Titanium dioxide filler for nylon as well as preparation method and application of titanium dioxide filler
By coating alumina and SiO2 on the surface of titanium dioxide and grafting PA6 oligomers, the degradation problem of titanium dioxide filler in polymer matrix is solved, the light reflectivity and mechanical properties are improved, and it is suitable for the preparation of high reflectivity PPA materials. .
Patent Information
- Application Number
- CN202411113983.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-22
AI Technical Summary
The titanium dioxide filler used in existing polymer matrix materials is easily catalyzed under the action of sunlight, water and oxygen, resulting in yellowing, powdering and loss of light from the resin matrix. The commonly used coupling agent cannot effectively improve the TiO2 and polymer matrix. Compatibility and dispersion affect the light reflectivity and mechanical properties of the material.
Using multi-layer inorganic and organic coating mechanism, first coat alumina on the surface of titanium dioxide, then coat SiO2 and etching to prepare a porous structure, and finally graft PA6 oligomer to improve the dispersion and light reflection ability of TiO2 in the nylon matrix , reduce photocatalytic activity.
The titanium dioxide filler for nylon with low photocatalytic activity, high light reflectivity and high dispersion has been achieved, which improves the weather resistance and mechanical properties of the composite material, and is suitable for the preparation of high reflectivity PPA materials.
Smart Images

Figure BDA0004993111320000061 
Figure BDA0004993111320000071 
Figure BDA0004993111320000072
Abstract
Description
Technical Field
[0001] The invention relates to the field of polymer composite materials, and in particular to a titanium dioxide filler for nylon and a preparation method and application thereof. Background Art
[0002] LED has the advantages of energy saving, environmental protection, long life and small size, and is widely used in various indication, display, decoration and lighting fields. However, LED lights have the problem of brightness decreasing after a long period of use. In order to solve the above problem, in addition to improving the performance of LED chips, we can also start from improving the whiteness and reflectivity of the bracket.
[0003] LED brackets are mainly made of polymer materials and metals through stamping, injection molding, and cutting and folding. Therefore, the polymer materials used in LEDs need to meet the performance requirements of high temperature resistance, dimensional stability, and aging resistance. Currently, commonly used materials include EMC (thermosetting epoxy resin), PCT (polyethylene terephthalate), LCP (liquid crystal polymer), and PPA (polyphthalamide). Compared with the first three, PPA takes into account both initial whiteness and excellent mechanical properties. Among them, PA9T and PA10T have better processing performance and dimensional stability, so they are suitable for manufacturing precision parts. PA9T is a high-temperature resistant nylon developed by Japan, and the current market price is relatively high; PA10T is a high-temperature resistant nylon independently developed by my country, with performance comparable to PA9T.
[0004] Titanium dioxide (TiO2) is a widely used white pigment with excellent hiding power, whiteness and light reflectivity. However, TiO2 has strong photoactivity. When exposed to sunlight, water and oxygen, it will catalytically degrade the polymer matrix material, causing the resin matrix to turn yellow, pulverize and lose gloss. Therefore, inorganic materials such as silicon, aluminum and zirconium are often coated on the surface of TiO2 to cover up its lattice defects and reduce its photocatalytic ability. However, after the TiO2 surface is coated with inorganic materials, the reflection ability of TiO2 to visible light will be reduced at the same time. Further coating the TiO2 surface with a porous film can improve the reflection and scattering ability of visible light.
[0005] In the process of preparing nano-titanium dioxide composite materials, nano-TiO2 is prone to agglomeration when melt-blended with polymers due to its small particle size, large specific surface area, and high surface energy. Therefore, coupling agents are often used to organically modify the surface of TiO2 to improve the compatibility and dispersibility of TiO2 with polymer matrices. However, the commonly used coupling agents have short organic chains and often have only a small number of functional groups that can interact with the matrix, which has limited effect in improving the compatibility of TiO2 with polymer matrices.
[0006] The present invention intends to adopt a multi-layer inorganic and organic coating mechanism to prepare a TiO2 filler for nylon with low photocatalytic activity, high light reflectivity and high dispersibility. Summary of the invention
[0007] The present invention provides a titanium dioxide filler for nylon and a preparation method and application thereof. The present invention first coats alumina (Al2O3) on the surface of titanium dioxide (TiO2) to reduce the photocatalytic ability of TiO2; then coats SiO2 and etches to prepare a porous structure of TiO2@Al2O3@v-SiO2 to further improve the light reflection ability of the inorganic filler; finally, grafts PA6 oligomers to increase the interaction force with the polymer, improves the dispersibility of the modified TiO2 in the nylon matrix, further improves the light reflection ability of TiO2, and the mechanical properties of the composite material.
