Waterproof photovoltaic cell backboard
By using a combined structure of a weather-resistant layer, a PET composite layer, a water-blocking layer and a black reflective coating on the photovoltaic cell backplane, the outdoor waterproofing and light reflectivity problems of photovoltaic cells are solved, achieving higher light reflectivity and light reflectivity. water capability, extending battery life.
Patent Information
- Application Number
- CN202322972253.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-03
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2033-11-03
AI Technical Summary
Photovoltaic cells are easily damaged by rain when installed outdoors, and existing technology is difficult to improve light reflectivity and waterproofing capabilities at the same time, affecting its power generation efficiency and service life.
A water-blocking photovoltaic cell backsheet structure composed of a weather-resistant layer, a PET composite layer, a water-blocking layer and a black reflective coating is used to enhance the overall performance of the photovoltaic cell by improving the reflectivity and water-blocking ability in the 780-1200nm band.
Significantly improves the light reflectivity and water-blocking ability of the photovoltaic cell backsheet, extending the battery life and improving overall performance.
Smart Images

Figure CN221805546U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to the technical field of photovoltaic power generation, in particular to a water-blocking photovoltaic cell back plate. Background Art
[0002] Photovoltaic cells can convert solar energy into electrical energy and provide clean energy. As energy and environmental issues become increasingly severe, the development of photovoltaic power generation technology has also attracted much attention. In order to improve the utilization rate of solar energy, people are currently committed to improving the light reflection efficiency of battery panels, so that solar energy is more likely to be absorbed by the battery, thereby further improving the power generation efficiency of solar cells.
[0003] Photovoltaic cells include numerous electrical components and need to maintain a dry environment. However, photovoltaic cells are often installed outdoors. When encountering rainy, snowy weather or high humidity, photovoltaic cells are often damaged by rain.
[0004] How to further improve the light reflectivity of photovoltaic cells while improving their waterproof ability has become a technical problem that needs to be solved urgently. Summary of the invention
[0005] The purpose of the utility model is to provide a water-blocking photovoltaic cell back sheet, which can greatly improve the near-infrared reflectivity in the 780-1200nm band and improve the water-blocking ability of the water-blocking photovoltaic cell back sheet, thereby improving the comprehensive performance of the photovoltaic cell. To achieve this purpose, the utility model adopts the following technical solutions:
[0006] A water-blocking photovoltaic cell back plate comprises a weather-resistant layer, a PET composite layer, a water-blocking layer and a black reflective coating layer which are arranged in sequence from outside to inside.
[0007] As an optional solution for the water-blocking photovoltaic cell backsheet, the weather-resistant layer is a weather-resistant film layer or a weather-resistant coating layer;
[0008] The weather-resistant film layer is one of PVDF film, PVF film, PO film, PET film, ETFE film and ECTFE film;
[0009] The weather-resistant coating layer is composed of one or more of polyvinylidene fluoride resin, silicone resin, trifluoro FEV resin, tetrafluoro FEV resin, acrylic resin, fluorine-modified acrylic resin, polyurethane resin, polyester resin, and epoxy resin;
[0010] The thickness of the weather-resistant layer is 10-30um;
[0011] Preferably, a second external bonding layer with a thickness of 0-20 μm is further included between the weather-resistant layer and the composite PET layer;
[0012] Further preferably, when the weather-resistant layer is one of PVDF film, PVF film, PO film, ETFE film and ECTFE film, the thickness of the second external bonding layer is not zero.
[0013] As an optional solution for the water-blocking photovoltaic cell backsheet, the composite PET layer is composed of a PET substrate layer and a PET reflective layer, the PET substrate layer is located on the inner side of the weather-resistant layer, and the water-blocking layer is connected to the PET reflective layer through a first external adhesive layer with a thickness of 5-20 μm;
[0014] The PET reflective layer is a PET film with a reflectivity of 70%-98% at 700-1200nm;
[0015] The thickness of the PET reflective layer is 25-200 μm; the thickness of the PET substrate layer is 100-600 μm.
[0016] As an optional solution for the water-blocking photovoltaic cell back sheet, an internal bonding layer with a thickness of 5-20 μm is further provided between the PET substrate layer and the PET reflective layer.
[0017] As an optional solution for the water-blocking photovoltaic cell backplane, the first external adhesive layer, the second external adhesive layer, and the internal adhesive layer are all one of a polyurethane adhesive layer, an acrylic resin adhesive layer, an epoxy resin adhesive layer, and a polyester adhesive layer.
