Carbon template sacrifice method for preparing multi-element metal oxide catalyst system with controllable morphology

Through a multi-pass storage tank and an improved suction filtration device, combined with electrochemical deposition technology, the problems in the existing technology of single catalyst components and morphology, cumbersome preparation process and unfriendly environment are solved, achieving high efficiency and flexibility of the catalyst. Preparation and sustainable use of resources.

CN221816102UInactive Publication Date: 2024-10-11HEBEI UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202420362043.3
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2024-02-26
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing carbon template sacrificial method to prepare metal oxide catalysts has the problems of single catalyst components and morphology, cumbersome preparation process, and unfriendly to the environment, and the waste liquid is not fully utilized, resulting in waste of resources and increased production costs.

Method used

Using a multi-channel precursor storage tank and an improved suction filtration device, the continuous processing of suction filtration and drying is achieved through a circular air flow dryer, eliminating the need to transfer the precursor material to the oven for drying, and under the vacuum suction filtration device An electrochemical test system was set up to deposit excess metal ions in the metal precursor solution onto the working electrode through electrochemical deposition to be used as a catalyst.

Benefits of technology

It achieves flexible control of catalyst components and morphology, simplifies the preparation process, improves metal ion utilization, reduces preparation costs, and reduces negative impact on the environment. It has flexible components, adjustable morphology, The process has the advantages of real-time controllability, safety and environmental friendliness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221816102U_ABST
    Figure CN221816102U_ABST
Patent Text Reader

Abstract

The utility model relates to a system for preparing a multi-element metal oxide catalyst with controllable morphology by a carbon template sacrifice method. The system comprises n metal precursor storage tanks, a multi-channel peristaltic pump, a flow meter, a carbon template storage tank, a filter cup, an annular pneumatic dryer, a filter head, a vacuum pump, an electrolytic bath and an electrochemical workstation, n = 2-5; wherein the n metal precursor storage tanks are respectively connected with the multi-channel peristaltic pump to form n groups of parallel feeding systems, n outlets of the multi-channel peristaltic pump are respectively connected with an inlet of the carbon template storage tank through the flow meter, an outlet of the carbon template storage tank is connected with an inlet of the filter cup through a pipeline, an outlet of the filter cup is connected with the upper end of the annular dryer, and the annular dryer is connected with the lower end of the annular dryer. The inlet of the filter head is connected with the lower end of the circular dryer, the vacuum pump is connected with the filter head, and the outlet of the filter head is communicated into the electrolytic bath. According to the utility model, the preparation process is simplified, the utilization rate of metal ions is improved, and the preparation cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model belongs to the technical field of catalyst manufacturing, and relates to a system for chemical synthesis using a carbon template sacrificial method, in particular to a multi-metal oxide catalyst preparation system with controllable morphology. Background Art

[0002] With the rapid development of renewable energy (such as solar and wind energy), the volatility and intermittency problems in the power system have become prominent. Using excess renewable energy for water electrolysis to produce hydrogen can convert electrical energy into hydrogen so that it can be burned or combined with fuel cells when needed, providing a stable energy supply, thereby achieving sustainable energy storage and utilization. The widespread application of water electrolysis hydrogen production technology will also further promote the development of related industries, including catalysts, electrolysis equipment, hydrogen storage and transportation. At the same time, with the maturity and large-scale application of water electrolysis hydrogen production technology, its cost will gradually decrease, further improving economic benefits. Catalysts are of great significance as key materials in the water electrolysis hydrogen production process. They can accelerate the reaction rate, improve selectivity, enhance stability and reduce energy consumption, providing key support for efficient and sustainable hydrogen energy preparation. Therefore, the efficient preparation of excellent catalysts is of great significance to the storage and application of sustainable energy.

