Composite metal part

By using a cold spraying process to form a nickel metal layer on the surface of the aluminum substrate, the problems of poor bonding force and deformation of aluminum-nickel composite metal parts are solved, high bonding strength and wear resistance are achieved, costs are reduced, and mechanical strength and mechanical strength are improved. cost-effective and expands application scenarios.

CN221895117UActive Publication Date: 2024-10-25SHENZHEN JINSHANGJIN NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202321954604.0
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-07-21
Publication Date
2024-10-25
Estimated Expiration
2033-07-21

AI Technical Summary

Technical Problem

The aluminum-nickel composite metal parts prepared in the prior art have problems such as poor bonding strength between the aluminum material and the nickel material, and are easy to fall off and deform.

Method used

A nickel metal layer is formed on the surface of the aluminum substrate through a cold spraying process to form a mechanical bond to ensure the bonding strength between the nickel metal layer and the aluminum substrate. The low temperature is maintained during the preparation process to avoid deformation. At the same time, the nickel metal layer can be selected thickness and nickel content to optimize performance.

Benefits of technology

It achieves high bonding strength and good wear resistance between aluminum substrate and nickel material, reduces costs, improves mechanical strength and cost performance, and expands the application scenarios of composite metal parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221895117U_ABST
    Figure CN221895117U_ABST
Patent Text Reader

Abstract

The utility model discloses a composite metal part. The composite metal piece comprises an aluminum base material and a nickel metal layer, and the nickel metal layer is formed in a local area of the surface of the aluminum base material through a cold spraying process. Wherein mechanical combination is formed between the nickel metal layer and the aluminum base material. According to the technical scheme, the nickel metal layer is formed on the surface of the aluminum base material through the cold spraying technology, mechanical combination is formed between the nickel metal layer and the aluminum base material, then the combination strength between the nickel metal layer and the aluminum base material is guaranteed, and the composite metal piece prepared based on the cold spraying technology cannot deform; and meanwhile, the composite metal part realizes perfect combination of light weight and high performance based on the material characteristics of the aluminum material and the nickel material, so that the mechanical strength and the cost performance of the composite metal part are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of metal materials, and in particular to a composite metal part. Background Art

[0002] Nickel and its alloys are widely used in key components and connectors in the industrial sector, particularly in high-load-bearing mechanical parts, due to their high hardness, high compressive strength, and excellent corrosion resistance. However, the high density of nickel alloys makes them expensive, which restricts their wider application.

[0003] Currently, casting pure nickel has the disadvantages of high cost and difficult processing. Existing technologies also produce aluminum-nickel composite metal parts to achieve the perfect combination of lightweight and high performance. However, these aluminum-nickel composite metal parts produced by existing technologies have the disadvantages of poor bonding between the aluminum and nickel materials, easy to fall off, and deformation. Utility Model Content

[0004] The present application provides a composite metal part, aiming to solve the problem that the composite metal parts prepared in the prior art have poor bonding strength between aluminum and nickel materials and are easily deformed.

[0005] To achieve the above objectives, the present application proposes a composite metal part, comprising:

[0006] Aluminum substrate;

[0007] A nickel metal layer is formed on a local area of ​​the surface of the aluminum substrate by a cold spraying process; wherein a mechanical bond is formed between the nickel metal layer and the aluminum substrate.

[0008] In this way, a nickel metal layer is formed on the surface of the aluminum substrate through a cold spraying process, forming a mechanical bond between the nickel metal layer and the aluminum substrate, thereby ensuring the bonding strength between the nickel metal layer and the aluminum substrate. Furthermore, the composite metal part produced using the cold spraying process does not deform due to the low temperature during the production process. Consequently, the composite metal part proposed in this application achieves a perfect combination of lightweight and high performance based on the material properties of aluminum and nickel, resulting in improved mechanical strength and cost-effectiveness.

[0009] In some embodiments, the nickel metal layer has a thickness in the range of 5 to 100 μm.

