Golden coated glass
By using a combination of Cu film layer, Co film layer and isolation barrier layer in gold-coated glass, the problems of high cost and poor effect in the existing technology are solved, achieving 24K pure gold color, high transmittance, low reflection and high heat transfer. performance for curtain wall and door and window applications.
Patent Information
- Application Number
- CN202420447829.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-08
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2034-03-08
AI Technical Summary
Existing gold-coated glass is expensive and a single metal film layer cannot meet the light intensity absorption and reflection effects at the same time. It is dark in color and prone to fading after use, and its market promotion is limited.
Cu film and Co film are used as the metal absorption layer, combined with the isolation barrier layer, dielectric interference layer and protective layer, to control the low-radiation gold-coated glass with 24K pure gold color and reduce production costs.
It achieves the effect of 24K pure gold color, while having high light transmittance, low reflection and high heat transfer performance, filling the gap of golden glass color in the market.
Smart Images

Figure CN221854470U_ABST
Abstract
Description
Technical Field
[0001] The utility model belongs to the technical field of coated glass, and in particular relates to golden coated glass. Background Art
[0002] Using golden-toned coated glass as curtain walls or doors and windows not only saves energy, but also demonstrates elegance and luxury. It is in line with the psychological needs of the current domestic and overseas markets and has certain market potential.
[0003] However, some existing gold-coated glasses use a pure gold film layer, such as the gold low-emissivity coated glass and its manufacturing method disclosed in Chinese patent CN 103407225 A. The patent uses a pure gold film layer, which is expensive and has great limitations on market promotion. In addition, a single pure gold film layer cannot simultaneously meet the requirements of both absorbing and reflecting light intensity, and the color is darker, which is prone to fading after long-term use.
[0004] Some use silver film layers and other metal film layers instead of pure gold film layers to achieve gold color. For example, Chinese patent CN104386921A discloses a gold double silver low-emissivity coated glass and its preparation method. In this patent, Ag+Cu is used instead of Au to achieve gold color. Although the production cost is saved compared with the pure gold film layer, the visible light transmittance, heat transfer coefficient and shading coefficient of this kind of glass are poor, and the energy-saving effect is not good. Utility Model Content
[0005] In order to solve the above technical problems, the utility model provides a golden coated glass, the appearance of which can achieve the effect of 24K pure gold color, and the glass has the performance of high transmittance, low reflection and high heat transfer.
[0006] The technical solution adopted by the utility model is as follows:
[0007] A golden coated glass comprises a glass substrate and a dielectric protection layer, a first dielectric interference layer, a first blocking isolation layer, a first metal absorption layer, a second metal absorption layer, a second blocking isolation layer, a second dielectric interference layer and a top protective layer which are sequentially stacked on the glass substrate; the first metal absorption layer is a Cu film layer, and the second metal absorption layer is a Co film layer.
[0008] The dielectric protection layer is Si 3 N 4 Layer or TiO x layer.
[0009] The thickness of the dielectric protection layer is 40-60 nm.
[0010] The first dielectric interference layer and the second dielectric interference layer are TiO x layer or ZnO layer.
[0011] The thicknesses of the first dielectric interference layer and the second dielectric interference layer are 20-40 nm and 15-30 nm respectively.
[0012] The first blocking isolation layer and the second blocking isolation layer are Ni layers, Cr layers or NiCr layers.
[0013] The thickness of the first blocking isolation layer and the second blocking isolation layer are both 1-5 nm.
[0014] The thickness of the first barrier isolation layer is preferably 3-4 nm.
[0015] The thickness of the second blocking isolation layer is preferably 2-3 nm.
[0016] The thickness of the first metal absorption layer and the second metal absorption layer are both 1 to 5 nm, preferably 1.5 to 2.5 nm.
[0017] The top protective layer is SiO 2 Layer, Si 3 N 4 Layer or TiO x layer.
[0018] The thickness of the top protective layer is 20-30 nm.
[0019] Compared with the prior art, the utility model has the following beneficial effects: the gold-coated glass provided by the utility model uses a Cu film layer composited with a Co film layer as a metal absorption layer, and cooperates with an isolation barrier layer, a dielectric interference layer, and a dielectric protection layer to adjust a 24K pure gold low-radiation gold-coated glass. The production cost is low, and the application in the field of curtain walls or door and window glass can solve the current market's pursuit of pure gold curtain walls and doors and windows, filling the gap in the color of gold glass curtain walls. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a schematic diagram of the structure of the gold-coated glass in the utility model, in which 1-glass substrate, 2-medium protection layer, 3-first dielectric interference layer, 4-first blocking isolation layer, 5-first metal absorption layer, 6-second metal absorption layer, 7-second blocking isolation layer, 8-second dielectric interference layer, 9-top protective layer;
[0021] Figure 2 This is a performance test diagram of the gold-coated glass in Example 1;
[0022] Figure 3 This is a performance test diagram of the gold-coated glass in Example 2;
[0023] Figure 4 This is a performance test diagram of the gold-coated glass in Example 3. DETAILED DESCRIPTION
[0024] The utility model provides a golden coated glass, comprising a glass substrate and a dielectric protection layer, a first dielectric interference layer, a first blocking isolation layer, a first metal absorption layer, a second metal absorption layer, a second blocking isolation layer, a second dielectric interference layer and a top protective layer which are sequentially stacked on the glass substrate; the first metal absorption layer is a Cu film layer, and the second metal absorption layer is a Co film layer.
[0025] The dielectric protection layer is Si 3 N 4 Layer or TiO x layer.
[0026] The thickness of the dielectric protection layer is 40-60 nm.