[0018] As an optional solution for the water-blocking photovoltaic cell backsheet, the water-blocking layer is one of a water-blocking composite layer or a water-blocking coating;
[0019] Preferably, the water-blocking composite layer is composed of a water-blocking functional layer and a first external bonding layer arranged from inside to outside;
[0020] The water-blocking functional layer is formed by curing one or more of an oxide film or graphene, silicon nitride, montmorillonite, mica powder, talc powder, and silazane with a resin;
[0021] The thickness of the water-blocking functional layer is 5-30 μm, and the thickness of the first external bonding layer is 5-20 μm;
[0022] Preferably, the water-blocking coating comprises 95-99 parts of resin, 0.5-2 parts of water-blocking agent, and 1-5 parts of curing agent;
[0023] The water-blocking agent is composed of one or more of oxides, graphene, silicon nitride, montmorillonite, mica powder, talc powder, and silazane.
[0024] As an optional solution for the water-blocking photovoltaic cell backplane, the black reflective coating is composed of 20-45 parts of weather-resistant functional resin, 3-8 parts of curing agent, 1-6 parts of organic and / or inorganic reflective pigment, 1-5 parts of auxiliary agent, and 50-75 parts of solvent (parts by weight);
[0025] Preferably, the black reflective coating has a thickness of 5-20 um.
[0026] As an optional solution for the water-blocking photovoltaic cell backplane, the weather-resistant functional resin includes at least one of polyvinylidene fluoride resin, silicone resin, trifluoro FEV resin, tetrafluoro FEV resin, acrylic resin, fluorine-modified acrylic resin, polyurethane resin, polyester resin, and epoxy resin;
[0027] Preferably, the curing agent includes at least one of an isocyanate curing agent, a melamine curing agent, and a melamine curing agent.
[0028] As an optional solution for the water-blocking photovoltaic cell backplane, the organic reflective pigments include azo, phthalocyanine, heterocyclic compounds, etc.
[0029] Preferably, the organic reflective pigment is one or more of quinacridone copper, dioxazine, phthalocyanine blue, anthraquinone blue, pigment yellow 150, and perylene black;
[0030] Further preferably, the inorganic reflective pigment includes at least one of copper chrome black, iron chrome black, cobalt blue, iron oxide red, titanium nickel yellow, and cobalt green.
[0031] As an optional solution for the water-blocking photovoltaic cell backsheet, the auxiliary agent includes one or more of a catalyst, a dispersant, a leveling agent, a defoaming agent, an anti-settling agent or a matting agent;
[0032] The solvent includes one or more of toluene, xylene, ethyl acetate, butyl acetate, propylene glycol methyl ether acetate, and dimethylformamide.
[0033] Beneficial effects of the utility model:
[0034] The water-blocking photovoltaic cell backboard provided by the utility model utilizes the light reflection function of the black reflective coating and the light reflection ability of the PET reflective layer to improve the light reflection ability of the photovoltaic cell backboard as a whole, and increases the reflectivity of the photovoltaic cell backboard in the 780-1200nm band to 60%-90%; and the provision of the water-blocking layer can greatly improve the water-blocking ability of the water-blocking photovoltaic cell backboard, greatly extending the service life of the photovoltaic cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a structural diagram of a photovoltaic cell backplane provided by a specific embodiment of the utility model;
[0036] Figure 2 This is a structural diagram of a photovoltaic cell backplane provided by another specific embodiment of the utility model;
[0037] In the figure:
[0038] 1. Weathering layer;
[0039] 2. PET composite layer;
[0040] 21. PET substrate layer;
[0041] 22. Internal bonding layer;
[0042] 23. PET reflective layer;
[0043] 3. Water-blocking layer;
[0044] 31. Water-blocking functional layer;
[0045] 32. a first external bonding layer;
[0046] 4. Black reflective coating;
[0047] 5. Second external bonding layer. Implementation
[0048] In order to make the technical problems solved by the present invention, the technical solutions adopted and the technical effects achieved more clearly, the technical solutions of the present invention are further explained below with reference to the accompanying drawings and through specific implementation methods.
