Low-carbon recyclable nylon pipeline for fuel system

By adopting low-carbon recyclable nylon pipelines with a multi-layer structure and using materials such as bio-based polyamide and modified polyamide, the recycling problem caused by the incompatibility of existing fuel system pipeline materials is solved, and environmental protection and cost are achieved. The improvement meets strict environmental protection regulations and functional requirements.

CN221913538UActive Publication Date: 2024-10-29YANGZHOU HUAGUANG NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202323234389.X
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-11-29
Publication Date
2024-10-29
Estimated Expiration
2033-11-29

AI Technical Summary

Technical Problem

Existing fuel system pipelines cannot be fully recycled due to incompatible materials. They have high carbon emissions and high costs, making it difficult to meet strict environmental regulations.

Method used

Low-carbon recyclable nylon pipelines with a multi-layer structure, including protective layer, adhesive layer, barrier layer, structural layer and working condition layer, using bio-based polyamide, modified polyamide and other materials to ensure inter-layer compatibility And realize the recycling of pipelines.

Benefits of technology

It improves the environmental protection and cost-effectiveness of the pipeline, meets the multiple functional requirements of the fuel system, reduces carbon emissions and usage costs, and improves material utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221913538U_ABST
    Figure CN221913538U_ABST
Patent Text Reader

Abstract

The utility model discloses a low-carbon recyclable nylon pipeline for a fuel oil system, which belongs to the technical field of fuel oil pipelines and comprises a protective layer, a bonding layer, a barrier layer, a structural layer and a working condition layer which are sequentially arranged from outside to inside, and the protective layer is a bio-based polyamide PA11 layer or a polyamide PA12 layer. The bonding layer is a modified polyamide PA12 layer or a first modified polyamide PA6 layer, the blocking layer is a polyamide MXD6 layer or a polyamide MXD9 layer, and the structural layer is a second modified polyamide PA6 layer; the working condition layer is a low-precipitation modified polyamide PA6 layer or a low-precipitation conductive modified polyamide PA6 layer or a conductive modified polyamide PA6 layer or a low-precipitation modified polyamide PA612 layer or a low-precipitation conductive modified polyamide PA612 layer. The pipeline adopts various compatible nylon layers, and the whole material of the pipeline can be recycled; the performance of a pipeline product is improved, the overall material utilization rate is increased, carbon emission is reduced, and meanwhile the manufacturing cost and the using cost of the pipeline are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model belongs to the technical field of fuel pipelines, and in particular relates to a low-carbon recyclable nylon pipeline used in a fuel system. Background Art

[0002] At present, automobile fuel system pipelines and thermal management system pipelines often use metal pipes, plastic pipes, rubber pipes and other pipe types, among which plastic pipes are the most widely used. However, with the increasingly stringent emission regulations of various countries and the fierce cost reduction competition between traditional models and new energy vehicles, strict requirements have been put forward for pipelines.

[0003] Due to the problems of evaporative emissions and precipitates in fuel system pipelines, most plastic pipes now use EVOH, ETFE, EFEP and other materials as barrier layers. The application of a large number of fluororesins such as ethylene-vinyl alcohol copolymer, ethylene-tetrafluoroethylene copolymer, and modified ethylene-tetrafluoroethylene copolymer has solved the problems of permeation emissions required by regulations. However, this multi-layer structure of pipelines is not compatible with each other, and there is no way to completely recycle the waste generated during the extrusion process and the scrapping of the pipelines after production or use. The carbon emissions of its entire life cycle are not low, and it is not truly environmentally friendly. Utility Model Content

[0004] The technical problem solved by the utility model is to provide a low-carbon recyclable nylon pipeline for a fuel system so that the pipeline can be recycled, thereby reducing carbon emissions and costs.

[0005] Technical solution: In order to solve the above technical problems, the technical solution adopted by the utility model is as follows:

[0006] A low-carbon recyclable nylon pipeline for a fuel system comprises a protective layer, an adhesive layer, a barrier layer, a structural layer and a working condition layer which are arranged in sequence from the outside to the inside, wherein the protective layer is a bio-based polyamide PA11 layer or a polyamide PA12 layer, the adhesive layer is a modified polyamide PA12 layer or a first modified polyamide PA6 layer, the barrier layer is a polyamide MXD6 layer or a polyamide MXD9 layer, the structural layer is a second modified polyamide PA6 layer, and the working condition layer is a low precipitation modified polyamide PA6 layer or a low precipitation conductive modified polyamide PA6 layer or a conductive modified polyamide PA6 layer or a low precipitation modified polyamide PA612 layer or a low precipitation conductive modified polyamide PA612 layer.

