Polyamide preparation device

By using the cavity and detection system of the magnetic seal device in the polyamide preparation device, the pressure and water content in the cavity are monitored and adjusted in real time to prevent condensation and reflux of water vapor, thus solving the problems of poor stability and safety during the polyamide preparation process. High stability and safe polymerization are achieved.

CN221889833UActive Publication Date: 2024-10-25SHANGHAI ZHONGHUA TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202323664123.9
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-12-29
Publication Date
2024-10-25
Estimated Expiration
2033-12-29

AI Technical Summary

Technical Problem

In the preparation process of polyamide, the magnetic seal device leads to problems of poor product stability and unsafe production. This is mainly due to the condensation and reflux of water vapor, which leads to inaccurate temperature control, affects the stability of process parameters, and may even cause the material to solidify and damage the polymerization device.

Method used

A polyamide preparation device is designed, which uses a magnetic sealing element to connect the cavity to the reaction kettle. The pressure and water content detection elements are used to monitor and adjust the pressure and water content in the cavity in real time to prevent the backflow of condensed water and ensure the material in the kettle. Uniformity and temperature control.

Benefits of technology

It effectively solves the problems of poor product stability and production safety, improves the stability of polyamide between batches, and ensures the safety and efficiency of polymerization reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221889833U_ABST
    Figure CN221889833U_ABST
Patent Text Reader

Abstract

The utility model provides a polyamide preparation device. The preparation device comprises a magnetic sealing element, a driving shaft and a reaction kettle, a cavity is formed in the magnetic sealing element, the magnetic sealing element is arranged at the top of the reaction kettle, one end of the driving shaft is arranged in the reaction kettle, and the other end of the driving shaft is arranged in the cavity; the polyamide preparation device further comprises a balance module, and the structure of the balance module is a first structure or a second structure. The utility model can effectively solve the problem of condensation reflux of gas-phase water vapor in polyamide production, and can keep the uniformity of materials in the kettle all the time, thereby obtaining products with stable performance and polyamide products with higher batch stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to a preparation device for polyamide. Background Art

[0002] In industrial production, the salt solution polymerization method is mostly used to prepare diacid diamine type polyamide. This method is to first prepare a certain concentration of nylon salt solution with monomer diamine and diacid, and then increase the temperature and pressure to carry out the polymerization reaction. This method usually has the advantages of controllable polymerization temperature, avoidance of local overheating, low system viscosity, and small amount of gel during polymerization. However, this method needs to be carried out under high temperature and high pressure process conditions; because a large amount of water is used as the reaction medium, a gas phase mainly composed of water vapor is formed inside the reaction system during the prepolymerization stage and prepolymerization stage of the raw material polymerization reaction. This polymerization reaction usually uses a reactor as a high temperature and high pressure reaction site, and the reactor needs to be equipped with a sealing device to ensure its airtightness.

[0003] There are two main designs for reactor seals: mechanical seals and magnetic seals. A balance tank must be included in a mechanical seal. In a mechanical seal, there are two unconnected cavities in front and behind the seal ring. Generally, the seal ring is a non-pressure-bearing component. The function of the balance tank is to balance the pressure of the cavities in front and behind the seal ring to prevent the seal ring from being damaged prematurely. If a mechanical seal is used to seal the reactor, since the medium in the balance tank is usually liquid, there is a risk that the liquid will leak into the reactor and contaminate the materials in the reactor. Therefore, mechanical seals are usually used in places with lower pressures and reaction systems with low requirements for material cleanliness.

[0004] In order to avoid contamination of the materials in the reactor and enable the reactor to withstand higher process pressure, the reactor is usually equipped with a magnetic sealing stirring device. Usually, the conventional magnetic sealing cavity is connected to the inside of the reactor, and its sealing effect is achieved through a closed cavity rather than the sealing ring in the mechanical sealing device.

[0005] However, the reactor equipped with a magnetic sealing device has poor stability between product batches. In severe cases, it may cause the material to solidify and damage the polymerization device, resulting in serious production accidents.

[0006] Therefore, there is an urgent need to provide a polyamide preparation device and method with high product stability and safe production. Utility Model Content

[0007] The utility model provides a polyamide preparation device to overcome the defects of the prior art that the raw materials are easily contaminated, the product stability is poor when using a magnetic sealing device, and the production is unsafe. The utility model can effectively solve the problem of condensation and reflux of gas phase water vapor in polyamide production, and always keep the uniformity of the materials in the kettle, so as to obtain a product with stable performance and a polyamide product with high batch stability.