[0003] In the laboratory, the carbon template sacrificial method is a commonly used method for synthesizing metal oxide catalysts. The carbon template is evenly dispersed in the precursor solution by an ultrasonic cleaner, and allowed to stand for a period of time so that the carbon template can fully adsorb the metal ions in the precursor solution. Then, the excess precursor solution is filtered into the filtration bottle, and the carbon template adsorbed with metal ions is retained. The carbon template adsorbed with metal ions is further transferred to an oven for drying, and finally heat-treated to obtain the catalyst. However, the carbon template adsorbed with metal ions obtained by this preparation system needs to be transferred to an oven for drying and then heat-treated. The preparation process is cumbersome, and only a metal oxide catalyst with a single morphology and fixed components can be obtained each time. The excess precursor solution produced after filtration is directly treated as waste liquid, resulting in a waste of resources and waste liquid treatment may involve environmental and safety issues. Therefore, we need to adopt a more efficient and environmentally friendly method to prepare catalysts.

[0004] At present, some preparation processes for metal oxide catalysts prepared by carbon template sacrificial method have been reported. For example, a three-dimensional metal oxide catalyst preparation process is reported in document 10.1002 / adfm.201605017. The precursor solution is prepared in a beaker, and then the three-dimensional carbon template is poured into the precursor solution. The three-dimensional carbon template is evenly dispersed in the precursor solution by an ultrasonic cleaner. The resulting suspension is allowed to stand for a period of time and then filtered and washed. The excess precursor solution flows into the filtration bottle and is poured into the waste liquid barrel after the filtration is completed. At the same time, the carbon template adsorbed with metal ions is retained and further transferred to an oven for drying, and finally heat-treated to obtain a metal oxide catalyst. It is worth noting that the catalyst preparation system can only produce catalyst products with fixed components and morphology each time. If you want to adjust the components, you can only prepare the precursor solution again, and the precursor material needs to be transferred back and forth in different environments, and the preparation process is cumbersome. In addition, the excess precursor solution produced after filtration is not fully utilized, and these valuable metal components are wasted, which invisibly increases the production cost. Utility Model Content

[0005] The purpose of the utility model is to solve the problems of one-time preparation of metal oxide catalyst components and single morphology in the laboratory, as well as the cumbersome preparation process and unfriendly to the environment, and to provide a multi-metal oxide catalyst system with controllable morphology prepared by a carbon template sacrificial method. In the system, the adjustment of different components of metal oxides is achieved through a multi-channel precursor storage tank; at the same time, the suction filtration device is improved, and a ring-shaped air flow dryer is designed between the filter cup and the filter head, so as to achieve the purpose of continuous treatment of suction filtration and drying, eliminating the step of transferring the precursor material to the oven for drying, and directly performing heat treatment, which greatly saves time and cost; and the electrochemical test system is arranged below the vacuum filtration device, and the metal ions in the excess metal precursor solution are deposited on the working electrode by electrochemical deposition, and the working electrode deposited with metal particles can be further used as a catalyst. The utility model simplifies the preparation process, improves the utilization rate of metal ions, reduces the preparation cost, and contributes to sustainable development.

[0006] The technical solution of the utility model is:

[0007] A carbon template sacrificial method for preparing a multi-metal oxide catalyst system with controllable morphology, the system comprising n metal precursor storage tanks, a multi-channel peristaltic pump, a flow meter, a carbon template storage tank, a filter cup, a circular air flow dryer, a filter head, a vacuum pump, an electrolytic cell and an electrochemical workstation; n=2-5;

[0008] Among them, n metal precursor storage tanks are respectively connected to multi-channel peristaltic pumps to form n parallel feeding systems, and the n outlets of the multi-channel peristaltic pumps are respectively connected to the inlet of the carbon template storage tank through a flow meter, and the outlet of the carbon template storage tank is connected to the inlet of the filter cup through a pipeline, and the outlet of the filter cup is connected to the upper end of the annular dryer, and the inlet of the filter head is connected to the lower end of the annular dryer, and the vacuum pump is connected to the filter head, and the outlet of the filter head is connected to the electrolytic cell;