[0008] The technical solution of the present invention is as follows:
[0009] A method for preparing titanium dioxide filler for nylon comprises the following steps:
[0010] (1) adjusting the pH of TiO2 aqueous dispersion to 9, adding Al2(SO4)3·18H2O aqueous solution dropwise at 60-90°C and stirring for 0.5-2h, then standing at 50-90°C for 1-5h, filtering, washing (with deionized water), and drying (80°C for more than 2h) to obtain TiO2@Al2O3 (alumina-coated titanium dioxide);
[0011] Preferably, TiO2 is in the rutile crystal form with a size of 200 to 400 nm;
[0012] The mass ratio of TiO2 to Al2(SO4)3·18H2O is 3:1 to 1:1, with the optimum being 2:1;
[0013] The concentration of the TiO2 aqueous dispersion is preferably 30 g / 100 mL; the pH is adjusted to 9 using a 10% NaOH aqueous solution and a 10% HCl aqueous solution;
[0014] The preferred concentration of Al2(SO4)3·18H2O aqueous solution is 30 g / 100 mL;
[0015] (2) dispersing TiO2@Al2O3 in a mixed solvent of ammonium hydroxide, deionized water and ethanol to obtain a TiO2@Al2O3 dispersion, dropping tetraethyl orthosilicate (TEOS) into the TiO2@Al2O3 dispersion and stirring it evenly, then standing it at 50-70°C for 1-3 hours, centrifuging it (7000 rpm, 30 minutes), washing the precipitate (with deionized water), and drying it (80°C, more than 2 hours) to obtain TiO2@Al2O3@SiO2;
[0016] Preferably, the volume ratio of ammonium hydroxide, deionized water and ethanol in the mixed solvent is 1:4:10;
[0017] The preferred concentration of TiO2@Al2O3 dispersion is 3g / 100mL;
[0018] The mass ratio of ethyl orthosilicate to TiO2@Al2O3 is 1:2 to 2:1;
[0019] (3) Dispersing TiO2@Al2O3@SiO2 in a polyvinyl pyrrolidone (PVP) aqueous solution to obtain a TiO2@Al2O3@SiO2 dispersion, standing at 80-100°C for 3-5 hours to load the polyvinyl pyrrolidone on the surface of TiO2@Al2O3@SiO2, then cooling to room temperature, adding a NaOH aqueous solution to the TiO2@Al2O3@SiO2 dispersion, etching SiO2 for 1-4 hours (optimally 2 hours), then washing (with deionized water), and drying (80°C, 2 hours or more) to obtain TiO2@Al2O3@v-SiO2;
[0020] Preferably the concentration of the polyvinyl pyrrolidone aqueous solution is 10 g / 100 mL;
[0021] The concentration of the TiO2@Al2O3@SiO2 dispersion is preferably 3 to 10 g / 100 mL;
[0022] The preferred concentration of NaOH aqueous solution is 10 g / 100 mL;
[0023] Preferably, the volume ratio of the NaOH aqueous solution to the PVP aqueous solution is 1:1 to 1:3;
[0024] (4) placing TiO2@Al2O3@v-SiO2 in a high-speed mixer, adding a coupling agent solution containing an amino group and stirring, followed by washing (with deionized water) and drying (80°C, more than 2 hours) to obtain amino-treated TiO2@Al2O3@v-SiO2;
[0025] The coupling agent containing terminal amino group is selected from one or more of KH-550, A-1110, A-1120, KBM-603 and KBM-602;
[0026] In the solution of the coupling agent containing terminal amino groups, the solvent is ethanol and water; preferably, the mass ratio of the coupling agent containing terminal amino groups, ethanol and water is 10:50:50;
[0027] The mass ratio of the coupling agent containing terminal amino groups to TiO2@Al2O3@v-SiO2 is 1:100 to 5:100, with the optimal value being 2:100;
[0028] The stirring speed of the high-speed mixer is preferably 1000 to 2000 rpm / min, and the stirring time is 5 to 10 min;
[0029] (5) melting caprolactam (CL), adding aminated TiO2@Al2O3@v-SiO2 and a catalyst to carry out polymerization reaction, and vacuum dehydration at the same time. After the polymerization is completed, PA6-modified TiO2@Al2O3@v-SiO2, i.e., the titanium dioxide filler for nylon, is obtained;
[0030] Caprolactam is analytically pure and preferably melts at 100°C;
[0031] The mass ratio of caprolactam to amination TiO2@Al2O3@v-SiO2 is 15:85 to 20:80;
[0032] The catalyst is sodium hydroxide, and the preferred molar ratio of the catalyst to caprolactam is 2:10;
[0033] Preferably, the vacuum is evacuated to below -0.085 MPa for dehydration;
[0034] The polymerization reaction temperature is 230-250°C, optimally 240°C, and the polymerization reaction time is 1-2h.