[0049] As attached Figure 1 and Figure 2 As shown: This embodiment provides a water-blocking photovoltaic cell backplane, which is composed of a weather-resistant layer 1, a PET composite layer 2, a water-blocking layer 3 and a black reflective coating 4 arranged in sequence;
[0050] In order to protect the internal structure of the photovoltaic cell, prevent air impurities from damaging the cell, and protect the stable environment inside the photovoltaic cell, as an optional solution for the photovoltaic cell panel, the weather-resistant layer 1 is a weather-resistant film layer or a weather-resistant coating layer;
[0051] The weather-resistant film layer is one of PVDF film, PVF film, PO film, PET film, ETFE film and ECTFE film;
[0052] The weather-resistant coating layer is composed of one or more of polyvinylidene fluoride resin, silicone resin, trifluoro FEV resin, tetrafluoro FEV resin, acrylic resin, fluorine-modified acrylic resin, polyurethane resin, polyester resin, and epoxy resin;
[0053] The thickness of the weather-resistant layer 1 is 10-30 um;
[0054] Preferably, a second external bonding layer 5 with a thickness of 0-20 μm is further included between the weather-resistant layer 1 and the composite PET layer 2;
[0055] Further preferably, when the weather-resistant layer 1 is one of PVDF film, PVF film, PO film, ETFE film and ECTFE film, the thickness of the second external bonding layer 5 is not zero.
[0056] In order to improve the support function of the sheet, ensure that the photovoltaic cell has reliable mechanical properties, and improve the light reflection effect, as an optional solution for the photovoltaic cell panel, the PET composite layer 2 is composed of a PET substrate layer 21 and a PET reflective layer 23, the PET substrate layer 21 is located on the inner side of the weather-resistant layer 1, and the water-blocking layer 3 is connected to the PET reflective layer 23;
[0057] The PET reflective layer 23 is a PET film with a reflectivity of 70%-98% at 780-1200nm;
[0058] The thickness of the PET reflective layer 23 is 25-200 μm; the thickness of the PET substrate layer 21 is 100-600 μm.
[0059] In order to improve the water-blocking ability of the water-blocking photovoltaic cell backsheet, the water-blocking layer 3 is a water-blocking composite layer or a water-blocking coating;
[0060] Preferably, the water-blocking composite layer is composed of a water-blocking functional layer 31 and a first external bonding layer 32 arranged from inside to outside;
[0061] The water-blocking functional layer 31 is formed by curing an oxide film or one or more of graphene, silicon nitride, montmorillonite, mica powder, talc powder, and silazane with a resin;
[0062] The thickness of the water-blocking functional layer 31 is 5-30 μm, and the thickness of the first external bonding layer 32 is 5-20 μm;
[0063] Preferably, the water-blocking coating comprises 93-97.5 parts of resin, 0.5-5 parts of water-blocking agent, and 2-6.5 parts of curing agent;
[0064] The water-blocking agent is composed of one or more of oxides, graphene, silicon nitride, montmorillonite, mica powder, talc powder, and silazane;
[0065] The thickness of the water-blocking coating is 5-30 μm.
[0066] In order to improve the light reflection ability of the photovoltaic cell backplane, as an optional solution for the photovoltaic cell panel, the black reflective coating 4 is composed of 20-45 parts of weather-resistant functional resin, 3-8 parts of curing agent, 1-6 parts of organic and / or inorganic reflective pigment, 1-5 parts of auxiliary agent, and 50-75 parts of solvent (parts by weight);
[0067] The thickness of the black reflective coating 4 is 5-20um;
[0068] The weather-resistant functional resin includes at least one of polyvinylidene fluoride resin, silicone resin, trifluoro FEV resin, tetrafluoro FEV resin, acrylic resin, fluorine-modified acrylic resin, polyurethane resin, polyester resin, and epoxy resin;
[0069] Preferably, the curing agent includes at least one of an isocyanate curing agent, a melamine curing agent, and a melamine curing agent.
[0070] The organic reflective pigments include azo, phthalocyanine, heterocyclic compounds, etc.
[0071] Preferably, the organic reflective pigment is one or more of quinacridone copper, dioxazine, phthalocyanine blue, anthraquinone blue, pigment yellow 150, and perylene black;
[0072] Further preferably, the inorganic reflective pigment includes at least one of copper chrome black, iron chrome black, cobalt blue, iron oxide red, titanium nickel yellow, and cobalt green.
[0073] The auxiliary agent includes one or more of a catalyst, a dispersant, a leveling agent, a defoaming agent, an anti-settling agent or a matting agent;
[0074] The solvent includes one or more of toluene, xylene, ethyl acetate, butyl acetate, propylene glycol methyl ether acetate, and dimethylformamide.
