thereby reducing the hydrogen concentration of the oxide semiconductor layer. Furthermore, the transistor including this gate insulating layer can be used as a FeFET (Ferroelectric Field Effect Transistor).

[0520] Furthermore, by surrounding a transistor using metal oxides with an insulating layer that suppresses the permeation of impurities and oxygen, the electrical characteristics of the transistor can be stabilized. For example, the insulating layer that suppresses the permeation of impurities and oxygen can be a single layer or a stack of insulating layers selected from one or more of boron, carbon, nitrogen, oxygen, fluorine, magnesium, aluminum, silicon, phosphorus, chlorine, argon, gallium, germanium, yttrium, zirconium, lanthanum, neodymium, hafnium, and tantalum. Specifically, the material used for the insulating layer that suppresses the permeation of impurities and oxygen can be metal oxides such as aluminum oxide, magnesium oxide, germanium oxide, yttrium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, hafnium oxide, and tantalum oxide, as well as nitrides such as aluminum nitride and silicon nitride, and oxynitrides such as silicon oxynitride.

[0521] Specifically, materials used as insulating layers that suppress the permeation of impurities such as water and hydrogen, as well as oxygen, include, for example, metal oxides such as aluminum oxide, magnesium oxide, germanium oxide, yttrium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, hafnium oxide, tantalum oxide, and oxides containing aluminum and hafnium (hafnium aluminate). Additionally, nitrides such as aluminum nitride, titanium aluminum nitride, and silicon nitride can be used as examples. Furthermore, nitrogen oxides such as silicon oxynitride can be used as examples. Moreover, gallium oxide can be used as an insulating layer material that suppresses oxygen permeation.

[0522] Furthermore, the insulating layer, such as the gate insulating layer, that contacts the oxide semiconductor layer or is disposed near the oxide semiconductor layer is preferably an insulating layer having regions containing excess oxygen. For example, by making the insulating layer having regions containing excess oxygen contact the oxide semiconductor layer or located near the oxide semiconductor layer, oxygen vacancies in the oxide semiconductor layer can be reduced. Regarding insulating layers that easily form regions containing excess oxygen, please refer to the description in <Structure of Semiconductor Devices>.

[0523] A hydrogen-barrier insulating layer is preferably used as an insulating layer in contact with or near the oxide semiconductor layer. This insulating layer's hydrogen-barrier properties suppress hydrogen diffusion into the oxide semiconductor layer. In other words, a hydrogen-barrier insulating layer is an insulating layer that functions to suppress hydrogen diffusion.

[0524] Examples of insulating materials that can trap or fix hydrogen include oxides containing hafnium, oxides containing magnesium, oxides containing aluminum, oxides containing both aluminum and hafnium (hafnium aluminate), and hafnium silicate. Furthermore, these metal oxides may also contain zirconium; for example, oxides containing both hafnium and zirconium can be cited.

[0525] An insulating layer with the function of capturing or fixing hydrogen preferably has an amorphous structure. In metal oxides with an amorphous structure, the ability to capture or fix hydrogen is high because some oxygen atoms have dangling bonds. Therefore, by making the insulating layer have an amorphous structure, the function of capturing or fixing hydrogen can be improved.

[0526] By giving the insulating layer an amorphous structure, the formation of grain boundaries can be suppressed. Suppressing grain boundary formation improves the flatness of the insulating layer. This results in a more uniform thickness distribution of the insulating layer, reducing extremely thin sections and thus improving its withstand voltage. Furthermore, the thickness distribution of the film disposed on the insulating layer can be made more uniform. Moreover, by suppressing grain boundary formation in the insulating layer, leakage current originating from defect states at grain boundaries can be reduced. Therefore, the insulating layer can be used as an insulating film with low leakage current.

[0527] Furthermore, the function of capturing or fixing the corresponding substance can also be described as possessing the property that the corresponding substance is not easily diffused. Therefore, the function of capturing or fixing the corresponding substance can also be referred to as barrier property.

[0528] In this specification, the term "barrier insulating layer" refers to an insulating layer that possesses barrier properties. Furthermore, barrier properties refer to the property that makes it difficult for the corresponding substance to diffuse (also known as the property that makes it difficult for the corresponding substance to pass through, the property that the corresponding substance has low permeability, or the function of inhibiting the diffusion of the corresponding substance). Note that hydrogen, as described as the corresponding substance, refers to hydrogen atoms, hydrogen molecules, water molecules, and OH-. - At least one of the following: substances bonded to hydrogen. Furthermore, unless otherwise specified, the impurity described as the corresponding substance refers to impurities in the channel forming region or semiconductor layer, such as at least one of hydrogen atoms, hydrogen molecules, water molecules, nitrogen atoms, nitrogen molecules, nitrogen oxide molecules (N₂O, NO, NO₂, etc.), copper atoms, etc. Furthermore, the oxygen described as the corresponding substance refers to at least one of oxygen atoms and oxygen molecules, for example.

[0529] Materials that can be used as hydrogen barrier insulating layers include aluminum oxide, magnesium oxide, hafnium oxide, zirconium oxide, oxides containing aluminum and hafnium (hafnium aluminate), oxides containing hafnium and zirconium (hafnium zirconium oxide), silicon nitride, or silicon oxynitride.

[0530] Inorganic insulating layers, exemplified as insulating layers that trap or fix hydrogen and those that inhibit hydrogen diffusion, also possess oxygen-barrier properties. Materials that serve as oxygen-barrier insulating layers include, for example, oxides containing one or both of aluminum and hafnium, magnesium oxide, zinc gallium oxide, silicon nitride, and silicon oxynitride. Furthermore, oxides containing one or both of aluminum and hafnium include, for example, aluminum oxide, hafnium oxide, oxides containing aluminum and hafnium (hafnium aluminate), and hafnium silicate.

[0531] [Conductive layer]

[0532] The conductive layers (conductive layer 220, conductive layer 240, conductive layer 240a, conductive layer 240b, conductive layer 243a, conductive layer 243b, conductive layer 246, conductive layer 255, conductive layer 260, conductive layer 265, etc.) included in the semiconductor device preferably use a metallic element selected from aluminum, chromium, copper, silver, gold, platinum, zinc, tantalum, nickel, titanium, iron, cobalt, molybdenum, tungsten, hafnium, vanadium, niobium, manganese, magnesium, zirconium, beryllium, indium, ruthenium, palladium, iridium, strontium, and lanthanum, an alloy containing the above-mentioned metallic elements, or an alloy combining the above-mentioned metallic elements. As alloys containing the above-mentioned metallic elements, nitrides or oxides of the alloys may also be used. For example, tantalum nitride, titanium nitride, nitrides containing titanium and aluminum, nitrides containing tantalum and aluminum, ruthenium oxide, ruthenium nitride, oxides containing strontium and ruthenium, oxides containing lanthanum and nickel, etc., are preferred. In addition, semiconductors with high conductivity, such as polycrystalline silicon containing impurity elements such as phosphorus, and silicides such as nickel silicides can also be used.

[0533] Furthermore, nitrogen-containing conductive materials such as tantalum nitrides, titanium nitrides, molybdenum nitrides, tungsten nitrides, ruthenium nitrides, tantalum and aluminum nitrides, or titanium and aluminum nitrides; oxygen-containing conductive materials such as ruthenium oxide, oxides containing strontium and ruthenium, or oxides containing lanthanum and nickel; and materials containing metallic elements such as titanium, tantalum, or ruthenium are preferred because they are conductive materials that are not easily oxidized, have the function of inhibiting oxygen diffusion, or maintain conductivity even when absorbing oxygen. Examples of oxygen-containing conductive materials include indium oxide containing tungsten oxide, indium oxide containing titanium oxide, ITO, indium tin oxide containing titanium oxide, ITSO, In-Zn oxide, and indium zinc oxide containing tungsten oxide. In this specification, conductive films deposited using oxygen-containing conductive materials are sometimes referred to as oxide conductive films.