[0035] The invention relates to a titanium dioxide filler for nylon prepared by the preparation method, and the filler can be used in PPA (polyphthalamide).
[0036] The present invention also relates to a high reflectivity PPA, which has the following formula: 69-79wt% of PPA resin, 20-30wt% of PA6-modified TiO2@Al2O3@v-SiO2 (i.e., the titanium dioxide filler for nylon described in the present invention), and 0.5-1wt% of antioxidant; all components add up to 100wt%;
[0037] PPA resin is selected from one or more high temperature resistant nylons such as PA9T and PA10T;
[0038] The antioxidant is a compound of a hindered phenol antioxidant and a phosphite antioxidant; the best one is a combination of N,N-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine and tris(2,4-di-tert-butyl)phenyl phosphite, and the mass ratio of the two is 1:1 to 2:1.
[0039] The preparation method of the high reflectivity PPA of the present invention is as follows:
[0040] (1) Before sample preparation, each raw material component was placed in an oven at 80-120°C and dried for 4-12 hours to remove moisture;
[0041] (2) According to the formula, the dried PPA, antioxidant and PA6-modified TiO2@Al2O3@v-SiO2 were placed in a high-speed mixer and mixed at a speed of 1500 rpm for 5 min to complete the premix;
[0042] (3) The premix was extruded into granules by an extruder at a temperature of 320-330° C. and a screw speed of 80 rpm, and then a specimen was prepared by an injection molding machine at a temperature of 320-330° C. and an injection molding pressure of 60 bar.
[0043] The advantages of the present invention are:
[0044] 1. Using Al2O3 to wrap TiO2 can cover up TiO2 lattice defects, effectively reduce the photocatalytic performance of the material, and improve the weather resistance of the prepared composite material. At the same time, wrapping SiO2 with etched holes on the surface of TiO2@Al2O3 can effectively improve the material's reflectivity to visible light.
[0045] 2. Amino-functionalized TiO2@Al2O3@v-SiO2 was polymerized with caprolactam to prepare PA6-modified TiO2@Al2O3@v-SiO2 composite materials, which have excellent compatibility with materials such as PA10T and can improve the mechanical properties of the materials while increasing the reflectivity of the composite materials to visible light. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 : Schematic diagram of the TiO2@Al2O3@v-SiO2 structure of the present invention.
[0047] Figure 2 : Schematic diagram of amino functionalization of TiO2@Al2O3@v-SiO2 and CL polymerization process. DETAILED DESCRIPTION
[0048] The present invention is further described below by means of specific embodiments, but the protection scope of the present invention is not limited thereto.
[0049] In the following examples, PA10T: resin H101, Huisheng (Taizhou) New Material Technology Co., Ltd.; antioxidant 1098: Shanghai McLean Biochemical Technology Co., Ltd.; antioxidant 168: Shanghai McLean Biochemical Technology Co., Ltd.
[0050] Example 1
[0051] The preparation steps of PA6 modified TiO2@Al2O3@v-SiO2 are as follows:
[0052] (1) 100 mL of 30 g / 100 mL TiO2 aqueous dispersion was adjusted to pH 9 using 10% NaOH aqueous solution and 10% HCl aqueous solution, and 50 mL of 30 g / 100 mL of 18-hydrated aluminum sulfate Al2(SO4)3·18H2O aqueous solution was slowly added at 80°C within 1 hour and stirred. After the reaction was completed, the mixture was allowed to stand at 80°C for 2 hours, filtered, washed with deionized water for more than three times, and dried in an oven at 80°C for more than 2 hours to obtain titanium dioxide TiO2@Al2O3 coated with alumina.
