Testing device and system for welding cracks of laser and laser arc hybrid welding
By designing a symmetrically arranged laser and laser arc hybrid welding crack test device for restraint plates and test plates, the problem that the Tieken test in the existing technology does not conform to actual working conditions has been solved, achieving more accurate welding crack assessment and improving test efficiency. efficiency.
Patent Information
- Application Number
- CN202420379721.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-28
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2034-02-28
AI Technical Summary
The existing technology lacks effective welding crack test standards. In particular, the gap and groove forms in the Tieyan test do not meet the actual working conditions, resulting in inaccurate assessment of crack sensitivity in laser and laser arc hybrid welding.
A welding crack testing device including a symmetrically arranged restraint plate and a laser and laser arc hybrid welding with a predetermined gap is designed. The first test plate and the second test plate are set on the restraint plate and a symmetrical third test plate is formed on it. The first groove and the second groove form a test weld, which is used to simulate actual working conditions for crack testing.
The device has a simple structure and is easy to operate, which improves the efficiency of welding crack testing, solves the problem that gaps and groove forms in Tieyan tests do not conform to actual working conditions, and provides more accurate crack evaluation results.
Smart Images

Figure CN221870662U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to the technical field of welding test devices, in particular to a test device and system for welding cracks of laser and laser arc composite welding. Background Art
[0002] High-strength steel has been widely used in aerospace, automobile manufacturing, engineering machinery, shipbuilding, and military industries due to its advantages such as high specific strength, good plasticity and toughness, and easy machining.
[0003] Laser and laser-arc hybrid welding have been developed rapidly due to their fast welding speed, deep penetration, small welding deformation and other characteristics. At present, they are also widely used in the above industries, especially in thick plate welding applications, which greatly improves welding quality and production efficiency. In addition to cold cracks, hot cracks are also common defects in high-strength steel welding, especially laser welding, when laser and laser-arc hybrid welding high-strength steel plates.
[0004] Since laser welding and laser arc hybrid welding are newly developed high-efficiency welding technologies in recent years, there is currently no reference welding crack test standard. The iron-abrasive test is often used to evaluate the crack sensitivity of laser arc hybrid welding. However, the gap and groove form of the iron-abrasive test do not meet the actual working conditions. Utility Model Content
[0005] Therefore, the utility model provides a testing device and system for welding cracks of laser and laser arc hybrid welding.
[0006] In order to solve the above technical problems, the utility model provides a test device for welding cracks of laser and laser arc hybrid welding, including: two restraint plates, and the two restraint plates are symmetrically arranged, and a predetermined gap is provided between the two restraint plates; a first test plate and a second test plate, and are arranged on the restraint plates and located on the welding area of the restraint plates, the first test plate is provided with a first groove, the second test plate is provided with a second groove, the first groove and the second groove are symmetrically arranged, and the first groove and the second groove form a test weld.
[0007] Furthermore, the first test plate, the second test plate, and the restraint plate are connected by welding.
[0008] Furthermore, an angle θ1 between the first groove and a straight line where the first test plate side wall is located is 25° to 35°.
[0009] Furthermore, the side wall of the second test plate having the second groove is a welding surface, and an angle θ2 between the welding surface and a straight line where the side wall of the second test plate is located is 0-3°.
[0010] Furthermore, an angle θ3 between the second groove and a straight line where the second test plate side wall is located is 25° to 35°.
[0011] Furthermore, the welding area is the two end portions of the restraint plate.
[0012] Furthermore, the length of the restraint plate is greater than the sum of the widths of the first test plate and the second test plate.
[0013] The utility model also provides a test system for welding cracks of laser and laser arc composite welding, comprising the test device for welding cracks of laser and laser arc composite welding.
[0014] The technical solution of the utility model has the following advantages:
[0015] The utility model provides a test device for welding cracks of laser and laser arc hybrid welding, comprising: two restraint plates, which are symmetrically arranged and have a predetermined gap between the two restraint plates; a first test plate and a second test plate, which are arranged on the restraint plates and located on the welding area of the restraint plates, wherein the first test plate is provided with a first groove, and the second test plate is provided with a second groove, the first groove and the second groove are symmetrically arranged, and the first groove and the second groove form a test weld.
[0016] By setting two restraint plates, and the two restraint plates are symmetrically arranged, it is convenient to place the first test plate and the second test plate on the two restraint plates, that is, on the welding area on the restraint plates, so as to achieve the connection between the first test plate and the second test plate and the restraint plates. At the same time, a first groove is set on the first test plate, and a second groove is set on the second test plate. The two first test plates and the second test plates with grooves are symmetrically arranged to form a test weld, that is, the test weld can be subsequently operated.
[0017] The laser and laser arc hybrid welding crack test device has a relatively simple structure and is easy to operate, which is convenient for later welding crack tests and improves the efficiency of the test. The laser and laser arc hybrid welding crack test device can solve the problem that the gap and groove form in the current iron research test do not meet the actual working conditions.