[0007] Furthermore, the thickness of the protective layer is a, 0.1mm≤a≤0.5mm.

[0008] Furthermore, the thickness of the adhesive layer is b, 0.03mm≤b≤0.4mm.

[0009] Furthermore, the thickness of the barrier layer is c, 0.05mm≤c≤0.4mm.

[0010] Furthermore, the thickness of the structural layer is d, 0.2mm≤d≤0.8mm.

[0011] Furthermore, the thickness of the working condition layer is e, 0.05mm≤e≤0.5mm.

[0012] Furthermore, the total wall thickness of the nylon pipe from the protective layer to the working layer is f, 0.43mm≤f≤2.6mm.

[0013] Furthermore, the protective layer is a bio-based polyamide PA11 layer, the adhesive layer is a first modified polyamide PA6 layer, the barrier layer is a polyamide MXD6 layer, the structural layer is a second modified polyamide PA6 layer, and the working layer is a low precipitation modified polyamide PA612 layer.

[0014] Furthermore, the protective layer is a polyamide PA12 layer, the adhesive layer is a modified polyamide PA12 layer, the barrier layer is a polyamide MXD6 layer, the structural layer is a second modified polyamide PA6 layer, and the working layer is a conductive modified polyamide PA6 layer.

[0015] Furthermore, the protective layer is a bio-based polyamide PA11 layer, the adhesive layer is a first modified polyamide PA6 layer, the barrier layer is a polyamide MXD6 layer, the structural layer is a second modified polyamide PA6 layer, and the working layer is a low-precipitation conductive modified polyamide PA612 layer.

[0016] Beneficial effects: Compared with the prior art, the utility model has the following advantages:

[0017] 1. The utility model pipeline adopts a variety of compatible nylon layers, and the interlayer structure design of the multi-layer nylon layer can better meet the requirements of existing regulations on pipelines and pipeline mechanical properties. At the same time, the overall material of the pipeline can be recycled, and the pipeline is environmentally friendly and cost-effective;

[0018] 2. Meet various functional requirements such as steam pipelines and conductive pipelines in automobile fuel systems;

[0019] 3. It not only improves the performance of pipeline products, increases the overall material utilization rate, and reduces carbon emissions, but also reduces the manufacturing cost and use cost of pipelines. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a schematic diagram of the partial cross-sectional structure of the pipeline in Example 1 of the utility model. DETAILED DESCRIPTION

[0021] The present invention will be further explained below in conjunction with specific embodiments. The embodiments are implemented based on the technical solution of the present invention. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0022] Example 1