[0053] (2) 100 mL of 3 g / 100 mL TiO2@Al2O3 particles were dispersed in a mixed solvent of ammonium hydroxide, deionized water and ethanol in a volume ratio of 1:4:10 and stirred to obtain a TiO2@Al2O3 dispersion. Then 3 g of tetraethyl orthosilicate (TEOS) was slowly added dropwise to the TiO2@Al2O3 dispersion and stirred, and then allowed to stand at 60°C for 2 h. Finally, the dispersion was centrifuged at 7000 rpm for 30 min, and the precipitate was washed with deionized water for more than three times and dried in an oven at 80°C for more than 2 h to obtain TiO2@Al2O3@SiO2.
[0054] (3) Disperse 5 g of TiO2@Al2O3@SiO2 in 100 mL of 10 g / 100 mL polyvinyl pyrrolidone (PVP) aqueous solution, stir to obtain a TiO2@Al2O3@SiO2 dispersion, and place at 100 °C for 1 h to load PVP on the surface of TiO2@Al2O3@SiO2. After the dispersion is cooled to room temperature, add 100 mL of 10 g / 100 mL NaOH aqueous solution to the TiO2@Al2O3@SiO2 dispersion, etch for 2 h, then wash with deionized water for more than three times, and dry in an oven at 80 °C for more than 2 h to prepare TiO2@Al2O3@v-SiO2.
[0055] (4) 1 kg of TiO2@Al2O3@v-SiO2 was placed in a high-speed mixer, 200 g of KH-550 ethanol aqueous solution was added and stirred at 2000 rpm for 5 min, then washed with deionized water for more than three times, and dried in an oven at 80°C for more than 2 h to prepare amino TiO2@Al2O3@v-SiO2.
[0056] (5) 20 g of caprolactam (CL) was melted at 100 °C, and 80 g of amino-treated TiO2@Al2O3@v-SiO2 and 4 g of sodium hydroxide were added. The mixture was polymerized at 250 °C for 1 h, and the mixture was vacuumed to below -0.085 MPa for dehydration. After the polymerization, PA6-modified TiO2@Al2O3@v-SiO2 was obtained.
[0057] The formula of PA10T composite material is as follows:
[0058] PA10T 79wt%, PA6 modified TiO2@Al2O3@v-SiO2 20wt%, antioxidant (antioxidant 168 and antioxidant 1098 are mixed in a mass ratio of 1:1, and this antioxidant is used in subsequent examples) 1wt%.
[0059] Example 2
[0060] The preparation steps of PA6 modified TiO2@Al2O3@v-SiO2 are as follows:
[0061] (1) 100 mL of 30 g / 100 mL TiO2 aqueous dispersion was adjusted to pH 9 using 10% NaOH aqueous solution and 10% HCl aqueous solution, and 30 mL of 30 g / 100 mL of 18-hydrated aluminum sulfate Al2(SO4)3·18H2O aqueous solution was slowly added at 60°C within 0.5 h and stirred. After the reaction was completed, the mixture was allowed to stand at 60°C for 2 h, filtered, washed with deionized water for more than three times, and dried in an oven at 80°C for more than 2 h to obtain titanium dioxide TiO2@Al2O3 coated with alumina.
[0062] (2) 100 mL of 3 g / 100 mL TiO2@Al2O3 particles were dispersed in a mixed solvent of ammonium hydroxide, deionized water and ethanol in a volume ratio of 1:4:10 and stirred to obtain a TiO2@Al2O3 dispersion. Then 3 g of tetraethyl orthosilicate (TEOS) was slowly added dropwise to the TiO2@Al2O3 dispersion and stirred, and then allowed to stand at 60°C for 2 h. Finally, the dispersion was centrifuged at 7000 rpm for 30 min, and the precipitate was washed with deionized water for more than three times and dried in an oven at 80°C for more than 2 h to obtain TiO2@Al2O3@SiO2.
[0063] (3) Disperse 5 g of TiO2@Al2O3@SiO2 in 100 mL of 10 g / 100 mL polyvinyl pyrrolidone (PVP) aqueous solution, stir to obtain a TiO2@Al2O3@SiO2 dispersion, and place at 100 °C for 1 h to load PVP on the surface of TiO2@Al2O3@SiO2. After the dispersion is cooled to room temperature, add 100 mL of 10 g / 100 mL NaOH aqueous solution to the TiO2@Al2O3@SiO2 dispersion, etch for 2 h, then wash with deionized water for more than three times, and dry in an oven at 80 °C for more than 2 h to prepare TiO2@Al2O3@v-SiO2.