[0008] During the production process, the polyamide produced by the reactor equipped with a magnetic sealing device has poor stability, and some batches cannot meet the required product performance requirements. In the process of studying the reasons for this result, the inventors found that because the magnetic sealing cavity is connected to the reactor, when the temperature and pressure of the reactor are increased, water vapor in the reaction system will enter the magnetic sealing cavity and condense to form condensed water, and then flow back into the reactor, causing the problem that the temperature in the reactor cannot be accurately controlled, thereby causing other production process parameters to fluctuate. The fluctuation of this process parameter is the reason for the poor stability between product batches. In severe cases, the reflux of condensed water may even cause the material to solidify and damage the polymerization device, resulting in very serious production accidents. The utility model solves the above technical problems through the following technical solutions:

[0009] The utility model provides a polyamide preparation device, which comprises a magnetic sealing element, a driving shaft and a reactor, wherein a cavity is provided inside the magnetic sealing element and the magnetic sealing element is arranged on the top of the reactor, one end of the driving shaft is arranged inside the reactor, and the other end is arranged in the cavity;

[0010] The polyamide preparation device further comprises a balancing module, and the structure of the balancing module is structure one or structure two:

[0011] The structure 1 comprises an intake pipe, a first exhaust pipe, and a pressure measuring element, a first signal processing element and a first feedback element which are electrically connected in sequence; the first exhaust pipe and the intake pipe are both in communication with the cavity, and the first exhaust pipe and the intake pipe are respectively provided with a first control valve and a second control valve; the pressure measuring element is arranged inside the reactor and the cavity, and is used to monitor the internal pressure of the reactor and the cavity respectively; the first signal processing element is used to judge whether the difference between the internal pressure of the reactor and the cavity meets the set condition, and if so, it is converted into a pressure control signal, or to judge whether the internal pressure of the reactor and / or the cavity reaches the rated pressure, and if not, it is converted into a pressure control signal; the first feedback element is respectively connected with the first control valve and the second control valve, and is used to control the first control valve or the second control valve in real time according to the pressure control signal, so as to adjust the internal pressure of the cavity;

[0012] The second structure includes a second exhaust pipe, and a water content detection element, a second signal processing element and a second feedback element which are electrically connected in sequence; the second exhaust pipe is communicated with the cavity, and a third control valve is provided on the second exhaust pipe; the water content detection element is arranged inside the cavity, and is used to detect the internal water content of the cavity; the second signal processing element is used to judge whether the internal water content exceeds a threshold value, and determine whether it is necessary to send a water content control signal to the second feedback element; the second feedback element is connected to the third control valve, and is used to control the opening and closing of the third control valve according to the water content control signal.

[0013] In the utility model, the pressure measuring element of the structure one can collect the internal pressure of the cavity in the magnetic sealing element and the reactor, and determine whether the pressure difference between the two meets the set conditions through the signal processing element. If so, it is converted into a pressure control signal, and the opening and closing of the second control valve is controlled to adjust the air intake of the protective gas, and the pressure of the cavity in the magnetic sealing element is supplemented to balance the pressure of the cavity in the magnetic sealing element and the inside of the reactor; or, the pressure measuring element of the structure one can also collect the internal pressure of the cavity in the magnetic sealing element and the reactor, and determine whether the internal pressure of the reactor and / or the cavity reaches the rated pressure through the signal processing element. If the rated pressure is not reached, it is converted into a pressure control signal, and the opening and closing of the second control valve is controlled to adjust the air intake of the protective gas, and the pressure of the cavity in the magnetic sealing element is supplemented to make the reactor and / or the cavity reach the rated pressure.

[0014] In the utility model, the water content detection element of the structure 2 can collect the water content inside the cavity in the magnetic sealing element, and control the opening and closing of the third control valve to discharge the condensed water in the cavity in time to prevent the condensed water from flowing back.

[0015] In the utility model, the magnetic sealing element can be a magnetic cylinder in the art.

[0016] In some embodiments, the reactor is provided with a third exhaust pipe, and the third exhaust pipe is provided with a fourth control valve.

[0017] In a specific embodiment, the fourth control valve is connected to the first feedback element and is used to adjust the fourth control valve according to the pressure control signal, thereby controlling the internal pressure of the reactor to balance the internal pressure of the cavity with the internal pressure of the reactor.

[0018] In a specific implementation, the fourth control valve is connected to the second feedback element, and the fourth control valve is adjusted according to the water content control signal to control the internal pressure of the reactor.

[0019] In the present invention, the polyamide preparation device as described above can be used to prepare polyamide, which includes the following steps: sequentially concentrating, prepolymerizing and post-polymerizing the polyamide salt solution; and the polyamide preparation method also includes the following method 1 or method 2:

[0020] Mode 1: In the step of concentration and the step of prepolymerization, the internal pressures of the reactor and the cavity are monitored and compared, and it is determined whether the difference between the internal pressures of the reactor and the cavity meets a set condition. If the set condition is met, it is converted into a pressure control signal; or, it is determined whether the internal pressures of the reactor and / or the cavity reach a rated pressure. If the rated pressure is not reached, it is converted into a pressure control signal; according to the pressure control signal, the second control valve is controlled to adjust the flow rate of the protective gas entering the cavity to maintain the pressure in the cavity balanced with the pressure of the reactor;

[0021] Method 2: In the concentration step and the prepolymerization step, the internal water content of the cavity is detected to determine whether the internal water content exceeds a threshold value, and whether it is necessary to send a water content control signal to the second feedback element; according to the water content control signal, the third control valve is controlled to discharge liquid water in the cavity.

