Filter stick

By covering the nanofiber membrane layer on the rope and fleece structure material and spinning the filter rod using electrospinning technology, the difficulty of rolling the fleece structure material into a rod is solved, achieving lightweight, uniform filtration effect and convenient recycling.

CN221931278UActive Publication Date: 2024-11-01NANTONG CELLULOSE FIBERS CO LTD +2
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202323431554.0
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-12-15
Publication Date
2024-11-01
Estimated Expiration
2033-12-15

AI Technical Summary

Technical Problem

There are difficulties in rolling into filter rods and are difficult to successfully apply.

Method used

Using rope and velvet structure material, the nanofiber membrane layer is covered on its outer peripheral surface, and the nanofiber membrane is spun in the electrostatic field using electrostatic field with electrostatic spinning technology to closely adhere to the "test tube brush-shaped" cluster fiber velvet, forming rope and velvet structure material It is a filter rod with filter element and nanofiber membrane as the shell.

Benefits of technology

The difficulty of rolling into a rod is overcome, lightweight, uniform filter quality, stable structural quality, and easy to mass production. In the preferred embodiment, all materials are cellulose diacetate, which is convenient for recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221931278U_ABST
    Figure CN221931278U_ABST
Patent Text Reader

Abstract

The filter stick comprises a filter element, the filter element comprises at least one or more than one rope velvet structure material, and the peripheral surface of the rope velvet structure material is covered with a nanofiber membrane layer shell to form the filter stick. The nanofiber membrane layer is composed of a plurality of single layers. The rope wool structure material comprises a core wire and fiber wool extending outwards along the axis of the core wire. The utility model also discloses a preparation method of the filter stick, which comprises the following steps: preparing a spinning solution by using a fiber-forming polymer, taking a rope velvet structure material as a receiving body, and spinning a nanofiber membrane layer on the surface of the rope velvet structure material by adopting an electrostatic spinning technology, so as to form the filter stick which takes the rope velvet structure material as a filter element and takes the nanofiber membrane as a shell. The nanofiber membrane spun by the utility model is attached to fiber fluff of a rope fluff structure material, has the characteristics of light weight, uniform and stable filtering quality and the like, is easy to produce in batches, is single in material, and is convenient to recycle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model belongs to the field of cigarettes and relates to a filter rod structure. Background Art

[0002] Regarding the preparation of cigarette filters, Li et al. prepared cellulose acetate fiber needle-punched felt from waste cigarette filters through fiber loosening, fiber degumming, fiber combing, fiber laying, lamination and needle punching processes. The felt has a good removal effect on ammonia-like unfriendly gases. The technology was disclosed in the article 157243, issue 845, 2022 of "Science of the Total Environment". The title of the article is: Kinetic optimization of odor adsorption with acetate fiber cloth prepared from waste cigarette filter, Science of The Total Environment, 2022, 845, 157243. Duan et al. dissolved waste cigarette filters and lanthanum cerium manganese oxide perovskite nanoparticles in a mixed solvent, and used electrospinning technology to produce a double perovskite-doped cellulose acetate composite nanofiber membrane, which can be used for formaldehyde decomposition and air purification at room temperature. The technology was disclosed in Cellulose, Issue 30, 2023, Pages 5795-5809, with the title: From waste to wealth: a cellulose-based fibrous membrane from recycled cigarettes supported with dual perovskite forformaldehyde degradation at room temperature, Cellulose, 2023, 30, 5795-5809. Compared with conventional filter rod materials, the fluff of velvet structure materials is soft, and there are great difficulties in rolling them into filter rods. It is urgent to develop new methods to successfully apply them. Utility Model Content

[0003] Aiming at the problem that it is difficult to roll the chenille yarn structure material into a rod in the prior art, the utility model provides a filter rod.

[0004] In order to achieve the above purpose, the solution of the utility model is:

[0005] A filter rod comprises a filter element, wherein the filter element comprises at least one or more chord structure materials, and the outer peripheral surface of the chord structure material is covered with a nanofiber membrane layer shell to form the filter rod.

[0006] Optionally, the material of the velvet structure material and the nanofiber membrane is a fiber-forming polymer, preferably at least one of cellulose diacetate, polyacrylonitrile, polylactic acid, and polyisophthalamide, preferably a single material, more preferably cellulose diacetate.