[0010] In this way, by setting the thickness of the nickel metal layer within the range of 5 to 100 μm, the nickel metal layer can maintain better mechanical properties, and at the same time, after being combined with the aluminum substrate, it can maintain the mechanical properties of the aluminum substrate, making it easier to obtain complex shapes or special performance components.

[0011] In some embodiments, the bonding strength between the aluminum substrate and the nickel metal layer is no less than 5 MPa.

[0012] In this way, when the bonding strength between the aluminum substrate and the nickel metal layer is not less than 5MPa, the bonding strength between the aluminum substrate and the nickel metal layer can be fully guaranteed, preventing the nickel metal layer from falling off or being peeled off from the aluminum substrate, thereby meeting usage requirements.

[0013] In some embodiments, when a standard wear resistance test is performed under a load of 5 to 50 N, the wear rate of the nickel metal layer is between 3.3×10 -6 mm 3 / (m·N).

[0014] Thus, in the wear resistance standard test under a load of 5 to 50 N, the wear rate of the nickel metal layer is 3.3×10 - 6 mm 3 / (m·N), it can prevent the nickel metal layer from being lost too quickly, further fully ensuring the service life of the bulk composite metal parts.

[0015] In some embodiments, the nickel content in the nickel metal layer is in a range of 80% to 99.99%.

[0016] In this way, the nickel content in the nickel metal layer is within the range of 80% to 99.99%, making its nickel content close to the level of pure nickel, thereby making the formed nickel metal layer have properties similar to those of pure nickel material, ensuring the performance of the composite metal part.

[0017] In some embodiments, the composite metal member further includes a solderable layer formed on the nickel metal layer.

[0018] In this way, a nickel metal layer is formed between the aluminum substrate and the weldable layer. The nickel metal layer can enhance the structural strength, and the nickel metal layer is combined with the aluminum substrate and the weldable layer respectively, which can increase the bonding force between the layers, making the composite metal parts more firmly bonded. At the same time, the weldable layer improves the welding performance of the composite metal parts.

[0019] In some embodiments, the solderable layer is a tin metal layer.

[0020] In this way, the tin metal layer is used as a solderable layer, and based on the material properties of the tin metal, good solderability can be provided for the composite metal part.

[0021] In some embodiments, the composite metal member is used as a welding member between electronic components, a soldering member of a printed circuit board, or a connecting member between mechanical parts.

[0022] In this way, the composite metal parts can be used as welding parts between electronic components or soldering parts of printed circuit boards or connecting parts between mechanical parts, thereby improving the application scenarios of the composite metal parts. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a schematic structural diagram of a composite metal part in one embodiment of the present application;

[0024] Figure 2 A schematic diagram of a local area of ​​an aluminum substrate according to an embodiment of the present application;

[0025] Figure 3 Schematic diagram of the structure of a composite metal part with a weldable layer in one embodiment of the present application. DETAILED DESCRIPTION

[0026] The following will be combined with the drawings in the embodiments of this application to clearly and completely describe the technical solutions in the embodiments of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of the embodiments. Based on the embodiments of this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

[0027] It should be noted that all directional indications in the embodiments of the present application (such as up, down, left, right, front, back, etc.) are only used to explain the relative position relationship, movement status, etc. between the various components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.

[0028] It should also be noted that when an element is referred to as being "fixed on" or "disposed on" another element, it may be directly on the other element or there may be an intermediate element. When an element is referred to as being "connected to" another element, it may be directly connected to the other element or there may be an intermediate element.

[0029] In addition, the descriptions of "first", "second", etc. in this application are for descriptive purposes only and should not be understood as indicating or implying their relative importance or implicitly indicating the number of the technical features indicated. Therefore, the features defined as "first" or "second" may explicitly or implicitly include at least one of such features. In addition, the technical solutions between the various embodiments can be combined with each other, but this must be based on the fact that they can be implemented by ordinary technicians in this field. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by this application.