[0075] In order to achieve a stable connection to the photovoltaic cell backsheet and improve the overall performance of the photovoltaic cell backsheet, as an optional solution for the photovoltaic cell panel, the first external bonding layer 32, the second external bonding layer 5, and the internal bonding layer 22 all include at least one of a polyurethane adhesive layer, an acrylic resin adhesive layer, an epoxy resin adhesive layer, or a polyester adhesive layer;
[0076] The technical solution of the present invention is further described below by specific implementation methods. Those skilled in the art should understand that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0077] The auxiliary materials used in this utility model are as follows:
[0078] Catalyst: PU-20, T-25;
[0079] Matting agent: Grace C803, Evonik OK-500;
[0080] Dispersant: BYK9010, EFKA4401;
[0081] Leveling agent: Digo 496, FLOW300;
[0082] Anti-settling agent: BYK-410, BYK-420;
[0083] Defoaming agent: BYK-A500, BYK-066N. Example
[0084] A water-blocking photovoltaic cell backplane comprises a weather-resistant layer 1, wherein the weather-resistant layer 1 is a polyvinylidene fluoride resin coating with a thickness of 10 μm; the weather-resistant layer 1 is connected to a PET composite layer 2, wherein the PET composite layer 2 comprises a 150 μm PET substrate layer 21 and a 35 μm PET reflective layer 23, wherein the PET reflective layer 23 is a PET film with a reflectivity of 90% at 780-1200 nm; the PET reflective layer 23 is connected to a water-blocking functional layer 31 via a first external bonding layer 32, wherein the first external bonding layer 32 is an acrylic resin adhesive; the water-blocking functional layer 31 is an aluminum oxide film with a thickness of 15 μm; and the other side of the water-blocking functional layer 31 is a black reflective coating 4.
[0085] Among them, the black reflective coating includes:
[0086] 40 parts of weather-resistant functional resin, specifically, the weather-resistant functional resin is fluorocarbon resin;
[0087] 4 parts of a curing agent, specifically, the curing agent is a melamine curing agent;
[0088] 3 parts of organic reflective pigment, specifically, the organic reflective pigment is a mixture of perylene black and dioxazine violet, and the addition ratio of perylene black to dioxazine violet is 5:1;
[0089] 3 parts of additives, specifically, the additives are a mixture of Grace OK500, EFKA4401, and FLOW300, and the addition ratio of Grace OK500, EFKA4401, and FLOW300 is 2:3:1;
[0090] 50 parts of solvent, wherein the solvent is butyl acetate. Example
[0091] A water-blocking photovoltaic cell backsheet, comprising a weather-resistant layer 1, wherein the weather-resistant layer 1 is a polyvinylidene fluoride film with a thickness of 20 μm; the weather-resistant layer 1 is connected to a PET composite layer 2 via a second external adhesive layer 5 with a thickness of 15 μm, wherein the PET composite layer 2 comprises a PET substrate layer 21 with a thickness of 300 μm and a PET reflective layer 23 with a thickness of 120 μm, wherein the PET reflective layer 23 is a PET film with a reflectivity of 75% at 700-1200 nm, and the PET reflective layer 23 is connected to a water-blocking layer 3, wherein the water-blocking layer 3 is a graphene water-blocking coating with a thickness of 20 μm, and the other side of the water-blocking layer 3 is a black reflective coating 4;
[0092] Among them, the black reflective coating includes:
[0093] 20 parts of weather-resistant functional resin, specifically, the weather-resistant functional resin is a mixture of acrylic resin and amino resin, and the addition ratio of the acrylic resin to the amino resin is 1:2;
[0094] 5 parts of a curing agent, specifically, the curing agent is an isocyanate curing agent;
[0095] 2 parts of organic reflective pigment, specifically, the organic reflective pigment is a phthalocyanine pigment;
[0096] 1 part of an inorganic reflective pigment, specifically, the inorganic reflective pigment is copper chrome black;
[0097] 4 parts of additives, specifically, the additives are a mixture of BYK-A500, PU-20, and EFKA4401, and the addition ratio of BYK-A500, PU-20, and EFKA4401 is 1:1:1;
[0098] 68 parts of solvent, wherein the solvent is propylene glycol methyl ether acetate. Example
[0099] A photovoltaic cell backplane comprises a weather-resistant layer 1, wherein the weather-resistant layer 1 is a PVDF film; the weather-resistant layer 1 is connected to a PET composite layer 2 via a second external bonding layer 5, wherein the PET composite layer 2 comprises a PET reflective layer 23 with a thickness of 150 μm and a PET substrate layer 21 with a thickness of 500 μm, wherein the PET reflective layer 23 and the PET substrate layer 21 comprise an internal bonding layer 22; the PET reflective layer 23 is a PET film with a reflectivity of 80% at 700-1200 nm; the PET reflective layer 23 is connected to a water-blocking layer 3, wherein the second external bonding layer 5 and the internal bonding layer are both polyester adhesives; the water-blocking layer 3 is a montmorillonite water-blocking coating with a thickness of 10 μm, and the other side of the water-blocking layer 3 is a black reflective coating 4.