[0007] Optionally, the nanofiber membrane layer is composed of several single layers.

[0008] The thickness of the nanofiber membrane layer is 0.01 to 4.5 mm, preferably 0.1 to 1 mm.

[0009] The filter rod has a diameter of 4-9 mm and a porosity of 20%-99.9%, preferably 50%-99.5%, and more preferably 90%-99%.

[0010] Optionally, the velvet structural material comprises a core wire and fiber fluff extending outwardly along the axis of the core wire; the core wire and the axis of the filter rod may coincide with or be parallel.

[0011] Optionally, the three-dimensional appearance of the velvet structure material may be similar to a "test tube brush", with the fiber fluff scattering outward from the axis, or forming a fixed angle with the axial direction of the core wire, preferably in the range of 45-135°, more preferably 80-100°.

[0012] Optionally, the fiber fluff is fixedly arranged on the section from the core axis to form but not limited to a flat straight structure, a Y-shaped structure, a cross structure, or a snowflake structure. The "Y-shaped structure, cross structure, or snowflake structure" refers to a pattern formed by the radial projection of the fiber fluff on a sufficiently long section of chenille material on the core.

[0013] Optionally, the connection point between the fiber fluff and the core wire is spiral or ring-shaped along the axis of the core wire. Optionally, the ring-shaped means that, like a ring, a ring of fiber fluff is placed on the core wire at a certain distance, and the rings are not connected; the spiral structure has a pitch of 0.2-50mm, preferably 1.2-5mm.

[0014] Optionally, the central thickness of the thread-shaped structure corresponds to the diameter of the core material, the thread thickness is proportional to the diameter of the fiber fluff, and the thread pitch corresponds to the inverse of the twist of the velvet structure material.

[0015] Optionally, the fiber fluff is arranged in a periodic structure along the axial direction of the core wire, including one or more combinations of cones, cylinders, and truncated cones; optionally, the circumferential spacing of the periodic arrangement structure is 0.5-80 mm, preferably 5-30 mm.

[0016] Optionally, the ends of the fiber fluff are in contact with the inner wall of the nanofiber membrane layer shell.

[0017] Optionally, the fiber fluff has a fiber fineness of 0.5-133 dtex, preferably a fiber fineness of 2.0-22 dtex.

[0018] Optionally, the core wire is made of a degradable or recyclable material.

[0019] Optionally, the core wire has a fineness of at least 2 tex, preferably 5-80 tex; a strength of at least 2N, optionally, a strength of at least 10N.

[0020] The preparation method of the chenille structural material comprises the following steps:

[0021] (1) Any fiber bundle is selected as the velvet yarn, any one of filament, single yarn and ply yarn is used as the core yarn, a gauge with different neck width is selected, the rotating head speed, twist direction, spindle speed and roller speed are adjusted, and the velvet structure material is obtained by the integrated spinning technology of "velvet yarn cutting-core yarn twisting";

[0022] Optionally, any one of filament yarn, single yarn and ply yarn is used as the core yarn, and velvet yarn of the same material is selected;

[0023] It should be noted that, for the lanyard structural material in which the connection points between the fiber fluff and the core wire form a spiral wire with the core wire as the axis: the diameter of the column core is proportional to the fineness of the core material.

[0024] The thread thickness is approximately proportional to the fiber denier / density, mainly due to the difference in fiber cross-sectional shape.

[0025] The thread pitch is proportional to the roller speed / spindle speed.

[0026] Optionally, the chord velvet structural material may be core-wrapped in a bundling-like manner on the periphery of the chord velvet structural material to improve the firmness of the fiber fluff in the chord velvet structural material.

[0027] In addition, there are other processes that can achieve the embedding of fibers in loops, and then the nesting of loops to form long chenille structural materials, which will not be described here.

[0028] (2) One spun velvet structure material or at least one spun velvet structure material is combined and twisted to form velvet structure materials of different thicknesses.

[0029] The preparation method of the filter rod comprises the following steps: preparing a spinning solution with a fiber-forming polymer, using a velvet structural material as a receiver, and using electrostatic spinning technology to spin a nanofiber membrane layer on the surface of the velvet structural material, thereby forming a filter rod with the velvet structural material as a filter core and the nanofiber membrane as an outer shell.

