Packaging material for molding, packaging case, and power storage device
By using a multi-layer structure and specific reinforced particles in lithium-ion battery packaging materials, the problem of insufficient puncture strength of lithium-ion battery packaging materials during molding processing is solved, achieving high puncture strength and improving molding processability, ensuring the battery's durability Security and Capacity.
Patent Information
- Application Number
- CN202322847885.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Priority Date
- 2023-09-07
- Filing Date
- 2023-10-23
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2033-10-23
AI Technical Summary
Existing lithium-ion battery packaging materials are prone to pinholes during the molding process, resulting in reduced puncture strength, making it difficult to balance the battery's large capacity and safety requirements.
A packaging material composed of a metal foil layer, a heat-resistant resin layer, a heat-fusible resin layer, an inner adhesive layer, and an outer adhesive layer. The inner adhesive layer contains inner reinforcement particles that meet specific requirements, and the outer adhesive layer contains inner reinforcement particles that meet specific requirements. The adhesive layer contains outer reinforcing particles, which improve the puncture strength by adjusting the coating amount and layer structure.
It significantly improves the puncture strength and molding processability of packaging materials, enhances the durability against external forces and impacts, and ensures the safety and capacity of the battery.
Smart Images

Figure CN221794043U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to a packaging material for molding, a packaging shell and an electric storage device. It should be noted that the packaging material can be used as a packaging material for non-fixed (laptop computers, mobile phones, car-mounted, etc.) and fixed electric storage devices (lithium ion batteries, etc.), and can also be used as a packaging material for food and medicine.
[0002] Here, in the present specification and claims, for convenience of explanation, the reinforcing agent and reinforcing particles contained in the inner adhesive layer are referred to as inner reinforcing agent and inner reinforcing particles, and the reinforcing agent and reinforcing particles contained in the outer adhesive layer are referred to as outer reinforcing agent and outer reinforcing particles.
[0003] In addition, in the present specification and claims, unless otherwise clearly indicated herein, various physical property values (specific surface area, tensile strength at break, tensile elongation at break, etc.) are values at room temperature. Background Art
[0004] Among various power storage devices, for example, lithium-ion batteries used in mobile devices (e.g., smartphones, tablet computers, and laptop computers), the battery body is packaged with a packaging material. As the packaging material, for example, a packaging material formed of a metal-resin laminated material in which a resin film is laminated on the inner surface and the outer surface of a metal foil is used. For the packaging material, in order to form a space for accommodating the battery body, a predetermined forming process such as a drawing process (e.g., a deep drawing process, a stretching process) can be performed.
[0005] Such batteries are generally required to be thinner and lighter. If the metal foil and resin films are thinned in the packaging material to meet this requirement, the probability of pinholes being generated during the molding of the packaging material becomes higher. On the other hand, if the molding depth is shallower to suppress the generation of pinholes, it becomes difficult to cope with the increase in battery capacity. In addition, if the resin film is thinned, the puncture strength of the packaging material is reduced, and the battery is easily broken due to external impact.
[0006] The packaging materials used for non-stationary (mobile, portable, etc.) power storage devices, such as the lithium-ion batteries for mobile devices, are more likely to be damaged by external forces such as impact, vibration, and external pressure than those used for stationary power storage devices. Therefore, packaging materials formed of metal-resin laminates are also required to have mechanical strength that can withstand external forces, especially excellent puncture resistance.
[0007] In order to improve the puncture strength of packaging materials, Patent Document 1 discloses the use of biaxially stretched polyester or biaxially stretched polyamide films as the outer layer of packaging materials. In addition, Patent Document 2 discloses the use of a heat-fusible resin film formed by laminating and integrating covering layers containing random copolymer polypropylene on the inner and outer surfaces of an intermediate layer containing block copolymer polypropylene as the inner layer of packaging materials. In addition, as a document that discloses improving the puncture strength of packaging materials, there is, for example, Patent Document 3.
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2022-50325 (paragraph
[0022] , etc.)
[0010] Patent Document 2: Japanese Patent Application Publication No. 2015-143107 (paragraph
[0028] , etc.)
[0011] Patent Document 3: Japanese Patent Application Publication No. 2020-161326 Utility Model Content
[0012] Issues to be Solved by Utility Models
[0013] In recent years, as the capacity of power storage devices such as lithium-ion batteries has increased, the safety of power storage devices has become increasingly important, and packaging materials are being required to have higher puncture strength.
[0014] The present invention is made in view of the above technical background, and the purpose of the present invention is to provide a packaging material and a packaging shell for molding with high puncture strength, and a storage device using the packaging material. Other purposes and advantages of the present invention can be confirmed from the following preferred embodiments.
[0015] Means for solving problems
[0016] The utility model provides the following means.
[0017] 1) A packaging material for molding, comprising a metal foil layer, a heat-resistant resin layer disposed on the outer surface side of the metal foil layer, and a heat-fusible resin layer disposed on the inner surface side of the metal foil layer, an outer adhesive layer being disposed between the metal foil layer and the heat-resistant resin layer, and an inner adhesive layer being disposed between the metal foil layer and the heat-fusible resin layer,
[0018] The inner adhesive layer contains an inner reinforcing agent.
[0019] As the inner reinforcing agent, inner reinforcing particles satisfying the following requirements 1 and 2 were used.
[0020] Requirement 1: The number average particle size of the inner reinforcing particles is within a range of 0.01 μm to 3 μm.
[0021] Requirement 2: The specific surface area of the inner reinforcing particles is 1 m 2 / g or above.
[0022] 2) The molding packaging material as described in the above item 1, wherein the inner adhesive layer is formed of a cured film of an inner adhesive composition containing an inner adhesive and the inner reinforcing agent,
[0023] The tensile elongation at break of the cured film of the inner adhesive composition is defined as L1.
[0024] When the tensile elongation at break of a cured film of an inside adhesive composition containing the inside adhesive but not containing the inside reinforcing agent is defined as L10,
[0025] The aforementioned L1 satisfies the following Relationship 1.
[0026] 15%≤{(L1-L10) / L10}×100%≤250%…(Formula 1).
[0027] 3) The molding packaging material as described in item 1 or 2 above, wherein the inner adhesive layer has a thickness of 2 g / m 2 ~10g / m 2 The coating amount in the range of is provided between the metal foil layer and the heat-fusible resin layer,
[0028] The content of the inner reinforcing agent in the inner adhesive layer is 0.2 g / m 2 ~1.0g / m 2 within the range.
[0029] 4) The molding packaging material according to any one of the above 1 to 3, wherein the outer adhesive layer contains an outer reinforcing agent.
[0030] As the outer reinforcing agent, outer reinforcing particles satisfying the following requirements 3 and 4 were used.
[0031] Requirement 3: The number average particle size of the outer reinforcing particles is within a range of 0.01 μm to 3 μm.
[0032] Requirement 4: The specific surface area of the outer reinforcing particles is 1 m 2 / g or above.
[0033] 5) The molding packaging material as described in the above item 4, wherein the outer adhesive layer is formed of a cured film of an outer adhesive composition containing an outer adhesive and the outer reinforcing agent,
[0034] The tensile elongation at break of the cured film of the outer adhesive composition is defined as L2.
[0035] When the tensile elongation at break of a cured film of an external adhesive composition containing the external adhesive but not containing the external reinforcing agent is defined as L20,
[0036] The aforementioned L2 satisfies the following Relationship 2.
[0037] 15%≤{(L2-L20) / L20}×100%≤250%…(Formula 2).
[0038] 6) A packaging case, which is formed by deep drawing or stretching the packaging material for molding as described in any one of 1 to 5 above.
[0039] 7) An electric storage device comprising an electric storage device body and a packaging case packaging the electric storage device body,
[0040] As the package case, there is provided the package case described in the above Item 6.
[0041] Utility Model Effect
[0042] The utility model achieves the following effects.
[0043] In the above item 1, the inner reinforcing particles satisfy the above requirement 1, thereby the fracture path in the inner adhesive layer becomes longer, and the fracture strength (tensile fracture strength, etc.) and elongation at break (tensile fracture elongation, etc.) of the inner adhesive layer are improved. In addition, the inner reinforcing particles satisfy the above requirement 2, thereby the interaction between the inner reinforcing particles and the inner adhesive molecules becomes stronger, and the fracture strength of the inner adhesive layer is further improved. Therefore, the puncture strength of the packaging material can be improved.
[0044] In the above Item 2, the tensile elongation at break L1 of the cured film of the inner adhesive composition satisfies the above Relationship 1, whereby the inner adhesive layer in the packaging material has high followability to the deformation of the metal foil layer, thereby reliably improving the puncture strength of the packaging material.
[0045] In the above item 3, the inner adhesive layer is 2g / m 2 ~10g / m 2 The coating amount in the range of is set between the heat-resistant resin layer and the metal foil layer, and the content of the inner reinforcing agent in the inner adhesive layer is 0.2 g / m 2 ~1.0g / m 2 In the range of , the breaking strength and breaking elongation of the inner adhesive layer are reliably improved. Therefore, the puncture strength of the packaging material can be reliably improved.
[0046] In the above item 4, the outer reinforcing particles satisfy the above requirement 3, thereby the fracture path in the outer adhesive layer becomes longer, and the fracture strength (tensile fracture strength, etc.) and elongation at break (tensile fracture elongation, etc.) of the outer adhesive layer are improved. In addition, the outer reinforcing particles satisfy the above requirement 4, thereby the interaction between the outer reinforcing particles and the outer adhesive molecules becomes stronger, and the fracture strength of the outer adhesive layer is further improved. Therefore, the puncture strength of the packaging material can be further improved.
[0047] In the above Item 5, the tensile elongation at break L2 of the cured film of the outer adhesive composition satisfies the above Relationship 2, whereby the outer adhesive layer in the packaging material has high followability to the deformation of the metal foil layer, thereby reliably improving the puncture strength of the packaging material.
[0048] In the aforementioned item 6, a package casing having high puncture strength can be provided.
[0049] In the aforementioned item 7, the power storage device includes the package case described in the aforementioned item 6, and therefore has high durability against external forces such as impact, vibration, and external pressure. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 This is a schematic cross-sectional view of a molding packaging material according to a first embodiment of the present invention.
[0051] Figure 2 This is a schematic cross-sectional view of a molding packaging material according to a second embodiment of the present invention.
[0052] Figure 3 This is a schematic cross-sectional view of a molding packaging material according to a third embodiment of the present invention.
[0053] Figure 4 This is a schematic cross-sectional view of a molding packaging material according to a fourth embodiment of the present invention.
[0054] Figure 5 This is a schematic cross-sectional view of a molding packaging material according to a fifth embodiment of the present invention.
[0055] Figure 6 This is a schematic cross-sectional view of a power storage device according to one embodiment of the present invention.
[0056] Figure 7 It is a schematic perspective view showing the power storage device in an exploded state.
[0057] Description of Reference Numerals
[0058] 1A~1E: Packaging materials
[0059] 2: Metal foil layer
[0060] 3: Heat-resistant resin layer
[0061] 4: Thermally fusible resin layer
[0062] 5.5R: Outer adhesive layer
[0063] 6R: Inner adhesive layer
[0064] 7: Matt coating
[0065] 8: Black coloring layer
[0066] 30: Lithium-ion battery (power storage device)
[0067] 31: Lithium-ion battery main body (power storage device main body) DETAILED DESCRIPTION
[0068] Some embodiments of the present invention are described below with reference to the accompanying drawings.
[0069] like Figure 1 As shown in FIG. 1 , a molding packaging material 1A according to a first embodiment of the present invention includes an inner surface 1 a and an outer surface 1 b .
[0070] The packaging material 1A is basically formed of a laminated body including a metal foil layer 2, a heat-resistant resin layer 3 disposed on the outer surface side of the metal foil layer 2, and a heat-fusible resin layer 4 disposed on the inner surface side of the metal foil layer 2 in a laminated state, an outer adhesive layer 5 is provided between the metal foil layer 2 and the heat-resistant resin layer 3, and an inner adhesive layer 6R is provided between the metal foil layer 2 and the heat-fusible resin layer 4. These layers are joined (bonded) and integrated in a laminated state.
[0071] The heat-fusible resin layer 4 is disposed on the inner surface 1a of the packaging material 1A, and thus the inner surface 1a of the packaging material 1A is formed by the inner surface of the heat-fusible resin layer 4. The heat-resistant resin layer 3 is also called the base material layer of the packaging material 1A, and is disposed on the outer surface 1b side of the metal foil layer 2 of the packaging material 1A.