[0534] Furthermore, multiple conductive layers formed from the aforementioned materials can be stacked. For example, a stacked structure combining materials containing the aforementioned metallic elements and conductive materials containing oxygen can also be used. Furthermore, a stacked structure combining materials containing the aforementioned metallic elements and conductive materials containing nitrogen can also be used. Additionally, a stacked structure combining materials containing the aforementioned metallic elements, conductive materials containing oxygen, and conductive materials containing nitrogen can also be used.

[0535] Furthermore, when using metal oxides in the channel formation region of a transistor, a stacked structure combining a material containing the aforementioned metal element and an oxygen-containing conductive material is preferably used as the conductive layer serving as the gate electrode. In this case, it is preferable to provide the oxygen-containing conductive material on one side of the channel formation region. By providing the oxygen-containing conductive material on one side of the channel formation region, oxygen detached from this conductive material can be easily supplied to the channel formation region.

[0536] [Substrate]

[0537] Substrates for forming transistors can be, for example, insulating substrates, semiconductor substrates, or conductive substrates. Examples of insulating substrates include glass substrates, quartz substrates, sapphire substrates, stabilized zirconium oxide substrates (yttrium-stabilized zirconium oxide substrates, etc.), and resin substrates. Examples of semiconductor substrates include semiconductor substrates made of silicon or germanium, or compound semiconductor substrates composed of silicon carbide, silicon-germanium, gallium arsenide, indium phosphide, zinc oxide, and gallium oxide. Furthermore, semiconductor substrates having insulating regions within the aforementioned semiconductor substrates, such as SOI (Silicon on Insulator) substrates, can also be used. Examples of conductive substrates include graphite substrates, metal substrates, alloy substrates, and conductive resin substrates. Alternatively, substrates containing metal nitrides or metal oxides can be used. Furthermore, examples include insulating substrates with conductors or semiconductors, semiconductor substrates with conductors or insulators, and conductive substrates with semiconductors or insulators. Substrates on which components are disposed can also be used. Examples of components mounted on a substrate include capacitors, resistors, switching elements, light-emitting elements, and storage elements.

[0538] The above is a description of the materials that can be used in the semiconductor device of this embodiment.

[0539] This embodiment can be appropriately combined with other embodiments. Furthermore, in this specification, where multiple structural examples are shown in one embodiment, these structural examples can be appropriately combined.

[0540] (Implementation Method 3)

[0541] In this embodiment, refer to Figures 29A to 35 This invention describes a storage device according to one aspect of the present invention. The storage device according to one aspect of the present invention includes a storage cell. The storage cell includes at least a transistor. For example, the storage cell includes a transistor and a capacitor.

[0542] <Example 1 of storage device structure>

[0543] Reference Figures 29A to 29C Describe the structure of a storage device, including storage units. Figure 29A It is a plan view of a storage device including storage unit 150. Figure 29B It is along Figure 29A The cross-sectional view of the dotted line A1-A2 shown. Figure 29C It is along Figure 29A The cross-sectional view shown is the dotted-dash line A3-A4.

[0544] Figures 29A to 29C The storage device shown includes: an insulating layer 140 on a substrate (not shown); a conductive layer 110 on the insulating layer 140; storage cells 150 on the conductive layer 110; an insulating layer 180 on the conductive layer 110; and an insulating layer 280. The insulating layers 140 and 180 serve as interlayer films. The conductive layer 110 serves as wiring.

[0545] The storage cell 150 includes a capacitor 100 on the conductive layer 110 and a transistor 200 on the capacitor 100.

[0546] The capacitor 100 includes a conductive layer 115 on the conductive layer 110, an insulating layer 130 on the conductive layer 115, and a conductive layer 220_1 on the insulating layer 130. The conductive layer 220_1 serves as one of a pair of electrodes (sometimes referred to as the upper electrode), the conductive layer 115 serves as the other of the pair of electrodes (sometimes referred to as the lower electrode), and the insulating layer 130 serves as the dielectric. That is, the capacitor 100 constitutes a MIM (Metal-Insulator-Metal) capacitor. Furthermore, the conductive layer 220_2 disposed on the conductive layer 220_1 can also be considered as part of the upper electrode of the capacitor 100.

[0547] like Figure 29B and Figure 29C As shown, the insulating layer 180 is provided with an opening 190 reaching the conductive layer 110. At least a portion of the conductive layer 115 is disposed in the opening 190. Note that the conductive layer 115 has a region in the opening 190 that contacts the top surface of the conductive layer 110, a region in the opening 190 that contacts the side surface of the insulating layer 180, and a region that contacts at least a portion of the top surface of the insulating layer 180. The insulating layer 130 is disposed such that at least a portion of it is located in the opening 190. The conductive layer 220_1 is disposed such that at least a portion of it is located in the opening 190. Furthermore, as Figure 29B and Figure 29C As shown, the conductive layer 220_1 is preferably provided in a manner that embeds it into the opening 190. Furthermore, the films disposed inside the opening 190 are preferably formed using the ALD method. This results in good film coverage. For example, the conductive layer 115, the insulating layer 130, and the conductive layer 220_1 are all preferably formed using the ALD method.

[0548] The capacitor 100 has a structure in which the upper and lower electrodes are opposed to each other with a dielectric material not only on the bottom surface but also on the side surface within the opening 190, thus increasing the electrostatic capacitance per unit area. Therefore, the deeper the opening 190, the larger the electrostatic capacitance of the capacitor 100 can be. In this way, by increasing the electrostatic capacitance per unit area of ​​the capacitor 100, the read operation of the storage device can be stabilized. Furthermore, it can promote the miniaturization or high integration of storage devices.

[0549] Figure 29B and Figure 29C An example is shown where the sidewalls of the opening 190 are perpendicular to the top surface of the conductive layer 110, and the opening 190 is circular when viewed from a plan view. By employing this structure, miniaturization or high integration of the storage device can be achieved.

[0550] A conductive layer 115 and an insulating layer 130 are stacked along the sidewall of the opening 190 and the top surface of the conductive layer 110. Furthermore, a conductive layer 220_1 is provided on the insulating layer 130 in a manner that is embedded in the opening 190. A capacitor 100 having this structure can be referred to as a trench capacitor or a grooved capacitor.

[0551] The conductive layer 110 is used as the wiring CAL described below, and may be provided in a strip shape, for example. Note that strip shape refers to a shape having a region extending in a certain direction (e.g., the X direction, Y direction, or Z direction).

[0552] As the conductive layer 110, a single layer or a stack of conductive materials described in [Conductor] of Embodiment 2 can be used. As the conductive layer 110, for example, a highly conductive material such as tungsten can be used. By using a highly conductive material, the conductivity of the conductive layer 110 can be improved, thereby enabling the conductive layer 110 to fully perform its function as a wiring CAL.

[0553] As the conductive layer 115, it is preferable to use a conductive material that is not easily oxidized, either as a single layer or in a stack, or a conductive material that has the function of inhibiting oxygen diffusion. For example, titanium nitride or ITSO can also be used. Alternatively, for example, a structure in which titanium nitride is stacked on top of tungsten can also be used. Alternatively, for example, a structure in which first titanium nitride, tungsten, and second titanium nitride are stacked sequentially can also be used. By adopting this structure, oxidation of the conductive layer 115 due to the insulating layer 130 can be suppressed when an oxide is used as the insulating layer 130. Furthermore, oxidation of the conductive layer 115 due to the insulating layer 180 can be suppressed when an oxide is used as the insulating layer 180.

[0554] The insulating layer 130 is provided in contact with the top and side surfaces of the conductive layer 115. That is, the insulating layer 130 preferably covers the side ends of the conductive layer 110. This prevents short circuits between the conductive layer 115 and the conductive layer 220_1.

