Plating layer structure plated with white gun color pearl tin-nickel alloy
Through the polymeric thiocyanate copper plating process and multi-layer plating structure, the problems of contamination of the traditional cyanide copper plating process and insufficient corrosion resistance of pearl nickel plating are solved, and high bonding force and corrosion resistance of the surface of steel parts are achieved. Plating provides a safer and more efficient decorative effect.
Patent Information
- Application Number
- CN202323360853.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-11
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2033-12-11
AI Technical Summary
The traditional cyanide copper plating process has problems of high pollution and high risks when preparing steel parts, and the pearl nickel coating has poor discoloration resistance and low corrosion resistance, and cannot effectively replace the hexavalent chromium decorative chromium plating layer.
The polymerized thiocyanate copper plating process is used instead of cyanide copper plating to prepare the pre-copper layer, and based on it, acid copper plating, pearl nickel plating and white gun-colored pearl tin-nickel alloy plating are formed in sequence. Through this layer structure, the Coating strength and corrosion resistance.
It achieves a good combination of the surface of the steel parts and the pre-plated copper layer, increases the thickness and brightness of the coating, provides anti-corrosion and decorative effects, and slows down the corrosion of the pearl nickel coating through the high corrosion resistance of the white gun-colored pearl tin-nickel alloy coating. The corrosion speed overcomes the pollution and risk problems of traditional processes and fills the gap in the domestic market for white gun-colored pearl tin-nickel alloy coatings.
Smart Images

Figure CN221877206U_ABST
Abstract
Description
Technical Field
[0001] The utility model belongs to the field of metal electroplating, and in particular relates to a plating structure of a white gun-colored pearl tin-nickel alloy. Background Art
[0002] Electroplating white gunmetal tin-nickel alloy is used to prepare a bright tin-nickel alloy coating. The coating is dark white, has a uniform alloy content, and has extremely high corrosion resistance. It is an ideal anti-corrosion coating and functional coating, and is usually used to replace hexavalent chromium decorative chrome plating.
[0003] Pearl nickel plating is soft and elegant, and has been widely used in instrumentation and hardware industries. However, pearl nickel plating has poor anti-discoloration ability and low corrosion resistance.
[0004] White gunmetal pearl tin-nickel alloy plating has a more elegant appearance than pearl nickel plating and has excellent corrosion resistance, but it has not yet been developed and applied.
[0005] According to the traditional process, steel parts are prepared with a pre-copper layer by cyanide copper plating, followed by pyrophosphate copper plating, acid copper plating, bright nickel plating, etc. However, it is not yet mature to replace cyanide copper plating with the current divalent copper cyanide-free copper plating process, and the problem of coating bonding strength still needs further research. [1] .
[0006] The polythiocyanate copper plating process is a newly developed cyanide-free copper plating process. It uses polycuprous thiocyanate as the main salt and polysodium thiocyanate as the coordination agent. Its process characteristics and performance are close to traditional cyanide copper plating. It is currently in the development and trial stage.
[0007] References: [1] Qin Zuzu, Li Jiansan, Xu Jinlai, Research progress of cyanide-free copper plating technology at home and abroad [J], Electroplating and Finishing, 2015, 34(3): 149-152. Summary of the invention
[0008] In order to solve the high pollution problem of the cyanide pre-plated copper layer prepared by the traditional method for steel parts, the utility model provides a plating structure of a white gun-colored pearl tin-nickel alloy. In order to achieve the above purpose, the utility model adopts the following technical solutions:
[0009] A coating structure of a white gun-colored pearl tin-nickel alloy, characterized in that it comprises a steel substrate, and a polymerized thiocyanate pre-plated copper layer, an acid copper plating layer, a pearl nickel plating layer, and a white gun-colored pearl tin-nickel alloy plating layer sequentially prepared on the steel substrate;
[0010] The thickness of the polymerized thiocyanate pre-plated copper layer is 1-4 μm.
[0011] Preferably, the thickness of the acid copper plating layer is 15 to 25 μm.
[0012] Preferably, the thickness of the pearl nickel plating layer is 3-5 μm.