[0022] In the utility model, the first method controls the pressure balance between the cavity and the reactor so that water vapor cannot enter the cavity and condense and reflux.

[0023] In the utility model, the second method timely discharges the water in the cavity, thereby preventing the water vapor from condensing and flowing back.

[0024] In some embodiments, the set condition includes a difference between the internal pressure of the reactor and the internal pressure of the cavity being greater than or equal to 0.01 MPa.

[0025] In a specific implementation, when the difference between the internal pressure of the reactor and the internal pressure of the cavity is greater than or equal to 0.01 MPa, the comparison result of the pressure difference is converted into the control signal, and the first control valve or the second control valve is controlled.

[0026] In a specific embodiment, when the difference between the internal pressure of the reactor and the internal pressure of the cavity is less than 0.01 MPa, no control signal is generated.

[0027] In some embodiments, when the liquid level inside the cavity is greater than or equal to the first preset liquid level, the water content signal is converted into the control signal, and the third control valve is controlled; preferably, the first preset liquid level is greater than or equal to 2%, where % is the percentage of the height of the first preset liquid level to the height of the cavity, for example, the first preset liquid level is greater than or equal to 3%, or greater than or equal to 5%.

[0028] In some embodiments, when the liquid level inside the cavity is less than a second preset liquid level, no control signal is generated; preferably, the second preset liquid level is less than 2%, where % is the percentage of the height of the second preset liquid level to the height of the cavity, for example, the second preset liquid level is less than 1%, or less than 0.5%.

[0029] In some embodiments, when the pressure of the cavity is less than the rated pressure, the second control valve is opened according to the pressure control signal to introduce protective gas into the cavity to increase the pressure of the cavity to the pressure of the reactor.

[0030] In some embodiments, when the water content of the cavity is greater than a threshold value, the third control valve is opened according to the control signal to discharge the liquid water in the cavity.

[0031] In some embodiments, the rated pressure of the cavity and the reactor is set to 1.0 MPa, and when the internal pressure of the cavity and the reactor is lower than 1.0 MPa, the second control valve is automatically adjusted.

[0032] In some embodiments, the pressure relief rate of the fourth control valve on the third exhaust pipe of the reactor is 0.5-3.5 MPa / h, for example, 2.5 MPa / h.

[0033] In some embodiments, the polyamide salt solution is obtained by a salt-forming reaction between a diamine and a diacid.

[0034] In a specific embodiment, the temperature of the salt-forming reaction is 150° C. or below.

[0035] In a specific embodiment, the molar ratio of the diamine monomer to the diacid monomer is (0.8-1.2):1, preferably (0.9-1.1):1.

[0036] In a specific embodiment, the monomer of the diacid is one or more of succinic acid, glutaric acid, adipic acid, suberic acid, sebacic acid, dodecanedioic acid, terephthalic acid and isophthalic acid, preferably one or more of adipic acid, sebacic acid or dodecanedioic acid.

[0037] In a specific embodiment, the monomer of the diamine is one or more of m-xylylenediamine, terephthalic acid, zero-xylylenediamine, decanediamine, pentamethylenediamine, dodecanediamine, hexamethylenediamine and butanediamine.

[0038] In some embodiments, the concentration of the polyamide salt solution is 30-70 wt.%.

[0039] In some embodiments, the pH value of the polyamide salt solution is 5.8-9.2, preferably 7.0-8.5.

[0040] In the utility model, the above-mentioned salt formation method is not only convenient for adjusting the molar ratio of the diacid and the diamine, but also the polyamide salt solution is in a homogeneous state with low viscosity, which is convenient for pipeline transmission of the salt solution and easy to operate for feeding.

[0041] In some embodiments, the concentration temperature is 150-210°C, such as 160°C or 180°C.

[0042] In some embodiments, the concentration pressure is 0.3-1.0 MPa, such as 0.6 MPa or 0.8 MPa.

[0043] In some embodiments, the concentration of the polyamide salt solution after the concentration is 60-85 wt.%.

[0044] In the utility model, through the concentration, the water in the system can be discharged at the bottom temperature, reducing energy consumption and operation complexity, and shortening the subsequent material heating time and drainage cycle, further improving the efficiency of the entire process.

[0045] In some embodiments, in the first method, the protective gas includes nitrogen.

[0046] In some implementations, in the second method, the third control valve is opened and closed intermittently; preferably, the intermittent time interval is 5 minutes.

[0047] In some embodiments, the prepolymerization temperature is 210-260°C, such as 230°C or 255°C.