[0072] A chemical conversion film 2a for improving the corrosion resistance of the metal foil layer 2 is formed on at least one of the inner surface and the outer surface of the metal foil layer 2. In the first embodiment, the chemical conversion films 2a and 2a are respectively formed on the inner surface and the outer surface of the metal foil layer 2. Each chemical conversion film 2a is formed by subjecting the surface of the metal foil to a chemical conversion treatment.
[0073] The packaging material 1A may be Figure 6 and 7 The packaging shown is used for a power storage device such as a battery device. Specifically, the power storage device is a lithium ion battery 30, for example.
[0074] like Figure 7 As shown, a lithium-ion battery 30 as an electric storage device includes a lithium-ion battery body 31 as the main body of the electric storage device, and a package case 20 that accommodates the battery body 31 in a state of surrounding the battery body 31. The package case 20 includes a container-shaped package case body 21 opened at the top, and a flat plate-shaped cover body 22 that closes the opening of the package case body 21 as components of the package case 20.
[0075] The package case body 21 is formed by deep drawing or stretching the packaging material 1A into a container shape with its inner surface 1a facing inward. That is, the package case body 21 is formed of a deep drawing or stretching product of the packaging material 1A.
[0076] A recess 21b for housing the battery body 31 is provided at the center of the inner surface 1a of the package case body 21. A flange 21a protruding outward is provided at the upper end of a side wall 21c disposed on the outer periphery of the package case body 21 as a predetermined joining portion.
[0077] The cover body 22 is a cover body obtained by using the packaging material 1A in a flat state without being subjected to molding. The outer peripheral portion 22 a of the cover body 22 is a predetermined joining portion of the cover body 22 .
[0078] In the battery 30, the battery body 31 is accommodated and arranged in the recess 21b of the package case body 21, and the cover body 22 is arranged on the package case body 21 in such a manner that the inner surface 1a thereof faces the battery body 31 side (lower side), and the heat-fusible resin layer 4 of the flange portion 21a of the package case body 21 and the heat-fusible resin layer 4 of the outer peripheral portion 22a of the cover body 22 are heat-fused (joined) in a sealed state by heat sealing, thereby forming a structure as shown in FIG. Figure 6 As shown, the battery 30 is in a state where the battery main body 31 is accommodated in the package case 20 .
[0079] It should be noted that Figure 6 The reference numeral “ 23 ” in FIG. 2 denotes a heat-sealed portion (heat-welded portion) between the heat-weldable resin layer 4 of the flange portion 21 a of the package case body 21 and the heat-weldable resin layer 4 of the outer peripheral portion 22 a of the lid 22 .
[0080] The tab (not shown) connected to the battery body 31 is usually led out from the battery body 31 to the outside of the package case 20 through the heat-sealed portion 23 .
[0081] Next, the structure of the packaging material 1A and the method for producing the packaging material 1A according to the first embodiment will be described in detail below.
[0082] (Heat-resistant resin layer)
[0083] The heat-resistant resin layer 3 is formed of, for example, a heat-resistant resin film. The type of the heat-resistant resin layer (heat-resistant resin film) 3 is not limited. As the heat-resistant resin layer 3, polyamide film, polyester film, etc. can be used, and their stretched films are preferably used. Among them, as the heat-resistant resin layer 3, from the aspects of excellent molding processability and strength, biaxially stretched polyamide film, biaxially stretched polybutylene terephthalate (PBT) film, biaxially stretched polyethylene terephthalate (PET) film or biaxially stretched polyethylene naphthalate (PEN) film is preferably used.
[0084] In addition, biaxially stretched polyamide films are particularly preferably used as the heat-resistant resin layer 3 in view of excellent puncture strength and molding processability. The type of polyamide film is not limited, and examples of the polyamide film include nylon 6 film, nylon 6,6 film, nylon MXD film, and the like.
[0085] The thickness of the heat-resistant resin layer 3 is not limited, but is preferably in the range of 9 μm to 50 μm. When a polyester film is used as the heat-resistant resin layer 3, the thickness is preferably in the range of 9 μm to 50 μm, and when a polyamide film is used, the thickness is preferably in the range of 10 μm to 50 μm. By making the thickness greater than the lower limit of the above-mentioned preferred range, it is possible to reliably ensure strength sufficient for the packaging material 1A, and by making the thickness less than the upper limit of the above-mentioned preferred range, it is possible to reliably reduce the processing stress acting on the packaging material 1A during deep drawing and stretching, and it is possible to reliably improve the formability of the packaging material 1A.
[0086] (Thermal Fusible Resin Layer)
[0087] The heat-fusible resin layer 4 is a layer that plays the role of providing the packaging material 1A with excellent chemical resistance to highly corrosive electrolytes used in the power storage device 30 such as lithium ion batteries and imparting heat sealability to the packaging material 1A.
[0088] The heat-fusible resin layer 4 is formed of, for example, a heat-fusible resin film. The type of the heat-fusible resin layer (heat-fusible resin film) 4 is not limited, and as the heat-fusible resin layer 4, a heat-fusible resin unstretched film can be preferably used. As the heat-fusible resin unstretched film, from the perspective of excellent chemical resistance and heat sealing properties, it is preferred to use an unstretched film formed of at least one heat-fusible resin selected from the group consisting of polyethylene, polypropylene, olefin copolymers, their acid-modified products, and ionomers. In particular, from the perspective of excellent puncture strength, it is preferred to use a three-layer co-extruded polypropylene film in which a coating layer containing a random copolymer polypropylene is laminated and integrated on both sides of an intermediate layer containing a block copolymer polypropylene. It should be noted that the layer thickness ratio of the unstretched three-layer co-extruded polypropylene film is not limited, and is preferably in the range of ethylene-propylene random copolymer (rPP): ethylene-propylene block copolymer (bPP): ethylene-propylene random copolymer (rPP) = 1 to 1.5: 7 to 8: 1 to 1.5.
[0089] The thickness of the heat-fusible resin layer 4 is not limited, but is preferably in the range of 20 μm to 80 μm. By making the thickness 20 μm or more, the generation of pinholes in the molded product can be reliably suppressed. By making the thickness 80 μm or less, the amount of resin used can be reliably reduced, and the manufacturing cost of the packaging material 1A can be reliably reduced. Among them, the thickness of the heat-fusible resin layer 4 is particularly preferably in the range of 30 μm to 50 μm.
[0090] (Metal foil layer)
[0091] The metal foil layer 2 is a layer that plays a role in providing the packaging material 1A with gas barrier properties for suppressing the intrusion of oxygen and moisture.
[0092] The metal foil layer 2 is formed of, for example, a metal foil. The type of the metal foil layer 2 is not limited, and aluminum foil, copper foil, stainless steel foil, etc. can be used as the metal foil layer 2, and aluminum foil is usually used. As the aluminum foil, an Al-Fe alloy foil containing 0.7 mass % to 1.7 mass % of Fe in particular has excellent strength and ductility, and can obtain good molding processability.
[0093] The thickness of the metal foil layer 2 is not limited, and can preferably be in the range of 20 μm to 100 μm. By making the thickness 20 μm or more, the generation of pinholes can be reliably suppressed during rolling when manufacturing the metal foil. By making the thickness 100 μm or less, the processing stress acting on the packaging material 1A during deep drawing and stretching can be reliably reduced, and the formability of the packaging material 1A can be reliably improved.
[0094] (Chemical conversion coating of metal foil layer)
[0095] The chemical conversion film 2a is a film (layer) for improving the corrosion resistance of the metal foil layer 2, and can be formed, for example, by subjecting the surface of the metal foil constituting the metal foil layer 2 to a chromate treatment or a non-chromium type chemical conversion treatment using a zirconium compound or the like. For example, in the case of a chromate treatment, an aqueous solution of any one of the following mixtures 1) to 3) is applied to the surface of the metal foil subjected to a degreasing treatment and then dried.
[0096] 1) A mixture of phosphoric acid, chromic acid, and at least one of a metal salt of fluoride and a non-metal salt of fluoride
[0097] 2) A mixture of any one of an acrylic resin, a chitosan derivative resin and a phenolic resin, at least one of chromic acid and a chromium (III) salt, and phosphoric acid
[0098] 3) A mixture of any one of an acrylic resin, a chitosan derivative resin and a phenolic resin, at least one of chromic acid and a chromium (III) salt, at least one of a metal salt of fluoride and a non-metal salt of fluoride, and phosphoric acid.
[0099] The amount of chromium deposited in the chemical conversion film 2a is not limited, but is preferably 0.1 mg / m2 on one side of the metal foil. 2 ~50 mg / m 2 The range is particularly preferably 2 mg / m 2 ~20 mg / m 2 The thickness of the chemical conversion film 2a is not limited, but is preferably in the range of 0.001 μm to 0.1 μm. Due to the chemical conversion film 2a having such a chromium deposition amount or thickness, the corrosion resistance of the metal foil layer 2 can be reliably improved.
[0100] In the first embodiment, the chemical conversion film 2a is formed on the inner surface and the outer surface of the metal foil layer 2 as described above. However, in the present invention, the chemical conversion film 2a may be formed on only one of the inner surface and the outer surface of the metal foil layer 2.
[0101] (Outer adhesive layer)
[0102] The outer adhesive layer 5 is a layer responsible for the bonding between the metal foil layer 2 and the layer arranged on the outer surface side of the metal foil layer 2. In the first embodiment, it is a layer responsible for the bonding between the metal foil layer 2 (specifically, the outer surface chemical conversion film 2a of the metal foil layer 2) and the heat-resistant resin layer 3.
[0103] The outer adhesive layer 5 is formed of a cured film of an outer adhesive composition containing an outer adhesive. In the first embodiment, the outer adhesive composition does not contain an outer reinforcing agent.
[0104] Hereinafter, in order to distinguish the outer adhesive composition containing the outer adhesive and the outer reinforcing agent from the outer adhesive composition containing the outer adhesive but not containing the outer reinforcing agent as described above, the former is also referred to as "the outer adhesive composition containing the outer reinforcing agent", and the latter is referred to as "the outer adhesive composition not containing the outer reinforcing agent". Therefore, in the first embodiment, the outer adhesive layer 5 is formed of a cured film of the outer adhesive composition not containing the outer reinforcing agent.
[0105] The type of the external adhesive is not limited, and as the external adhesive, polyurethane adhesives, acrylic adhesives, polyacrylate adhesives, modified polypropylene adhesives, polyester adhesives, polyamide adhesives, epoxy adhesives, etc. can be used.
[0106] In addition, the outer adhesive is preferably an adhesive that can be used as an adhesive for dry lamination (for example, a urethane adhesive, an olefin adhesive). Specifically, as such an outer adhesive, for example, an adhesive containing a two-component curing polyester urethane resin formed of a polyester resin as a main agent of the outer adhesive and a polyfunctional isocyanate compound as a curing agent can be used.
[0107] Polyester resin is a copolymer made of dicarboxylic acid and diol as raw materials, and preferred materials and compositions are as follows.
[0108] As dicarboxylic acids, both aliphatic dicarboxylic acids and aromatic dicarboxylic acids are preferably used. In addition, the odd or even number of methylene groups in the methylene chain of aliphatic dicarboxylic acids is a factor that affects the crystallinity of the resin. Dicarboxylic acids with an even number of methylene groups produce highly crystalline and hard resins. Therefore, as dicarboxylic acids, aliphatic dicarboxylic acids with an even number of methylene groups are preferably used. As aliphatic dicarboxylic acids with an even number of methylene groups, succinic acid (methylene group number is 2), adipic acid (methylene group number is 4), suberic acid (methylene group number is 6) and sebacic acid (methylene group number is 8) can be exemplified.
[0109] Examples of the aromatic dicarboxylic acid include isophthalic acid, terephthalic acid, naphthalene dicarboxylic acid, and phthalic anhydride.
[0110] In addition, it is preferred that the content of aromatic dicarboxylic acid relative to the total amount of aliphatic dicarboxylic acid and aromatic dicarboxylic acid is within the range of 40 mol% to 80 mol%, in other words, the content of aliphatic dicarboxylic acid is limited to the range of 20 mol% to 60 mol%. In this case, a resin with high bonding strength and good molding processability is generated, and a packaging material with good molding processability and high side wall can be made into a packaging shell, and the interlayer peeling of the metal foil layer 2 and the heat-resistant resin layer 3 can be reliably suppressed. In addition, by making the content of aromatic dicarboxylic acid more than 40 mol%, the agglomeration peeling caused by the reduction of film properties can be reliably suppressed, and then the interlayer peeling can be reliably suppressed. By making the content of aromatic dicarboxylic acid less than 80%, the reduction of the adhesion performance caused by the curing of the resin can be reliably suppressed. The content of particularly preferred aromatic dicarboxylic acid is within the range of 50 mol% to 70 mol%.