[0018] The utility model summary is provided to introduce a selection of concepts in a simplified form, which will be further described in the following detailed description. The utility model summary is not intended to identify key features or essential features of the present disclosure, nor is it intended to limit the scope of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the specific implementation methods of the utility model or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the utility model. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0020] Figure 1 A schematic diagram of the structure of a test device for laser and laser arc hybrid welding cracks provided by the utility model;
[0021] Figure 2 A schematic diagram of the structure of a test device for laser and laser arc hybrid welding cracks provided by the utility model;
[0022] Figure 3 A schematic diagram of the structure of a test device for laser and laser arc hybrid welding cracks provided by the utility model;
[0023] Figure 4 The utility model provides a schematic structural diagram of a test device for welding cracks of laser and laser arc hybrid welding.
[0024] Description of reference numerals:
[0025] 1. Restraint plate; 2. First test plate; 3. Second test plate; 4. Welding area; 5. First groove; 6. Second groove; 7. Test weld. DETAILED DESCRIPTION
[0026] In the following, only certain exemplary embodiments are briefly described. As those skilled in the art will appreciate, the described embodiments may be modified in various different ways without departing from the spirit or scope of the present disclosure. Therefore, the drawings and description are to be regarded as illustrative in nature and not restrictive.
[0027] In the description of the present disclosure, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the present disclosure and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present disclosure. In addition, the terms "first" and "second" are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present disclosure, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.
[0028] In the description of the present disclosure, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or can communicate with each other; it can be directly connected, or indirectly connected through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present disclosure can be understood according to specific circumstances.
[0029] In the present disclosure, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply means that the first feature is lower in level than the second feature.
[0030] The disclosure below provides many different embodiments or examples to realize different structures of the present disclosure. In order to simplify the disclosure of the present disclosure, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present disclosure. In addition, the present disclosure can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplicity and clarity, and does not itself indicate the relationship between the various embodiments and / or settings discussed. In addition, the present disclosure provides various specific examples of processes and materials, but those of ordinary skill in the art can be aware of the application of other processes and / or the use of other materials.
[0031] The preferred embodiments of the present disclosure are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present disclosure, and are not used to limit the present disclosure.
[0032] See also Figures 1 to 4 As shown, the utility model provides a test device for welding cracks of laser and laser arc hybrid welding, including: a restraint plate 1, which has two, and the two restraint plates 1 are symmetrically arranged, and a predetermined gap is provided between the two restraint plates 1; a first test plate 2 and a second test plate 3, and are arranged on the restraint plate 1 and located on the welding area 4 of the restraint plate 1, the first test plate 2 is provided with a first groove 5, the second test plate 3 is provided with a second groove 6, the first groove 5 and the second groove 6 are symmetrically arranged, and the first groove 5 and the second groove 6 form a test weld 7.
[0033] By setting two restraint plates 1, and the two restraint plates 1 are symmetrically arranged, it is convenient to set the first test plate 2 and the second test plate 3 on the two restraint plates 1, that is, set them on the welding area 4 on the restraint plates 1, so as to achieve the connection between the first test plate 2 and the second test plate 3 and the restraint plate 1. At the same time, a first groove 5 is set on the first test plate 2, and a second groove 6 is set on the second test plate 3. The two first test plates 2 and the second test plates 3 with grooves are symmetrically arranged to form a test weld 7, that is, the test weld 7 can be subjected to subsequent operations.
[0034] The laser and laser arc hybrid welding crack test device has a relatively simple structure and is easy to operate, which is convenient for later welding crack tests and improves the efficiency of the test. The laser and laser arc hybrid welding crack test device can solve the problem that the gap and groove form in the current iron research test do not meet the actual working conditions.
[0035] The first test plate 2 and the second test plate 3 are welded to the restraining plate 1. That is, the first test plate 2 and the second test plate 3 are welded to the welding area 4 of the restraining plate 1, and a restraining weld is formed with the restraining plate 1. The first test plate 2 and the second test plate 3 are also welded to form a test weld 7.
[0036] In some optional embodiments, the angle θ1 between the first groove 5 and the straight line where the side wall of the first test plate 2 is located is 25° to 35°. The side wall of the second test plate 3 having the second groove 6 is a welding surface, and the angle θ2 between the welding surface and the straight line where the side wall of the second test plate 3 is located is 0 to 3°. The angle θ3 between the second groove 6 and the straight line where the side wall of the second test plate 3 is located is 25° to 35°.
[0037] Specifically, the welding area 4 is the two end portions of the restraining plate 1. Of course, the welding area 4 can also be adjusted according to actual conditions.
[0038] There are four welding areas 4 , and the first test plate 2 , the second test plate 3 and the restraint plate 1 can form four test welds 7 .