[0013] Preferably, the thickness of the white gunmetal pearl tin-nickel alloy plating layer is 0.2-0.3 μm.
[0014] The surface of steel parts is pre-copper-plated with polythiocyanate, and good bonding can be formed between the coating and the steel substrate. Acid copper plating is used to increase the thickness and brightness of the coating to achieve anti-corrosion and decorative effects. Pearl nickel is plated on the copper plating layer. The electrode potential of the pearl nickel plating is relatively negative, and it is an anodic coating with respect to the copper plating layer. This coating structure can better block the corrosion of the corrosive medium toward the substrate. White gun-colored pearl tin-nickel alloy is plated on the pearl nickel plating, and the electrode potential of the prepared coating is positive than that of the pearl nickel plating. When this coating structure is corroded, the corrosive medium first corrodes the pearl nickel plating and corrodes in the lateral direction, but the white gun-colored pearl tin-nickel alloy coating has high corrosion resistance and can effectively slow down the corrosion rate of the pearl nickel plating.
[0015] Compared with the prior art, the utility model has the following beneficial effects:
[0016] 1. The utility model discloses a coating structure of a white gun-colored pearl tin-nickel alloy, which adopts a polymerized thiocyanate copper plating process instead of a cyanide copper plating process to prepare a pre-plated copper layer, thus overcoming the high pollution and high risk problems caused by the use of cyanide;
[0017] 2. The coating structure of the white gun-colored pearl tin-nickel alloy plated disclosed by the utility model fills the blank of the white gun-colored pearl tin-nickel alloy plated in the domestic market. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The drawings described herein are used to provide a further understanding of the present invention, constitute a part of the present application, and do not constitute an improper limitation of the present invention. In the drawings:
[0019] Figure 1 It is a schematic diagram of the coating structure of Example 1 and Example 2 of the utility model. Implementation
[0020] The present invention will be described in detail below in conjunction with the accompanying drawings and specific embodiments. The schematic embodiments and descriptions of the present invention are used to explain the present invention but are not intended to limit the present invention.
[0021] A polymerized thiocyanate pre-plated copper layer, an acid copper plating layer, a pearl nickel plating layer, and a white gun-colored pearl tin-nickel alloy plating layer are sequentially prepared on a steel substrate from the inside to the outside.
[0022] The existing pre-treatment process is used to degrease, remove rust and activate the steel substrate.
[0023] After pretreatment of steel parts, a polythiocyanate copper plating process is adopted to prepare a polythiocyanate pre-plated copper layer.
[0024] Preferably, the thickness of the polymerized thiocyanate pre-copper plating layer is 1 to 4 μm.
[0025] Preferably, the polymerized thiocyanate pre-copper plating layer is prepared by using Zunyi Huitong's HT-810 polymerized thiocyanate copper plating process:
[0026] Polymeric cuprous thiocyanate 17-23 g / L, polymeric sodium thiocyanate 100-160 g / L, potassium sodium tartrate 8-12 g / L, HT-810 brightener 1-2 mL / L, HT-810 moving agent 2-4 mL / L, plating tank temperature 45°C-55°C, plating solution pH range 12-13, cathode current density 0.5-1.0 A / dm 2 , cathode movement 4~6m / min, anode current density ≤0.5A / dm 2 , use oxygen-free electrolytic copper corners (or copper particles) as anodes.
[0027] After the steel parts are pre-coppered with polymerized thiocyanate, the acid copper coating is prepared by the current acid copper plating process.
[0028] Preferably, the thickness of the acid copper plating layer is 15 to 25 μm.
[0029] After the steel parts are plated with acid copper, the pearl nickel coating is prepared by the current pearl nickel plating process.
[0030] Preferably, the thickness of the pearl nickel plating layer is 3-5 μm.
[0031] After the steel parts are plated with pearl nickel, the current white gun-colored tin-nickel alloy plating process is adopted to prepare the white gun-colored pearl tin-nickel alloy plating layer.
[0032] Preferably, the thickness of the white gunmetal pearl tin-nickel alloy plating layer is 0.2-0.3 μm.