[0111] Examples of the diol include ethylene glycol, propylene glycol, 1,3-butanediol, 1,4-butanediol, diethylene glycol, dipropylene glycol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, octanediol, 1,4-cyclohexanediol, and 2-butyl-2-ethyl-1,3-propanediol.
[0112] The molecular weight of the polyester resin is not limited, but it is preferred to set the number average molecular weight (Mn) in the range of 8,000 to 25,000, and the weight average molecular weight (Mw) in the range of 15,000 to 50,000, and further set their ratio (Mw / Mn) in the range of 1.3 to 2.5. By setting the number average molecular weight (Mn) to be 8,000 or more and the weight average molecular weight (Mw) to be 15,000 or more, suitable coating film strength and heat resistance can be reliably obtained. By setting the number average molecular weight (Mn) to be 25,000 or less and the weight average molecular weight (Mw) to be 50,000 or less, it will not be excessively hardened, and suitable coating film elongation can be reliably obtained. In addition, by setting their ratio (Mw / Mn) in the range of 1.3 to 2.5, a suitable molecular weight distribution is obtained, and the balance between the adhesive coating adaptability (wide distribution) and performance (narrow distribution) can be reliably ensured. In the polyester resin, a particularly preferred number average molecular weight (Mn) is in the range of 10,000 to 23,000, a particularly preferred weight average molecular weight (Mw) is in the range of 20,000 to 40,000, and a particularly preferred ratio (Mw / Mn) is in the range of 1.5 to 2.3.
[0113] The molecular weight of the polyester resin can be adjusted by chain extension using a multifunctional isocyanate. That is, if the polyester component in the main agent is connected using NCO, a polymer with a hydroxyl group at the end is generated, and the molecular weight of the polyester resin can be adjusted by adjusting the equivalent ratio of the isocyanate group to the hydroxyl group of the polyester. It is preferred to use a polyester resin obtained by connecting them in a manner such that their equivalent ratio (OH / NCO) is in the range of 1.01 to 10. In addition, as other methods for adjusting the molecular weight, the change of the reaction conditions of the polycondensation reaction of dicarboxylic acid and diol (adjustment of the molar ratio of dicarboxylic acid to diol) can be cited. In addition, epoxy resins and acrylic resins can also be added to the main agent of the adhesive as additives.
[0114] The type of the polyfunctional isocyanate compound as a curing agent is not limited. As the polyfunctional isocyanate compound, various isocyanate compounds of aromatic, aliphatic, alicyclic, etc. can be used. As a specific example, one or more polyfunctional isocyanate modified substances in diisocyanates such as hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI) from aliphatic, toluene diisocyanate (TDI) from aromatic, diphenylmethane diisocyanate (MDI) can be cited. The modification means is not limited. As the modification means, in addition to the adducts formed with polyfunctional active hydrogen compounds such as water, glycerol, trimethylolpropane, the polyfunctional isocyanate modified substances obtained by polymerization reactions such as isocyanurate esterification, carbodiimidization, polymerization, etc. can also be cited. One or more of them can also be mixed and used. In addition, in order to increase the bonding strength after curing and obtain the effect of inhibiting the peeling of the heat-resistant resin layer 3, it is preferred to contain more than 50 mol% of aromatic isocyanate compounds. The content of the aromatic isocyanate compound is particularly preferably 70 mol% or more.
[0115] In the two-component curing polyester urethane resin, the mixing ratio of the main agent and the curing agent is not limited, and they can be preferably mixed in a ratio of 2 to 25 moles of isocyanate functional groups (-NCO) relative to 1 mole of polyol hydroxyl groups (-OH). By making their molar ratio (-NCO) / (-OH) greater than 2, the curing reaction can be reliably and fully carried out, and suitable coating film strength and heat resistance can be reliably obtained. By making (-NCO) / (-OH) less than 25, the curing of the coating film caused by excessive reaction with functional groups other than polyols can be reliably suppressed, and suitable elongation can be reliably obtained. The particularly preferred molar ratio (-NCO) / (-OH) of polyol hydroxyl groups to isocyanate functional groups is in the range of 5 to 20.
[0116] (Inner adhesive layer)
[0117] The inner adhesive layer 6R is a layer responsible for the bonding between the metal foil layer 2 and the layer arranged on the inner surface side of the metal foil layer 2. In the first embodiment, it is a layer responsible for the bonding between the metal foil layer 2 (specifically, the inner surface chemical conversion film 2a of the metal foil layer 2) and the thermally fusible resin layer 4.
[0118] The inside adhesive layer 6R is formed of a cured film of an inside adhesive composition containing an inside adhesive and an inside reinforcing agent.
[0119] Hereinafter, in order to distinguish the above-mentioned inside adhesive composition containing the inside adhesive and the inside reinforcing agent from the inside adhesive composition containing the inside adhesive but not containing the inside reinforcing agent, the former is also referred to as "the inside adhesive composition containing the inside reinforcing agent", and the latter is referred to as "the inside adhesive composition not containing the inside reinforcing agent". Therefore, in the first embodiment, the inside adhesive layer 6R is formed of a cured film of the inside adhesive composition containing the inside reinforcing agent.
[0120] The type of the inner adhesive is not limited, and as the inner adhesive, polyurethane adhesives, acrylic adhesives, epoxy adhesives, polyolefin adhesives (e.g., acid-modified polypropylene adhesives), elastic adhesives, fluorine adhesives, etc. can be used. Among them, acrylic adhesives and polyolefin adhesives are preferably used, in which case the electrolyte resistance and water vapor barrier properties of the packaging material 1A can be improved.
[0121] As the inner reinforcing agent, inner reinforcing particles can be used. As the inner reinforcing particles, at least one of inorganic particles and organic particles can be used.
[0122] As inorganic particles, for example, fillers listed in "Table 1 Types and properties of fillers" in "Reinforcement (One) Inorganic Reinforcers (Bujin (その1) Inorganic Reinforcers)" by Shiraki Yoshikazu, Journal of the Rubber Association of Japan, Vol. 53, No. 1, pp. 17-33, 1980, and carbon black can be used. Specifically, as inorganic particles, at least one particle selected from the group consisting of calcium carbonate (CaCO3), magnesium carbonate, calcium / magnesium carbonate, silicate, silicon dioxide (silicic acid: SiO2), aluminum hydrate, barium sulfate, calcium sulfate, calcium sulfite and carbon black (CB) is preferably used.
[0123] As the organic particles, it is preferable to use particles (beads) of at least one selected from the group consisting of acrylic resin, styrene resin, and fluororesin.
[0124] Therefore, as the inner reinforcing particles, at least one selected from the group consisting of the above-mentioned inorganic particles and the above-mentioned organic particles is preferably used. In addition, the inorganic particles and the organic particles may be used in combination.
[0125] In addition, the inner reinforcing particles must satisfy the following requirements 1 and 2.
[0126] Requirement 1: The number average particle size of the inner reinforcing particles is within a range of 0.01 μm to 3 μm.
[0127] Requirement 2: The specific surface area of the inner reinforcing particles is 1m 2 / g or above.
[0128] By making the inner reinforcing particles satisfy the above requirement 1, the fracture path in the inner adhesive layer 6R becomes longer, and the fracture strength (tensile fracture strength, etc.) and fracture elongation (tensile fracture elongation, etc.) of the inner adhesive layer 6R are improved. In addition, by making the inner reinforcing particles satisfy the above requirement 2, the interaction between the inner reinforcing particles and the inner adhesive molecules becomes stronger, and the fracture strength of the inner adhesive layer 6R is further improved. Therefore, the puncture strength of the packaging material 1A can be improved.
[0129] Furthermore, generally, if the puncture strength of a packaging material increases, the molding processability of the packaging material tends to increase. Therefore, by increasing the puncture strength of the packaging material 1A, the molding processability of the packaging material 1A can also be improved.
[0130] In the above-mentioned requirement 1, the number average particle size of the inner reinforcing particles is 0.01 μm or more, thereby preventing the inner adhesive layer 6R from becoming hard due to the inclusion of the inner reinforcing particles. The number average particle size of the inner reinforcing particles is 3 μm or less, thereby reliably obtaining the reinforcing effect of the inner adhesive layer 6R brought about by the inclusion of the inner reinforcing particles. In addition, if the number average particle size of the inner reinforcing particles is less than 0.01 μm, when the inner reinforcing particles are dispersed in the inner adhesive, the inner reinforcing particles are easily agglomerated, and it is difficult to evenly disperse the inner reinforcing particles in the inner adhesive. The preferred lower limit of the number average particle size of the inner reinforcing particles is 0.03 μm, the preferred upper limit is 1.0 μm, and the more preferred upper limit is 0.5 μm.
[0131] In the above requirement 2, the preferred lower limit of the specific surface area of the inner reinforcing particles is 10 m 2 / g, the preferred upper limit is 500m 2 / g. If the specific surface area is greater than 500m 2 / g, the interaction between the inner reinforcing particles and the inner adhesive molecules is saturated, and the improvement of the breaking strength of the inner adhesive layer 6R is not observed. Therefore, the specific surface area is preferably 500m 2 / g or less. A more preferred upper limit is 450m 2 / g.
[0132] In addition, the inner reinforcing particles are preferably particles with insulating properties. In this case, the electrical insulation of the portion closer to the inner surface 1a than the metal foil layer 3 of the packaging material 1A can be improved. Therefore, for example, even if the inner surface 1a of the packaging material 1A is damaged by cracks, scratches, etc. due to frequent or strong contact of the packaged objects such as the storage device body 31 packaged by the packaging material 1A with the inner surface 1a of the packaging material 1A, the reduction in the electrical insulation of the packaging material 1A caused by the damage can be suppressed. In order to reliably achieve such an effect, the volume resistivity of the insulating inner reinforcing particles is preferably 1×10 12 Ωcm or more.
[0133] As such inner reinforcing particles having insulating properties, at least one selected from the group consisting of insulating inorganic particles and organic particles as described below is preferably used. Insulating inorganic particles and organic particles may also be used in combination.
[0134] Examples of the insulating inorganic particles include particles of calcium carbonate (CaCO 3 ), magnesium carbonate, calcium-magnesium carbonate, silicate, silicon dioxide (silicic acid: SiO 2 ), aluminum hydrate, barium sulfate, calcium sulfate, and calcium sulfite.
[0135] Examples of the organic particles include particles (beads) of acrylic resin, styrene resin, and fluororesin. In addition, generally, organic particles have insulating properties.
[0136] When the tensile elongation at break of a cured film of the inside adhesive composition containing the inside reinforcing agent is L1 and the tensile elongation at break of a cured film of the inside adhesive composition not containing the inside reinforcing agent is L10, L1 preferably satisfies the following relational expression 1.
[0137] 15%≤{(L1-L10) / L10}×100%≤250%…(Formula 1).
[0138] By making L1 satisfy the above-mentioned relational expression 1, in the packaging material 1A, the inner adhesive layer 6R has high followability to the deformation of the metal foil layer 2. Therefore, the puncture strength of the packaging material 1A can be reliably improved, and the moldability of the packaging material 1A can also be reliably improved.
[0139] In the above-mentioned relational expression 1, {(L1-L10) / L10}×100% as the median side thereof refers to the improvement rate ΔL1 of the tensile elongation at break of the cured film of the inner adhesive composition (inner adhesive layer 6R) achieved by containing the inner reinforcing agent (i.e., ΔL1={(L1-L10) / L10}×100%). The improvement rate ΔL1 is particularly preferably in the range of 20% to 230%, and further, ΔL1 is very preferably in the range of 50% to 230%.
[0140] In the inner reinforcing agent (inner reinforcing particles), functional groups can be added by subjecting the inner reinforcing agent to a silane-based or titanium-based coupling agent treatment or a surface treatment based on a synthetic polymer, etc. In this case, the surface activity of the inner reinforcing agent can be increased, thereby improving the interfacial adhesion between the inner reinforcing agent and the inner adhesive.
[0141] When dispersing the inner reinforcing agent in the inner adhesive in order to make the inner reinforcing agent contained in the inner adhesive, it is preferable to use a disperser for dispersion. In addition, a dispersant such as a surfactant may be used for the dispersion.