[0030] Optionally, the nanofiber membrane layer is spun from a plurality of single layers or layers.

[0031] Optionally, the polymer is at least one of cellulose diacetate, polyacrylonitrile, polylactic acid, and poly(m-phenylene isophthalamide).

[0032] Furthermore, the method for preparing the filter rod comprises the following steps:

[0033] (1) Spinning solution preparation: Weigh a certain amount of fiber-forming polymer and add it to the mixed solvent, stirring until the spinning solution is uniform;

[0034] (2) Using filament as core thread and fiber tow as velvet yarn, selecting gauges of different specifications and models, adjusting parameters such as rotary head speed, twist direction, spindle speed, and roller speed, and obtaining velvet structural materials through the integrated spinning technology of "velvet yarn cutting-core thread twisting";

[0035] (3) The spinning solution prepared in step (1) is transferred to an electrospinning machine, and the velvet structure material prepared in step (2) is used as a receiving body, and a filter rod is obtained by electrospinning technology; in other words, the filter rod of the utility model is obtained by wrapping a nanofiber membrane layer around the outer periphery of the entire velvet structure material.

[0036] Optionally, in step (1), the polymer is a fiber-forming polymer, preferably a single material; the polymer includes but is not limited to cellulose diacetate, polyacrylonitrile, polylactic acid, polyisophthalamide, etc., preferably cellulose diacetate or cellulose diacetate fiber material from washed and recycled cigarette butts. It should be noted that the polymer can be made of different materials, but it is more convenient to recycle a single material. From this perspective, it is preferred to use a single material. More preferably, all materials of the utility model are cellulose diacetate fibers, which can be directly dissolved together for recycling and respinning.

[0037] Optionally, in step (1), the polymer is stirred at 20-60° C. for 0.5-3 h until the spinning solution is uniform.

[0038] Optionally, in step (1), the mixed solvent is one of dimethylacetamide, dimethylformamide, and acetone, or a combination of acetone and dimethylacetamide or dimethylformamide.

[0039] Preferably, in step (1), the mass ratio of acetone to dimethylacetamide in the mixed solvent is 2:1 or the mass ratio of acetone to dimethylacetamide is 2:1.

[0040] Optionally, in step (1), the mass fraction of the cellulose diacetate in the spinning solution is 5 to 18% by weight.

[0041] Optionally, in step (2), the core wire fineness is at least 2 tex, preferably between 5 and 80 tex; the fiber fineness of the fiber bundle is 0.5-133 dtex, preferably the fiber fineness is 2.2-22 dtex.

[0042] Optionally, in step (2), the corresponding gauge neck width is 0.8-10 mm, preferably 1.5-4.5 mm; or, the rotating head speed in step (2) is 4000-30000 r / min, preferably 12000-15000 r / min; or, the twist direction in step (2) is S twist or Z twist; or, the spindle speed in step (2) is 100-4000 r / min, preferably 400-3000 r / min; or, in step (2); the roller speed is set at 4-20 m / min.

[0043] Optionally, in step (3), the electrospinning process parameters are set to a positive pressure range of 10 to 15 kV, a negative pressure range of 0 to -5 kV, a receiving distance of 10 to 20 cm, and the receiving body is driven by active constant-speed transmission motors at both ends, with a rotation speed set to 300 to 1000 rpm, and the entire spinning process time is maintained at 40 to 120 min.

[0044] Due to the adoption of the above technical solution, the beneficial effects of the utility model include: the utility model proposes to use diacetyl cellulose to configure the spinning solution, use the velvet structure material as the receiver, and use the electrostatic spinning technology to spin a layer of nanofiber membrane on the surface of the velvet structure material, thus forming a filter rod with the velvet structure material as the filter element and the nanofiber membrane as the shell. In this structure, the nanofiber membrane spun in the electrostatic field fits tightly to the "test tube brush-like" clusters of fluff, overcoming the difficulty of rolling into a rod, and has the characteristics of light weight and uniform filtering quality. The product structure has stable quality and is easy to mass produce. In the preferred embodiment, all materials are diacetyl cellulose, which is very convenient to recycle. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 The figure is a schematic diagram of the outline of an embodiment of the cigarette filter rod of the utility model.