[0555] Alternatively, the side ends of the insulating layer 130 can be aligned or substantially aligned with the side ends of the conductive layer 115. By employing this structure, the insulating layer 130 and the conductive layer 115 can be formed using the same mask, thereby simplifying the manufacturing process of the storage device.

[0556] High-k material is preferably used for insulating layer 130. By using high-k material for insulating layer 130, the thickness of insulating layer 130 can be increased to a level that can suppress leakage current and sufficiently ensure the electrostatic capacitance of capacitor 100.

[0557] Furthermore, as the insulating layer 130, it is preferable to use an insulator made of a high-k material, and more preferably, a laminated structure of a high-k material and a material with a dielectric strength greater than that of the high-k material is used. For example, as the insulating layer 130, an insulating film in which zirconium oxide, alumina, and zirconium oxide are stacked sequentially can be used. Alternatively, for example, an insulating film in which zirconium oxide, alumina, zirconium oxide, and alumina are stacked sequentially can be used. Furthermore, for example, an insulating film in which hafnium zirconium oxide, alumina, hafnium zirconium oxide, and alumina are stacked sequentially can be used. By using an insulating layer with a high dielectric strength, such as alumina, the dielectric strength can be increased, thereby suppressing electrostatic breakdown of the capacitor 100.

[0558] Furthermore, a ferroelectric material can also be used as the insulating layer 130. For details regarding ferroelectric materials, please refer to the description in Embodiment 2.

[0559] Metal oxides containing one or both of hafnium and zirconium can exhibit ferroelectricity even in thin films of a few nm, and are therefore preferred for use in the insulating layer 130. The thickness of the insulating layer 130 can be 100 nm or less, more preferably 50 nm or less, further preferably 20 nm or less, and even more preferably 10 nm or less (typically, 2 nm or more and 9 nm or less). Furthermore, for example, the thickness is preferably 8 nm or more and 12 nm or less. By using a ferroelectric layer that can be thinned, the capacitor 100 can be combined with miniaturized semiconductor elements such as transistors to form a semiconductor device.

[0560] Furthermore, metal oxides containing one or both of hafnium and zirconium can exhibit ferroelectricity even when their area is extremely small, and are therefore preferred for insulating layer 130. For example, the ferroelectric layer can have an area (occupied area) of 100 μm when viewed from a plane. 2 Below, 10μm 2 Below, 1μm 2 Below or 0.1μm 2 The following can also exhibit ferroelectric properties. Furthermore, sometimes ferroelectric layers can exist even with a planar surface area (occupied area) of 10000 nm.2 Below or 1000nm 2 The following also exhibit ferroelectric properties. By reducing the area of ​​the ferroelectric layer, the occupied area of ​​the capacitor 100 can be reduced.

[0561] Ferroelectric materials are insulators that exhibit the property of becoming internally polarized under the influence of an applied electric field and maintaining this polarization even when the electric field is zero. Therefore, non-volatile storage elements can be formed by using a capacitor (hereinafter sometimes referred to as a ferroelectric capacitor) that uses this material as the dielectric. Non-volatile storage elements using ferroelectric capacitors are sometimes called FeRAM (Ferroelectric Random Access Memory), ferroelectric memory, etc. For example, a ferroelectric memory includes a transistor and a ferroelectric capacitor, with one of the source and drain terminals of the transistor connected to a terminal of the ferroelectric capacitor. Thus, when a ferroelectric capacitor is used as capacitor 100, the storage device shown in this embodiment is used as a ferroelectric memory.

[0562] The conductive layer 220_1 is disposed in contact with a portion of the top surface of the insulating layer 130. Preferably, the side portion of the conductive layer 220_1 is located inside the side portion of the conductive layer 115 in both the X and Y directions. Note that in a structure where the insulating layer 130 covers the side portion of the conductive layer 115, the side portion of the conductive layer 220_1 may also be located outside the side portion of the conductive layer 115.

[0563] Insulating layer 180 is used as an interlayer film, so its relative permittivity is preferably low. By using a material with a low relative permittivity for the interlayer film, parasitic capacitance generated between wirings can be reduced.

[0564] Note that in Figure 29B and Figure 29C The diagram shows the insulating layer 180 as a single layer, but the invention is not limited thereto. The insulating layer 180 may also have a stacked structure of two or more layers.

[0565] Figure 30A This diagram shows an example of a region 101 in which the conductive layer 115 has a corner bend within the recess of the conductive layer 110. Therefore, compared to a case where region 101 has a corner (right angle or acute angle) when viewed in cross-section, electric field concentration on the insulating layer 130 near region 101 can be suppressed. Furthermore, the end 103 of the conductive layer 115 is positioned at a height from the reference plane lower than the top surface of the insulating layer 180. Therefore, compared to a case where the end 103 is located on the insulating layer 180, electric field concentration on the insulating layer 130 near the end 103 can be suppressed. Thus, by suppressing electric field concentration on the insulating layer 130, insulation breakdown of the insulating layer 130 can be suppressed, thereby providing a highly reliable storage device.

[0566] Figure 30B It is shown Figure 30A The diagram shows an example where end 103 is located on insulating layer 180. Figure 30B In the example shown, the region 102 formed by the top surface of the insulating layer 180 and the side surface in the opening 190 has a curved portion. Furthermore, in Figure 30B In the example shown, end 103 has a tapered shape. Because region 102 has a bend and end 103 has a tapered shape, even though end 103 is located on insulating layer 180, electric field concentration on insulating layer 130 near region 102 and end 103 can be suppressed. Therefore, insulation breakdown of insulating layer 130 can be suppressed, and a highly reliable storage device can be provided.

[0567] Figure 30C It is shown in Figure 30B The figure shows an example of an insulating layer 187 disposed on the insulating layer 130, for example, in the region of the insulating layer 130 that overlaps with the insulating layer 180. By providing the insulating layer 187, the electric field concentration on the insulating layer 130 can sometimes be appropriately suppressed.

[0568] In addition, an insulating layer 280 is disposed on the capacitor 100. The insulating layer 280 has a portion located on the insulating layer 130 and a portion located on the conductive layer 220.

[0569] Regarding transistor 200, please refer to embodiment 2 ( Figure 18B The description of transistor 200A shown is omitted here. Furthermore, the transistors included in the memory cell 150 are not limited to transistor 200A; the transistors shown in Embodiment 2 may also be used. Additionally, planar, GAA (Gate All Around), or LGAA (Lateral Gate All Around) transistors may also be used.

[0570] like Figures 29A to 29CAs shown, transistor 200 overlaps with capacitor 100. Furthermore, the groove 291 where a portion of the transistor 200 is disposed has a region overlapping with the opening 190 where a portion of the capacitor 100 is disposed. Specifically, conductive layer 220 is used as one of the source and drain electrodes of transistor 200 and as the upper electrode of capacitor 100, thereby allowing transistor 200 and capacitor 100 to share some constituent elements. By employing this structure, transistor 200 and capacitor 100 can be disposed in a manner that does not significantly increase the occupied area when viewed from a planar perspective. This reduces the occupied area of ​​memory cell 150, allowing for a high-density configuration of memory cells 150 to increase the storage capacity of the memory device. In other words, high integration of the memory device can be achieved. Figure 29B and Figure 29C An example is shown where the width of the opening 190 is smaller than the width of the groove 291. There are no particular limitations on the relationship between the width of the opening 190 and the width of the groove 291. From a miniaturization point of view, the width of the opening 190 is preferably equal to or smaller than the width of the groove 291.

[0571] Furthermore, by placing the transistor 200 above the capacitor 100, the transistor 200 is not affected by the heat treatment during the manufacture of the capacitor 100. Therefore, it is possible to suppress the degradation of the electrical characteristics of the transistor 200, such as threshold voltage fluctuations and increased parasitic resistance, as well as the increase in uneven electrical characteristics caused by such degradation.