[0023] like Figure 1As shown, a low-carbon recyclable nylon pipeline for a fuel system, the nylon pipeline body is in a hollow cylindrical shape and is formed by five-layer co-extrusion, including a protective layer 1, an adhesive layer 2, a barrier layer 3, a structural layer 4 and a working layer 5 arranged in sequence from the outside to the inside, the protective layer 1 is a bio-based polyamide PA11 layer or a polyamide PA12 layer, the protective layer 1 is the outermost layer, and is made of PA11 or PA12 long-chain nylon material, such as PA12 L25 W40X BLACK, PA12 RILSAN MA 4411 BLACK, PA11BESN BLACK P40 TL or PA12 LX9002 material. In this embodiment, PA12 L25 W40 X BLACK is selected to meet the aging durability requirements of the use environment; the adhesive layer 2 is a modified polyamide PA12 layer or a first modified polyamide PA6 layer, and is made of PA12XE3795 NAT, PA6 R473, PA6 R463, RILSAN MA 4411 BLACK, PA11BESN BLACK P40 TL or PA12 LX9002 material. TIEFLEX S442 or VETAMID·SX8002 material, PA12 XE3795 NAT is selected in this embodiment, which can effectively bond the protective layer 1 and the barrier layer 3; the barrier layer 3 is a polyamide MXD6 layer or a polyamide MXD9 layer, which is made of semi-aromatic polyamide MXD6 or MXD9 material, such as MXD6 BXT2000-0203 material. Due to the presence of the benzene ring structure, it has a very stable structure and has high barrier properties to various fuel vapors, which can meet the emission performance requirements; the structural layer 4 is a second modified polyamide PA6 layer, which is different from the first modified polyamide PA6 layer in material (the same material can also be used), and the second modified polyamide PA6 layer is made of modified polyamide PA6 material, such as PA6BRZ347W, PA6 B210HS-EX or PA6 ORGALLOY LE60 material. PA6 is selected in this embodiment. BRZ347W can be effectively bonded to the semi-aromatic polyamide MXD6 or MXD9 of the barrier layer 3, and can also be effectively bonded to various modified polyamide PA6 and modified polyamide PA612 of the working layer 5, playing the multiple functions of strengthening the overall structure of the pipeline and bonding two adjacent layers; the working layer 5 is a low precipitation modified polyamide PA6 layer or a low precipitation conductive modified polyamide PA6 layer or a conductive modified polyamide PA6 layer or a low precipitation modified polyamide PA612 layer or a low precipitation conductive modified polyamide PA612 layer, and the working layer 5 is the innermost layer. According to the different working conditions of the pipeline in the fuel system, for example, the fuel steam pipeline and the general fuel pipeline can adopt low precipitation modified polyamide PA6 or low precipitation modified polyamide PA612, such as PA6 R073, PA612 DX9380 or PA612 LN6261HIbk materials;Conductive requirements The fuel line can use conductive modified polyamide PA6 or low precipitation conductive modified polyamide PA612 or low precipitation conductive modified polyamide PA6 layer, such as PA6 B240HS-CE BK, PA612 DX9180 or PA612 LN6255HIEbk materials. This embodiment is a general fuel line, and PA6 R073 material is selected. ;

[0024] like Figure 1 As shown, the thickness of the protective layer 1 is a, 0.1mm≤a≤0.5mm, and a=0.2mm in this embodiment; the thickness of the adhesive layer 2 is b, 0.03mm≤b≤0.4mm, and b=0.05mm in this embodiment; the thickness of the barrier layer 3 is c, 0.05mm≤c≤0.4mm, and c=0.1mm in this embodiment; the thickness of the structural layer 4 is d, 0.2mm≤d≤0.8mm, and d=0.5mm in this embodiment. Since the thickness of the structural layer 4 is relatively thick, it occupies a large proportion of the overall pipeline. The material ratio is large (reaching half), and after the pipeline is recycled and granulated as a whole, the modified polyamide PA6 material accounts for a large proportion, and the pipeline can be recycled; the thickness of the working layer 5 is e, 0.05mm≤e≤0.5mm, and in this embodiment e=0.15mm, and the working layer 5 also increases the proportion of modified polyamide PA6 material during recycling; the total wall thickness of the nylon pipeline from the protective layer 1 to the working layer 5 is f, 0.43mm≤f≤2.6mm, and in this embodiment f=a+b+c+d+e=1mm.

[0025] Example 2

[0026] The difference from Example 1 is that the protective layer 1 is made of PA11 P40TL material with a thickness of a=0.2 mm; the adhesive layer 2 is made of PA6 R473 material with a thickness of b=0.05 mm; the barrier layer 3 is made of MXD6 BXT2000-0203 material with a thickness of c=0.1 mm; the structural layer 4 is made of PA6 B210HS-EX material with a thickness of d=0.5 mm; the working layer 5 is made of PA612 DX9380 material with a thickness of e=0.15 mm;

[0027] Example 3

[0028] The difference from Example 1 is that the protective layer 1 is made of PA12 L25 W40 X BLACK material with a thickness of a=0.2 mm; the adhesive layer 2 is made of PA12 XE3795 NAT material with a thickness of b=0.05 mm; the barrier layer 3 is made of MXD6 BXT2000-0203 material with a thickness of c=0.1 mm; the structural layer 4 is made of PA6 BRZ347W material with a thickness of d=0.5 mm; the working layer 5 is made of PA6B240HS-CE BK material with a thickness of e=0.15 mm;