[0046] Figure 2 It is a longitudinal schematic diagram of an embodiment of a filter rod made of chenille structural material of the utility model.

[0047] Figure 3 This is a schematic diagram of the spiral structure of an embodiment of the chenille structural material of the utility model.

[0048] Figure 4 Schematic diagram of the principle of preparing a chenille structure material structure for the utility model Figure 1 .

[0049] Figure 5Schematic diagram of the principle of preparing a chenille structure material structure for the utility model Figure 2 .

[0050] Fig. 6A It is a longitudinal schematic diagram of an embodiment of the "straight-line" chenille structural material of the utility model.

[0051] Figure 6B It is a horizontal schematic diagram of an embodiment of the "straight-line" chenille structural material of the utility model.

[0052] Fig. 7A It is a horizontal schematic diagram of an embodiment of the "Y-shaped" chenille structural material of the utility model.

[0053] Figure 7B It is a horizontal schematic diagram of an embodiment of the "cross-shaped" chenille structural material of the utility model.

[0054] Figure 7C It is a horizontal schematic diagram of an embodiment of the "snowflake type" chenille structural material of the utility model.

[0055] Markings in the figure: 1, rotating head; 2, velvet yarn; 4, gauge; 5, chenille yarn; 6, blade;

[0056] 10, filter rod; 10-1, fiber fluff; 10-2, core wire; 10-3, nanofiber membrane layer shell. DETAILED DESCRIPTION

[0057] The utility model filter rod comprises a filter core part and a nanofiber membrane layer shell, the filter core part comprises a chord structure material, the chord structure material comprises a core line and fiber fluff arranged along the core line and extending outward from the axis; the core line coincides with or is parallel to the axis of the outer layer wrapping material. The fiber fluff of the chord structure material is scattered outward from the axis; the ends of the fiber fluff are in contact with the inner wall of the outer layer wrapping material; the connection point between the fiber fluff and the core line is spiral or annular along the axis of the core line.

[0058] Specifically, a filter rod 10 is composed of an inner velvet structure material composed of fiber fluff 10-1, a core wire 10-2, and a nanofiber membrane layer outer shell 10-3. The velvet structure material can be a special form similar to a "test tube brush shape", which is made of, but not limited to, diacetate fiber as the velvet yarn, and ordinary yarn as the core yarn, which is spun on a fancy spinning machine with a twisted core wire 10-2 as the axis, and a special form of velvet structure material composed of fiber fluff 10-1 is arranged on it. Please refer to Figure 1 Its internal pore structure is mainly determined by the spatial distribution of fiber hair 10-1 of the velvet structure material.

[0059] Optionally, the connection point between the fiber fluff 10-1 and the core wire 10-2 forms a spiral line or a ring with the core wire 10-2 as the axis; further, the extension direction of the spiral line diverges in a spiral (spiral) toward the outer circumference, showing a periodic, uniform and regular distribution.

[0060] Optionally, the fiber fluff 10 - 1 is arranged in a periodic structure along the axial direction of the core wire 10 - 2 .

[0061] Optionally, the ends of the fiber fluff 10 - 1 are in contact with the inner wall of the outer wrapping material.

[0062] The filter rod of the utility model can provide a new smoke flow channel. The main factors include the materials used for the core wire and fiber fluff, fiber denier, and fiber root number, which affect the main physical indicators of the filter rod including porosity, and then produce different effects on smoke components, cooling and suction resistance.

[0063] The utility model achieves the specified requirements through the process to adapt to the inner cavity size of the filter rod with a circumference of 14-28 mm, and adopts at least one lanyard structural material containing a core wire and fiber fluff.

[0064] A production process of an embodiment of a velvet structural material: two core wires clamp hundreds of short fibers through twisting, and the fibers actually present a certain spiral arrangement between each node; similar to the arrangement of spiraling stairs, similar to the process of twisting hemp rope, certain fibers are clamped in the nodes, and the spatial arrangement of the fibers also presents a certain rotation with the curvature of the hemp rope (caused by twisting), and may not be on the same plane, but is a periodic, extended, divergent arrangement in the cylinder along the axis of the core material.