[0572] Figures 31A to 31C This illustrates a storage device that uses the transistor 200E described in Embodiment 2, which is included as a storage cell 150. Figure 31A It is a plan view of a storage device including storage unit 150. Figure 31B It is along Figure 31A The cross-sectional view of the dotted line A1-A2 shown. Figure 31C It is along Figure 31A The cross-sectional view shown is the dotted-dash line A3-A4.

[0573] In addition, such as Figure 31B and Figure 31C As shown, the side ends of the insulating layer 130 can also be aligned or substantially aligned with the side ends of the conductive layer 220. By adopting this structure, the insulating layer 130 and the conductive layer 220 can be formed using the same mask, thereby simplifying the manufacturing process of the storage device.

[0574] Figure 37A An example of a circuit diagram of the storage device shown in this embodiment is illustrated. For example... Figure 37A As shown, Figures 29A to 29CThe structure shown is used as a storage cell. Storage cell 951 includes transistor M1 and capacitor CA. Here, transistor M1 corresponds to transistor 200, and capacitor CA corresponds to capacitor 100.

[0575] One of the source and drain terminals of transistor M1 is connected to one of the electrodes of capacitor CA. The other of the source and drain terminals of transistor M1 is connected to wiring BIL. The gate of transistor M1 is connected to wiring WOL. The other of the electrodes of capacitor CA is connected to wiring CAL.

[0576] Here, wiring BIL corresponds to conductive layer 246, wiring WOL corresponds to conductive layer 260, and wiring CAL corresponds to conductive layer 110. For example... Figures 29A to 29C As shown, preferably, conductive layer 260 extends in the X direction and conductive layer 246 extends in the Y direction. By employing this structure, the wiring BIL and wiring WOL intersect each other. Furthermore, in Figure 29C The intermediate wiring CAL (conductive layer 110) is parallel to the wiring WOL (conductive layer 260). However, the invention is not limited to this. For example, the wiring CAL can also be parallel to the wiring BIL (conductive layer 246).

[0577] Note that the storage unit will be described in detail in the following implementation.

[0578] <Example 2 of storage device structure>

[0579] Figure 32A and Figure 32B It is a cross-sectional view of a memory device including transistors 200a and 200b.

[0580] Figure 32A and Figure 32B The storage device shown includes an insulating layer 140 on a substrate (not shown), a storage cell 150 on the insulating layer 140, an insulating layer 280a on the insulating layer 140, and an insulating layer 280b above the insulating layer 280a. The insulating layers 140, 280a, and 280b are used as interlayer films.

[0581] The storage cell 150 includes a transistor 200a on an insulating layer 140 and a transistor 200b on the transistor 200a.

[0582] Regarding transistors 200a and 200b, refer to transistor 200D in embodiment 2 (see [reference]). Figure 26C ) and transistor 200A (refer to Figure 18BThe description of the structure of conductive layer 220a and semiconductor layer 230a is omitted here. For example, regarding the structure of conductive layer 220a and semiconductor layer 230a, the conductive layer 220 is referred to as conductive layer 220a and the semiconductor layer 230 as semiconductor layer 230a, etc., which can be found in [reference needed]. Figure 26C The explanation is as follows. Furthermore, for example, regarding the structure of conductive layer 220b and semiconductor layer 230b, by referring to conductive layer 220 as conductive layer 220b and semiconductor layer 230 as semiconductor layer 230b, etc., please refer to... Figure 18B Explanation.

[0583] Insulating layers 280a and 280b can adopt the same structure as that used for insulating layer 280.

[0584] The transistors included in the storage cell 150 are not limited to a combination of transistors 200a and 200b, and one or more of the transistors shown in Embodiment 2 can be used.

[0585] exist Figure 32A and Figure 32B In the storage cell 150 shown, a capacitor generated between the conductive layer 220b and the conductive layer 240a can be used, thereby allowing data to be retained without forming a separate capacitor.

[0586] The preferred shortest distance from the top surface of conductive layer 240a to conductive layer 220b is the same as the distance from the top surface of conductive layer 246 to the gate wiring. Figure 32A The shortest distance between conductive layer 260 and conductive layer 220b is short. This increases the capacitance generated between conductive layer 220b and conductive layer 240a. Furthermore, it reduces the parasitic capacitance generated between conductive layer 246 and the gate wiring. For example, the structure of transistor 200A described in Embodiment 2 can be used as transistor 200b.

[0587] like Figure 32A and Figure 32B As shown, transistor 200b overlaps with transistor 200a. Furthermore, the groove 291 where a portion of the transistor 200b is disposed has a region that overlaps with the opening 290 where a portion of the transistor 200a is disposed. In particular, since the conductive layer 220b is used as one of the source and drain electrodes of transistor 200b and as the gate electrode of transistor 200a, transistors 200b and 200a share some constituent elements. By adopting this structure, transistors 200b and 200a can be disposed in a manner that does not significantly increase the occupied area when viewed from a planar perspective. Therefore, the occupied area of ​​the memory cell 150 can be reduced, thereby increasing the storage capacity of the memory device by arranging the memory cells 150 at a high density. In other words, high integration of the memory device can be achieved.

[0588] Figure 37E Another example of a circuit diagram showing the storage device illustrated in this embodiment is provided. Figure 37E As shown, Figure 32A and Figure 32B The structure shown is used as a storage cell. Storage cell 955 includes transistor M2 and transistor M3. Here, transistor M2 corresponds to transistor 200b, and transistor M3 corresponds to transistor 200a.

[0589] One of the source and drain of transistor M2 is connected to the gate of transistor M3. The other of the source and drain of transistor M2 is connected to wiring WBL. The gate of transistor M2 is connected to wiring WOL. One of the source and drain of transistor M3 is connected to wiring RBL. The other of the source and drain of transistor M3 is connected to wiring SL.

[0590] Here, wiring WBL corresponds to conductive layer 246, and wiring WOL corresponds to conductive layer 260. For example... Figure 32A and Figure 32B As shown, preferably, conductive layer 260 extends in the X direction and conductive layer 246 extends in the Y direction. With this structure, wiring WBL and wiring WOL intersect each other.

[0591] Furthermore, transistor M2 may also include a back gate. Similarly, transistor M3 may also include a back gate.

[0592] <Example 3 of storage device structure>

[0593] The memory cell 150, including the transistor 200 and capacitor 100 shown in this embodiment, can be used as a memory cell of a memory device. The transistor 200 is an OS transistor. Because the off-state current of the transistor 200 is small, using this transistor in a memory device allows for long-term retention of stored content. In other words, since refresh operations are not required or occur at extremely low frequencies, the power consumption of the memory device can be significantly reduced. Furthermore, because the transistor 200 has high frequency characteristics, high-speed reading and writing to the memory device are possible.

[0594] A storage cell array can be constructed by arranging the storage cells 150 in a three-dimensional and matrix manner.

[0595] Figure 33A This is a floor plan of the storage device. Figure 33A An example is shown where two × two storage cells (storage cells 150a to 150d) are arranged in the X and Y directions.

[0596] Figure 33B It is along Figure 33A The cross-sectional view shown is the dotted-dash line A1-A2. Figure 33A and Figure 33B In the middle, two storage units (in Figure 33B In this configuration, storage cells 150a and 150b are connected to a common wiring (conductive layer 246).

[0597] Figure 37B The circuit diagram corresponding to two memory cells is shown. (Example) Figure 37B As shown, the storage device 952 includes two storage cells. One storage cell includes a transistor M1 and a capacitor CA1, and the other storage cell includes a transistor M2 and a capacitor CA2. For example, when using... Figure 37B and Figure 33B In the corresponding cases, transistor M1 corresponds to transistor 200a, capacitor CA1 corresponds to capacitor 100a, transistor M2 corresponds to transistor 200b, and capacitor CA2 corresponds to capacitor 100b.