[0064] (4) 1 kg of TiO2@Al2O3@v-SiO2 was placed in a high-speed mixer, 200 g of KH-550 ethanol aqueous solution was added and stirred at 2000 rpm for 5 min, then washed with deionized water for more than three times, and dried in an oven at 80°C for more than 2 h to prepare amino TiO2@Al2O3@v-SiO2.
[0065] (5) 20 g of caprolactam (CL) was melted at 100 °C, and 80 g of amino-treated TiO2@Al2O3@v-SiO2 and 4 g of sodium hydroxide were added. The mixture was polymerized at 250 °C for 2 h, and the mixture was vacuumed to below -0.085 MPa for dehydration. After the polymerization, PA6-modified TiO2@Al2O3@v-SiO2 was obtained.
[0066] The formula of PA10T composite material is as follows:
[0067] PA10T 79wt%, PA6 modified TiO2@Al2O3@v-SiO2 20wt%, antioxidant 1wt%.
[0068] Example 3
[0069] The preparation steps of PA6 modified TiO2@Al2O3@v-SiO2 are as follows:
[0070] (1) 100 mL of 30 g / 100 mL TiO2 aqueous dispersion was adjusted to pH 9 using 10% NaOH aqueous solution and 10% HCl aqueous solution, and 100 mL of 30 g / 100 mL of 18-hydrated aluminum sulfate Al2(SO4)3·18H2O aqueous solution was slowly added at 80°C for 2 h and stirred. After the reaction was completed, the mixture was allowed to stand at 70°C for 2 h, filtered, washed with deionized water for more than three times, and dried in an oven at 80°C for more than 2 h to obtain titanium dioxide TiO2@Al2O3 coated with alumina.
[0071] (2) 100 mL of 3 g / 100 mL TiO2@Al2O3 particles were dispersed in a mixed solvent of ammonium hydroxide, deionized water and ethanol in a volume ratio of 1:4:10 and stirred to obtain a TiO2@Al2O3 dispersion. Then 3 g of tetraethyl orthosilicate (TEOS) was slowly added dropwise to the TiO2@Al2O3 dispersion and stirred, and then allowed to stand at 60°C for 2 h. Finally, the dispersion was centrifuged at 7000 rpm for 30 min, and the precipitate was washed with deionized water for more than three times and dried in an oven at 80°C for more than 2 h to obtain TiO2@Al2O3@SiO2.
[0072] (3) Disperse 5 g of TiO2@Al2O3@SiO2 in 100 mL of 10 g / 100 mL polyvinyl pyrrolidone (PVP) aqueous solution, stir to obtain a TiO2@Al2O3@SiO2 dispersion, and place at 100 °C for 1 h to load PVP on the surface of TiO2@Al2O3@SiO2. After the dispersion is cooled to room temperature, add 100 mL of 10 g / 100 mL NaOH aqueous solution to the TiO2@Al2O3@SiO2 dispersion, etch for 2 h, then wash with deionized water for more than three times, and dry in an oven at 80 °C for more than 2 h to prepare TiO2@Al2O3@v-SiO2.
[0073] (4) 1 kg of TiO2@Al2O3@v-SiO2 was placed in a high-speed mixer, 200 g of KH-550 ethanol aqueous solution was added and stirred at 2000 rpm for 5 min, then washed with deionized water for more than three times, and dried in an oven at 80°C for more than 2 h to prepare amino TiO2@Al2O3@v-SiO2.
[0074] (5) 20 g of caprolactam (CL) was melted at 100 °C, and 80 g of amino-treated TiO2@Al2O3@v-SiO2 and 4 g of sodium hydroxide were added. The mixture was polymerized at 250 °C for 1 h, and the mixture was vacuumed to below -0.085 MPa for dehydration. After the polymerization, PA6-modified TiO2@Al2O3@v-SiO2 was obtained.
[0075] The formula of PA10T composite material is as follows:
[0076] PA10T 79wt%, PA6 modified TiO2@Al2O3@v-SiO2 20wt%, antioxidant 1wt%.