[0009] Each of the n metal precursor storage tanks and the carbon template storage tank is provided with a mechanical stirring paddle;

[0010] The material of the pipeline is chlorinated polyethylene, and the inner diameter of the chlorinated polyethylene pipe is 10 mm;

[0011] The inner diameter of the filter sand core of the suction filtration is 50 mm;

[0012] The aperture of the annular airflow dryer tuyere is 4 mm, and the inner diameter of the annular ring is consistent with the filter head;

[0013] The electrolytic cell is equipped with a counter electrode, a reference electrode and a working electrode;

[0014] The counter electrode is a platinum sheet or a graphite rod; the reference electrode is a saturated calomel electrode, a silver-silver chloride electrode or a mercury-mercury oxide electrode; the working electrode is conductive glass, nickel foam or copper foam;

[0015] The length, width and height of the electrolytic cell are 15 cm*15 cm*10 cm;

[0016] The essential features of this utility model are:

[0017] In the current laboratory catalyst preparation system, the carbon template sacrificial process for synthesizing metal oxide catalysts has the problem of cumbersome process. First, the materials need to be transferred back and forth between different containers, which increases the complexity of the operation. Secondly, the waste liquid generated by this process cannot be reused, which not only increases production costs but also has a negative impact on the environment. In addition, the catalyst synthesized once is usually a metal oxide catalyst with fixed components, which greatly increases the experimental cycle.

[0018] The utility model realizes flexible regulation of catalyst components and components by feeding in parallel with a multi-channel storage tank and a peristaltic pump; in addition, different types of carbon templates can be selected according to different experimental requirements, so as to prepare a multi-metal oxide catalyst with controllable morphology. This design makes the preparation of the catalyst more flexible, greatly improves the preparation efficiency, and shortens the experimental cycle. In addition, by designing a circular airflow dryer between the filter cup and the filter head, the filtration and drying processes can be carried out continuously, eliminating the step of transferring the precursor material to the oven for drying, and directly performing heat treatment after drying, which greatly saves time and cost; at the same time, the electrochemical test system is arranged below the vacuum filtration device, and the metal ions in the excess metal precursor solution are deposited on the working electrode by electrochemical deposition, and the working electrode deposited with metal particles can be further used as a catalyst, and the excess precursor solution produced by the filtration can be electro-deposited through the electrolytic cell without further treatment to achieve the purpose of reuse, reducing production costs and further improving resource utilization efficiency.

[0019] The beneficial effects of the utility model are:

[0020] Compared with the traditional preparation system, the utility model can realize customized preparation of morphology and metal oxide components by adding a metal precursor storage tank and adding a carbon template with a specific morphology according to different experimental requirements or existing conditions when synthesizing catalysts of metal oxides with different morphologies and components. After the mixed solution of the carbon template and a variety of metal precursor solutions is filtered, the carbon template adsorbed with metal ions is left on the filter membrane and further dried by a circular airflow dryer, and can be directly heat-treated after being taken out, eliminating the step of transferring the precursor to the oven, simplifying the preparation process, saving about 1 hour, and the continuity of the whole system can also save manpower. In the traditional preparation process, the excess precursor solution will flow into the suction filtration bottle and further poured into the waste liquid barrel as waste liquid. The waste liquid contains recyclable metal components. If it is poured directly into the waste liquid barrel, these valuable metal components will not be able to be recycled, resulting in a waste of resources. Therefore, an electrochemical test system is designed under the suction filtration device, and the excess metal precursor solution flows into the electrolytic cell. At the same time, the working electrode, the counter electrode and the reference electrode are inserted into the electrolytic cell to form a three-electrode system and submerged in the solution, and connected to the electrochemical workstation. The required current density, potential and reaction time and other parameters are set according to the rate and quality of electrodeposition. When the required deposition time is reached or the target deposition quality is reached, the electrochemical reaction is stopped, and the working electrode on which the metal atoms are deposited can be further utilized as a catalyst. And the excess precursor solution can be used without further treatment, thereby reducing the preparation cost and contributing to sustainable development. The utility model is suitable for the production of multi-component and multi-morphology metal oxide catalyst products, and has the advantages of flexible and variable components, adjustable morphology, real-time controllable process, safety and environmental friendliness. In the embodiment, we successfully synthesized binary MnCo2O4 metal oxides and quinary (FeCoNiMnCu)3O4 metal oxides with three-dimensional network structures, from the attached Figure 3 and attached Figure 4 Scanning transmission electron microscopy characterization images show that the morphology is a three-dimensional network structure, and the different metal elements are evenly distributed. Through statistics, it is found that the average particle size of MnCo2O4 metal oxide is 10 nanometers (see Appendix Figure 5 ), which shows that the quality of the catalyst is better than other similar products. In addition, the MnCo2O4 metal oxide and (FeCoNiMnCu)3O4 metal oxide loaded on the working electrode obtained by further electrodeposition showed excellent OER performance (attached Figure 6 , 7). BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the technical solutions in the embodiments of the utility model, the drawings required for describing the prior art in the utility model will be introduced below. The drawings are derived from the embodiments of the utility model. Ordinary technicians in this field can also obtain other drawings based on these drawings without paying creative work.

[0022] Figure 1 This is a device diagram of a multi-metal oxide catalyst preparation system with controllable morphology provided by the utility model;

[0023] Among them, 1-metal precursor I storage tank, 2-metal precursor II storage tank, 3-metal precursor III storage tank, 4-multi-channel peristaltic pump, 5-flow meter, 6-carbon template storage tank, 7-filter cup, 8-annular air flow dryer, 9-filter head, 10-vacuum pump, 11-counter electrode, 12-reference electrode, 13-working electrode, 14-electrolyzer, 15-electrochemical workstation;

[0024] Figure 2 It is a schematic diagram of a circular airflow dryer in a multi-metal oxide catalyst preparation system with controllable morphology provided by the utility model;

[0025] Figure 3 is a STEM image of the three-dimensional network MnCo2O4 synthesized in Example 1;

[0026] Figure 4 is a STEM image of the three-dimensional network (FeCoNiMnCu)3O4 synthesized in Example 2;

[0027] Figure 5 is a particle size distribution diagram of the three-dimensional network MnCo2O4 synthesized in Example 1;

[0028] Figure 6 is the LSV curve of the MnCo2O4 oxide obtained by electrodeposition in Example 1;

[0029] Figure 7 is the LSV curve of (FeCoNiMnCu)3O4 oxide obtained by electrodeposition in Example 2; DETAILED DESCRIPTION

[0030] In order to make those skilled in the art more familiar with the specific technical solutions and advantages of the embodiments of the utility model, the following embodiments will introduce the technical solutions and implementation processes in detail and completely. Without departing from the spirit and essence of the utility model, modifications and replacements made to the methods, steps or conditions of the utility model are within the scope of the utility model. Unless otherwise specified, the technical means used in the embodiments are conventional means well known to those skilled in the art.

[0031] The utility model provides a carbon template sacrificial method for preparing a multi-metal oxide catalyst system with controllable morphology. Figure 1 As shown, it includes a metal precursor I storage tank 1, a metal precursor II storage tank 2, a metal precursor III storage tank 3, a multi-channel peristaltic pump 4, a flow meter 5, a carbon template storage tank 6, a filter cup 7, a circular air flow dryer 8, a filter head 9, a vacuum pump 10, a counter electrode 11, a reference electrode 12, a working electrode 13, an electrolytic cell 14, and an electrochemical workstation 15;