[0598] One of the source and drain of transistor M1 is connected to one of the electrodes of capacitor CA1. The other of the source and drain of transistor M1 is connected to wiring BIL. The gate of transistor M1 is connected to wiring WOL1. The other of the electrodes of capacitor CA1 is connected to wiring CAL. One of the source and drain of transistor M2 is connected to one of the electrodes of capacitor CA2. The other of the source and drain of transistor M2 is connected to wiring BIL. The gate of transistor M2 is connected to wiring WOL2. The other of the electrodes of capacitor CA2 is connected to wiring CAL.

[0599] Here, wiring BIL corresponds to conductive layer 246, wiring WOL1 corresponds to conductive layer 260, wiring WOL2 corresponds to another conductive layer 260, and wiring CAL corresponds to conductive layer 110.

[0600] Figure 33A and Figure 33B The memory cells 150a and 150b shown both have the same structure as memory cell 150. Memory cell 150a includes a capacitor 100a and a transistor 200a, and memory cell 150b includes a capacitor 100b and a transistor 200b. Furthermore, Figure 33A The storage cells 150c and 150d shown also have the same structure as storage cell 150. Therefore, in Figure 33A and Figure 33B In the storage device shown, for those having the same Figures 29A to 29C Components with the same function as those in the shown storage device are marked with the same symbols. Furthermore, for details regarding storage cells 150a to 150d, please refer to the description of storage cell 150 in <Example 1 of Storage Device Structure>.

[0601] like Figure 33A and Figure 33B As shown, conductive layers 260 used for wiring WOL are respectively disposed in memory cells 150a and 150b. Furthermore, as... Figure 33A As shown, a conductive layer 260 is provided in a manner shared between memory cells 150a and 150c, and another conductive layer 260 is provided in a manner shared between memory cells 150b and 150d. Furthermore, a conductive layer 246, serving as part of the wiring BIL, is provided in a manner shared between memory cells 150a and 150b. In other words, the conductive layer 246 is connected to the semiconductor layer 230 of memory cells 150a and 150b. Furthermore, another conductive layer 246 is provided in a manner shared between memory cells 150c and 150d.

[0602] Furthermore, memory cells 150a and 150b are axially symmetrical about the perpendicular bisector of the dashed line A1-A2. That is, transistors 200a and 200b are also axially symmetrical about the perpendicular bisector of the dashed line A1-A2. Here, conductive layer 240b serves as one of the source and drain electrodes of transistor 200a and another of the source and drain electrodes of transistor 200b. Moreover, transistors 200a and 200b share conductive layer 240b. By employing the above structure, a memory device capable of miniaturization or high integration can be provided.

[0603] In addition, the conductive layer 110 can be disposed in the memory cell 150a and the memory cell 150b respectively, or it can be disposed together in the memory cell 150a and the memory cell 150b.

[0604] also, Figure 34 This shows n layers (n is an integer greater than or equal to 3) stacked along the Z direction. Figure 33A The example shown is of four storage units. Figure 34 It is along Figure 33A The cross-sectional view of the dotted line A1-A2 shown.

[0605] Figure 34 The storage device shown includes n storage layers 160. Specifically, storage layer 160[1] is provided with storage layer 160[2], and storage layer 160[2] is further provided with (n-2) storage layers, with storage layer 160[n] being the topmost layer. There is no particular limitation on the number of storage cells included in a single storage layer 160, and it may include more than two storage cells.

[0606] The memory cells included in the n-layer memory layer 160 are connected to a readout amplifier (not shown) disposed beneath the n-layer memory layer 160 via conductive layers 245, 247, and 248. Both conductive layers 245 and 248 are disposed within openings formed in insulating layers 140, 180, 130, and 280, and are in contact with the bottom surface of conductive layer 246. Furthermore, conductive layer 247 is disposed within an opening formed in insulating layers 140, 180, 130, and 280, and is in contact with the top surface of conductive layer 246. Conductive materials suitable for conductive layer 240 can be used as conductive layers 245, 247, and 248.

[0607] Conductive layers 245, 246, and 248 are used as plugs or wiring for connecting circuit elements, wiring, electrodes, or terminals such as switches, transistors, capacitors, inductors, resistors, and diodes to the memory cell 150; for connecting two or more memory cells 150; or for connecting... Figure 34 The storage device shown has a plug or wiring located on or below it. For example, a conductive layer 245 may be used with... Figure 34 The structure shown depicts the connection of a read amplifier (not shown) beneath the storage device. In this case, the conductive layer 245 is used as part of the wiring BIL. Thus, by stacking the read amplifier (not shown), storage device, etc., the storage capacity per unit area can be increased.

[0608] In addition, as Figure 34 The storage unit shown can also be used Figure 31B and Figure 31C The capacitor 100 shown has a structure in which the side ends of the insulating layer 130 are aligned with the side ends of the conductive layer 220, preventing the insulating layer 130 from overlapping with the conductive layer 245. Therefore, the processing for forming the opening in the conductive layer 245 is easier. Furthermore, the same effect can be achieved when forming the opening in the conductive layer 247 or conductive layer 248.

[0609] like Figure 34 As shown, by stacking multiple storage cells, the cells can be configured in an integrated manner without increasing the footprint of the storage cell array. In other words, a 3D storage cell array can be constructed.

[0610] Figure 35 An example of a cross-sectional structure of a storage device having a layer containing memory cells stacked on top of a drive circuit including a sense amplifier is shown.

[0611] exist Figure 35In the middle, a storage cell 150 (transistor 200 and capacitor 100) is disposed above transistor 300.

[0612] Transistor 300 is one of the transistors included in the sense amplifier.

[0613] about Figure 35 The storage unit 150 shown can be referred to in the description of storage unit 150 in <Example 1 of the structure of storage device>.

[0614] like Figure 35 As shown, by employing a structure in which the read amplifier is arranged overlapping the memory cell 150, the bit line can be shortened. This reduces the bit line capacitance, thereby enabling high-speed driving of the memory device.

[0615] Figure 35 The storage device shown can correspond to the semiconductor device 900 described in Embodiment 4. Specifically, transistor 300 corresponds to the transistor included in the sense amplifier 927 in semiconductor device 900. Furthermore, storage cell 150 corresponds to storage cell 950.

[0616] Transistor 300 is disposed on substrate 311 and includes a conductive layer 316 serving as a gate, an insulating layer 315 serving as a gate insulating layer, a semiconductor region 313 formed by a portion of substrate 311, and low-resistance regions 314a and 314b serving as source or drain regions. Transistor 300 may be p-channel or n-channel. Substrate 311 preferably comprises silicon-based semiconductors, and more particularly, preferably comprises monocrystalline silicon.

[0617] Alternatively, substrate 311 can also be a structure in which a single-crystal oxide semiconductor film (typically an indium oxide film) is disposed on a stable zirconia substrate. As described in Embodiment 1, the indium oxide film deposited on the stable zirconia substrate contains a single crystal. By using a portion of this indium oxide film as semiconductor region 313, the field-effect mobility of transistor 300 can be improved. Furthermore, the reliability of transistor 300 can be improved.

[0618] Here, in Figure 35In the transistor 300 shown, the semiconductor region 313 (a portion of the substrate 311) forming the channel has a convex shape. Furthermore, a conductive layer 316 is provided such that it covers the sides and top surface of the semiconductor region 313 with an insulating layer 315 in between. The conductive layer 316 can also be made of a material with an adjustable work function. Because of the convex portion of the semiconductor substrate, this transistor 300 is also called a FIN-type transistor. Furthermore, an insulating layer for forming the convex portion can be provided in contact with the upper surface of the convex portion. Although the case where the convex portion is formed by processing a portion of the semiconductor substrate is shown here, a semiconductor film with a convex shape can also be formed by processing an SOI substrate.