[0039] In some optional embodiments, the length of the restraint plate 1 is greater than the sum of the widths of the first test plate 2 and the second test plate 3. This arrangement facilitates the connection of the first test plate 2 and the second test plate 3 with the restraint plate 1, provides a welding position for the first test plate 2 and the second test plate 3 to be welded to the restraint plate 1, and forms a weld, while increasing the stability of the connection.
[0040] The test process of laser and laser arc hybrid welding cracks includes the following steps:
[0041] Step 1: Follow Figure 1 and Figure 2 A first test plate 2 and a second test plate 3, and a restraining plate 1 used in a processing test;
[0042] Step 2: Follow Figure 3 and Figure 4 The first test plate 2, the second test plate 3 and the restraining plate 1 are rigidly fixed by welding;
[0043] Step 3: Weld the test weld 7 on the test device according to the welding process method, preheating temperature and process parameters used. After welding, place it together with the test device for 48 hours, and then inspect the surface and cross section of the test weld 7.
[0044] Among them, t1 in the test plate is set to adapt to the laser welding penetration depth, and its range is 8 to 20 mm; θ2 is set according to the melt width suitable for laser welding, and its angle range is 0 to 3°; θ1 and θ3 are set according to the actual angle of laser arc hybrid welding to make stress concentration points appear in the heat affected zone of the weld, making the entire device more prone to cracking, and its angle range is 25 to 35°.
[0045] At the same time, a method for detecting welding cracks in laser and laser arc hybrid welding is proposed, including the surface and cross section of the test weld 7.
[0046] Among them, the surface of the test weld is subjected to appearance inspection and penetration inspection, and the surface crack length and the test weld length are measured by a steel ruler, and the results are counted, and the crack rate is calculated according to formula 1;
[0047]
[0048] Where:
[0049] C f ——Surface crack rate, %;
[0050] L——test weld length, in millimeters (mm);
[0051] ∑l f ——Total length of surface cracks, in millimeters (mm).
[0052] Metallographic examination was performed on the cross section of the test weld, and the test weld was machined and dissected. Five cross sections were cut along the welding direction, and metallographic examination was performed on each cross section. The cross-sectional crack length and minimum weld height were statistically analyzed, and the cross-sectional crack rate of the weld was calculated according to Formula 2.
[0053]
[0054] Where:
[0055] C s ——Crack rate of profile, %;
[0056] H——minimum thickness of the test weld, in millimeters (mm);
[0057] H c ——Height of the root crack, in millimeters (mm).
[0058] Furthermore, an evaluation of the test results of laser and laser arc hybrid welding cracks is proposed. If cracks occur, the preheating temperature can be increased and the test can be carried out again to determine the final preheating temperature.
[0059] The utility model also provides a test system for welding cracks of laser and laser arc composite welding, comprising the test device for welding cracks of laser and laser arc composite welding.
[0060] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention of the utility model.
Claims
1. A test device for welding cracks of laser and laser arc hybrid welding, characterized in that: include: There are two restraint plates (1), and the two restraint plates (1) are symmetrically arranged, and a predetermined gap is provided between the two restraint plates (1); A first test plate (2) and a second test plate (3) are arranged on the restraining plate (1) and located on the welding area (4) of the restraining plate (1); a first groove (5) is arranged on the first test plate (2), and a second groove (6) is arranged on the second test plate (3); the first groove (5) and the second groove (6) are symmetrically arranged, and the first groove (5) and the second groove (6) form a test weld (7).
2. The testing device for welding cracks of laser and laser arc hybrid welding according to claim 1 is characterized in that: The first test plate (2), the second test plate (3), and the restraining plate (1) are connected by welding.
3. The testing device for welding cracks of laser and laser arc hybrid welding according to claim 2, characterized in that: The angle θ1 between the first groove (5) and the straight line on which the side wall of the first test plate (2) is located is 25° to 35°.
4. The test device for laser and laser arc hybrid welding cracks according to any one of claims 1 to 3, characterized in that: The side wall of the second test plate (3) having the second groove (6) is a welding surface, and the angle θ2 between the welding surface and the straight line where the side wall of the second test plate (3) is located is 0 to 3°.
5. The testing device for welding cracks of laser and laser arc hybrid welding according to claim 4, characterized in that: The angle θ3 between the second groove (6) and the straight line on which the side wall of the second test plate (3) is located is 25° to 35°.
6. The testing device for welding cracks of laser and laser arc hybrid welding according to claim 5, characterized in that: The welding area (4) is the two end portions of the restraining plate (1).
7. The testing device for welding cracks of laser and laser arc hybrid welding according to claim 6, characterized in that: The length of the restraining plate (1) is greater than the sum of the widths of the first test plate (2) and the second test plate (3).
8. A laser and laser arc hybrid welding crack test system, characterized in that: A testing device for welding cracks of laser and laser arc hybrid welding comprising any one of claims 1-7.
Citation Information
Cited By
Device and method for testing welding crack sensitivity of copper-nickel alloy pipe
CN121253794A