[0048] In some embodiments, the prepolymerization pressure is 0.5-3.5 MPa, such as 1.9 MPa or 2.8 MPa.

[0049] In some embodiments, the prepolymerization time is 0.5-3 h, such as 1 h.

[0050] In some embodiments, the prepolymerization includes depressurizing the reactor.

[0051] In a specific embodiment, the pressure release rate is 0.5-3.5 MPa / h, such as 2.0 MPa / h or 2.5 MPa / h.

[0052] In a specific implementation manner, after the pressure relief, the pressure of the reactor is normal pressure.

[0053] In a specific embodiment, the post-polymerization temperature is 250-310°C, such as 300°C.

[0054] In the utility model, whether the polymerization needs to be carried out under vacuum conditions is determined according to the viscosity of the final product.

[0055] In a specific embodiment, the post-polymerization pressure is normal pressure; or, the post-polymerization pressure is -0.03-0.06 MPa.

[0056] In a specific embodiment, the post-polymerization time is 0.5-2 h, such as 0.5 h.

[0057] In the utility model, a viscosity detection device is used to determine whether the viscosity of the post-polymerization product meets the requirement; if it has, the pressure in the reactor is flushed to normal pressure or slightly positive pressure by an inert gas, the discharge valve at the bottom of the reactor is opened to discharge the material, and then the material is cast through a casting head, cooled and solidified in a cooling tank, and then sliced ​​and granulated by a granulator, and then sieved, dried, and packaged to complete the production.

[0058] In a specific embodiment, after completing the post-polymerization step, the method for preparing polyamide further comprises: strip casting, cooling and pelletizing, screening, and drying.

[0059] In the present invention, those skilled in the art should know that polyamide can be called nylon, and resin is a general term for plastics, which can refer to polyamide / nylon.

[0060] In the present invention, those skilled in the art should know that the magnetic sealing element can be a magnetic cylinder.

[0061] On the basis of conforming to the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present utility model.

[0062] The reagents and raw materials used in the utility model are all commercially available.

[0063] The positive and progressive effects of the utility model are:

[0064] The utility model can effectively solve the problem of condensation and reflux of gas phase water vapor in polyamide production, and keep the uniformity of materials in the kettle at all times, so as to obtain products with stable performance and polyamide products with high batch stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] Figure 1 This is a schematic diagram of the structure of the polyamide preparation device in Example 1 of the present application.

[0066] Figure 2 This is a schematic diagram of the structure of the polyamide preparation device in Example 2 of the present application.

[0067] Figure 3 This is a schematic diagram of the structure of the polyamide preparation device of Comparative Example 1.

[0068] Description of reference numerals:

[0069] Magnetic sealing element 1

[0070] Drive shaft 2

[0071] Reactor 3

[0072] Cavity 4

[0073] Intake duct 1001

[0074] The first exhaust pipe 1002

[0075] Second exhaust duct 1003

[0076] The third exhaust pipe 1004

[0077] Load Cell 101

[0078] First signal processing element 102

[0079] The first feedback element 103

[0080] The first control valve 104

[0081] Second control valve 105

[0082] The third control valve 106

[0083] Fourth control valve 107

[0084] Water content detection element 108

[0085] The second signal processing unit 109

[0086] The second feedback element 110 . DETAILED DESCRIPTION

[0087] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods without specific conditions in the following examples are selected according to conventional methods and conditions, or according to the product specifications.

[0088] Example 1

[0089] Figure 1 Schematic diagram of the structure of the polyamide preparation device of this embodiment. The polyamide preparation device comprises a magnetic sealing element 1, a driving shaft 2 and a reaction kettle 3, a cavity 4 is provided inside the magnetic sealing element 1, and the magnetic sealing element 1 is arranged on the top of the reaction kettle 3, one end of the driving shaft 2 is arranged inside the reaction kettle 3, and the other end is arranged in the cavity 4;

[0090] The polyamide preparation device also includes a balancing module, and the balancing module has a structure 1:

[0091] Structure 1 includes an air intake pipe 1001, a first exhaust pipe 1002, and a pressure measuring element 101, a first signal processing element 102 and a first feedback element 103 which are electrically connected in sequence; the first exhaust pipe 1002 and the air intake pipe 1001 are both connected to the cavity 4, and the first exhaust pipe 1002 and the air intake pipe 1001 are respectively provided with a first control valve 104 and a second control valve 105; the pressure measuring element 101 is respectively provided inside the reactor 3 and the cavity 4, and is used to monitor the internal pressure of the reactor 3 and the cavity 4 respectively; the first signal processing element 102 is used to It is used to judge whether the difference between the internal pressure of the reactor 3 and the cavity 4 meets the set condition, that is, it is greater than or equal to 0.01MPa. If the set condition is met, it is converted into a pressure control signal, or it is used to judge whether the internal pressure of the reactor 3 and / or the cavity 4 reaches the rated pressure. If it does not reach the rated pressure, it is converted into a pressure control signal; the first feedback element 103 is connected to the first control valve 104 and the second control valve 105 respectively, and is used to control the first control valve 104 or the second control valve 105 in real time according to the pressure control signal, so as to adjust the internal pressure of the cavity 4;

[0092] The reactor 3 is provided with a third exhaust pipe 1004, on which a fourth control valve 107 is provided; the fourth control valve 107 is connected to the first feedback element 103, and is used to adjust the fourth control valve 107 according to the pressure control signal, thereby controlling the internal pressure of the reactor 3, so that the internal pressure of the cavity 4 is balanced with the internal pressure of the reactor 3.