[0619] Notice, Figure 35 The structure of transistor 300 shown is only an example and is not limited to the structure described above. Appropriate transistors can be used depending on the circuit structure or driving method.

[0620] Wiring layers, including interlayer films, wiring, and plugs, can also be provided between the various structures. Furthermore, multiple wiring layers can be provided depending on the design. Here, in conductive layers that function as plugs or wiring, the same symbol is sometimes used to represent multiple structures. Furthermore, in this specification, wiring and plugs connecting to wiring can also be considered as a single component. That is, a portion of the conductive layer is sometimes used as wiring, and a portion of the conductive layer is sometimes used as a plug.

[0621] For example, on transistor 300, insulating layers 320, 322, 324, and 326 are sequentially stacked as interlayer films. Furthermore, conductive layers 328 are embedded in insulating layers 320 and 322, and conductive layers 330 are embedded in insulating layers 324 and 326. Additionally, conductive layers 328 and 330 are used as connectors or wiring.

[0622] Furthermore, the insulating layer used as an interlayer film can be used as a planarization film covering the uneven shape underneath. For example, in order to improve the flatness of the top surface of the insulating layer 322, its top surface can also be planarized by a planarization process using CMP or the like.

[0623] Alternatively, a wiring layer can be provided on the insulating layer 326 and the conductive layer 330. For example, in Figure 35 In the middle, insulating layers 350, 352, and 354 are stacked in sequence. Furthermore, a conductive layer 356 is formed in insulating layers 350, 352, and 354. The conductive layer 356 is used as a plug or wiring.

[0624] The insulating layers described above, which can be used in semiconductor devices or storage devices, can be used as insulating layers 352 and 354, which are used as interlayer films.

[0625] As conductive layers used for plugs or wiring, such as conductive layers 328, 330, and 356, conductive materials suitable for conductive layer 240 can be used. High-melting-point materials such as tungsten or molybdenum, which combine heat resistance and conductivity, are preferred; tungsten is particularly preferred. Alternatively, low-resistance conductive materials such as aluminum or copper are preferred. Using low-resistance conductive materials reduces wiring resistance.

[0626] The conductive layer 240 included in transistor 200 is connected to the low-resistance region 314b, which serves as the source or drain region of transistor 300, through conductive layers 643, 642, 644, 645, 646, 356, 330, and 328.

[0627] Conductive layer 643 is embedded in insulating layers 285, 283, 250, and 280. Conductive layer 642 is disposed on insulating layer 130 and embedded in insulating layer 280. Conductive layer 642 can be manufactured using the same materials and processes as conductive layer 220. Conductive layer 644 is embedded in insulating layers 180 and 130. Conductive layer 645 is embedded in insulating layer 180. Conductive layer 645 can be manufactured using the same materials and processes as conductive layer 110. Conductive layer 646 is embedded in insulating layer 648. Transistor 300 and conductive layer 110 are insulated by insulating layer 648.

[0628] This embodiment can be appropriately combined with other embodiments. Furthermore, in this specification, where multiple structural examples are shown in one embodiment, these structural examples can be appropriately combined.

[0629] (Implementation Method 4)

[0630] In this embodiment, a semiconductor device 900 according to one aspect of the present invention is described. The semiconductor device 900 can be used as a storage device.

[0631] Figure 36 This is a block diagram illustrating a structural example of a semiconductor device 900. Figure 36 The semiconductor device 900 shown includes a driving circuit 910 and a memory array 920. The memory array 920 includes one or more memory cells 950. Figure 36 An example of a memory array 920 including multiple memory cells 950 configured in a matrix is ​​shown.

[0632] As storage unit 950, the storage device (storage unit 150, etc.) described in embodiment 3 can be used.

[0633] The drive circuit 910 includes a PSW 931 (power switch), a PSW 932, and peripheral circuit 915. The peripheral circuit 915 includes peripheral circuit 911, a control circuit 912, and a voltage generation circuit 928.

[0634] In the semiconductor device 900, circuits, signals, and voltages can be appropriately selected or omitted as needed. Alternatively, other circuits or signals can be added. Signals BW, CE, GW, CLK, WAKE, ADDR, WDA, PON1, and PON2 are signals input from the outside, while signal RDA is a signal output to the outside. Signal CLK is the clock signal.

[0635] In addition, signals BW, CE, and GW are control signals. Signal CE is the chip enable signal, signal GW is the global write enable signal, and signal BW is the byte write enable signal. Signal ADDR is the address signal. Signal WDA is the write data signal, and signal RDA is the read data signal. Signals PON1 and PON2 are power gating control signals. Alternatively, signals PON1 and PON2 can also be generated in the control circuit 912.

[0636] The control circuit 912 is a logic circuit that controls the overall operation of the semiconductor device 900. For example, the control circuit 912 performs logical operations on signals CE, GW, and BW to determine the operating mode of the semiconductor device 900 (e.g., write operation, read operation). Alternatively, the control circuit 912 generates control signals for the peripheral circuit 911 to execute the aforementioned operating mode.

[0637] The voltage generation circuit 928 has the function of generating a negative voltage. The signal WAKE has the function of controlling the input signal CLK to the voltage generation circuit 928. For example, when a signal of level H is applied as the signal WAKE, the signal CLK is input to the voltage generation circuit 928, and the voltage generation circuit 928 generates a negative voltage.

[0638] The peripheral circuit 911 is used to write and read data from the storage unit 950. The peripheral circuit 911 includes a row decoder 941, a column decoder 942, a row driver 923, a column driver 924, an input circuit 925, an output circuit 926, and a sense amplifier 927.

[0639] Row decoder 941 and column decoder 942 are used to decode the signal ADDR. Row decoder 941 is used to specify the row to be accessed, and column decoder 942 is used to specify the column to be accessed. Row driver 923 is used to select the row specified by row decoder 941. Column driver 924 has the following functions: writing data to memory cell 950; reading data from memory cell 950; and storing the read data.

[0640] Input circuit 925 has the function of holding signal WDA. The data held in input circuit 925 is output to column driver 924. The output data of input circuit 925 is the data written to memory cell 950 (Din). The data read from memory cell 950 by column driver 924 (Dout) is output to output circuit 926. Output circuit 926 has the function of holding Dout. In addition, output circuit 926 has the function of outputting Dout to the outside of semiconductor device 900. The data output from output circuit 926 is signal RDA.

[0641] PSW931 controls the supply of V to the external circuit 915. DD The PSW932 has the function of controlling the supply of V to the line driver 923. HM The function of the semiconductor device 900. Here, the high power supply potential of the semiconductor device 900 is V. DD The low power supply potential is GND (ground potential). Additionally, V HM It is a high power supply potential used to make the word line high, which is higher than V. DD The PSW931 is controlled to turn on / off using signal PON1, and the PSW932 is controlled to turn on / off using signal PON2. Figure 36 In the middle, the peripheral circuit 915 is supplied with V DD The number of power domains can be 1, but it can also be multiple. In this case, a power switch can be set for each power domain.

[0642] Reference Figures 37A to 37G This section describes an example of the structure of a storage cell that can be used in storage cell 950.

[0643] [DOSRAM]

[0644] Figure 37AAn example circuit structure of a DRAM (Dynamic Random Access Memory) type memory cell is shown. In this specification, DRAM using OS transistors is referred to as DOSRAM (Dynamic Oxide Semiconductor Random Access Memory). Memory cell 951 includes transistor M1 and capacitor CA.

[0645] Transistor M1 may also include a front gate (sometimes simply referred to as the gate) and a back gate. In this case, the back gate may also be connected to a wiring supplied with a constant potential or signal, and the front gate and the back gate may also be connected.

[0646] The first terminal of transistor M1 is connected to the first terminal of capacitor CA, the second terminal of transistor M1 is connected to wiring BIL, and the gate of transistor M1 is connected to wiring WOL. The second terminal of capacitor CA is connected to wiring CAL.