[0030] See Figure 1 as well as Figure 3 As shown, the present application proposes a composite metal part 100, including an aluminum substrate 10 and a nickel metal layer 20, wherein the nickel metal layer 20 is formed on a local area 110 on the surface of the aluminum substrate 10 by a cold spraying process; wherein a mechanical bond is formed between the nickel metal layer 20 and the aluminum substrate 10.

[0031] Cold spraying is a metal spraying process that does not require melting the metal particles being sprayed, resulting in a relatively low spraying temperature. During the spraying process, a supersonic gas-solid two-phase airflow shoots the metal particles onto the substrate, forming a dense coating that creates a strong bond between the substrate and the metal coating.

[0032] In the technical solution of this application, a composite metal part 100 is made of aluminum and nickel. Nickel metal particles are cold-sprayed onto a localized area 110 of an aluminum substrate 10 to form a nickel metal layer 20. The aluminum substrate 10 can be a basic structural part such as an aluminum sheet or block, and is not limited thereto.

[0033] The localized area 110 can be understood as a portion of the surface of the aluminum substrate 10, rather than the entire surface of the aluminum substrate 10. When the nickel metal layer 20 is to be provided on the surface of the aluminum substrate 10, the localized area can be selected based on actual usage requirements. Furthermore, the shape, size, and number of the localized areas 110 are not limited in this application, as long as the nickel metal layer 20 provided in the localized area meets the usage requirements.

[0034] Thus, the nickel metal layer 20 is formed on the surface of the aluminum substrate 10 via the cold spraying process, forming a mechanical bond between the nickel metal layer 20 and the aluminum substrate 10, thereby ensuring the bonding strength between the nickel metal layer 20 and the aluminum substrate 10. Furthermore, the composite metal part 100 produced via the cold spraying process does not deform due to the low temperature during the production process. Furthermore, the composite metal part 100 proposed in this application achieves a perfect combination of lightweight and high performance based on the material properties of aluminum and nickel, thereby improving both mechanical strength and cost-effectiveness.

[0035] Illustratively, the prepared composite metal part 100 includes the following excellent properties: (1) the aluminum substrate 10 and the nickel metal layer 20 each exert their own performance advantages, so that the overall performance of the composite metal part 100 reaches or exceeds that of pure metal materials; (2) the product cost is low, and there is no need to use an expensive pure nickel substrate, which greatly reduces costs; (3) the density of aluminum is only 1 / 3 of that of pure nickel, and the overall density of the composite metal part 100 is much lower than that of pure nickel, so the composite metal part 100 is light in weight.

[0036] In some embodiments, the thickness of the nickel metal layer 20 is in the range of 5 to 100 μm. The specific thickness can be selected based on actual use requirements or the thickness of the aluminum substrate 10. Thus, by setting the thickness of the nickel metal layer 20 in the range of 5 to 100 μm, the nickel metal layer 20 can maintain excellent mechanical properties. At the same time, after being combined with the aluminum substrate 10, the nickel metal layer 20 can maintain the mechanical properties of the aluminum substrate 10, making it easier to obtain components with complex shapes or special properties.

[0037] In some embodiments, the bonding strength between the aluminum substrate 10 and the nickel metal layer 20 is no less than 5 MPa.

[0038] In order to ensure that the bonding strength between the aluminum substrate 10 and the nickel metal layer 20 meets the requirements and has good bonding force, the selected local area 110 of the aluminum substrate 10 can be pretreated before the nickel metal powder is sprayed onto the aluminum substrate 10.

[0039] As will be understood, pretreatment involves a series of processes such as degreasing, grinding, and pickling localized areas of the aluminum substrate 10 to remove impurities and oil stains on the surface of the aluminum substrate 10 and form a rough microstructure. This ensures cleanliness while increasing the bonding area between the aluminum substrate 10 and the nickel metal layer 20, thereby improving the bonding between the aluminum substrate 10 and the nickel metal layer 20. After bonding, the bonding strength between the aluminum substrate 10 and the nickel metal layer 20 can be measured using a tensile testing machine.