[0033] Preferably, the white gunmetal pearl tin-nickel alloy coating is prepared by using the PGA-215 white gunmetal tin-nickel alloy plating process of Chaobang Chemical:
[0034] Nickel chloride hexahydrate 135~175g / L, PGA-215A additive 450~500mL / L, PGA-215B additive 30~60mL / L, PGA-215C additive 10~30mL / L, plating solution pH range 3.5~4.5, plating tank temperature 63℃~73℃, cathode current density 0.5~1.5A / dm 2 , the cathode moves 4 to 6 m / min.
[0035] Steel parts are plated with white gunmetal tin-nickel alloy and then passivated and dried:
[0036] The specific process is "oxidation with 5% volume fraction hydrogen peroxide → water washing → pure water washing → centrifuge dehydration → drying". Example 1
[0037] like Figure 1 As shown, a coating structure of a white gun-colored pearl tin-nickel alloy is provided, comprising a steel substrate 1, and a polymerized thiocyanate pre-plated copper layer 2, an acid copper coating layer 3, a pearl nickel coating layer 4, and a white gun-colored pearl tin-nickel alloy coating layer 5 which are sequentially prepared on the steel substrate 1 from the inside to the outside.
[0038] 1. Pre-treatment:
[0039] The steel substrate 1 is subjected to "alkaline chemical degreasing → water washing → acid washing → water washing → alkaline cathode electrolytic degreasing → water washing → alkaline anodic electrolytic degreasing → water washing → activation → water washing".
[0040] 2. Polythiocyanate pre-copper plating:
[0041] After pretreatment of the steel parts, the thiocyanate pre-plated copper layer 2 was prepared by Zunyi Huitong's HT-810 polymerized thiocyanate copper plating process, and the coating thickness was 2 μm.
[0042] Polymerized cuprous thiocyanate 18g / L, polymerized sodium thiocyanate 120g / L, potassium sodium tartrate 10g / L, HT-810 brightener 1.5mL / L, HT-810 moving agent 3mL / L, plating tank temperature 53℃, plating solution pH 12.8, cathode current density 0.7A / dm 2 , cathode movement 5m / min, anode current density 0.4A / dm 2 , use oxygen-free electrolytic copper corner as anode.
[0043] 3. Acid copper plating:
[0044] After the steel parts are pre-copper-plated with polymerized thiocyanate, an acid copper coating 3 is prepared by using the current acid copper plating process, and the coating thickness is 20 μm.
[0045] 4. Pearl nickel plating:
[0046] After the steel parts are plated with acid copper, a pearl nickel coating 4 is prepared by using the current pearl nickel coating process, and the coating thickness is 4 μm.
[0047] 5. White gun-colored pearl tin-nickel alloy:
[0048] After the steel parts are plated with pearl nickel, the white gun-colored pearl tin-nickel alloy coating 5 is prepared by the PGA-215 white gun-colored tin-nickel alloy plating process of Chaobang Chemical, and the coating thickness is 0.25 μm.
[0049] Nickel chloride hexahydrate 140g / L, PGA-215A additive 460mL / L, PGA-215B additive 40mL / L, PGA-215C additive 15mL / L, plating solution pH 4.2, plating tank temperature 68℃, cathode current density 0.8A / dm 2 , cathode moves 5m / min.
[0050] 6. Passivation and drying:
[0051] After the steel parts are plated with white gun-colored pearl tin-nickel alloy, they are "oxidized with 5% volume fraction hydrogen peroxide → washed with water → washed with pure water → dried". Example 2
[0052] like Figure 1 As shown, a coating structure of a white gun-colored pearl tin-nickel alloy is provided, comprising a steel substrate 1, and a polymerized thiocyanate pre-plated copper layer 2, an acid copper coating layer 3, a pearl nickel coating layer 4, and a white gun-colored pearl tin-nickel alloy coating layer 5 which are sequentially prepared on the steel substrate 1 from the inside to the outside.
[0053] 1. Pre-treatment:
[0054] The steel substrate 1 is subjected to "alkaline chemical degreasing → water washing → acid washing → water washing → alkaline cathode electrolytic degreasing → water washing → alkaline anodic electrolytic degreasing → water washing → activation → water washing".