[0647] The BIL (Bite Line) is used as the bit line, and the WOL (Word Line) is used as the word line. The CAL (Chip Line) is used to apply a specified potential to the second terminal of the capacitor CA. During data writing and reading, it is preferable to apply a low-level potential (sometimes called a reference potential) to the CAL.

[0648] Data writing and reading are performed by applying a high-level potential to the wiring WOL to turn on the transistor M1, thereby making the wiring BIL and the first terminal of the capacitor CA conductive (allowing current to flow).

[0649] Furthermore, the memory cell that can be used as memory cell 950 is not limited to memory cell 951, and the circuit structure can be changed. For example, memory cell 951 may not include capacitor CA and wiring CAL, and the first terminal of transistor M1 may be in an electrically floating state.

[0650] An OS transistor is preferably used as transistor M1. OS transistors have the characteristic of extremely low off-state current. By using an OS transistor as transistor M1, the leakage current of transistor M1 can be made very small. That is, transistor M1 can hold written data for a longer period, thereby reducing the refresh frequency of the memory cell. Furthermore, the memory cell refresh operation can be omitted. Moreover, because the leakage current is very small, multi-valued data or analog data can be held in memory cell 951.

[0651] In addition, such as Figure 37B As shown, a single wiring block can be set up for two or more DRAM memory cells.

[0652] [NOSRAM]

[0653] Figure 37C An example circuit structure of a gain-cell type memory cell including two transistors and one capacitor is shown. Memory cell 953 includes transistor M2, transistor M3, and capacitor CB. In this specification and the like, a memory device including a gain-cell type memory cell that uses the OS transistor for transistor M2 is referred to as NOSRAM (Nonvolatile Oxide Semiconductor RAM).

[0654] Transistor M2's first terminal is connected to capacitor CB's first terminal; transistor M2's second terminal is connected to wiring WBL; and transistor M2's gate is connected to wiring WOL. Capacitor CB's second terminal is connected to wiring CAL. Transistor M3's first terminal is connected to wiring RBL; transistor M3's second terminal is connected to wiring SL; and transistor M3's gate is connected to capacitor CB's first terminal.

[0655] Wiring WBL is used as the write bit line, wiring RBL as the read bit line, and wiring WOL as the word line. Wiring CAL is used to apply a predetermined potential to the second terminal of capacitor CB. During data writing, data holding, and data reading, it is preferable to apply a low-level potential (sometimes called the reference potential) to wiring CAL.

[0656] Data writing is performed by applying a high-level potential to wiring WOL, which turns on transistor M2 and thus connects wiring WBL to the first terminal of capacitor CB. Specifically, when transistor M2 is on, a potential corresponding to the information to be recorded is applied to wiring WBL to write that potential to the first terminal of capacitor CB and the gate of transistor M3. Then, a low-level potential is applied to wiring WOL, which turns off transistor M2, thereby maintaining the potential of the first terminal of capacitor CB and the potential of the gate of transistor M3.

[0657] Data is read out by applying a predetermined potential to the wiring SL. Since the current flowing between the source and drain of transistor M3 and the potential of the first terminal of transistor M3 are determined by the potential of the gate and the second terminal of transistor M3, the potential held by the first terminal of capacitor CB (or the gate of transistor M3) can be read by reading the potential of the wiring RBL connected to the first terminal of transistor M3. In other words, the information written to the memory cell can be read from the potential held by the first terminal of capacitor CB (or the gate of transistor M3).

[0658] For example, a structure that combines the wiring WBL and wiring RBL into a single wiring BIL can also be adopted. Figure 37D An example of the circuit structure of the memory cell in this case is shown. In memory cell 954, the wiring WBL and wiring RBL of memory cell 953 are combined into a single wiring BIL, and the second terminal of transistor M2 and the first terminal of transistor M3 are connected to the wiring BIL. That is, memory cell 954 operates by combining the write bit line and the read bit line into a single wiring BIL.

[0659] Figure 37E The memory cell 955 shown is an example where the capacitor CB and wiring CAL of memory cell 953 are omitted. Furthermore, Figure 37F The memory cell 956 shown is an example of omitting the capacitor CB and wiring CAL found in memory cell 954. This structure improves the integration density of the memory cells.

[0660] Note that it is preferable to use the OS transistor as at least transistor M2. In particular, it is preferable to use the OS transistor as both transistor M2 and transistor M3. By using the OS transistor as transistor M2, written data can be held for a longer period of time using transistor M2, thereby reducing the refresh frequency of the memory cell. Furthermore, the refresh operation of the memory cell can be omitted. In addition, since the leakage current is very small, multi-value data or analog data can be held in memory cells 953 to 956.

[0661] The memory cells 953 to 956, which use OS transistors as transistor M2, are a form of NOSRAM.

[0662] Si transistors can also be used as transistor M3. Si transistors can improve field-effect mobility and can be p-channel transistors, thus increasing the freedom of circuit design.

[0663] also, Figure 37G A gain-cell type memory cell 957 with three transistors and one capacitor is shown. The memory cell 957 includes transistors M4 to M6 and capacitor CC.

[0664] Transistor M4's first terminal is connected to capacitor CC's first terminal; transistor M4's second terminal is connected to wiring BIL; and transistor M4's gate is connected to wiring WOL. Capacitor CC's second terminal is connected to transistor M5's first terminal and wiring GNDL. Transistor M5's second terminal is connected to transistor M6's first terminal; transistor M5's gate is connected to capacitor CC's first terminal. Transistor M6's second terminal is connected to wiring BIL; and transistor M6's gate is connected to wiring RWL.

[0665] The BIL (Bite Line) is used as the bit line, the WOL (Write Word Line) is used as the write word line, and the RWL (Read Word Line) is used as the read word line. The GNDL (Ground Node Line) is used to supply a low-level potential.

[0666] Data writing is performed by applying a high-level potential to wiring WOL, which turns on transistor M4 and connects wiring BIL to the first terminal of capacitor CC. Specifically, when transistor M4 is on, a potential corresponding to the information to be recorded is applied to wiring BIL to write that potential to the first terminal of capacitor CC and the gate of transistor M5. Then, a low-level potential is applied to wiring WOL, which turns off transistor M4, thereby maintaining the potential of the first terminal of capacitor CC and the potential of the gate of transistor M5.

[0667] Data readout is performed by pre-charging the wiring BIL to a predetermined potential, then making the wiring BIL electrically floating and applying a high-level potential to the wiring RWL. By making the wiring RWL high, transistor M6 is turned on, and the wiring BIL and the second terminal of transistor M5 are connected. At this time, the potential of the wiring BIL is applied to the second terminal of transistor M5, but the potential of the second terminal of transistor M5 and the potential of the wiring BIL will change correspondingly to the potential held by the first terminal of capacitor CC (or the gate of transistor M5). Here, the potential held by the first terminal of capacitor CC (or the gate of transistor M5) can be read by reading the potential of the wiring BIL. In other words, the information written to the memory cell can be read from the potential held by the first terminal of capacitor CC (or the gate of transistor M5).

[0668] Note that it is preferable to use the OS transistor as at least transistor M4.

[0669] Si transistors can also be used as transistors M5 and M6. As mentioned above, the field-effect mobility of Si transistors is sometimes higher than that of OS transistors, depending on factors such as the crystallization state of the silicon used in the semiconductor layer.

[0670] The driving circuitry 910 and memory array 920 included in the semiconductor device 900 can also be disposed on the same plane. Furthermore, as... Figure 38A As shown, the driving circuit 910 and the memory array 920 can also overlap. By overlapping the driving circuit 910 and the memory array 920, the signal transmission distance can be shortened. Figure 38B As shown, multiple memory arrays 920 can also be stacked on the drive circuit 910.