[0077] Example 4
[0078] The preparation steps of PA6 modified TiO2@Al2O3@v-SiO2 are as follows:
[0079] (1) 100 mL of 30 g / 100 mL TiO2 aqueous dispersion was adjusted to pH 9 using 10% NaOH aqueous solution and 10% HCl aqueous solution, and 100 mL of 30 g / 100 mL of 18-hydrated aluminum sulfate Al2(SO4)3·18H2O aqueous solution was slowly added at 80°C for 2 h and stirred. After the reaction was completed, the mixture was allowed to stand at 70°C for 2 h, filtered, washed with deionized water for more than three times, and dried in an oven at 80°C for more than 2 h to obtain titanium dioxide TiO2@Al2O3 coated with alumina.
[0080] (2) 100 mL of 3 g / 100 mL TiO2@Al2O3 particles were dispersed in a mixed solvent of ammonium hydroxide, deionized water and ethanol in a volume ratio of 1:4:10 and stirred to obtain a TiO2@Al2O3 dispersion. Then 1 g of tetraethyl orthosilicate (TEOS) was slowly added dropwise to the TiO2@Al2O3 dispersion and stirred, and then allowed to stand at 60°C for 2 h. Finally, the dispersion was centrifuged at 7000 rpm for 30 min, and the precipitate was washed with deionized water for more than three times and dried in an oven at 80°C for more than 2 h to obtain TiO2@Al2O3@SiO2.
[0081] (3) Disperse 5 g of TiO2@Al2O3@SiO2 in 100 mL of 10 g / 100 mL polyvinyl pyrrolidone (PVP) aqueous solution, stir to obtain a TiO2@Al2O3@SiO2 dispersion, and place at 100 °C for 1 h to load PVP on the surface of TiO2@Al2O3@SiO2. After the dispersion is cooled to room temperature, add 100 mL of 10 g / 100 mL NaOH aqueous solution to the TiO2@Al2O3@SiO2 dispersion, etch for 1 h, then wash with deionized water for more than three times, and dry in an oven at 80 °C for more than 2 h to prepare TiO2@Al2O3@v-SiO2.
[0082] (4) 1 kg of TiO2@Al2O3@v-SiO2 was placed in a high-speed mixer, 200 g of KH-550 ethanol aqueous solution was added and stirred at 2000 rpm for 5 min, then washed with deionized water for more than three times, and dried in an oven at 80°C for more than 2 h to prepare amino TiO2@Al2O3@v-SiO2.
[0083] (5) 20 g of caprolactam (CL) was melted at 100 °C, and 80 g of amino-treated TiO2@Al2O3@v-SiO2 and 4 g of sodium hydroxide were added. The mixture was polymerized at 250 °C for 1 h, and the mixture was vacuumed to below -0.085 MPa for dehydration. After the polymerization, PA6-modified TiO2@Al2O3@v-SiO2 was obtained.
[0084] The formula of PA10T composite material is as follows:
[0085] PA10T 79wt%, PA6 modified TiO2@Al2O3@v-SiO2 20wt%, antioxidant 1wt%.
[0086] Example 5
[0087] The preparation steps of PA6 modified TiO2@Al2O3@v-SiO2 are as follows:
[0088] (1) 100 mL of 30 g / 100 mL TiO2 aqueous dispersion was adjusted to pH 9 using 10% NaOH aqueous solution and 10% HCl aqueous solution, and 100 mL of 30 g / 100 mL of 18-hydrated aluminum sulfate Al2(SO4)3·18H2O aqueous solution was slowly added at 80°C within 1 hour and stirred. After the reaction was completed, the mixture was allowed to stand at 70°C for 2 hours, filtered, washed with deionized water for more than three times, and dried in an oven at 80°C for more than 2 hours to obtain titanium dioxide TiO2@Al2O3 coated with alumina.
[0089] (2) 100 mL of 3 g / 100 mL TiO2@Al2O3 particles were dispersed in a mixed solvent of ammonium hydroxide, deionized water and ethanol in a volume ratio of 1:4:10 and stirred to obtain a TiO2@Al2O3 dispersion. Then 1 g of tetraethyl orthosilicate (TEOS) was slowly added dropwise to the TiO2@Al2O3 dispersion and stirred, and then allowed to stand at 60°C for 2 h. Finally, the dispersion was centrifuged at 7000 rpm for 30 min, and the precipitate was washed with deionized water for more than three times and dried in an oven at 80°C for more than 2 h to obtain TiO2@Al2O3@SiO2.