[0093] Embodiment 2-6

[0094] Example 2 is a method for preparing polyamide, which uses the polyamide preparation device of Example 1 to prepare PA6T / 66 resin, comprising the following steps:

[0095] S1. Salt formation

[0096] At 120° C., a PA6T / 66 salt solution with a concentration of 54 wt % was prepared (test conditions: the pH value of the PA6T / 66 salt solution at 25° C. and a concentration of 10 wt % was 7.4), which was used to prepare the PA6T / 66 resin;

[0097] S2, Concentration

[0098] After the PA6T / 66 salt solution is added to the reactor 3, the temperature of the material in the reactor 3 is raised to 180°C by the heat medium in the jacket. During the heating process, the pressure in the reactor 3 increases. At this time, the pressure balance module starts to work synchronously. Its operation mode is to use the pressure sensor connected to the reactor 3 as a pressure measuring element 101 to detect the pressure changes in the cavity 4 and the reactor 3 in real time. The difference between the internal pressure of the reactor and the internal pressure of the cavity is greater than or equal to 0.01MPa, and give an instruction to control the second control valve to open, fill nitrogen into the cavity 4 of the magnetic cylinder, and measure the amount. At the same time, the internal pressure change of the magnetic cylinder is detected to achieve synchronization between the pressure in the reactor 3 and the pressure in the magnetic cylinder. In the process of raising the temperature of the PA6T / 66 salt solution to 180°C, the pressure in the reactor 3 gradually increased to 0.8MPa. Under the regulation of the balance module, the pressure in the magnetic cylinder also maintained the same increasing rate as the pressure in the reactor 3, increasing to 0.8MPa, and the magnetic cylinder was filled with nitrogen atmosphere, and no condensed water was formed (displayed by the liquid water detection device);

[0099] Under the condition of constant pressure of 0.8 MPa, the concentration of the salt solution was increased from 54wt% to 66wt%, and the data showed that no condensed water was formed in the magnetic cylinder.

[0100] S3, pre-aggregation

[0101] The material temperature was raised to 230℃ and kept unchanged for 1h. The pressure in the kettle was controlled to be constant. The difference between the internal pressure of the reactor and the internal pressure of the cavity was greater than or equal to 0.01MPa. The second control valve was opened by giving a command. Through the balancing module, the pressure in the magnetic cylinder was kept consistent with that in the kettle, both of which were 2.8MPa. After the constant temperature and pressure were completed, the temperature in the kettle was gradually raised to 295℃, while the pressure in the kettle was kept constant. Under the action of the pressure balancing module, the pressure in the magnetic cylinder was kept synchronous, and the experiment proved that no condensed water was generated.

[0102] When the temperature in the kettle rises to 295°C, the pressure in the kettle begins to gradually decrease at a pressure relief rate of 2.5MPa / h. Under the action of the balancing module, the nitrogen in the magnetic cylinder is discharged through the exhaust pipe, gradually reducing the pressure in the magnetic cylinder, and no condensed water is formed in the magnetic cylinder.

[0103] S4, post-polymerization

[0104] When the pressure is released to normal pressure, the temperature in the kettle is controlled to rise steadily to 300°C, and no temperature fluctuation occurs during the process. After reacting at this temperature and normal pressure for 30 minutes, the reaction is terminated, and the molten material is pressed out of the casting strip from the casting strip head by nitrogen, and then cooled in a cooling water tank, pelletized, sieved, dried, and packaged to obtain the final PA6T / 66 product.

[0105] Examples 3-6 adopt the same process scheme as Example 2 (including preparation equipment and preparation method) and are repeated experiments of Example 2.

[0106] Comparative Examples 1-5

[0107] Figure 3 Schematic diagram of the structure of the polyamide preparation device of Comparative Examples 1 to 5. The polyamide preparation device is a conventional reaction device in the art, which does not contain a pressure balance module, and the other structures are the same as those of Example 3.