[0671] Next, an example of an arithmetic processing device that may include the aforementioned storage device or other semiconductor device will be described.

[0672] Figure 39This is a block diagram of the arithmetic unit 960. Figure 39 The computing device 960 shown can be used, for example, as a CPU. Furthermore, the computing device 960 can also be used with processors such as GPUs (Graphics Processing Units), TPUs (Tensor Processing Units), and NPUs (Neural Processing Units), which have more (tens to hundreds) processor cores than a CPU capable of parallel processing.

[0673] Figure 39 The illustrated arithmetic unit 960 includes, on substrate 961: an ALU 962 (ALU: Arithmetic Logic Unit), an ALU controller 962c, an instruction decoder 963, an interrupt controller 964, a timing controller 965, a register 966, a register controller 967, a bus interface 968, a cache 969, and a cache interface 969i. The substrate 961 can be a semiconductor substrate, an SOI substrate, a glass substrate, etc. It may also include a rewritable ROM and a ROM interface. The cache 969 and the cache interface 969i can also be located on different chips.

[0674] The cache 969 is connected to the main memory located on different chips via the cache interface 969i. The cache interface 969i has the function of supplying a portion of the data stored in the main memory to the cache 969. In addition, the cache interface 969i has the function of outputting a portion of the data held in the cache 969 to the ALU 962 or register 966, etc., via the bus interface 968.

[0675] As described later, the memory array 920 can be arranged in a manner that stacks on the computing device 960. The memory array 920 can be used as a cache. In this case, the cache interface 969i can have the function of supplying data held in the memory array 920 to the cache 969. Furthermore, in this case, it is preferable that a portion of the cache interface 969i includes a drive circuit 910.

[0676] Note that you can also omit cache 969 and use only memory array 920 as a cache.

[0677] Figure 39 The arithmetic device 960 shown is merely an example with a simplified structure; therefore, the actual arithmetic device 960 has various structures depending on its application. For example, it is preferable to include... Figure 39The computing device 960 shown has a multi-core structure, which consists of a single core and multiple cores that operate simultaneously. The more cores, the better the computing performance. More cores are preferred; for example, two cores are preferred, four cores are more preferred, eight cores are even more preferred, twelve cores are still more preferred, and sixteen cores or more are even more preferred. Furthermore, when used in servers or other applications requiring very high computing performance, a multi-core structure with 16 or more cores is preferred, more preferably 32 or more cores, and more preferably 64 or more cores. Additionally, the number of bits that can be processed in the internal computing circuitry, data bus, etc., of the computing device 960 can be, for example, 8 bits, 16 bits, 32 bits, 64 bits, etc.

[0678] Instructions input to the arithmetic unit 960 via the bus interface 968 are input to the instruction decoder 963 and, after being decoded, are input to the ALU controller 962c, interrupt controller 964, register controller 967, and timing controller 965.

[0679] The ALU controller 962c, interrupt controller 964, register controller 967, and timing controller 965 perform various controls based on the decoded instructions. Specifically, the ALU controller 962c generates signals to control the operation of the ALU 962. Furthermore, when executing the program of the arithmetic unit 960, the interrupt controller 964 determines and processes interrupt requests from external input / output devices, peripheral circuits, etc., based on their priority, mask state, etc. The register controller 967 generates the address of register 966 and reads and writes register 966 according to the state of the arithmetic unit 960.

[0680] Furthermore, the timing controller 965 generates signals to control the operating timing of the ALU 962, ALU controller 962c, instruction decoder 963, interrupt controller 964, and register controller 967. For example, the timing controller 965 includes an internal clock generator that generates an internal clock signal base...

Claims

1. A method for manufacturing a metal oxide layer, comprising the following steps: The first step in forming the crystalline part; The second step of forming a metal oxide layer with an amorphous structure on the crystalline portion; and The third step involves heat treatment to allow the metal oxide layer to crystallize and grow using the crystallized portion as a nucleus. wherein The metal oxide layer contains indium.

2. The method for manufacturing a metal oxide layer according to claim 1, In the first step, the crystalline portion is formed on the layer with the groove. In the second step, the metal oxide layer is formed in a manner that covers the trench portion. Furthermore, in the third step, the metal oxide layer is crystallized and grown along the groove.

3. A method for manufacturing a metal oxide layer, comprising the following steps: The first step in forming the crystalline part; and The second step involves forming a single-crystal metal oxide layer on the crystallized portion using the crystallized portion as a seed crystal. wherein The metal oxide layer contains indium. In the first step, a groove is formed and the crystalline portion is formed on a layer with a curved surface at the upper end of the groove. Furthermore, in the second step, the metal oxide layer is formed in a manner that covers the groove portion.

4. A method for manufacturing a metal oxide layer, comprising the following steps: The first step in forming the crystalline part; The second step of forming a metal oxide layer with an amorphous structure on the crystalline portion; and The third step involves heat treatment to allow the metal oxide layer to crystallize and grow using the crystallized portion as a nucleus. wherein The metal oxide layer contains indium. In the first step, a groove is formed and the crystalline portion is formed on a layer with a curved surface at the upper end of the groove. In the second step, the metal oxide layer is formed in a manner that covers the trench portion. Furthermore, in the third step, the metal oxide layer is crystallized and grown along the groove.

5. The method for manufacturing a metal oxide layer according to claim 3, In the second step, the metal oxide layer is formed under conditions where the substrate temperature is above 100°C and below 300°C.

6. The method for manufacturing a metal oxide layer according to claim 3, In the second step, the metal oxide layer is formed under conditions where the substrate temperature is above 150°C and below 250°C.

7. The method for manufacturing a metal oxide layer according to claim 3 or 4, The surface described therein has a portion with a radius of curvature of more than 1 nm and less than 500 nm.

8. The method for manufacturing a metal oxide layer according to claim 3 or 4, The curved surface has a portion whose radius of curvature is greater than the thickness of the metal oxide layer.

9. The method for manufacturing a metal oxide layer according to claim 3 or 4, The layer contains an insulating material.

10. The method for manufacturing a metal oxide layer according to claim 3 or 4, The layer contains a conductive material.

11. The method for manufacturing a metal oxide layer according to claim 3 or 4, The layer therein has a curved surface at the bottom of the groove.

12. The method for manufacturing a metal oxide layer according to any one of claims 1, 3, and 4, The metal oxide layer is formed using a sputtering method. Furthermore, a hydrogen-containing gas is used as the sputtering gas.

13. The method for manufacturing a metal oxide layer according to claim 1 or 4, The heat treatment involves performing a first heat treatment and a second heat treatment sequentially. Furthermore, the temperature of the second heating treatment is higher than the temperature of the first heating treatment.

14. The method for manufacturing a metal oxide layer according to claim 13, The first heating treatment is carried out in an atmosphere containing hydrogen and nitrogen.

15. The method for manufacturing a metal oxide layer according to claim 13, The hydrogen concentration in the metal oxide layer is reduced by performing the second heat treatment.

16. The method for manufacturing a metal oxide layer according to claim 1 or 4, The metal oxide layer after the heat treatment contains grains in the portion overlapping with the crystalline portion.

17. The method for manufacturing a metal oxide layer according to claim 16, The crystal orientation of the grains is <111> .

18. The method for manufacturing a metal oxide layer according to claim 17, The crystal orientation of the crystalline portion is as follows: <001> .

19. The method for manufacturing a metal oxide layer according to claim 18, The crystalline portion contains indium, gallium, and zinc. Furthermore, the composition of the crystallized portion is In:Ga:Zn=1:1:1 [atomic ratio] or near that, or In:Ga:Zn=1:3:2 [atomic ratio] or near that.

20. The method for manufacturing a metal oxide layer according to claim 16, The crystalline portion contains indium oxide.

Citation Information

Patent Citations

  • Semiconductor device

    JP2011151383A

  • Semiconductor integrated circuit

    JP2012257187A