[0142] The method for dispersing the inner reinforcing agent in the inner adhesive is not limited, but the following method is preferable.
[0143] That is, an ink containing a high concentration of the inner reinforcing agent (also referred to as "ink containing a high concentration of the inner reinforcing agent") is prepared in advance. Then, the ink is added to the inner adhesive (preferably the main agent of the inner adhesive) so that the content of the inner reinforcing agent becomes a predetermined ratio and mixed, thereby dispersing the inner reinforcing agent in the inner adhesive.
[0144] The ink can be prepared, for example, as follows.
[0145] That is, an inner reinforcing agent is added to a varnish (a mixture of a resin and a solvent) and mixed to prepare a base of ink, to which auxiliary agents (surfactants, viscosity regulators, antistatic agents, antioxidants, dispersants, leveling agents, anti-settling agents, defoaming agents, etc.) are added, and kneading and dispersion are performed using a disperser, thereby uniformly dispersing the inner reinforcing agent in the varnish, thereby preparing the above-mentioned ink containing a high concentration of the inner reinforcing agent.
[0146] As the resin for the varnish, one or a combination of two or more selected from the group consisting of a copolymer of vinyl chloride and vinyl acetate, chlorinated rubber, chlorinated polypropylene, acrylic resin, polyamide resin, polyurethane resin, polyester resin and nitrocellulose can be used. In particular, as the resin, it is preferred to use a resin of the same type (more preferably the same composition) as the main agent of the inner adhesive, thereby making the ink and the main agent of the inner adhesive easily compatible (mixable).
[0147] As the paint solvent, one selected from the group consisting of toluene, methyl ethyl ketone, methylcyclohexane, ethyl acetate and isopropyl alcohol or a combination of two or more thereof can be used. In particular, ethyl acetate, methyl ethyl ketone, methylcyclohexane, etc., which can also be used as the inner adhesive solvent, are preferably used as the solvent. In addition, toluene, methyl ethyl ketone, etc. can be used as a cosolvent as needed.
[0148] The ink is preferably prepared using a paint resin, a paint solvent, an inner reinforcing agent, and an auxiliary agent in the following mixing ratio.
[0149] Resin: 15% to 25% by mass
[0150] Solvent: 40% to 70% by mass
[0151] Internal reinforcing agent: 5% to 50% by mass
[0152] Auxiliary agent: 1% to 5% by mass.
[0153] In addition, it is preferred that the inner reinforcing agent is dispersed uniformly in the ink at a high concentration. In order to prepare such an ink, as the above-mentioned disperser, a paint shaker, a ball mill, a grinder, a sand mill, a bead mill, a Dynomill, a roller mill, an ultrasonic grinder, a high-pressure collision disperser, etc. can be used. In addition, one disperser can be used for one or more dispersion treatments, or two or more dispersers can be used in combination for multiple dispersion treatments.
[0154] As described above, the ink containing the inner reinforcing agent at a high concentration is added to the inner adhesive (preferably the main agent thereof) so that the content of the inner reinforcing agent becomes a predetermined ratio, and the mixture is uniformly mixed and dispersed, thereby reliably suppressing the formation of secondary agglomerated particles between the inner reinforcing agents, thereby reliably making the inner reinforcing agent uniformly dispersed in the inner adhesive (the main agent thereof). Thus, even if the inner reinforcing agent is added to the inner adhesive (the main agent thereof) and left for several months, the inner adhesive (the main agent thereof) in which the inner reinforcing agent is well dispersed can be reliably obtained.
[0155] When the inner reinforcing agent is added to the main agent of the inner adhesive, for example, by reacting the main agent of the inner adhesive obtained as described above and well dispersed with the inner reinforcing agent with a curing agent (for example, an isocyanate curing agent), a cured film of the inner adhesive composition (i.e., the inner adhesive layer 6R) with very few coating defects caused by the secondary agglomerated particles of the inner reinforcing agent can be reliably formed. Thus, the tensile elongation at break L1 of the cured film is reliably improved compared to the cured film of the inner adhesive composition not containing the inner reinforcing agent, and the cured film of the inner adhesive composition can reliably follow the deformation and puncture deformation during the molding process. Therefore, the inner adhesive layer 6R can reliably maintain good adhesion.
[0156] For example, when a polyolefin adhesive is used as the inner adhesive, it is preferred to use an acid-modified polypropylene resin (acid-modified PP resin) as its main agent. In addition, when an acid-modified polypropylene resin is used as the main agent, it is preferred to use an acid-modified polypropylene resin as a paint resin and methylcyclohexane, methyl ethyl ketone or a mixed solvent thereof as a paint solvent.
[0157] The content of the inner reinforcing agent relative to the total amount of the inner reinforcing agent and the main agent of the inner adhesive (for example, acid-modified polypropylene resin) is preferably in the range of 2% to 10% by mass. It should be noted that, in detail, the content refers to the solid content, that is, the content does not include the mass of the solvent. The following are the same.
[0158] The inner adhesive layer 6R is preferably 2 g / m 2 ~10g / m 2 The coating amount in the range of is provided between the metal foil layer 2 and the heat-fusible resin layer 4. In addition, the content of the inner reinforcing agent in the inner adhesive layer 6R is preferably 0.2 g / m 2 ~1.0g / m 2 By making the coating amount of the inner adhesive layer 6R within the above range and the content of the inner reinforcing agent within the above range, the breaking strength and breaking elongation of the inner adhesive layer 6R are reliably improved. Therefore, the puncture strength of the packaging material 1A can be reliably improved, and the molding processability of the packaging material 1A can also be reliably improved. It should be noted that the coating amount of the inner adhesive layer 6R mentioned above refers to the solid component coating amount in detail, and the content of the inner reinforcing agent mentioned above refers to the solid component content in detail. The following are the same.
[0159] The more preferred lower limit of the coating amount of the inner adhesive layer 6R is 4 g / m 2 The more preferred upper limit is 9 g / m 2 The lower limit of the content of the inner reinforcing agent is more preferably 0.2 g / m 2 The more preferred upper limit is 0.7 g / m 2 .
[0160] The method for laminating (joining) the metal foil layer 2 and the heat-fusible resin layer 4 is not limited, but dry lamination is preferred.
[0161] (Method for producing packaging material)
[0162] An example of a preferred method for producing the packaging material 1A is as follows.
[0163] A metal foil layer 2 having a chemical conversion film 2a formed on the inner surface and the outer surface is prepared. Next, an outer adhesive composition is applied in a layer to the outer surface of the metal foil layer 2 by a predetermined coating method, and the solvent in the composition is dried and evaporated. Then, the outer surface of the metal foil layer 2 is bonded to the inner surface of the heat-resistant resin layer 3, and the composition is aged at a predetermined temperature according to the curing conditions of the composition, thereby curing the composition.
[0164] Next, the inner adhesive composition is applied in a layer to the inner surface of the metal foil layer 2 using a prescribed coating method, and the solvent in the composition is dried and evaporated. Then, the inner surface of the metal foil layer 2 is bonded to the outer surface of the thermally fusible resin layer 4, and the composition is aged at a prescribed temperature according to the curing conditions of the composition, thereby curing the composition.
[0165] Thus, the heat-resistant resin layer 3 is bonded to the outer surface of the metal foil layer 2 via the outer adhesive layer 5 , and the thermally fusible resin layer 4 is bonded to the inner surface of the metal foil layer 2 via the inner adhesive layer 6R, thereby obtaining the packaging material 1A.
[0166] The coating method is not limited, and specific examples thereof include gravure coating, reverse roll coating, and lip roll coating.
[0167] However, the packaging material according to the present invention is not limited to the packaging material manufactured by the above-mentioned manufacturing method of the packaging material 1A, and may be a packaging material manufactured by other methods.
[0168] The molding packaging material according to the present invention is not limited to the packaging material 1A of the first embodiment, and may be other packaging materials such as Figures 2 to 5 2 to 5th embodiment packaging materials 1B to 1E are shown in the figures. These packaging materials 1B to 1E can be used, for example, in the power storage device 30 (see Figure 6 and 7 ) packaging.
[0169] In these figures, the same reference numerals are given to elements that play the same role as the elements of the packaging material 1A of the first embodiment. In addition, the outer adhesive layer marked with reference numeral "5" does not contain an outer reinforcing agent like the outer adhesive layer of the packaging material 1A of the first embodiment, and the outer adhesive layer marked with reference numeral "5R" contains an outer reinforcing agent. Hereinafter, the second to fifth embodiments will be described with the focus on the differences from the first embodiment.
[0170] Figure 2In the second embodiment shown, the outer adhesive layer 5R of the packaging material 1B contains an outer reinforcing agent, and more specifically, is formed of a cured film of an outer adhesive composition containing an outer adhesive and an outer reinforcing agent, that is, a cured film of an outer adhesive composition containing an outer reinforcing agent.
[0171] As the external reinforcing agent, external reinforcing particles can be used. As the external reinforcing particles, at least one of inorganic particles and organic particles can be used.
[0172] As the inorganic particles, it is preferred to use at least one particle selected from the group consisting of calcium carbonate (CaCO 3 ), magnesium carbonate, calcium / magnesium carbonate, silicate, silicon dioxide (silicic acid: SiO 2 ), aluminum hydrate, barium sulfate, calcium sulfate, calcium sulfite and carbon black (CB).
[0173] As the organic particles, it is preferable to use particles of at least one selected from the group consisting of acrylic resin, styrene resin, and fluororesin.
[0174] Therefore, as the outer reinforcing particles, at least one selected from the group consisting of the above-mentioned inorganic particles and the above-mentioned organic particles can be used. In addition, the inorganic particles and the organic particles can also be used in combination.
[0175] Furthermore, the outer reinforcing particles preferably satisfy the following requirements 3 and 4.
[0176] Requirement 3: The number average particle size of the outer reinforcing particles is within the range of 0.01 μm to 3 μm.
[0177] Requirement 4: The specific surface area of the outer reinforcement particles is 1m 2 / g or above.
[0178] By making the outer reinforcing particles satisfy the above requirement 3, the fracture path in the outer adhesive layer 5R becomes longer, and the fracture strength (tensile fracture strength, etc.) and fracture elongation (tensile fracture elongation, etc.) of the outer adhesive layer 5R are improved. In addition, by making the outer reinforcing particles satisfy the above requirement 4, the interaction between the outer reinforcing particles and the outer adhesive molecules becomes stronger, and the fracture strength of the outer adhesive layer 5R is further improved. Therefore, the puncture strength of the packaging material 1B can be further improved.
[0179] Furthermore, generally, as the puncture strength of a packaging material increases, the molding processability of the packaging material tends to increase. Therefore, by further increasing the puncture strength of the packaging material 1B, the molding processability of the packaging material 1B can be further improved.
[0180] In the above requirement 3, the number average particle size of the outer reinforcing particles is 0.01 μm or more, thereby reliably suppressing the hardening of the outer adhesive layer 5R due to the inclusion of the outer reinforcing particles, and reliably improving the elongation at break of the outer adhesive layer 5R. The number average particle size of the outer reinforcing particles is 3 μm or less, thereby reliably obtaining the reinforcing effect of the outer adhesive layer 5R brought about by the inclusion of the outer reinforcing particles. The preferred lower limit of the number average particle size of the outer reinforcing particles is 0.03 μm, and the preferred upper limit is 0.5 μm.
[0181] In the above requirement 4, the more preferred lower limit of the specific surface area of the outer reinforcing particles is 10 m 2 / g, and the more preferred upper limit is 500m 2 / g. If the specific surface area is greater than 500m 2 / g, the interaction between the outer reinforcing particles and the outer adhesive molecules is saturated, and the improvement of the breaking strength of the outer adhesive layer 5R is not observed. Therefore, the specific surface area is preferably 500m 2 / g or less. A more preferred upper limit is 450m 2 / g.
[0182] In addition, when the tensile elongation at break of the cured film of the outer adhesive composition containing the outer reinforcing agent (i.e., the outer adhesive composition containing the outer adhesive and the outer reinforcing agent) is set to L2, and the tensile elongation at break of the cured film of the outer adhesive composition not containing the outer reinforcing agent (i.e., the outer adhesive composition containing the outer adhesive but not containing the outer reinforcing agent) is set to L20, L2 preferably satisfies the following Relationship 2.
[0183] 15%≤{(L2-L20) / L20}×100%≤250%…(Formula 2).
[0184] By making L2 satisfy the above-mentioned relational expression 2, in the packaging material 1B, the outer adhesive layer 5R has high followability to the deformation of the metal foil layer 2. Therefore, the puncture strength of the packaging material 1B can be more reliably improved, and the moldability of the packaging material 1B can also be more reliably improved.