[0108] Comparative Example 1 is a method for preparing polyamide, which uses Figure 3 The polyamide preparation device is used to prepare PA6T / 66 resin, comprising the following steps:

[0109] S1. Salt formation

[0110] At 120° C., a PA6T / 66 salt solution with a concentration of 54 wt % was prepared (test conditions: the pH value of the PA6T / 66 salt solution at 25° C. and a concentration of 10 wt % was 7.4), which was used to prepare the PA6T / 66 resin;

[0111] S2, Concentration

[0112] After the PA6T / 66 salt solution was added to the reactor, the temperature of the material in the reactor was raised to 180°C by the heat medium in the jacket. During the heating process, the pressure in the reactor gradually increased to 0.8 MPa. Due to the absence of a balancing module, the temperature vs. time curve was more turbulent than that in the embodiment during the heating process, and temperature fluctuations occasionally occurred.

[0113] Under the condition of constant pressure of 0.8 MPa, the concentration of the salt solution was increased from 54 wt % to 66 wt %. Similarly, the temperature vs. time curve was more volatile than that of Examples 2-6, with occasional temperature fluctuations, and the fluctuations intensified to a magnitude of ±5°C.

[0114] S3, pre-aggregation

[0115] The material temperature was raised to 230°C and kept constant for 1 hour, and the pressure in the kettle was controlled to be constant at 2.8 MPa. After the constant temperature and pressure were completed, the temperature in the kettle was gradually raised to 295°C, and the pressure in the kettle was kept constant at 2.8 MPa during the heating process.

[0116] When the temperature in the kettle rises to 295°C, the pressure in the kettle begins to be gradually reduced at a pressure relief rate of 2.5MPa / h.

[0117] S4, post-polymerization

[0118] When the pressure is released to normal pressure, the temperature in the kettle is controlled to rise steadily to 300°C. After reacting at this temperature and normal pressure for 30 minutes, the reaction is terminated, and the molten material is pressed out of the casting strip from the casting strip head by nitrogen, and then cooled in a cooling water tank, pelletized, sieved, dried, and packaged to obtain the final PA6T / 66 product.

[0119] Comparative Examples 2-5 adopt the same process scheme as Comparative Example 1 (including preparation equipment and preparation method) and are repeated experiments of Comparative Example 1.

[0120] Example 7

[0121] Figure 2 Schematic diagram of the structure of the polyamide preparation device of this embodiment. The polyamide preparation device comprises a magnetic sealing element 1, a driving shaft 2 and a reaction kettle 3, a cavity 4 is provided inside the magnetic sealing element 1, and the magnetic sealing element 1 is arranged on the top of the reaction kettle 3, one end of the driving shaft 2 is arranged inside the reaction kettle 3, and the other end is arranged in the cavity 4;

[0122] The polyamide preparation device also includes a balancing module, and the structure of the balancing module is structure 2:

[0123] Structure 2 includes a second exhaust pipe 1003, and a water content detection element 108, a second signal processing element and a second feedback element which are electrically connected in sequence; the second exhaust pipe 1003 is communicated with the cavity 4, and a third control valve 106 is provided on the second exhaust pipe 1003; the water content detection element 108 is arranged inside the cavity 4, and is used to detect the internal water content of the cavity 4; the second signal processing element is used to determine whether the internal water content exceeds a threshold value, that is, greater than or equal to 2% (% is the percentage of the height of the first preset liquid level to the height of the cavity), and determine whether it is necessary to send a water content control signal to the second feedback element; the second feedback element is connected to the third control valve 106, and is used to control the opening and closing of the third control valve 106 according to the water content control signal.

[0124] The reactor 3 is provided with a third exhaust pipe 1004 , on which a fourth control valve 107 is provided; the fourth control valve 107 is connected to the second feedback element, and the fourth control valve 107 is adjusted according to the water content control signal, thereby controlling the internal pressure of the reactor 3 .

[0125] Examples 8-12

[0126] Example 8 is a method for preparing polyamide, which uses the polyamide preparation device of Example 3 to prepare MXD6 resin, comprising the following steps:

[0127] S1. Salt formation

[0128] At 90° C., a 51 wt% MXD6 salt solution was prepared (test conditions: the pH value of the MXD6 salt solution at 25° C. and a concentration of 10 wt% was 6.9) for preparing MXD6 resin;

[0129] S2, Concentration

[0130] After the MXD6 salt solution is added to the reactor 3, the temperature of the material in the reactor 3 is raised to 160°C by the heat medium in the jacket. During the temperature rise process, the pressure in the reactor 3 is gradually raised to 0.6MPa. In this process, the water content in the cavity 4 is measured. When the liquid level inside the cavity 4 is greater than or equal to the first preset liquid level, the water content signal is converted into the control signal, and the third control valve is controlled to intermittently drain the magnetic cylinder at intervals of 5 minutes to remove the water in the magnetic cylinder; wherein the first preset liquid level is greater than or equal to 2%, and % is the percentage of the height of the first preset liquid level to the height of the cavity.

[0131] Under the constant pressure condition of 0.6MPa, the concentration of the salt solution is increased from 51wt% to 70wt%, and the water content in the cavity 4 is measured. When the liquid level inside the cavity 4 is greater than or equal to the first preset liquid level, the water content signal is converted into the control signal, and the third control valve is controlled. This process is accompanied by intermittent magnetic cylinder exhaust operation, and the water in the magnetic cylinder is removed at intervals of 5min.