[0055] 2. Polythiocyanate pre-copper plating:
[0056] After pretreatment of the steel parts, the polythiocyanate pre-plated copper layer 2 was prepared by using the HT-810 polythiocyanate copper plating process of Zunyi Huitong, and the coating thickness was 4 μm.
[0057] Polymerized cuprous thiocyanate 22g / L, polymerized sodium thiocyanate 150g / L, potassium sodium tartrate 10g / L, HT-810 brightener 1.5mL / L, HT-810 moving agent 3mL / L, plating tank temperature 52℃, plating solution pH 12.5, cathode current density 0.8A / dm 2 , cathode movement 5m / min, anode current density 0.3A / dm 2 , using oxygen-free electrolytic copper particles as anode.
[0058] 3. Acid copper plating:
[0059] After the steel parts are pre-copper-plated with polymerized thiocyanate, an acid copper coating 3 is prepared by using the current acid copper plating process, and the coating thickness is 18 μm.
[0060] 4. Pearl nickel plating:
[0061] After the steel parts are plated with acid copper, a pearl nickel coating 4 is prepared by using the current pearl nickel coating process, and the coating thickness is 4 μm.
[0062] 5. White gun-colored pearl tin-nickel alloy:
[0063] After the steel parts are plated with pearl nickel, the white gun-colored pearl tin-nickel alloy coating 5 is prepared by the PGA-215 white gun-colored tin-nickel alloy plating process of Chaobang Chemical, and the coating thickness is 0.25 μm.
[0064] Nickel chloride hexahydrate 170g / L, PGA-215A additive 480mL / L, PGA-215B additive 50mL / L, PGA-215C additive 25mL / L, plating solution pH 3.8, plating tank temperature 64℃, cathode current density 1.2A / dm 2 , cathode moves 5m / min.
[0065] 6. Passivation and drying:
[0066] After the steel parts are plated with white gun-colored pearl tin-nickel alloy, they are "oxidized with 5% volume fraction hydrogen peroxide → washed with water → washed with pure water → dried".
[0067] Test Example 1:
[0068] The white gun-colored pearl tin-nickel alloy samples prepared in Example 1 and Example 2 were tested for coating adhesion by a thermal shock test method in accordance with GB / T 5270-2005 "Review of test methods for adhesion strength of electrodeposited and chemically deposited metal coatings on metal substrates". The samples were placed in a heating furnace and heated to 220°C for 30 minutes, then taken out and suddenly cooled in water at room temperature. The coating did not blister or fall off, and its adhesion was good.
[0069] Test Example 2:
[0070] The white gun-colored pearl tin-nickel alloy samples prepared in Example 1 and Example 2 were subjected to an acetic acid salt spray test for 54 hours in accordance with GB / T 10125-2021 "Artificial atmosphere corrosion test salt spray test". No red rust was generated on the surface of the samples, and the prepared coating had good corrosion resistance.
[0071] The technical solutions provided by the embodiments of the present utility model are described in detail above. The principles and implementation methods of the embodiments of the present utility model are described in detail in this article using specific examples. The description of the above embodiments is only applicable to help understand the principles of the embodiments of the present utility model. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present utility model, which all belong to the protection scope of the present utility model.
Claims
1. A coating structure of a white gun-colored pearl tin-nickel alloy, characterized in that: It comprises a steel substrate, and a polymerized thiocyanate pre-plated copper layer, an acid copper plating layer, a pearl nickel plating layer, and a white gun-colored pearl tin-nickel alloy plating layer which are sequentially prepared on the steel substrate; The thickness of the polymerized thiocyanate pre-plated copper layer is 1-4 μm.
2. The coating structure of the white gunmetal pearl tin-nickel alloy as claimed in claim 1, characterized in that: The thickness of the acid copper plating layer is 15 to 25 μm.
3. The coating structure of the white gunmetal pearl tin-nickel alloy as claimed in claim 1, characterized in that: The thickness of the pearl nickel plating layer is 3-5 μm.
4. The coating structure of the white gunmetal pearl tin-nickel alloy as claimed in claim 1, characterized in that: The thickness of the white gunmetal pearl tin-nickel alloy plating layer is 0.2-0.3 μm.