[0029] Example 4

[0030] The difference from Example 1 is that the protective layer 1 is made of PA11 P40TL material with a thickness of a=0.2 mm; the adhesive layer 2 is made of PA6 R473 material with a thickness of b=0.05 mm; the barrier layer 3 is made of MXD6 BXT2000-0203 material with a thickness of c=0.1 mm; the structural layer 4 is made of PA6 B210HS-EX material with a thickness of d=0.5 mm; the working layer 5 is made of PA612 DX9180 material with a thickness of e=0.15 mm;

[0031] The bio-based polyamide PA11, polyamide PA12, modified polyamide PA12, polyamide MXD6, polyamide MXD9, polyamide PA6, modified polyamide PA6, low precipitation modified polyamide PA6, low precipitation conductive modified polyamide PA6, conductive modified polyamide PA6, low precipitation modified polyamide PA612 and low precipitation conductive modified polyamide PA612 of Examples 1-4 are all existing materials.

[0032] Comparative Example 1

[0033] The pipeline in Comparative Example 1 is the existing technology, and it also adopts a five-layer structure, including a first layer, a second layer, a third layer, a fourth layer and a fifth layer arranged in sequence from the outside to the inside. The first layer is made of PA12 RILSAN MA 4411BLACK material with a thickness of 0.4 mm; the second layer is made of RILSAN TIEFLEX S442 material with a thickness of 0.05 mm; the third layer is made of EVOH F101B material with a thickness of 0.1 mm; the fourth layer is made of RILSAN TIEFLEX S442 material with a thickness of 0.05 mm; the fifth layer is made of PA12 RILSANMA 4411 BLACK material with a thickness of 0.4 mm; the materials of each layer in Comparative Example 1 are all existing materials, and the multi-layer structure pipeline cannot be recycled because its materials are not compatible.

[0034] Comparative Example 2

[0035] The pipeline in Comparative Example 2 is the existing technology, and it also adopts a five-layer structure, including the first layer, the second layer, the third layer, the fourth layer and the fifth layer arranged from the outside to the inside. The first layer is made of PA12 RILSAN MA 4411BLACK material with a thickness of 0.4 mm; the second layer is made of RILSAN TIEFLEX S442 material with a thickness of 0.1 mm; the third layer is made of EVOH LA170B material with a thickness of 0.1 mm; the fourth layer is made of VETAMID SX8002 material with a thickness of 0.3 mm; the fifth layer is made of ETFE AH5000 material with a thickness of 0.1 mm; the materials of each layer in Comparative Example 2 are all existing materials, and the multi-layer structure pipeline cannot be recycled because its materials are not compatible.

[0036] Comparative Example 3

[0037] The pipeline in Comparative Example 3 is the existing technology, and it also adopts a five-layer structure, including the first layer, the second layer, the third layer, the fourth layer and the fifth layer arranged from the outside to the inside. The first layer is made of PA12 RILSAN MA 4411 BLACK material with a thickness of 0.4 mm; the second layer is made of RILSAN TIEFLEX S442 material with a thickness of 0.05 mm; the third layer is made of EVOH F101B material with a thickness of 0.1 mm; the fourth layer is made of RILSAN TIEFLEX S442 material with a thickness of 0.05 mm; the fifth layer is made of PA12 AESNBLACK P202 CTL material with a thickness of 0.4 mm; the materials of each layer in Comparative Example 3 are all existing materials, and the multi-layer structure pipeline cannot be recycled because its materials are not compatible.

[0038] Comparative Example 4

[0039] The pipeline in Comparative Example 4 is the existing technology, and it also adopts a five-layer structure, including the first layer, the second layer, the third layer, the fourth layer and the fifth layer arranged from the outside to the inside. The first layer is made of PA12 RILSAN MA 4411BLACK material with a thickness of 0.4 mm; the second layer is made of RILSAN TIEFLEX S442 material with a thickness of 0.1 mm; the third layer is made of EVOH LA170B material with a thickness of 0.1 mm; the fourth layer is made of VETAMID SX8002 material with a thickness of 0.3 mm; the fifth layer is made of EFEP RP5000AS material with a thickness of 0.1 mm; the materials of each layer in Comparative Example 4 are all existing materials, and the multi-layer structure pipeline cannot be recycled because its materials are not compatible.