[0090] (3) Disperse 5 g of TiO2@Al2O3@SiO2 in 100 mL of 10 g / 100 mL polyvinyl pyrrolidone (PVP) aqueous solution, stir to obtain a TiO2@Al2O3@SiO2 dispersion, and place at 100 °C for 1 h to load PVP on the surface of TiO2@Al2O3@SiO2. After the dispersion is cooled to room temperature, add 100 mL of 10 g / 100 mL NaOH aqueous solution to the TiO2@Al2O3@SiO2 dispersion, etch for 1 h, then wash with deionized water for more than three times, and dry in an oven at 80 °C for more than 2 h to prepare TiO2@Al2O3@v-SiO2.
[0091] (4) 1 kg of TiO2@Al2O3@v-SiO2 was placed in a high-speed mixer, 100 g of KH-550 ethanol aqueous solution was added and stirred at 2000 rpm for 5 min, then washed with deionized water for more than three times, and dried in an oven at 80 °C for more than 2 h to prepare amino TiO2@Al2O3@v-SiO2.
[0092] (5) 15 g of caprolactam (CL) was melted at 100 °C, and 85 g of amino-treated TiO2@Al2O3@v-SiO2 and 3 g of sodium hydroxide were added. The mixture was polymerized at 250 °C for 1 h, and the mixture was vacuumed to below -0.085 MPa for dehydration. After the polymerization, PA6-modified TiO2@Al2O3@v-SiO2 was obtained.
[0093] The formula of PA10T composite material is as follows:
[0094] PA10T 79wt%, PA6 modified TiO2@Al2O3@v-SiO2 20wt%, antioxidant 1wt%.
[0095] Comparative Example 1
[0096] The difference from the embodiment is that no inorganic filler is added, only PA10T is added, and the composite material formula is as follows: PA10T 99wt%, antioxidant 1wt%.
[0097] Comparative Example 2
[0098] The difference from the embodiment is that unmodified TiO2 is added, and the composite material formula is as follows: PA10T 79wt%, TiO2 20wt%, antioxidant 1wt%.
[0099] Example performance test results
[0100] Performance test: With reference to the national standards "GB / T 1040 Determination of tensile properties of plastics", "GB / T 2913 Test method for whiteness of plastics" and "GB / T 16422.3 Laboratory light source exposure test method Part 3: Fluorescent ultraviolet lamp", the tensile strength and whiteness of the PA10T composite materials prepared in the embodiments and comparative examples were tested under ultraviolet light irradiation for different times, and the reflectivity of the samples to light of a wavelength of 460 nm at different irradiation times was tested by a UV-visible spectrophotometer. The results are shown in Tables 1 to 3.
[0101] Table 1 Whiteness test results of PA10T composite materials under different UV aging times (unit: %)
[0102]
[0103] Table 2 Test results of the reflectivity of PA10T composite materials at a wavelength of 460 nm under different UV aging times (unit: %)
[0104]
[0105] Table 3 Test results of tensile properties of PA10T composite materials under different UV aging times (unit: MPa)
[0106]
[0107] It can be seen from the data in Table 1 that adding TiO2 to PA10T can effectively improve the whiteness of the composite material; the data in Table 2 show that SiO2 wrapped with etched holes can effectively improve the reflectivity of the composite material, which means that the application of this material in LED brackets can make the LED have better luminous efficiency; finally, the tensile test results in Table 3 show that grafting polymer molecular chains on the surface of inorganic materials is beneficial to improving the composite tensile strength.
[0108] Combining Tables 1 to 3, it can be found that Al2O3 effectively inhibits the photocatalytic effect of TiO2 and can increase the stability of the composite material under ultraviolet light, thus broadening the possibility of outdoor application of composite materials, such as automotive headlights, street lamps, advertising screens and other application scenarios.