[0032] Among them, three metal precursor storage tanks are respectively connected to the multi-channel peristaltic pump 4 to form three parallel feeding systems, and the three outlets of the multi-channel peristaltic pump 4 are respectively connected to the inlet of the carbon template storage tank 6 through a flow meter, and the outlet of the carbon template storage tank 6 is connected to the inlet of the filter cup 7 through a pipeline, and the outlet of the filter cup 7 is connected to the upper end of the annular dryer 8, and the inlet of the filter head is connected to the lower end of the annular dryer 8, and the vacuum pump 10 is connected to the filter head 9, and the outlet of the filter head 9 is also connected to the electrolytic cell 14;

[0033] The metal precursor I storage tank 1, the metal precursor II storage tank 2, the metal precursor III storage tank 3, and the carbon template storage tank 6 have the same structure, and are all provided with mechanical stirring paddles;

[0034] The material of the pipeline is chlorinated polyethylene, and the inner diameter of the chlorinated polyethylene pipe is 10 mm;

[0035] The inner diameter of the filter sand core of the suction filtration is 50 mm;

[0036] The aperture of the annular airflow dryer tuyere is 4 mm, and the inner diameter of the annular ring is consistent with the filter head; it is connected to the glass airflow dryer device through a pipeline (the glass airflow dryer is JC-C30 type);

[0037] The inner diameter of the filter cup is 50 mm and the capacity is 1 liter;

[0038] The electrolytic cell is equipped with a counter electrode, a reference electrode and a working electrode;

[0039] The counter electrode is a platinum sheet or a graphite rod, and the utility model specifically is a platinum sheet;

[0040] The reference electrode is one of a saturated calomel electrode, a silver-silver chloride electrode and a mercury oxide electrode, and the utility model is specifically a silver-silver chloride electrode;

[0041] The working electrode is one of conductive glass, nickel foam and copper foam, and the present invention specifically uses conductive glass;

[0042] The length, width and height of the electrolytic cell are 15 cm*15 cm*10 cm;

[0043] The chlorinated polyethylene pipe has excellent corrosion resistance, can withstand the erosion of a variety of strong acids, strong alkalis, organic solvents and corrosive gases, has good stability in a wide range of chemical media, and is not easily corroded and dissolved. It also has an extremely low friction coefficient and a smooth surface, which can reduce the resistance and energy loss of the fluid when passing through the pipeline. Compared with quartz tubes and metal tubes, chlorinated polyethylene is more suitable for use in chemical synthesis, because quartz tubes may be corroded in certain strong acid and alkali environments, and metal tubes are prone to rust and corrosion in certain corrosive media.

[0044] Metal precursor I, metal precursor II, metal precursor III and carbon template are dissolved in corresponding storage tanks respectively, the multi-channel peristaltic pump is turned on, the flow rate of the multi-channel peristaltic pump is set according to the components and components of the target product, the liquid inlet switch of the multi-channel peristaltic pump is turned on to allow the metal precursor mixed solution to flow into the carbon template storage tank for impregnation and adsorption of metal ions, and when the carbon template fully adsorbs the metal ions, the vacuum pump is turned on for filtration, and the carbon template adsorbing the metal ions is retained on the filter membrane for drying, and finally heat treatment is performed, and the excess precursor solution flows into the electrolytic cell for electrochemical deposition.

[0045] The multi-channel peristaltic pump is connected to a flow meter, which can monitor the output flow of the multi-channel peristaltic pump in real time. According to the feedback signal of the flow meter, the working parameters of the multi-channel peristaltic pump are adjusted to achieve the required flow control, thereby achieving fine regulation of the multi-metal oxide components and improving product quality.

[0046] The storage tank contains a mechanical stirring paddle, which stirs the material to fully dissolve the soluble material and evenly disperse the insoluble material, which is beneficial to ensure the quality of the product. The carbon template storage tank contains a mechanical stirring paddle, which stirs the carbon template and the metal precursor mixed solution to ensure that the carbon template is fully in contact with the metal precursor mixed solution, so that the carbon template evenly adsorbs different metal ions, thereby ensuring the quality of the product.