[0040] The comparison between Example 1-2 and Comparative Example 1-2 is shown in Table 1

[0041]

[0042]

[0043] Table 1 Comparison of Examples 3-4 and Comparative Examples 3-4 See Table 2

[0044]

[0045]

[0046] Table 2

[0047] Precipitates in Table 1 and Table 2: Refer to TL 52712 standard, according to SAE J2260 test method Solubleconstituents (soluble components): <6g m2;

[0048] Insoluble constituents: <0.7 g m2;

[0049] Electrical conductivity: According to SAE J2260 test method

[0050] The surface resistivity determined by the resistance value measured on the sample (inner wall of the pipeline) should not be greater than 10 6 Ω. Mechanical performance requirements: axial yield strength: ≥24MPa;

[0051] Radial yield strength: ≥25MPa;

[0052] Axial elongation at break: ≥170%;

[0053] Radial elongation at break: ≥170%;

[0054] Interlayer adhesion: ≥2.5N mm.

[0055] The above is only a preferred embodiment of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A low-carbon recyclable nylon pipeline for fuel system, It is characterized in that The invention comprises a protective layer (1), an adhesive layer (2), a barrier layer (3), a structural layer (4) and a working condition layer (5) which are arranged in sequence from the outside to the inside, wherein the protective layer (1) is a bio-based polyamide PA11 layer or a polyamide PA12 layer, the adhesive layer (2) is a modified polyamide PA12 layer or a first modified polyamide PA6 layer, the barrier layer (3) is a polyamide MXD6 layer or a polyamide MXD9 layer, the structural layer (4) is a second modified polyamide PA6 layer, and the working condition layer (5) is a low precipitation type modified polyamide PA6 layer or a low precipitation conductive modified polyamide PA6 layer or a conductive modified polyamide PA6 layer or a low precipitation modified polyamide PA612 layer or a low precipitation conductive modified polyamide PA612 layer.

2. The low-carbon recyclable nylon pipeline for a fuel system according to claim 1, It is characterized in that The thickness of the protective layer (1) is a, 0.1 mm ≤ a ≤ 0.5 mm.

3. The low-carbon recyclable nylon pipeline for a fuel system according to claim 1, It is characterized in that The thickness of the adhesive layer (2) is b, 0.03 mm ≤ b ≤ 0.4 mm.

4. The low-carbon recyclable nylon pipeline for a fuel system according to claim 1, It is characterized in that The thickness of the barrier layer (3) is c, 0.05 mm ≤ c ≤ 0.4 mm.

5. The low-carbon recyclable nylon pipeline for a fuel system according to claim 1, It is characterized in that The thickness of the structural layer (4) is d, 0.2 mm≤d≤0.8 mm.

6. The low-carbon recyclable nylon pipeline for a fuel system according to claim 1, It is characterized in that The thickness of the working condition layer (5) is e, 0.05mm≤e≤0.5mm.

7. The low-carbon recyclable nylon pipeline for a fuel system according to claim 1, It is characterized in that The total wall thickness of the nylon pipe from the protective layer (1) to the working layer (5) is f, and 0.43 mm ≤ f ≤ 2.6 mm.

8. The low-carbon recyclable nylon pipeline for a fuel system according to claim 1, It is characterized in that The protective layer (1) is a bio-based polyamide PA11 layer, the adhesive layer (2) is a first modified polyamide PA6 layer, the barrier layer (3) is a polyamide MXD6 layer, the structural layer (4) is a second modified polyamide PA6 layer, and the working layer (5) is a low-precipitation modified polyamide PA612 layer.

9. The low-carbon recyclable nylon pipeline for a fuel system according to claim 1, It is characterized in that The protective layer (1) is a polyamide PA12 layer, the adhesive layer (2) is a modified polyamide PA12 layer, the barrier layer (3) is a polyamide MXD6 layer, the structural layer (4) is a second modified polyamide PA6 layer, and the working layer (5) is a conductive modified polyamide PA6 layer.

10. The low-carbon recyclable nylon pipeline for a fuel system according to claim 1, It is characterized in that The protective layer (1) is a bio-based polyamide PA11 layer, the adhesive layer (2) is a first modified polyamide PA6 layer, the barrier layer (3) is a polyamide MXD6 layer, the structural layer (4) is a second modified polyamide PA6 layer, and the working layer (5) is a low-precipitation conductive modified polyamide PA612 layer.