[0027] The first dielectric interference layer is TiO x layer or ZnO layer.
[0028] The thickness of the first dielectric interference layer is 20-40 nm.
[0029] The first barrier isolation layer is a Ni layer, a Cr layer or a NiCr layer.
[0030] The thickness of the first blocking isolation layer is 1-5 nm, preferably 3-4 nm.
[0031] The thickness of the first metal absorption layer and the second metal absorption layer are both 1-5 nm, preferably 1.5-2.5 nm and 1.6 nm respectively.
[0032] The second blocking isolation layer is a Ni layer, a Cr layer or a NiCr layer.
[0033] The thickness of the second blocking isolation layer is 1-5 nm, preferably 2-3 nm.
[0034] The second dielectric interference layer is TiO x layer or ZnO layer.
[0035] The thickness of the second dielectric interference layer is 15-30 nm.
[0036] The top protective layer is SiO 2 Layer, Si 3 N 4 Layer or TiO x layer.
[0037] The thickness of the top protective layer is 20-30 nm.
[0038] The gold-colored coated glass provided by the utility model can obtain low-radiation gold-colored coated glass with a 24K pure gold color appearance through the coordination of film layers of specific thickness.
[0039] The utility model is described in detail below in conjunction with embodiments.
[0040] Examples 1 to 3
[0041] A golden coated glass comprises a glass substrate and a dielectric protection layer, a first dielectric interference layer, a first blocking isolation layer, a first metal absorption layer, a second metal absorption layer, a second blocking isolation layer, a second dielectric interference layer and a top protective layer which are sequentially stacked on the glass substrate; the first metal absorption layer is a Cu film layer, the second metal absorption layer is a Co film layer
[0042] The materials and thicknesses of the various film layers of the gold-coated glass in each embodiment are shown in Table 1.
[0043] Table 1
[0044] Example 1 Example 2 Example 3 Glass substrate 6mm white glass 6mm white glass 6mm white glass Dielectric protection layer <![CDATA[53nm thick Si 3 N 4 > <![CDATA[48nm thick Si 3 N 4 > <![CDATA[58nm thick TiO 2 > First dielectric interference layer <![CDATA[25nm thick TiO 2 > 30nm thick ZnO 37nm thick ZnO First barrier layer 3.3nm thick NiCr 3.1nm thick NiCr 3.6nm thick NiCr First metal absorption layer 2.2nm thick Cu 1.9nm thick Cu 1.8nm thick Cu Second metal absorption layer 1.6nm thick Co 2.1nm thick Co 1.7nm thick Co Second barrier layer 2.5nm thick Cr 2.3nm thick Cr 2.6nm thick Cr Second dielectric interference layer 16nm thick ZnO <![CDATA[25nm thick TiO 2 > <![CDATA[23nm thick TiO 2 > Top protective layer <![CDATA[28nm thick Si 3 N 4 > <![CDATA[22nm thick Si 3 N 4 > <![CDATA[25nm thick Si 3 N 4 >
[0045] The performance parameters of the gold-coated glass in each embodiment are shown in Tables 2 and 3.
[0046] Table 2
[0047]
[0048]
[0049] Table 3
[0050]
[0051] It can be seen from Table 2 and Table 3 above that the gold-coated glass provided by the utility model has a 24K pure gold color and has the performance of high transmittance, low reflection and high heat transfer.
[0052] The gold-coated glass in each embodiment and ordinary white glass are made into hollow glass, and the structure of the hollow glass is: 6mm gold-coated / 12mm 85% argon spacer / 6mm white glass. The properties of the hollow glass are shown in Table 4.
[0053] Table 4
[0054]
[0055] The detailed description of a gold-coated glass with reference to the above embodiment is illustrative rather than restrictive, and several embodiments can be listed according to the limited scope. Therefore, changes and modifications without departing from the overall concept of the utility model should fall within the scope of protection of the utility model.
Claims
1. A golden coated glass, characterized in that: It includes a glass substrate and a dielectric protection layer, a first dielectric interference layer, a first blocking isolation layer, a first metal absorption layer, a second metal absorption layer, a second blocking isolation layer, a second dielectric interference layer and a top protective layer which are sequentially stacked on the glass substrate; the first metal absorption layer is a Cu film layer, and the second metal absorption layer is a Co film layer.
2. The gold-coated glass according to claim 1, characterized in that: The dielectric protection layer is a Si3N4 layer or a TiO x layer.
3. The gold-coated glass according to claim 1, characterized in that: The thickness of the dielectric protection layer is 40-60 nm.
4. The gold-coated glass according to claim 1, characterized in that: The first dielectric interference layer and the second dielectric interference layer are TiO x layer or ZnO layer.
5. The gold-coated glass according to claim 1, characterized in that: The thicknesses of the first dielectric interference layer and the second dielectric interference layer are 20-40 nm and 15-30 nm respectively.
6. The gold-coated glass according to claim 1, characterized in that: The first blocking isolation layer and the second blocking isolation layer are Ni layers, Cr layers or NiCr layers.
7. The gold-coated glass according to claim 1, characterized in that: The thickness of the first blocking isolation layer and the second blocking isolation layer are both 1-5 nm.
8. The gold-coated glass according to claim 1, characterized in that: The thickness of the first metal absorption layer and the second metal absorption layer are both 1-5 nm.
9. The gold-coated glass according to claim 1, characterized in that: The top protective layer is a SiO2 layer, a Si3N4 layer or a TiO x layer.
10. The gold-coated glass according to claim 1, characterized in that: The thickness of the top protective layer is 20-30 nm.