[0185] In the above-mentioned relational expression 2, {(L2-L20) / L20}×100% as the median side thereof refers to the improvement rate ΔL2 of the tensile elongation at break of the cured film of the outer adhesive composition (outer adhesive layer 5R) achieved by containing the outer reinforcing agent (i.e., ΔL2={(L2-L20) / L20}×100%). The improvement rate ΔL2 is particularly preferably in the range of 20% to 230%, and further, ΔL2 is very preferably in the range of 50% to 230%.
[0186] In the external reinforcing agent (external reinforcing particles), functional groups can be imparted by subjecting the external adhesive to a silane-based or titanium-based coupling agent treatment or a surface treatment based on a synthetic polymer or the like. In this case, the surface activity of the external reinforcing agent can be increased, thereby increasing the interfacial adhesion between the external reinforcing agent and the external adhesive.
[0187] When dispersing the external reinforcing agent in the external adhesive in order to include the external reinforcing agent in the external adhesive, it is preferable to use a disperser for dispersion. In addition, a dispersant such as a surfactant may be used for the dispersion.
[0188] The method for dispersing the outer reinforcing agent in the outer adhesive is not limited, and the same method as the method for dispersing the inner reinforcing agent in the inner adhesive described above can be preferably used.
[0189] For example, when an outer adhesive based on a two-component curable polyester urethane resin is used as the outer adhesive, a varnish containing a polyester resin (varnish resin) of the same type as the main component of the outer adhesive and ethyl acetate (varnish solvent) is prepared, an outer reinforcing agent and an auxiliary agent are added to the varnish, and kneading and dispersion are performed using a disperser, thereby uniformly dispersing the outer reinforcing agent in the varnish, thereby preparing an ink containing a high concentration of the outer reinforcing agent (also referred to as "ink containing a high concentration of the outer reinforcing agent").
[0190] Next, the ink is added to the main agent of the external adhesive so that the content of the external reinforcing agent becomes a predetermined ratio, and the mixture is uniformly mixed and dispersed, thereby reliably suppressing the generation of secondary aggregated particles between the external reinforcing agents, and reliably dispersing the external reinforcing agent uniformly in the main agent of the external adhesive. Thus, a main agent of the external adhesive having good dispersibility of the external reinforcing agent can be obtained, in which the external reinforcing agent does not precipitate even after being added to the main agent and left for several months.
[0191] In this ink, the preferred mixing ratio of the varnish resin, the varnish solvent, the external reinforcing agent, and the auxiliary agent is the same as that of the ink containing the high concentration of the internal reinforcing agent described above.
[0192] The content of the external reinforcing agent relative to the total amount of the external reinforcing agent and the main agent of the external adhesive is preferably in the range of 2 mass % to 10 mass %. It should be noted that, in detail, the content refers to the solid content. The following are the same.
[0193] The outer adhesive layer 5R is preferably 2 g / m 2 ~10g / m 2 The coating amount in the range of is set between the metal foil layer 2 and the heat-resistant resin layer 3. In addition, the content of the outer reinforcing agent in the outer adhesive layer 5R is preferably 0.2 g / m2 ~1.0g / m 2 By making the coating amount of the outer adhesive layer 5R within the above range and the content of the outer reinforcing agent within the above range, the breaking strength and breaking elongation of the outer adhesive layer 5R are reliably improved. Therefore, the puncture strength of the packaging material 1B can be reliably improved, and the molding processability of the packaging material 1B can also be reliably improved. It should be noted that the coating amount of the outer adhesive layer 5R mentioned above refers to the solid component coating amount in detail, and the content of the outer reinforcing agent mentioned above refers to the solid component content in detail. The following are the same.
[0194] The more preferred lower limit of the coating amount of the outer adhesive layer 5R is 4 g / m 2 The more preferred upper limit is 9 g / m 2 The more preferred lower limit of the content of the above-mentioned outer reinforcing agent is 0.2 g / m 2 The more preferred upper limit is 0.7 g / m 2 .
[0195] Figure 3 In the third embodiment shown, the outer adhesive layer 5R of the packaging material 1C contains an outer reinforcing agent, and more specifically, is formed of a cured film of an outer adhesive composition containing an outer adhesive and an outer reinforcing agent, that is, a cured film of an outer adhesive composition containing an outer reinforcing agent.
[0196] Furthermore, the packaging material 1C includes a matte coating layer 7 formed in a laminated manner on the outer surface of the heat-resistant resin layer 3 .
[0197] (Matt coating)
[0198] The matte coating layer 7 is a layer for imparting good sliding properties to the outer surface 1 b of the packaging material 1C and improving the molding processability of the packaging material 1C.
[0199] The type of the matte coating 7 is not limited. For example, the matte coating 7 is formed by a cured film of a resin composition containing inorganic particles and organic particles dispersed in a heat-resistant resin component. Among them, the matte coating 7 is preferably formed by a cured film of a resin composition containing 20% to 40% by mass of inorganic particles with a number average particle size of 1 μm to 10 μm and 5% to 15% by mass of organic particles with a number average particle size of 5 μm to 15 μm in a two-component curable heat-resistant resin.
[0200] As the heat-resistant resin, for example, at least one selected from the group consisting of acrylic resin, epoxy resin, polyester resin, urethane resin, polyolefin resin and fluorine resin can be used. In particular, as the heat-resistant resin, a fluorine resin based on tetrafluoroethylene or fluorine ethylene-vinyl ether copolymer is preferably used in view of excellent heat resistance and chemical resistance.
[0201] In the matte coating 7, the type of inorganic particles is not limited. As the inorganic particles, for example, at least one particle selected from the group consisting of silica, alumina, calcium oxide, calcium carbonate, calcium sulfate, barium sulfate and calcium silicate can be used, among which silica particles are preferably used.
[0202] In the matte coating 7, the type of organic particles is not limited. As the organic particles (organic beads), for example, at least one selected from the group consisting of polyethylene wax, polytetrafluoroethylene wax, acrylic resin particles, urethane resin particles, polyethylene resin particles, and polystyrene resin particles can be used. Among them, polyethylene wax, polytetrafluoroethylene wax, and polyethylene resin particles are preferably used.
[0203] The matte coating layer 7 can be formed, for example, by applying a matte coating composition containing the above-mentioned inorganic particles and / or organic particles and a heat-resistant resin in a layer form on the outer surface of the heat-resistant resin layer 3 and curing the composition.
[0204] The thickness of the matte coating 7 after curing (drying) is preferably in the range of 0.5 μm to 5 μm. By setting the thickness to be 0.5 μm or more, the sliding property of the outer surface 1b of the packaging material 1C is reliably improved. By setting the thickness to be 5 μm or less, the manufacturing cost of the packaging material 1C can be reliably reduced. The particularly preferred thickness is in the range of 1 μm to 3 μm.
[0205] The glossiness value of the surface (outer surface) of the matte coating 7 is a value measured at a 60° reflection angle based on JIS (Japanese Industrial Standard) Z8741, and is preferably set in the range of 1% to 15%. The glossiness value can be measured at a 60° reflection angle using a glossiness meter "micro-TRI-glo ss-s" manufactured by BYK, for example.
[0206] The timing of the step of forming the matte coating layer 7 is not limited, but the matte coating layer forming step is preferably performed after the step of bonding the heat-resistant resin layer 3 to the metal foil layer 2 via the outer adhesive layer 5R.
[0207] Figure 4In the fourth embodiment shown, the outer adhesive layer 5 of the packaging material 1D does not contain an outer reinforcing agent and is therefore formed of a cured film of an outer adhesive composition that does not contain an outer reinforcing agent.
[0208] In addition, the packaging material 1D includes a matte coating layer 7 formed in a laminated manner on the outer surface of the heat-resistant resin layer 3. The structure of the matte coating layer 7 is similar to that of the third embodiment ( Figure 3 ) is the same as the matte coating 7.
[0209] Furthermore, the packaging material 1D includes a black colored layer 8 formed in a laminated state on the inner surface of the heat-resistant resin layer 3 . Specifically, the black colored layer 8 is provided between the outer adhesive layer 5 and the heat-resistant resin layer 3 .
[0210] (Black coloring layer)
[0211] The black colored layer 8 is a layer for masking the color and gloss of the metal foil layer 2 on the outer surface 1 b of the packaging material 1D.
[0212] The structure of the black coloring layer 8 is not limited, but the black coloring layer 8 preferably contains carbon black (CB), diamine, polyol, and a curing agent. However, the present invention is not limited to such a structure of the black coloring layer 8.
[0213] The content of carbon black in the black coloring layer 8 is not limited, and it is preferably in the range of 15 mass % to 60 mass %. In addition, the content of the total amount of diamine, polyol and curing agent in the black coloring layer 8 is not limited, and it is preferably in the range of 40 mass % to 85 mass %. Among them, the content of carbon black is preferably in the range of 20 mass % to 50 mass %. It should be noted that, in detail, their contents all refer to the solid content. The following are the same.
[0214] The thickness of the black colored layer 8 is not limited, but is preferably in the range of 1 μm to 4 μm. By setting the thickness to be 1 μm or more, the color and gloss of the metal foil layer 2 can be reliably shielded.
[0215] The method for forming the black colored layer 8 is not limited, and examples thereof include a gravure printing method, a reverse roll coating method, and a lip roll coating method.
[0216] The particle size of carbon black is not limited, but it is preferable to use carbon black having a number average particle size within a range of 0.01 μm to 3 μm.
[0217] The type of diamine is not limited. As the diamine, for example, one or more selected from the group consisting of ethylenediamine, dimerdiamine, 2-hydroxyethylethylenediamine, 2-hydroxyethylpropylenediamine, dicyclohexylmethanediamine and 2-hydroxyethylpropylenediamine can be used.
[0218] The type of the polyol is not limited, but as the polyol, it is preferable to use one or two or more selected from the group consisting of polyurethane polyols, polyester polyols, and polyether polyols.
[0219] In the black coloring layer 8, the type of curing agent is not limited, and for example, isocyanate compounds can be cited. As isocyanate compounds, for example, various isocyanate compounds of aromatic, aliphatic, and alicyclic systems can be used. As specific examples thereof, toluene diisocyanate (TDI), diphenylmethane diisocyanate, hexamethylene diisocyanate (HDI), and isophorone diisocyanate can be cited.
[0220] Figure 5 In the fifth embodiment shown, the outer adhesive layer 5R of the packaging material 1E contains an outer reinforcing agent, and more specifically, is formed of a cured film of an outer adhesive composition containing an outer adhesive and an outer reinforcing agent, that is, a cured film of an outer adhesive composition containing an outer reinforcing agent.
[0221] In addition, the packaging material 1E includes a matte coating layer 7 formed in a laminated manner on the outer surface of the heat-resistant resin layer 3. The structure of the matte coating layer 7 is similar to that of the third embodiment ( Figure 3 ) is the same as the matte coating 7.
[0222] In addition, the packaging material 1E includes a black coloring layer 8 formed in a laminated manner on the inner surface of the heat-resistant resin layer 3. Specifically, the black coloring layer 8 is provided between the outer adhesive layer 5R and the heat-resistant resin layer 3. The configuration of the black coloring layer 8 is, for example, similar to that of the fourth embodiment ( Figure 4 ) is the same as the black colored layer 8.
[0223] Although some embodiments of the present invention have been described above, the present invention is not limited to these embodiments, and it goes without saying that various changes can be made within the scope not departing from the gist of the present invention.
[0224] Example
[0225] Specific examples and comparative examples of the present invention are shown below. However, the present invention is not limited to the following examples.
[0226] Here, in the following Examples 1 to 10 and the following Comparative Examples 1 to 4, aluminum foil of the same material is used as the metal foil layer 2. The material is aluminum alloy symbol A8079 specified by JIS H4160. The thickness of all aluminum foils is 35 μm. In addition, chemical conversion coatings 2a obtained by the same chemical conversion treatment as in Example 1 are formed on the inner and outer surfaces of all aluminum foils.
[0227] In addition, in the following embodiments 1 to 10 and the following comparative examples 1 to 4, as the heat-resistant resin layer 3, all the same monolayer biaxially stretched nylon (ONY) films are used. The thickness of all the films is 15 μm. In addition, for the inner surface of all the films (i.e., the bonding surface with the metal foil layer 2 in the film), corona treatment is implemented in advance in order to improve the wettability with the outer adhesive composition. In addition, in embodiments 7 to 10 and comparative examples 3 to 4, a matte coating 7 of the same composition is formed on the outer surface of the film, and in embodiments 8 to 10 and comparative examples 3 to 4, a black coloring layer 8 of the same composition is formed on the inner surface of the film.