[0040] In this way, when the bonding strength between the aluminum substrate 10 and the nickel metal layer 20 is not less than 5 MPa, the bonding stability between the aluminum substrate 10 and the nickel metal layer 20 is fully guaranteed, preventing the nickel metal layer 20 from falling off or being peeled off from the aluminum substrate 10, thereby increasing the service life and meeting the use requirements.

[0041] In some embodiments, when the wear resistance standard test is performed under a load of 5 to 50 N, the wear rate of the nickel metal layer 20 is 3.3×10 -6 mm 3 / (m·N).

[0042] One conventional test involves a dry sand / rubber wheel abrasion test, which involves abrading a standard specimen using sand particles of controlled size and composition. The abrasive is introduced between the test specimen and a rotating wheel of a chlorobutyl rubber tire or rim of a specified hardness. The test specimen (composite metal part 100) is pressed against the rotating wheel with a specified force by a lever arm while a controlled flow of sand particles abrades the test surface. The rotation of the grinding wheel causes its contact surface to move in the direction of the sand flow. The specific protocol of the standard abrasion resistance test will not be repeated here, and the mass loss is further converted to volume loss in cubic millimeters.

[0043] Thus, in the wear resistance standard test under a load of 5 to 50 N, the wear rate of the nickel metal layer 20 is 3.3×10 - 6 mm 3 When the value is within the range of 0.0147 W / (m·N), the nickel metal layer 20 can be prevented from being worn out too quickly, thereby fully ensuring the service life of the composite metal component 100 .

[0044] In some embodiments, after the composite metal part 100 is prepared, it can be placed in a corrosive solution for corrosion resistance testing. A corrosion resistance test chamber containing a 5% NaCl corrosive solution can be provided. The composite metal part 100 is immersed in the corrosive solution for 500 hours. After removal, the surface of the nickel metal layer 20 can be inspected for obvious signs of corrosion. The absence of these signs indicates good corrosion resistance.

[0045] In some embodiments, SEM analysis can also be performed to observe the mechanical engagement between the nickel metal layer 20 and the aluminum substrate 10 using a scanning electron microscope. No obvious cracks are observed at the interface of the nickel metal layer 20. When the nickel metal layer 20 is uniform and dense, the surface quality and appearance of the nickel metal layer 20 can meet ideal requirements.

[0046] In some embodiments, the nickel content of the nickel metal layer 20 is in the range of 80% to 99.99%, thus making the nickel content close to that of pure nickel, and thus making the formed nickel metal layer 20 have properties similar to those of pure nickel, thereby ensuring the performance of the composite metal part 100.

[0047] It is understood that the nickel content in the nickel metal layer 20 is within the range of 80% to 99.99%, that is, the nickel content in the nickel metal powder used is within the range of 80% to 99.99%. During the cold spraying process, the state and performance of the nickel metal powder will not change substantially.

[0048] Optionally, the particle size of the nickel metal powder is 3 to 50 μm. A cold spraying process is to use a self-cooling spraying device to spray high-purity nickel powder on a local area 110 on the pretreated aluminum substrate 10 using high-pressure gas at a spraying temperature of 200 to 900°C; the distance between the nozzle and the surface is 10 to 30 mm, and the gas velocity is 300 to 900 m / s; the spraying angle is perpendicular to the surface, and the spraying is performed 2 to 3 times on the same trajectory to obtain a nickel metal layer 20 with a coating thickness of 10 to 100 μm on the surface of the aluminum substrate 10.

[0049] When cold spraying is performed, other areas of the aluminum substrate 10 other than the local area 110 can be covered by a self-made masking fixture to ensure the area range of the cold spraying.

[0050] Furthermore, the composite metal part 100 may be subjected to post-processing operations, such as cleaning and drying the composite metal part 100 prepared by cold spraying.

[0051] See Figure 3 As shown, in some embodiments, the composite metal member 100 further includes a solderable layer 30 formed on the nickel metal layer 20 .