[0047] A circular airflow dryer is connected between the filter cup and the filter head. After the filtration is completed, the airflow dryer is started to dry the carbon template that has fully adsorbed metal ions. There is no need to transfer it to an oven for further drying. It can be directly heat treated after being taken out. This design eliminates the step of transferring the precursor to the oven, simplifies the preparation process, improves the continuity of the material preparation process, and greatly saves time costs.

[0048] The lower end of the filter head is connected to an electrolytic cell. After the suspension is filtered, the excess metal precursor mixed solution flows into the electrolytic cell. The working electrode (conductive glass), the reference electrode (silver-silver chloride electrode) and the counter electrode (platinum sheet) are installed in the electrolytic cell to form a three-electrode system and are immersed in the solution. The electrochemical workstation is connected to set the required current density, potential and reaction time parameters according to the rate and quality of electrodeposition. When the required deposition time or the target deposition quality is reached, the electrochemical reaction is stopped. The conductive glass deposited with metal can be further used as a catalyst, which improves the utilization rate of metal ions, reduces the preparation cost, and contributes to sustainable development.

[0049] The material pushing device is a multi-channel peristaltic pump, which pushes the fluid by compressing a hose. The hose has no direct contact with other components inside the pump, so non-contact fluid delivery can be achieved, and the material can be pushed at a fixed flow rate, which can be adjusted within a large range.

[0050] This morphology-controllable multi-metal oxide catalyst preparation system is suitable for preparing catalysts by carbon template method, and is mainly used for various metal oxide catalysts in the field of hydrogen production by water electrolysis. It can prepare three-dimensional network metal oxide catalysts, spherical metal oxide catalysts and other products. The system can prepare multi-metal oxide catalysts, and realize the regulation of different components of metal oxides by adjusting the solution feed of different metal precursors. This method can flexibly adjust the components of the catalyst to meet different reaction conditions and requirements. Multi-metal oxide catalysts usually have higher activity and selectivity than single metal oxides, which can improve the efficiency of hydrogen production by water electrolysis. It can also reduce the generation of waste and reduce the impact on the environment through recycling and reuse. In addition, the system usually adopts mild reaction conditions, avoids high temperature and high energy consumption processes, and helps to reduce energy consumption and environmental pollution in the preparation process.

[0051] The following is a specific example of preparing a three-dimensional network structure multi-metal oxide using the morphology controllable multi-metal oxide catalyst preparation system provided by the utility model:

[0052] Example 1

[0053] Accurately weigh 29.1 grams of cobalt nitrate hexahydrate, dissolve it in 500 milliliters of deionized water and put it into the first metal precursor storage tank for stirring until it is completely dissolved. Similarly, weigh 25.1 grams of manganese nitrate tetrahydrate, dissolve it in 500 milliliters of deionized water and put it into the second metal precursor storage tank for stirring until it is completely dissolved. Weigh 1.6 grams of three-dimensional carbon template and put it into the carbon template storage tank 6. The total volume of the material is 1 liter. Turn on the multi-channel peristaltic pump, and set the channel flow rate of the multi-channel peristaltic pump for conveying the cobalt nitrate hexahydrate metal precursor solution to 50 milliliters per minute, and the channel flow rate of the multi-channel peristaltic pump for conveying the manganese nitrate tetrahydrate metal precursor solution to 25 milliliters per minute. When all the cobalt nitrate hexahydrate metal precursor solution flows into the carbon template storage tank, the multi-channel peristaltic pump stops working, and the remaining manganese nitrate tetrahydrate metal precursor solution is prepared for next use. The mixture in the carbon template storage tank is fully stirred so that the carbon template is fully mixed with the two metal precursor solutions, so that different metal ions are uniformly adsorbed on the carbon template. Wait until the carbon template fully absorbs the metal ions and then filter it out. After the filtration is completed, the three-dimensional carbon template that fully absorbs the metal ions is further dried in a circular air flow dryer, and finally heat treated to obtain about 800 mg of a three-dimensional network MnCo2O4 metal oxide. At the same time, the excess metal precursor mixed solution flows into the electrolytic cell and is reused as an electrolyte for electrodeposition. At a constant potential of -0.7V, MnCo oxide is obtained by electrodeposition on conductive glass, and the deposition time is determined to be 1.0h to achieve a suitable thickness of the MnCo oxide. The OER performance of the MnCo oxide obtained by electrodeposition was tested by electrochemical testing. Figure 6 The LSV curve shows that MnCo oxide has excellent OER performance. Therefore, this method can improve the utilization rate of metal ions, reduce costs and be environmentally friendly. Please refer to Figure 3 and Figure 5 Scanning transmission electron microscopy (STEM) observation revealed that the morphology of MnCo2O4 metal oxide is a three-dimensional network structure. Further high-resolution transmission electron microscopy (HRTEM) revealed that its average particle size is 10 nanometers. This result shows that the quality of this product is superior to other similar products.