[0228] In the following Examples 1 to 10 and Comparative Examples 1 to 4, the same unstretched three-layer coextruded polypropylene (CPP) film was used as the heat-fusible resin layer 4. The thickness of all the films was 30 μm, and the layer thickness ratio was rPP:bPP:rPP=1:8:1. In addition, the outer surface of all the films (i.e., the bonding surface of the film with the metal foil layer 2) was pre-corona treated in order to improve the wettability with the inner adhesive composition.
[0229] <Example 1>
[0230] A chemical conversion film 2a is formed on the inner and outer surfaces of the aluminum foil as the metal foil layer 2. The chemical conversion film 2a is formed by applying a chemical conversion treatment solution composed of polyacrylic acid, a trivalent chromium compound, water and an alcohol to the inner and outer surfaces of the aluminum foil and then drying at 150°C. The chromium deposition amount of the chemical conversion film 2a is 10 mg / m2 on one side of the aluminum foil. 2 The thickness of each chemical conversion film 2a is 0.01 μm.
[0231] The above-mentioned biaxially stretched nylon (ONY) film was prepared as the heat-resistant resin layer 3. The TD hot water shrinkage of the film was 2.7%, the MD hot water shrinkage was 2.0%, the difference in hot water shrinkage between TD and MD (TD-MD) was 0.7%, the TD elastic modulus was 1.7 GPa, the MD elastic modulus was 2.7 GPa, the TD breaking strength was 361 MPa, the MD breaking strength was 280 MPa, and the number average molecular weight of the polyamide was 25,000.
[0232] As the outer adhesive composition constituting the outer adhesive layer 5, an outer adhesive composition containing an outer adhesive but not containing an outer reinforcing agent, that is, an outer adhesive composition not containing an outer reinforcing agent is prepared. In the outer adhesive composition, a two-component curing polyester urethane resin is used as the outer adhesive. The preparation method of the outer adhesive composition is as follows.
[0233] First, a polyester resin (polyester polyol) as the main agent of a two-liquid curable polyester urethane resin was prepared by the following method. That is, 30 mol parts of neopentyl glycol, 30 mol parts of ethylene glycol, and 40 mol parts of 1,6-hexanediol were melted at 80°C, and the melt was subjected to a condensation reaction at 210°C for 20 hours with stirring with 30 mol parts of adipic acid (methylene number is 4) as an aliphatic dicarboxylic acid and 70 mol parts of isophthalic acid as an aromatic dicarboxylic acid, thereby obtaining a polyester polyol as the main agent. The number average molecular weight (Mn) of the polyester polyol is 12,000, the weight average molecular weight (Mw) is 20,500, and their ratio (Mw / Mn) is 1.7. Furthermore, 60 parts by mass of ethyl acetate are added to 40 parts by mass of the polyester polyol to prepare a flowing polyester polyol resin solution. Its hydroxyl value is 2.2 mgKOH / g (solution value).
[0234] Next, 7.1 parts by mass of an adduct of toluene diisocyanate (TDI) (aromatic) and trimethylolpropane (TMP) (NCO: 13.0% by mass, solid content: 75% by mass) as a curing agent was added to 100 parts by mass of the polyester polyol resin solution as the main agent, and 34.1 parts by mass of ethyl acetate was further added, and stirred and mixed to prepare an outer adhesive composition (i.e., a two-component curable polyester urethane resin) not containing an outer reinforcing agent. In the outer adhesive composition, the molar ratio (-NCO) / (-OH) of the isocyanate functional group (-NCO) to the polyester polyol hydroxyl group (-OH) was 10.
[0235] Next, a cured film of the outer adhesive composition was prepared by the following method, and its physical properties were evaluated.
[0236] That is, the outer adhesive composition is applied in a layer on a non-adhesive untreated polypropylene film so that the thickness after drying is 10 μm, the solvent in the composition is dried and evaporated, and then the composition is aged at 60° C. until the residual isocyanate is 5% by mass or less, thereby curing. Then, the cured product is peeled off from the untreated polypropylene film, thereby preparing a cured film (10 μm in thickness) of the outer adhesive composition.
[0237] The cured film was cut into 15 mm width to collect a test piece, and then the test piece was subjected to a tensile test to measure the tensile breaking strength and tensile breaking elongation of the test piece. As a result, the tensile breaking strength was 30 MPa and the tensile breaking elongation was 18%.
[0238] It should be noted that the above-mentioned tensile test was conducted under the conditions of a point distance of 50 mm and a tensile speed of 100 mm / min in accordance with JIS K7161-1:2014. The following are the same.
[0239] Next, at 5.0 g / m 2 The outer adhesive composition is applied in a layer on the outer surface of the aluminum foil with a coating amount (specifically, the solid content coating amount. The same below) to dry and evaporate the solvent in the composition. Then, the outer surface of the aluminum foil is bonded to the inner surface of the biaxially stretched nylon (ONY) film as the heat-resistant resin layer 3, and aged at 60°C to cure the composition.
[0240] Next, as an inner adhesive composition constituting the inner adhesive layer 6R, a silica particle (SiO2 particle: number average particle size of 0.4 μm, specific surface area of 10 m 2 / g) and an acid-modified polypropylene (PP) adhesive as an inner adhesive, that is, an inner adhesive composition containing silica particles. The preparation method of this composition is as follows.
[0241] First, 20 parts by mass of acid-modified polypropylene (acid-modified PP) having the same composition as the main agent of the inner adhesive as a varnish resin, 40 parts by mass of a mixed organic solvent of methylcyclohexane:methyl ethyl ketone = 8 parts by mass:2 parts by mass as a varnish solvent, 35 parts by mass of the above-mentioned silica particles as an inner reinforcing agent, and 5 parts by mass of auxiliary agents (dispersant and anti-settling agent) were mixed, and the mixture was kneaded and dispersed using a disperser, thereby preparing an ink containing a high concentration of silica particles (concentration of silica particles: 35% by mass).
[0242] Next, a predetermined amount of the ink was added to 15 parts by mass of an acid-modified polypropylene resin solution and 85 parts by mass of a mixed organic solvent of methylcyclohexane:methyl ethyl ketone=8 parts by mass:2 parts by mass, and mixed and dispersed using a disperser to prepare a main agent of an inner adhesive containing silica particles.
[0243] 0.9 parts by mass of a polymer (multifunctional isocyanate compound) of hexamethylene diisocyanate (HDI) as a curing agent was added to 100 parts by mass of the main agent in such a manner that the equivalent ratio (NCO / OH) was 1.8, and the mixture was stirred and mixed to prepare an inner adhesive composition containing silica particles (i.e., an acid-modified polypropylene adhesive containing silica particles). The content of silica particles in the inner adhesive composition (specifically, the solid content, the same below) was 4.5% by mass.
[0244] Next, a cured film of the inner adhesive composition was prepared by the following method, and its physical properties were evaluated.
[0245] That is, the inner adhesive composition is applied in a layer on a non-adhesive untreated polypropylene film so that the thickness after drying is 10 μm, the solvent in the composition is dried and evaporated, and then the composition is aged at 40° C. until the residual isocyanate is 5% by mass or less, thereby curing. Then, the cured product is peeled off from the untreated polypropylene film, thereby preparing a cured film (10 μm thick) of the inner adhesive composition.
[0246] The cured film was cut into 15 mm width to collect a test piece, and then the test piece was subjected to a tensile test to measure the tensile breaking strength and tensile breaking elongation L1 of the test piece. As a result, the tensile breaking strength was 25 MPa and the tensile breaking elongation L1 was 172%.
[0247] In addition, an inner adhesive composition containing an inner adhesive but not containing silica particles, i.e., an inner adhesive composition not containing silica particles, was prepared by the same method as the inner adhesive composition described above, without using an ink containing high concentration silica particles. Next, a cured film of the inner adhesive composition was prepared by the same method as the cured film of the inner adhesive composition containing silica particles described above.
[0248] The cured film was cut into a width of 15 mm to collect a test piece. Then, the test piece was subjected to a tensile test to measure the tensile breaking strength and tensile breaking elongation L10 of the test piece, and the improvement rate ΔL1 (={(L1-L10) / L10}×100%) of the tensile breaking elongation of the cured film of the inner adhesive composition achieved by containing silica particles was calculated. As a result, ΔL1 was 64%.
[0249] Next, at 5.5 g / m 2 The inner adhesive composition containing silica particles is applied in a layer on the inner surface of the aluminum foil with a coating amount (specifically, the solid content coating amount. The same applies below) and the solvent in the composition is dried and evaporated. Then, the inner surface of the aluminum foil is bonded to the outer surface of the above-mentioned unstretched three-layer coextruded polypropylene (CPP) film as the heat-fusible resin layer 4, and aged at 40°C to cure the composition. In this case, the content of silica particles in the inner adhesive layer 6R is 0.25 g / m 2 .
[0250] The packaging material was manufactured by the above method.
[0251] <Example 2>
[0252] A two-component curable polyester urethane resin used as the outer adhesive of Example 1 and silica particles (SiO2 particles: number average particle size of 0.4 μm, specific surface area of 10 m 2 / g) of an outer adhesive composition, that is, an outer adhesive composition containing silica particles.
[0253] First, 20 parts by mass of the polyester polyol of Example 1 as a paint resin, 40 parts by mass of ethyl acetate as a paint solvent, 35 parts by mass of the above-mentioned silica particles as an external reinforcing agent, and 5 parts by mass of auxiliary agents (dispersant and anti-settling agent) are mixed, and the mixture is kneaded and dispersed using a disperser to prepare an ink containing a high concentration of silica particles (concentration of silica particles: 35% by mass).
[0254] Next, a predetermined amount of the ink was added to 100 parts by mass of the polyester polyol resin solution of Example 1 and 64.4 parts by mass of ethyl acetate, and mixed and dispersed using a disperser to prepare a main agent of an external adhesive containing silica particles.
[0255] With respect to 100 parts by mass of the main agent, 7.1 parts by mass of an adduct of toluene diisocyanate (TDI) (aromatic system) and trimethylolpropane (TMP) as an aromatic isocyanate compound (NCO is 13.0% by mass, solid content is 75% by mass) was added as a curing agent, and 34.1 parts by mass of ethyl acetate was further added, and stirred and mixed to prepare an outer adhesive composition containing silica particles. In the outer adhesive composition, the molar ratio (-NCO) / (-OH) of the isocyanate functional group (-NCO) to the polyester polyol hydroxyl group (-OH) was 10. In addition, the content of silica particles in the outer adhesive composition was 4.9% by mass.
[0256] Next, a cured film of the outer adhesive composition was prepared by the following method, and its physical properties were evaluated.
[0257] That is, the outer adhesive composition is applied in a layer on a non-adhesive untreated polypropylene film so that the thickness after drying is 10 μm, the solvent in the composition is dried and evaporated, and then the composition is aged at 60° C. until the residual isocyanate is 5% by mass or less, thereby curing. Then, the cured product is peeled off from the untreated polypropylene film, thereby preparing a cured film (10 μm in thickness) of the outer adhesive composition.
[0258] The cured film was cut into pieces with a width of 15 mm to obtain test pieces. The test pieces were then subjected to a tensile test to measure the tensile breaking strength and tensile breaking elongation L2 of the test pieces. As a result, the tensile breaking strength was 35 MPa and the tensile breaking elongation L2 was 42%.
[0259] In addition, an external adhesive composition containing an external adhesive but not containing silica particles, i.e., an external adhesive composition not containing silica particles, was prepared by the same method as the above-mentioned external adhesive composition without using an ink containing high concentration silica particles. Then, a cured film of the external adhesive composition was prepared by the same method as the cured film of the above-mentioned external adhesive composition containing silica particles.
[0260] The cured film was cut into a width of 15 mm to collect a test piece. Then, the test piece was subjected to a tensile test to measure the tensile breaking strength and tensile breaking elongation L20 of the test piece, and the improvement rate ΔL2 (={(L2-L20) / L20}×100%) of the tensile breaking elongation of the cured film of the outer adhesive composition achieved by containing silica particles was calculated. As a result, ΔL2 was 133%.