[0132] S3, pre-aggregation

[0133] The material temperature is raised to 210°C and maintained unchanged for 1 hour, and the pressure in the kettle is controlled to be constant at 1.9MPa. This process is accompanied by intermittent magnetic cylinder exhaust operation, and the water in the magnetic cylinder is removed at intervals of 5 minutes. After the constant temperature and pressure are completed, the temperature in the kettle is gradually raised to 255°C, while the pressure in the kettle is maintained at a constant 1.9MPa; the water content in the cavity 4 is measured, and when the liquid level inside the cavity 4 is greater than or equal to the first preset liquid level, i.e., 2% (% is the percentage of the height of the first preset liquid level to the height of the cavity), the water content signal is converted into the control signal, and the third control valve is controlled. This process is accompanied by intermittent magnetic cylinder exhaust operation, and the water in the magnetic cylinder is removed at intervals of 5 minutes.

[0134] When the temperature in the kettle rises to 255℃, the pressure in the kettle begins to be gradually reduced at a pressure relief rate of 2.0MPa / h. This process is accompanied by intermittent magnetic cylinder exhaust operation at intervals of 5min to remove the moisture in the magnetic cylinder.

[0135] S4, post-polymerization

[0136] When the pressure is released to normal pressure, the temperature in the kettle is controlled to rise steadily to 260°C, and no temperature fluctuation occurs during the process. After reacting at this temperature and normal pressure for 30 minutes, the reaction is terminated, and the molten material is pressed out of the casting strip from the casting strip head by nitrogen, and then cooled in a cooling water tank, pelletized, sieved, dried, and packaged to obtain the final MXD6 product.

[0137] Examples 9-12 adopt the same process scheme as Example 8 (including preparation equipment and preparation method) and are repeated experiments of Example 8.

[0138] Comparative Examples 6-10

[0139] Comparative Example 6 is a method for preparing polyamide, which uses the polyamide preparation device of Comparative Example 1 to prepare MXD6 resin, comprising the following steps:

[0140] S1. Salt formation

[0141] At 90° C., a 51 wt% MXD6 salt solution was prepared (test conditions: the pH value of the MXD6 salt solution at 25° C. and a concentration of 10 wt% was 6.9) for preparing MXD6 resin;

[0142] S2, Concentration

[0143] After the MXD6 salt solution was added into the reactor, the temperature of the materials in the reactor was raised to 160°C by the heat medium in the jacket. During the heating process, the pressure in the reactor gradually increased to 0.6 MPa.

[0144] Under a constant pressure of 0.6 MPa, the concentration of the salt solution was increased from 51 wt % to 70 wt %.

[0145] S3, pre-aggregation

[0146] The material temperature was raised to 220°C and kept constant for 1 hour, and the pressure in the kettle was controlled to be constant at 1.9 MPa. After the constant temperature and pressure were completed, the temperature in the kettle was gradually raised to 255°C, while the pressure in the kettle was kept constant at 1.9 MPa.

[0147] When the temperature in the kettle rises to 255°C, the pressure in the kettle begins to be gradually reduced at a pressure relief rate of 2.0 MPa / h.

[0148] S4, post-polymerization

[0149] When the pressure is released to normal pressure, the temperature in the kettle is controlled to rise steadily to 260°C. After reacting at this temperature and normal pressure for 30 minutes, the reaction is terminated, and the molten material is pressed out of the casting strip from the casting strip head by nitrogen, and then cooled in a cooling water tank, pelletized, sieved, dried, and packaged to obtain the final MXD6 product.

[0150] Effect Example 1

[0151] This effect example tests the performance of the polyamide products of Examples 2-6, 8-12 and Comparative Examples 1-5, 6-10.

[0152] The following are the performance evaluation test methods:

[0153] 1) Relative viscosity: According to standard ISO 307, the polymer is dissolved in concentrated sulfuric acid and tested in a constant temperature water box at 25°C.

[0154] 2) Mn and PDI: tested using gel permeation chromatography (GPC) hexafluoroisopropanol system.

[0155] 3) Melting point Tm: Tested according to standard ISO11357. Specific steps: Differential scanning calorimeter (DSC) heating program: heat to 350°C at a rate of 10°C / min, stay for 5 minutes, then cool to 25°C at a rate of 10°C / min, stay for 5 minutes, and then heat to 350°C at a rate of 10°C / min. The temperature corresponding to the endothermic peak of the second heating curve is the melting point Tm.

[0156] 4) Terminal amine or terminal carboxyl group: quantitative analysis and measurement by potentiometric titration. Specific steps: Use a fully automatic point titrator to titrate the content of terminal amine or terminal carboxyl group, take 1g of polymer and dissolve it in hexafluoroisopropanol solution, after the sample is completely dissolved, use a calibrated hydrochloric acid standard solution or KOH-ethanol solution to titrate and test the content of terminal amine or terminal carboxyl group.