[0054] Example 2

[0055] Accurately weigh 9.7 grams of cobalt nitrate hexahydrate, dissolve it in 200 milliliters of deionized water, and put it into the first storage tank for stirring until completely dissolved. Weigh 8.37 grams of manganese nitrate tetrahydrate, dissolve it in 200 milliliters of deionized water, and put it into the second storage tank for stirring until completely dissolved. Similarly, weigh 13.47 grams of ferric nitrate nonahydrate, dissolve it in 200 milliliters of deionized water, and put it into the third metal precursor storage tank for stirring until completely dissolved. Weigh 9.7 grams of nickel nitrate hexahydrate, dissolve it in 200 milliliters of deionized water, and put it into the fourth metal precursor storage tank for stirring until completely dissolved. Weigh 6.25 grams of copper nitrate, dissolve it in 200 milliliters of deionized water, and put it into the fifth metal precursor storage tank for stirring until completely dissolved. Weigh 1.6 grams of three-dimensional carbon template and put it into the carbon template storage tank. The total volume of the materials is 1 liter. Turn on the multi-channel peristaltic pump, and the channel flow rate of the multi-channel peristaltic pump that transports the metal precursor solution is set to 20 milliliters per minute. After all five metal precursor solutions flow into the carbon template storage tank, they are fully stirred so that the carbon template and the metal precursor solutions are fully mixed, so that different metal ions are evenly adsorbed on the carbon template. After the carbon template fully adsorbs the metal ions, it is filtered. After the filtration is completed, the three-dimensional carbon template that fully adsorbs the metal ions is further dried by a circular air flow dryer, and finally heat treated to obtain a five-element (FeCoNiMnCu)3O4 metal oxide with a three-dimensional network shape. At the same time, the excess metal precursor mixed solution flows into the electrolytic cell and is reused as an electrolyte for electrodeposition. Under a constant potential of -0.7V, FeCoNiMnCu oxide is electrodeposited on conductive glass, and the deposition time is determined to be 0.5h to achieve a suitable thickness of the FeCoNiMnCu oxide. The OER performance of the FeCoNiMnCu oxide obtained by electrochemical testing was tested. Figure 7 The LSV curve shows that FeCoNiMnCu oxide has excellent OER performance. Therefore, this method can improve the utilization rate of metal ions, reduce costs and be environmentally friendly. Please refer to Figure 4 Scanning transmission electron microscopy (STEM) observation revealed that the morphology of (FeCoNiMnCu)3O4 metal oxide is a three-dimensional network structure.

[0056] Experiments have shown that the quality of the catalyst synthesized by this system is significantly higher than that of other similar products. The system uses independent precursor storage tanks and multi-channel peristaltic pumps to flexibly change the components of the metal oxide catalyst, which can meet the needs of catalyst products with different indicators and greatly improve the preparation efficiency.