[0261] Next, at 5.5 g / m 2 The outer adhesive composition containing silica particles is applied in a layer on the outer surface of the aluminum foil, and the solvent in the composition is dried and evaporated. Then, the outer surface of the aluminum foil is bonded to the inner surface of the biaxially stretched nylon (ONY) film as the heat-resistant resin layer 3, and aged at 60°C to cure the composition. In this case, the content of silica particles in the outer adhesive layer 5R is 0.27 g / m 2 .
[0262] Next, as an inner adhesive composition constituting the inner adhesive layer 6R, a silica particle (SiO2 particle: number average particle size of 0.4 μm, specific surface area of 10 m 2 / g) and an acid-modified polypropylene (PP) adhesive as an inner adhesive, that is, an inner adhesive composition containing silica particles. The preparation method of this composition is as follows.
[0263] First, 20 parts by mass of acid-modified polypropylene having the same composition as the main agent of the inner adhesive as a paint resin, 40 parts by mass of a mixed organic solvent of methylcyclohexane:methyl ethyl ketone = 8 parts by mass:2 parts by mass as a paint solvent, 35 parts by mass of the above-mentioned silica particles as an inner reinforcing agent, and 5 parts by mass of auxiliary agents (dispersant and anti-settling agent) were mixed, and the mixture was kneaded and dispersed using a disperser, thereby preparing an ink containing a high concentration of silica particles (concentration of silica particles: 35% by mass).
[0264] Next, a predetermined amount of the ink was added to 15 parts by mass of an acid-modified polypropylene resin solution and 85 parts by mass of a mixed organic solvent of methylcyclohexane:methyl ethyl ketone=8 parts by mass:2 parts by mass, and mixed and dispersed using a disperser to prepare a main agent of an inner adhesive containing silica particles.
[0265] 0.9 parts by mass of a polymer (polyfunctional isocyanate compound) of hexamethylene diisocyanate (HDI) as a curing agent was added to 100 parts by mass of the main agent so that the equivalent ratio (NCO / OH) was 1.8, and the mixture was mixed and stirred to prepare an inner adhesive composition containing silica particles (i.e., an acid-modified polypropylene adhesive containing silica particles). The content of silica particles in the inner adhesive composition was 3.5% by mass.
[0266] Next, a cured film of the inner adhesive composition containing silica particles was prepared by the following method, and its physical properties were evaluated.
[0267] That is, the inner adhesive composition is applied in a layer on a non-adhesive untreated polypropylene film so that the thickness after drying is 10 μm, the solvent in the composition is dried and evaporated, and then the composition is aged at 40° C. until the residual isocyanate is 5% by mass or less, thereby curing. Then, the cured product is peeled off from the untreated polypropylene film, thereby preparing a cured film (10 μm thick) of the inner adhesive composition.
[0268] The cured film was cut into 15 mm width to collect a test piece, and then the test piece was subjected to a tensile test to measure the tensile breaking strength and tensile breaking elongation L1 of the test piece. As a result, the tensile breaking strength was 23 MPa and the tensile breaking elongation L1 was 165%.
[0269] In addition, an inner adhesive composition containing an inner adhesive but not containing silica particles, i.e., an inner adhesive composition not containing silica particles, was prepared by the same method as the inner adhesive composition described above, without using an ink containing high concentration silica particles. Next, a cured film of the inner adhesive composition was prepared by the same method as the cured film of the inner adhesive composition containing silica particles described above.
[0270] The cured film was cut into a width of 15 mm to collect a test piece. Then, the test piece was subjected to a tensile test to measure the tensile breaking strength and tensile breaking elongation L10 of the test piece, and the improvement rate ΔL1 of the tensile breaking elongation of the cured film of the inner adhesive composition due to the inclusion of silica particles was calculated. As a result, ΔL1 was 57%.
[0271] Next, at 6.5 g / m 2 The inner adhesive composition containing silica particles is applied in a layer on the inner surface of the aluminum foil in an amount of 0.23 g / m2, and the solvent in the composition is dried and evaporated. Then, the inner surface of the aluminum foil is bonded to the outer surface of the unstretched three-layer coextruded polypropylene (CPP) film as the heat-fusible resin layer 4, and aged at 40°C to cure the composition. In this case, the content of silica particles in the inner adhesive layer 6R is 0.23 g / m2. 2 .
[0272] The packaging material was manufactured by the above method.
[0273] <Example 3>
[0274] In Example 1, the content of the silica particles as the inner reinforcing agent was set to 9.0 mass % and the coating amount of the inner adhesive composition was set to 12.5 g / m 2 , except for this, the same operation as in Example 1 was performed to conduct a tensile test of the cured film of each adhesive composition and to produce a packaging material. In this case, the content of the silica particles in the inner adhesive layer 6R was 1.13 g / m 2 .
[0275] In addition, the values of the tensile elongation at break and the increase rate ΔL2 of the cured film of the outer adhesive composition measured and calculated by the tensile test are recorded in the "Cured Film" column of the "Outer Adhesive Layer" in Table 1, and the values of the tensile elongation at break and the increase rate ΔL1 of the cured film of the inner adhesive composition measured and calculated by the tensile test are recorded in the "Cured Film" column of the "Inner Adhesive Layer" in Table 1. The same applies to Examples 4 to 10 and Comparative Examples 1 to 4.
[0276] <Example 4>
[0277] In Example 2, the outer reinforcing agent is calcium carbonate particles (CaCO3 particles: number average particle size of 0.03 μm, specific surface area of 130 m 2 / g) and the content of calcium carbonate particles in the outer adhesive composition was 4.5% by mass, and the coating amount of the outer adhesive composition was 5.5 g / m 2 , and the inner reinforcing agent is calcium carbonate particles (CaCo3 particles: the average particle size is 0.03 μm, the specific surface area is 130 m 2 / g) and the content of calcium carbonate particles in the inner adhesive composition is 5.0 mass %, and the coating amount of the inner adhesive composition is 5.0 g / m 2 , except for this, the same operation as in Example 2 was performed to conduct a tensile test of the cured film of each adhesive composition and to produce a packaging material. In this case, the content of calcium carbonate particles in the outer adhesive layer 5R was 0.25 g / m 2 The content of calcium carbonate particles in the inner adhesive layer 6R is 0.25 g / m 2 .
[0278] <Example 5>
[0279] In Example 1, the inner reinforcing agent is calcium carbonate particles (CaCO3 particles: number average particle size of 1.0 μm, specific surface area of 3.0 m 2 / g) and the content of calcium carbonate particles in the inner adhesive composition was 2.5 mass %, and the coating amount of the inner adhesive composition was 8.5 g / m 2 , except for this, the same operation as in Example 1 was performed to conduct a tensile test of the cured film of the inner adhesive composition and to manufacture a packaging material. In this case, the content of calcium carbonate particles in the inner adhesive layer 6R was 0.21 g / m 2 .
[0280] <Example 6>
[0281] In Example 1, the inner reinforcing agent is acrylic resin particles (with a number average particle size of 2.0 μm and a specific surface area of 2.5 m 2 / g) and the content of the acrylic resin particles in the inner adhesive composition was 4.0 mass %, and the coating amount of the inner adhesive composition was 5.5 g / m 2 , except for this, the same operation as in Example 1 was performed to conduct a tensile test of the cured film of the inner adhesive composition and to manufacture a packaging material. In this case, the content of the acrylic resin particles in the inner adhesive layer 6R was 0.22 g / m 2 .
[0282] <Example 7>
[0283] In Example 1, the outer reinforcing agent is carbon black (CB: number average particle size is 0.05 μm, specific surface area is 45 m 2 / g) and the carbon black content in the outer adhesive composition was 4.8 mass %, and the coating amount of the outer adhesive composition was 6.5 g / m 2 , except for this, the tensile test of the cured film of the outer adhesive composition was carried out in the same manner as in Example 1, and the outer surface of the aluminum foil was bonded to the inner surface of the biaxially stretched nylon film (heat-resistant resin layer 3), and the composition was cured by aging at 60°C. In this case, the carbon black content in the outer adhesive layer 5R was 0.31 g / m 2 .
[0284] Next, a film was prepared in which the inner adhesive (main agent) was acrylic polyol (a type of acrylic adhesive (main agent)) and the inner reinforcing agent was silica particles (SiO2 particles: number average particle size of 0.2 μm, specific surface area of 25 m 2 / g), and the content of silica particles in the inner adhesive composition is 7.5% by mass. Then, the inner adhesive composition is heated at 5.5 g / m 2 The inner surface of the aluminum foil was coated with a coating amount of 0.41 g / m2 to dry and evaporate the solvent in the composition. Then, the inner surface of the aluminum foil was bonded to the outer surface of the unstretched three-layer coextruded polypropylene film (thermo-fusible resin layer 4) and aged at 40°C to cure the composition. In this case, the content of the silica particles in the inner adhesive layer 6R was 0.41 g / m2. 2 In addition, in the same manner as in Example 1, a tensile test of the cured film of the inner adhesive composition was performed.
[0285] Next, a matte coating layer 7 is formed on the outer surface of the biaxially stretched nylon film (heat-resistant resin layer 3) by the following method.
[0286] That is, 70 parts by mass of fluoroethylene-acrylic acid ester copolymer as a heat-resistant resin, 10 parts by mass of barium sulfate particles (number average particle size of 2.0 μm) and 10 parts by mass of silica particles (number average particle size of 1.0 μm) as inorganic particles, 5 parts by mass of polytetrafluoroethylene wax (number average particle size of 10.0 μm) as wax, and 5 parts by mass of polyethylene resin particles (number average particle size of 5.0 μm) as organic particles (organic beads) were mixed to prepare a matte coating composition. Then, the matte coating composition was applied in a layered manner to a thickness of 2 μm after drying on the outer surface of a biaxially stretched nylon film, and aged for 5 days at 40° C., thereby forming a matte coating layer 7 (thickness of 2 μm) on the outer surface of the biaxially stretched nylon film.
[0287] The packaging material was manufactured by the above method.
[0288] <Example 8>
[0289] The black colored layer 8 was formed on the inner surface of the biaxially stretched nylon film (heat-resistant resin layer 3) by the following method.
[0290] That is, to a resin composition having a total content of 75% by mass of ethylenediamine, polyester polyol and toluene diisocyanate curing agent, carbon black (CB) having a number average particle size of 0.4 μm is added in such a manner that the content of carbon black becomes 25% by mass, and the mixture is uniformly mixed and dispersed to prepare a black ink. Then, the black ink is applied in layers to the inner surface of a biaxially stretched nylon film using a gravure roller and dried. The film is further placed under a 40°C environment for 1 day, thereby performing a cross-linking reaction while drying. Thus, a black coloring layer 8 (3 μm in thickness) is formed on the inner surface of the biaxially stretched nylon film.
[0291] Next, at 5.0 g / m 2 The same outer adhesive composition as in Example 1 is applied in a layer on the outer surface of the aluminum foil with a coating amount of, the solvent in the composition is dried and evaporated, and then the outer surface of the aluminum foil is bonded to the inner surface of the biaxially stretched nylon film (i.e., the black coloring layer 8) and aged at 60°C to cure the composition.
[0292] Next, the same acrylic adhesive as in Example 7 and carbon black (CB: number average particle size of 0.01 μm, specific surface area of 420 m 2 / g) of acrylic resin adhesive composition (i.e., inner adhesive composition containing carbon black), at 6.0 g / m 2The inner surface of the aluminum foil is coated with a coating amount of 0.48 g / m2 and the solvent in the composition is dried and evaporated. Then, the inner surface of the aluminum foil is bonded to the outer surface of the unstretched three-layer coextruded polypropylene film (thermo-fusible resin layer 4) and aged at 40°C to cure the composition. In this case, the carbon black content in the inner adhesive layer 6R is 0.48 g / m2. 2 In addition, in the same manner as in Example 1, a tensile test of the cured film of the inner adhesive composition was performed.
[0293] Next, a matte coating layer 7 was formed on the outer surface of the biaxially stretched nylon film by the same method as in Example 7, thereby producing a packaging material.
[0294] <Example 9>
[0295] A black colored layer 8 (3 mm in thickness) was formed on the inner surface of the biaxially stretched nylon film (heat-resistant resin layer 3) by the same method as in Example 8 using the same black ink as in Example 8.