[0052] As the name implies, the solderable layer 30 is a metal layer used for welding. Thus, the nickel metal layer 20 is formed between the aluminum substrate 10 and the solderable layer 30. The nickel metal layer 20 enhances structural strength. Furthermore, the nickel metal layer 20, in combination with the aluminum substrate 10 and the solderable layer 30, increases the bonding strength between the layers, making the composite metal part 100 more secure. Furthermore, the solderable layer 30 improves the welding performance of the composite metal part 100.

[0053] Optionally, the solderable layer 30 is a tin metal layer. The thickness of the tin metal layer is in the range of 10 to 100 μm. Similarly, the tin metal layer can also be bonded to the surface of the nickel metal layer 20 using a cold spray process. Thus, using the tin metal layer as the solderable layer 30 can provide the composite metal component 100 with good solderability due to the material properties of tin metal.

[0054] In some embodiments, the composite metal member 100 is used as a welder between electronic components, a soldering member for printed circuit boards, or a connector between mechanical components. Thus, the composite metal member 100 can be used as a welder between electronic components, a soldering member for printed circuit boards, or a connector between mechanical components, thereby expanding the application scenarios of the composite metal member 100.

[0055] For example, the composite metal part 100 is used for welding of FPC printed circuit boards, and mechanical and electrical connections between electronic components are achieved through soldering. The nickel metal layer 20 has a good bonding effect with the substrate and the solder, and also has certain anti-corrosion properties.

[0056] In a specific embodiment, the process of preparing the composite metal part 100 (nickel-coated aluminum sheet) includes:

[0057] 1) Provide 1100 aluminum alloy rolled sheet with a width of 40mm, a length of 1000mm and a thickness of 5mm.

[0058] 2) The surface of the aluminum sheet is chemically cleaned and impurities are removed, and then it is ground and polished.

[0059] 3) Using self-cooling spraying equipment, high-purity nickel powder is sprayed on a designated area on the pretreated aluminum alloy sheet using high-pressure gas at a spraying temperature of 500°C; the distance between the nozzle and the surface is 15 mm, and the gas velocity is 500 m / s; the spraying angle is perpendicular to the surface, and three spraying passes are performed on the same trajectory to form a nickel metal layer 20 with an average thickness of 50 μm in a local area 110 (1000 mm long and 5 mm wide) of the aluminum sheet.

[0060] 4) The surface of the nickel metal layer 20 is ground and polished to reduce surface unevenness and improve product appearance quality.

[0061] 5) Cleaning and drying the prepared composite metal part 100.

[0062] The above description is only a partial or preferred embodiment of the present application. Neither the text nor the drawings can limit the scope of protection of the present application. Any equivalent structural transformation made by using the contents of the present application specification and drawings under the overall concept of the present application, or direct / indirect application in other related technical fields, is included in the scope of protection of the present application.

Claims

1. A composite metal part, characterized in that: include: Aluminum substrate; The nickel metal layer is formed on a local area of ​​the surface of the aluminum substrate by a cold spraying process; wherein the local area is processed to form a surface to be bonded, and a mechanical bond is formed between the nickel metal layer and the aluminum substrate.

2. The composite metal part according to claim 1, characterized in that: The thickness of the nickel metal layer is in the range of 5 to 100 μm.

3. The composite metal part according to claim 1, characterized in that: The bonding strength between the aluminum substrate and the nickel metal layer is not less than 5 MPa.

4. The composite metal part according to claim 1, characterized in that: When the wear resistance standard test is carried out under a load of 5 to 50 N, the wear rate of the nickel metal layer is 3.3×10 -6 mm 3 / (m·N).

5. The composite metal part according to claim 1, characterized in that: The composite metal member further includes a weldable layer formed on the nickel metal layer.

6. The composite metal part according to claim 5, characterized in that: The solderable layer is a tin metal layer.

7. The composite metal part according to claim 1, characterized in that: The composite metal piece is used as a welding piece between electronic components, a soldering piece of a printed circuit board or a connecting piece between mechanical parts.