[0100] Among them, the black reflective coating includes:
[0101] 40 parts of weather-resistant functional resin, specifically, the weather-resistant functional resin is epoxy resin;
[0102] 8 parts of a curing agent, specifically, the curing agent is a mixture of an isocyanate curing agent and a melamine curing agent, and the addition ratio of the isocyanate curing agent to the melamine curing agent is 2:1;
[0103] 3 parts of an organic reflective pigment, specifically, the organic reflective pigment is perylene black;
[0104] 1 part of an inorganic reflective pigment, specifically, the inorganic reflective pigment is cobalt blue;
[0105] 1 part of an additive, specifically, the additive is a mixture of BYK-420 and Digo 496, and the addition ratio of BYK-420 to Digo 496 is 3:1;
[0106] 47 parts of a solvent, wherein the solvent is butyl acetate.
[0107] The above contents are only preferred embodiments of the present invention. For ordinary technicians in this field, according to the concept of the present invention, there will be changes in the specific implementation methods and application scopes. The contents of this specification should not be understood as limiting the present invention.
Claims
1. A water-blocking photovoltaic cell back sheet, characterized in that: The water-blocking photovoltaic cell back plate is composed of a weather-resistant layer, a PET composite layer, a water-blocking layer and a black reflective coating layer which are arranged in sequence from the outside to the inside.
2. The water-blocking photovoltaic cell back sheet according to claim 1, characterized in that: The weather-resistant layer is a weather-resistant film layer or a weather-resistant coating layer; The weather-resistant film layer is one of PVDF film, PVF film, PO film, PET film, ETFE film and ECTFE film; The thickness of the weather-resistant layer is 10-30 um.
3. The water-blocking photovoltaic cell back sheet according to claim 1, characterized in that: A second external bonding layer with a thickness of 0-20 μm is also included between the weather-resistant layer and the PET composite layer.
4. The water-blocking photovoltaic cell back sheet according to claim 1, characterized in that: When the weather-resistant layer is one of PVDF film, PVF film, PO film, ETFE film and ECTFE film, the thickness of the second external bonding layer is not zero.
5. The water-blocking photovoltaic cell back sheet according to claim 1, characterized in that: The PET composite layer is composed of a PET base layer and a PET reflective layer, the PET base layer is located inside the weather-resistant layer, and the water-blocking layer is connected to the PET reflective layer; The PET reflective layer is a PET film with a reflectivity of 70%-98% at 780-1200nm; The thickness of the PET reflective layer is 25-200 μm; the thickness of the PET substrate layer is 100-600 μm.
6. The photovoltaic cell back sheet according to claim 5, characterized in that: An internal bonding layer with a thickness of 5-20 μm is also arranged between the PET substrate layer and the PET reflective layer.
7. The photovoltaic cell back sheet according to claim 1, characterized in that: The water-blocking layer is a water-blocking composite layer or a water-blocking coating.
8. The photovoltaic cell back sheet according to claim 7, characterized in that: The water-blocking composite layer is composed of a water-blocking functional layer and a first external bonding layer arranged from inside to outside.
9. The photovoltaic cell back sheet according to claim 4, characterized in that: The second external adhesive layer is one of a polyurethane adhesive layer, an acrylic resin adhesive layer, an epoxy resin adhesive layer, and a polyester adhesive layer.
10. The photovoltaic cell back sheet according to claim 6, characterized in that: The internal bonding layer is one of a polyurethane adhesive layer, an acrylic resin adhesive layer, an epoxy resin adhesive layer, and a polyester adhesive layer.
11. The photovoltaic cell back sheet according to claim 8, characterized in that: The first external adhesive layer is one of a polyurethane adhesive layer, an acrylic resin adhesive layer, an epoxy resin adhesive layer, and a polyester adhesive layer.