[0296] Next, a two-component curable polyester urethane resin as in Example 1 was added as an outer adhesive in such a manner that the content of the silica particles was 4.3% by mass, and silica particles (SiO2 particles: number average particle size of 0.4 μm, specific surface area of 10 m 2 / g) of polyester urethane resin adhesive composition (i.e., outer adhesive composition containing silica particles), at 6.5 g / m 2 The outer surface of the aluminum foil is coated with a coating amount of 0.28 g / m 2 and the solvent in the composition is dried and evaporated. Then, the outer surface of the aluminum foil is bonded to the inner surface of the biaxially stretched nylon film (i.e., the black colored layer 8) and aged at 60° C. to cure the composition. In this case, the content of the silica particles in the outer adhesive layer 5R is 0.28 g / m 2. 2 In addition, in the same manner as in Example 1, a tensile test of the cured film of the outer adhesive composition was performed.
[0297] Next, the same acrylic adhesive as in Example 7 and carbon black (CB: number average particle size of 0.01 μm, specific surface area of 420 m 2 / g) of acrylic resin adhesive composition (i.e., inner adhesive composition containing carbon black), at 6.5 g / m 2The inner surface of the aluminum foil is coated with a coating amount of 0.20 g / m2 and the solvent in the composition is dried and evaporated. Then, the inner surface of the aluminum foil is bonded to the outer surface of the unstretched three-layer coextruded polypropylene film (thermo-fusible resin layer 4) and aged at 40°C to cure the composition. In this case, the carbon black content in the inner adhesive layer 6R is 0.20 g / m2. 2 In addition, in the same manner as in Example 1, a tensile test of the cured film of the inner adhesive composition was performed.
[0298] Next, a matte coating layer 7 was formed on the outer surface of the biaxially stretched nylon film by the same method as in Example 7, thereby producing a packaging material.
[0299] <Example 10>
[0300] A black colored layer 8 (3 mm in thickness) was formed on the inner surface of the biaxially stretched nylon film (heat-resistant resin layer 3) by the same method as in Example 8 using the same black ink as in Example 8.
[0301] Next, at 5.0 g / m 2 The same outer adhesive composition as in Example 1 is applied in a layer on the outer surface of the aluminum foil with a coating amount of, the solvent in the composition is dried and evaporated, and then the outer surface of the aluminum foil is bonded to the inner surface of the biaxially stretched nylon film (i.e., the black coloring layer 8) and aged at 60°C to cure the composition.
[0302] Next, the same acrylic adhesive as in Example 7 and calcium carbonate particles (CaCO particles: number average particle size of 0.02 μm, specific surface area of 210 m2) as an inner reinforcing agent were contained in a manner such that the content of calcium carbonate particles was 9.0 mass %. 2 / g) of acrylic resin adhesive composition (i.e., inner adhesive composition containing calcium carbonate particles), at 7.5 g / m 2 The inner surface of the aluminum foil is coated with a coating amount of 0.68 g / m2 and the solvent in the composition is dried and evaporated. Then, the inner surface of the aluminum foil is bonded to the outer surface of the unstretched three-layer coextruded polypropylene film (thermo-fusible resin layer 4) and aged at 40°C to cure the composition. In this case, the content of calcium carbonate particles in the inner adhesive layer 6R is 0.68 g / m2. 2 In addition, in the same manner as in Example 1, a tensile test of the cured film of the inner adhesive composition was performed.
[0303] Next, a matte coating layer 7 was formed on the outer surface of the biaxially stretched nylon film by the same method as in Example 7, thereby producing a packaging material.
[0304] <Comparative Example 1>
[0305] In Example 1, except that the inner reinforcing agent was not contained in the inner adhesive layer, the tensile test of the cured film of each adhesive composition was carried out in the same manner as in Example 1, and a packaging material was produced.
[0306] <Comparative Example 2>
[0307] In Example 1, the inner reinforcing agent is silica particles (SiO2 particles: number average particle size of 4.0 μm, specific surface area of 1.0 m 2 / g) and the content of the silica particles in the inner adhesive composition containing the silica particles was 3.5% by mass, and the coating amount of the inner adhesive composition was 6.5 g / m 2 , except for this, the same operation as in Example 1 was performed to conduct a tensile test of the cured film of the inner adhesive composition and to manufacture a packaging material. In this case, the content of the silica particles in the inner adhesive layer 6R was 0.23 g / m 2 .
[0308] <Comparative Example 3>
[0309] In Example 8, the inner adhesive layer did not contain the inner reinforcing agent, and the coating amount of the inner adhesive layer was 6.5 g / m 2 , except for this, the same operation as in Example 8 was carried out to perform a tensile test on the cured film of the inner adhesive composition and to produce a packaging material.
[0310] <Comparative Example 4>
[0311] In Example 8, the inner reinforcing agent is calcium carbonate particles (CaCO3 particles: number average particle size of 3.0 μm, specific surface area of 0.8 m 2 / g) and the content of calcium carbonate particles in the inner adhesive composition containing calcium carbonate particles is 4.5% by mass, and the coating amount of the inner adhesive composition is 4.5 g / m 2 , except for this, the same operation as in Example 8 was performed to conduct a tensile test of the cured film of the inner adhesive composition and to manufacture a packaging material. In this case, the content of calcium carbonate particles in the inner adhesive layer 6R was 0.20 g / m 2 .
[0312] (Measurement method of specific surface area)
[0313] Here, in Examples 1 to 10 and Comparative Examples 1 to 4, the specific surface areas of the inner reinforcing agent (inner reinforcing particles) and the outer reinforcing agent (outer reinforcing particles) were measured by the following method in accordance with JIS Z8330:2013.
[0314] That is, the enhancer was weighed and the pore distribution was measured using a gas adsorption type pore distribution measuring instrument (NOVA4200e: Seishin Enterprise Co., Ltd.) by using a N2 gas purge method (gas flow rate of 20 cm 3 / min, gas pressure of 20 kPa, heating temperature of 200°C, and treatment time of 2 hours) were used to pretreat the weighed reinforcing agent, and then the specific surface area of the reinforcing agent was measured by the BET multi-point method.
[0315] (Method for calculating number average particle size)
[0316] The number average particle size of the inner reinforcing particles and the outer reinforcing particles is determined by the following method.
[0317] A suspension of inner reinforcing particles was prepared, and the particle size distribution of the inner reinforcing particles was measured using a laser diffraction / scattering particle size distribution measuring apparatus (Partica LA-960V2: Horiba, Ltd.) to determine the number average particle size of the inner reinforcing particles. The number average particle size of the outer reinforcing particles was determined in the same manner.
[0318] (Evaluation of packaging materials)
[0319] The packaging materials of Examples 1 to 10 and Comparative Examples 1 to 4 were subjected to puncture strength measurement and moldability test. The results are shown in Tables 1 and 2 below.
[0320] [Table 1]
[0321]
[0322] [Table 2]
[0323]
[0324] <Punch Strength>
[0325] The puncture strength of the packaging material is measured in accordance with JIS Z1707: 2019. The puncture strength test at this time is performed according to the following steps 1 and 2.
[0326] Step 1: Fix the test piece collected from the packaging material with a fixture, and pierce a semicircular needle with a diameter of 1.0 mm and a tip radius of 0.5 mm from the heat-resistant resin layer side at a test speed of 50±5 mm / min, and measure the maximum force (N) until the needle penetrates.
[0327] Step 2: The number of test pieces collected from the packaging material is set to 5 or more, and the test pieces are collected so as to be averaged over the entire width of the packaging material.
[0328] The meanings of the symbols in the "Piercing Strength" column in Tables 1 and 2 are as follows: ◎ and ○ were regarded as passing the piercing strength test.
[0329] ◎: Puncture strength greater than 19N
[0330] ○: Puncture strength greater than 16N and less than 19N
[0331] ×: The puncture strength is 16N or less.
[0332] <Molding processability test>
[0333] A press machine manufactured by AMAD A Co., Ltd. was prepared, which was provided with a die having a punch shape of 33 mm×54 mm, a punch corner R of 2 mm, a punch shoulder R of 1.3 mm, and a die shape of a die shoulder R of 1 mm.
[0334] Then, a rectangular test plate of 100 mm in length and 125 mm in width was collected from the packaging material, and the test plate was deep-drawn using the above-mentioned press machine to form a formed product.
[0335] The presence or absence of pinholes and cracks in the corners of the molded product was confirmed by the transmitted light method in a dark room, and the "maximum molding depth (mm)" without pinholes and cracks was investigated to evaluate the molding processability of the packaging material. The evaluation criteria are as follows. It should be noted that ◎ and ○ are considered to be qualified in the molding processability test.
[0336] ◎: No cracks or pinholes when the maximum forming depth is 7mm or more
[0337] ○: No cracks or pinholes when the maximum forming depth is 6 mm or more and less than 7 mm
[0338] ×: There are cracks and / or pinholes when the maximum forming depth is less than 6 mm.
[0339] As can be seen from Tables 1 and 2, it was confirmed that the packaging materials of Examples 1 to 10 using the inner reinforcing particles satisfying the above requirements 1 and 2 had high puncture strength.
[0340] Furthermore, it can be confirmed that, as in Examples 1, 2, and 4 to 10, the coating amount of the inner adhesive layer 6R is 2 g / m 2 ~10g / m 2 The content of the inner reinforcing agent in the inner adhesive layer 6R is within the range of 0.2 g / m 2 ~1.0g / m 2 When it is within the range of , the improvement rate ΔL1 of the tensile elongation at break is large, so the molding processability of the packaging material is high.
[0341] This application claims priority to Japanese Patent Application No. 2022-169759 filed on October 24, 2022 and Japanese Patent Application No. 2023-145339 filed on September 7, 2023, the disclosures of which directly constitute a part of this application.
[0342] The terms and expressions used herein are for explanation and are not intended to be interpreted in a limiting sense. Any equivalents of the features shown and described herein are not excluded. It should be understood that various modifications are allowed within the scope of the claims of the present utility model.
[0343] Industrial Applicability
[0344] The utility model can be used in packaging materials, packaging shells and power storage devices for molding processing.
Claims
1. A packaging material for molding, comprising a metal foil layer, a heat-resistant resin layer disposed on the outer surface side of the metal foil layer, and a heat-fusible resin layer disposed on the inner surface side of the metal foil layer, characterized in that: An outer adhesive layer is provided between the metal foil layer and the heat-resistant resin layer, and an inner adhesive layer is provided between the metal foil layer and the heat-fusible resin layer. The inner adhesive layer contains an inner reinforcing agent, As the inner reinforcing agent, inner reinforcing particles satisfying the following requirements 1 and 2 are used. Requirement 1: The number average particle size of the inner reinforcing particles is in the range of 0.01 μm to 3 μm; Requirement 2: The specific surface area of the inner reinforcing particles is 1 m 2 / g or above.
2. The packaging material for molding processing according to claim 1, wherein The inner adhesive layer is formed of a cured film of an inner adhesive composition containing an inner adhesive and the inner reinforcing agent. The tensile elongation at break of the cured film of the inner adhesive composition is defined as L1. When the tensile elongation at break of a cured film of an inside adhesive composition containing the inside adhesive but not containing the inside reinforcing agent is defined as L10, The L1 satisfies the following relation 1, 15%≤{(L1-L10) / L10}×100%≤250%…(Formula 1).
3. The packaging material for molding processing according to claim 1 or 2, wherein: The inner adhesive layer is 2g / m 2 ~10g / m 2 A coating amount in a range of is provided between the metal foil layer and the thermally fusible resin layer, The content of the inner reinforcing agent in the inner adhesive layer is 0.2 g / m 2 ~1.0g / m 2 within the range.
4. The packaging material for molding processing according to claim 1 or 2, wherein: The outer adhesive layer contains an outer reinforcing agent, As the outer reinforcing agent, outer reinforcing particles satisfying the following requirements 3 and 4 are used. Requirement 3: The number average particle size of the outer reinforcement particles is in the range of 0.01 μm to 3 μm; Requirement 4: The specific surface area of the outer reinforcing particles is 1 m 2 / g or above.
5. The packaging material for molding processing according to claim 4, wherein The outer adhesive layer is formed of a cured film of an outer adhesive composition containing an outer adhesive and the outer reinforcing agent. The tensile elongation at break of the cured film of the outer adhesive composition is defined as L2, When the tensile elongation at break of a cured film of an external adhesive composition containing the external adhesive but not containing the external reinforcing agent is defined as L20, The L2 satisfies the following relational expression 2, 15%≤{(L2-L20) / L20}×100%≤250%…(Formula 2).
6. The packaging shell is characterized in that: The packaging case is formed by deep drawing or stretching the packaging material for molding according to any one of claims 1 to 5.
7. An electric storage device comprising an electric storage device body and a packaging case packaging the electric storage device body, characterized in that: As the packaging case, the packaging case according to claim 6 is provided.