[0157] 5) Chroma / YI: Tested according to standard HG / T 3862 Plastic Yellowness Index Test Method.

[0158] 6) Tensile properties: tensile strength, tensile modulus and elongation at break were tested according to standard GB / T 1040.2 / 1A.

[0159] 7) Bending properties: Test the sample's bending strength and bending modulus according to standard GB / T 9341.

[0160] 8) Yield rate: The product yield rate is obtained by comparing the actual yield rate with the theoretical yield rate.

[0161] The polyamides prepared in Examples 2-6, Examples 8-12 and Comparative Examples 1-5 and 6-10 were tested respectively. The properties of the polyamide products of Examples 2-6 are shown in Table 1; the properties of the polyamide products of Comparative Examples 1-5 are shown in Table 2; the properties of the polyamide products of Examples 8-12 are shown in Table 3; and the properties of the polyamide products of Comparative Examples 6-10 are shown in Table 4.

[0162] Table 1

[0163]

[0164] It can be seen from the data in Table 1 that the PA6T / 66 products produced by Examples 2-6 using the equipment and method have a high yield rate, the performance of the five batches of samples is very close, the error is small, and the batch-to-batch stability is high.

[0165] Table 2

[0166]

[0167] It can be seen from Table 2 that the temperature, pressure and torque fluctuate greatly in the concentration stage, constant temperature and pressure stage and pressure release stage. This causes the yield rate, relative viscosity, terminal amine group, YI value and tensile strength of the products of Comparative Examples 1-5 to fluctuate greatly. The average yield rate is lower than that of the embodiment.

[0168] Table 3

[0169]

[0170] It can be seen from the data in Table 3 that the MXD6 products produced by the equipment and method in Examples 8-12 have a high yield rate, the performance of the five batches of samples is very close, the error is small, and the batch-to-batch stability is high.

[0171] Table 4

[0172]

[0173] It can be seen from Table 4 that the temperature, pressure and torque fluctuate greatly in the concentration stage, constant temperature and pressure stage and pressure release stage. This causes the yield rate, relative viscosity, terminal amine group, YI value and tensile strength of the products of Comparative Examples 6-10 to fluctuate greatly. The average yield rate is lower than that of the embodiment.

Claims

1. A polyamide preparation device, comprising a magnetic sealing element, a driving shaft and a reactor, wherein a cavity is provided inside the magnetic sealing element and the magnetic sealing element is arranged on the top of the reactor, one end of the driving shaft is arranged inside the reactor, and the other end is arranged in the cavity; Features: The polyamide preparation device further comprises a balancing module, and the structure of the balancing module is structure one or structure two: The structure 1 comprises an intake pipe, a first exhaust pipe, and a pressure measuring element, a first signal processing element and a first feedback element which are electrically connected in sequence; the first exhaust pipe and the intake pipe are both connected to the cavity, and the first exhaust pipe and the intake pipe are respectively provided with a first control valve and a second control valve; the pressure measuring element is arranged inside the reactor and the cavity, and is used to monitor the internal pressure of the reactor and the cavity respectively; the first signal processing element is used to judge whether the difference between the internal pressure of the reactor and the cavity meets the set condition, and if so, it is converted into a pressure control signal, or to judge whether the internal pressure of the reactor and / or the cavity reaches the rated pressure, and if not, it is converted into a pressure control signal; the first feedback element is respectively connected to the first control valve and the second control valve, and is used to control the first control valve or the second control valve in real time according to the pressure control signal, so as to adjust the internal pressure of the cavity; The second structure includes a second exhaust pipe, and a water content detection element, a second signal processing element and a second feedback element which are electrically connected in sequence; the second exhaust pipe is communicated with the cavity, and a third control valve is provided on the second exhaust pipe; the water content detection element is arranged inside the cavity, and is used to detect the internal water content of the cavity; the second signal processing element is used to judge whether the internal water content exceeds a threshold value, and determine whether it is necessary to send a water content control signal to the second feedback element; the second feedback element is connected to the third control valve, and is used to control the opening and closing of the third control valve according to the water content control signal.

2. The polyamide preparation device according to claim 1, It is characterized in that The reactor is provided with a third exhaust pipeline, and the third exhaust pipeline is provided with a fourth control valve.

3. The polyamide preparation device according to claim 2, It is characterized in that The fourth control valve is connected to the first feedback element and is used to adjust the fourth control valve according to the pressure control signal, thereby controlling the internal pressure of the reactor and balancing the internal pressure of the cavity with the internal pressure of the reactor.

4. The polyamide preparation device according to claim 2, It is characterized in that The fourth control valve is connected to the second feedback element, and the fourth control valve is adjusted according to the water content control signal to control the internal pressure of the reactor.