[0057] From the above embodiments, it can be seen that the present invention can well achieve the regulation of different components of metal oxides by adding multiple precursor storage tanks and using a multi-channel peristaltic pump to feed different metal precursor solutions; the multi-channel peristaltic pump is connected to a flowmeter to monitor the output flow of the multi-channel peristaltic pump in real time. According to the feedback signal of the flowmeter, the working parameters of the multi-channel peristaltic pump are adjusted to achieve the required flow control, thereby realizing fine regulation of the metal oxide components; adding different types of carbon templates to the carbon template storage tank can further realize the regulation of different morphologies of multi-metal oxides, greatly improving the selectivity of catalyst types, and providing an effective strategy for customized design and optimization of multi-metal oxide catalysts; by improving the filtration device, a circular air flow dryer is designed between the filter cup and the filter head according to the shape characteristics of the filtration device, so as to achieve the purpose of continuous filtration and drying, eliminating the step of transferring the precursor material to the oven for drying, and directly performing heat treatment, which greatly saves time and cost; at the same time, after solid-liquid separation by filtration, the collection device of the excess precursor solution is improved, and an electrochemical test system is set under the vacuum filtration device. The excess precursor solution flows into the electrolytic cell, and the excess metal precursor solution can be deposited on the working electrode by electrochemical deposition through the electrochemical test system. The working electrode deposited with metal particles can be further used as a catalyst, thereby improving the utilization rate of metal ions, reducing the preparation cost, and contributing to sustainable development.

[0058] The above embodiments are more suitable implementation methods of the present invention, but the implementation methods of the present invention are not limited to the above embodiments. Without departing from the spirit and essence of the present invention, modifications and replacements made to the methods, steps or conditions of the present invention all belong to the protection scope of the present invention.

[0059] Matters not covered in this utility model are known technologies.

Claims

1. A carbon template sacrificial method for preparing a morphology-controllable multi-metal oxide catalyst system, characterized by: The system includes n metal precursor storage tanks, a multi-channel peristaltic pump, a flow meter, a carbon template storage tank, a filter cup, a circular air flow dryer, a filter head, a vacuum pump, an electrolytic cell and an electrochemical workstation; n = 2 to 5; Among them, n metal precursor storage tanks are respectively connected to multi-channel peristaltic pumps to form n parallel feeding systems, and the n outlets of the multi-channel peristaltic pumps are respectively connected to the inlet of the carbon template storage tank through a flow meter, and the outlet of the carbon template storage tank is connected to the inlet of the filter cup through a pipeline, and the outlet of the filter cup is connected to the upper end of the annular dryer, and the inlet of the filter head is connected to the lower end of the annular dryer, and the vacuum pump is connected to the filter head, and the outlet of the filter head is connected to the electrolytic cell; Mechanical stirring paddles are provided in the n metal precursor storage tanks and the carbon template storage tank.

2. The carbon template sacrificial method for preparing a morphology-controllable multi-metal oxide catalyst system as claimed in claim 1, characterized in that The material of the pipeline is chlorinated polyethylene, and the inner diameter of the chlorinated polyethylene pipe is 10 mm; The inner diameter of the filter sand core of the suction filtration is 50 mm; The aperture of the annular airflow dryer tuyere is 4 mm, and the inner diameter of the annular ring is consistent with the filter head; The length, width and height of the electrolytic cell are 15 cm*15 cm*10 cm.

3. The carbon template sacrificial method for preparing a morphology-controllable multi-metal oxide catalyst system as claimed in claim 1, characterized in that The electrolytic cell is equipped with a counter electrode, a reference electrode and a working electrode; The counter electrode is a platinum sheet or a graphite rod; the reference electrode is a saturated calomel electrode, a silver-silver chloride electrode or a mercury-mercury oxide electrode; and the working electrode is conductive glass, foamed nickel or foamed copper.