Claims
1. A method for preparing titanium dioxide filler for nylon, It is characterized in that The steps include: (1) Adjustment of TiO 2 The pH of the aqueous dispersion was adjusted to 9, and Al was added dropwise at 60-90°C. 2 (SO 4 ) 3 18H 2 O aqueous solution and stirred for 0.5-2h, then allowed to stand at 50-90°C for 1-5h, then filtered, washed, and dried to obtain TiO 2 @Al 2 O 3 ; (2) TiO 2 @Al 2 O 3 Dispersed in a mixed solvent of ammonium hydroxide, deionized water and ethanol, TiO 2 @Al 2 O 3 Dispersion liquid, add tetraethyl orthosilicate dropwise to TiO 2 @Al 2 O 3 The dispersion was stirred evenly, then allowed to stand at 50-70°C for 1-3 hours, centrifuged, the precipitate was washed, and dried to obtain TiO 2 @Al 2 O 3 @SiO 2 ; (3) TiO 2 @Al 2 O 3 @SiO 2 Dispersed in polyvinyl pyrrolidone aqueous solution to obtain TiO 2 @Al 2 O 3 @SiO 2 The dispersion was allowed to stand at 80-100°C for 3-5 hours to allow polyvinyl pyrrolidone to be loaded on the TiO 2 @Al 2 O 3 @SiO 2 surface, and then cooled to room temperature to TiO 2 @Al 2 O 3 @SiO 2 NaOH aqueous solution was added to the dispersion to 2 Etching was performed for 1 to 4 hours, followed by washing and drying to obtain TiO 2 @Al 2 O 3 @v-SiO 2 ; (4) TiO 2 @Al 2 O 3 @v-SiO 2 Place in a high-speed mixer, add a coupling agent solution containing terminal amino groups and stir, then wash and dry to obtain amino TiO 2 @Al 2 O 3 @v-SiO 2 ; (5) Melt caprolactam and add aminated TiO 2 @Al 2 O 3 @v-SiO 2 The catalyst is reacted with the catalyst for polymerization, and vacuum dehydration is performed at the same time. After the polymerization is completed, PA6 modified TiO 2 @Al 2 O 3 @v-SiO 2 , i.e. the titanium dioxide filler for nylon; The polymerization reaction temperature is 230-250°C, and the polymerization reaction time is 1-2h.
2. The method for preparing the titanium dioxide filler for nylon as claimed in claim 1, It is characterized in that In step (1), TiO 2 With Al 2 (SO 4 ) 3 18H 2 The mass ratio of O is 3:1 to 1:
1.
3. The method for preparing the titanium dioxide filler for nylon as claimed in claim 1, It is characterized in that In step (2), tetraethyl orthosilicate and TiO 2 @Al 2 O 3 The mass ratio is 1:2 to 2:
1.
4. The method for preparing the titanium dioxide filler for nylon as claimed in claim 1, It is characterized in that In step (4), the coupling agent containing terminal amino group is selected from one or more of KH-550, A-1110, A-1120, KBM-603 and KBM-602.
5. The method for preparing the titanium dioxide filler for nylon as claimed in claim 1, It is characterized in that In step (4), a coupling agent containing an amino group and TiO 2 @Al 2 O 3 @v-SiO 2 The mass ratio is 1:100~5:
100.
6. The method for preparing the titanium dioxide filler for nylon as claimed in claim 1, It is characterized in that In step (5), caprolactam and aminated TiO 2 @Al 2 O 3 @v-SiO 2 The mass ratio is 15:85~20:
80.
7. The method for preparing the titanium dioxide filler for nylon as claimed in claim 1, It is characterized in that In step (5), the catalyst is sodium hydroxide.
8. Titanium dioxide filler for nylon obtained by the preparation method according to any one of claims 1 to 7.
9. A high reflectivity PPA, It is characterized in that The recipe is as follows: PPA resin 69-79wt%, titanium dioxide filler for nylon according to claim 8 20-30wt%, antioxidant 0.5-1wt%; All components add up to 100 wt%.
10. The method for preparing the high reflectivity PPA according to claim 9, It is characterized in that The preparation method is as follows: (1) Before sample preparation, each raw material component was placed in an oven at 80-120°C and dried for 4-12 hours to remove moisture; (2) According to the formula, the dried PPA, antioxidant and titanium dioxide filler for nylon are placed in a high-speed mixer and mixed at a speed of 1500 rpm for 5 minutes to complete the premix; (3) The premix was extruded into granules by an extruder at a temperature of 320-330° C. and a screw speed of 80 rpm, and then a specimen was prepared by an injection molding machine at a temperature of 320-330° C. and an injection molding pressure of 60 bar.
Citation Information
Cited By
High-reflectivity composite material as well as preparation method and application thereof
CN120118500A
A high-reflectivity composite material, its preparation method and application
CN120118500B