[0065] Please refer to the attached picture, Fig. 6A , Figure 6B In the figure, the core wire 10-2 is composed of two or more core materials twisted with each other, the fiber fluff 10-1 is fiber fluff and fiber fluff clusters, an angle α is formed between the fiber fluff 10-1 and the core wire 10-2, and the nearly circular diameter of the lanyard structural material is d.

[0066] Fig. 7A , Figure 7B and Figure 7C The chenille structural material with any transverse cross section shown in the figure can be obtained by die extruding a chenille structural material with a corresponding radial transverse cross section.

[0067] It is particularly important to emphasize that the drawings of the present invention are for the purpose of facilitating understanding and schematically illustrating the basic structure and principle of the present invention. The scope of the present invention is not limited to the structures shown in the drawings. While meeting basic requirements, the core wires, fiber fluffs, and periodic structures of the present invention are not all absolutely regular and orderly.

[0068] Furthermore, a novel filter rod and a preparation method thereof are provided, wherein the preparation method of the novel filter rod comprises the following steps:

[0069] (1) Spinning solution preparation: Weigh a certain amount of cellulose diacetate polymer or cellulose diacetate fiber material from washed and recycled cigarette butts, add it to a mixed solvent, and stir at 20 to 60° C. for 0.5 to 3 h until the spinning solution is uniform;

[0070] (2) Using cellulose diacetate filaments with a bundle fineness of 55-150d and a root number of 15-72f as the core yarn, cellulose diacetate fiber bundles with a single filament of 2.2d-20d and a root number of 300-600f as the velvet yarn, selecting different specifications and models of gauges, adjusting the parameters such as the rotating head speed, twist direction, spindle speed, and roller speed, and obtaining a cellulose diacetate chenille structure material through the cutting-twisting spinning technology;

[0071] Alternatively, using cellulose diacetate filaments with a fineness of 5 to 80 tex as the core yarn and cellulose diacetate fiber tows with a fineness of 2.2-22 dtex as the fleece yarn, selecting different specifications of gauges, adjusting the rotating head speed, twist direction, spindle speed, roller speed and other parameters, through the "fleece yarn cutting-core twisting" integrated spinning technology ((please refer to Figure 5 ) to obtain a cellulose diacetate chenille structure material;

[0072] (3) The spinning solution prepared in step (1) is transferred to an electrospinning machine, and the velvet structure material obtained in step (2) is used as a receiving body. The filter rod is spun by electrospinning technology, and the process parameters of the electrospinning process are set as a positive pressure range of 10 to 15 kV, a negative pressure range of 0 to -5 kV, and a receiving distance of 10 to 20 cm. The receiving body is driven by active constant-speed transmission motors at both ends, and the speed is set to 300 to 1000 rpm. The entire spinning process time is maintained at 40 to 120 min. The spun nanofiber membrane is fitted with a "test tube brush-like" cluster of fluff, has the characteristics of light weight, uniform and stable filtration quality, etc., and is easy to mass produce. In a preferred embodiment, all materials are cellulose diacetate, which is easy to recycle.

[0073] The present invention is further described below in conjunction with specific embodiments.

[0074] A filter rod 10 includes a filter element, wherein the filter element comprises at least one or more velvet structural materials, and the outer peripheral surface of the velvet structural material is covered with a nanofiber membrane layer shell 10-3 to form the filter rod.

[0075] In one embodiment, the material of the velvet structure material and the nanofiber membrane is a fiber-forming polymer, preferably at least one of cellulose diacetate, polyacrylonitrile, polylactic acid, and polyisophthalamide, preferably a single material, more preferably cellulose diacetate.

[0076] In one embodiment, the nanofiber membrane layer is composed of several single layers.

[0077] The thickness of the nanofiber membrane layer is 0.01 to 4.5 mm, preferably 0.1 to 1 mm.

[0078] The filter rod has a diameter of 4-9 mm and a porosity of 20%-99.9%, preferably 50%-99.5%, and more preferably 90%-99%.

[0079] In one embodiment, the velvet structural material comprises a core wire 10-2 and fiber fluff 10-1 extending outwardly along the axis of the core wire 10-2; the core wire 10-2 and the axis of the filter rod may coincide with or be parallel.

[0080] In one embodiment, the three-dimensional appearance of the velvet structure material may be similar to a "test tube brush", and the fiber fluff 10-1 is scattered outward from the axis, or forms a fixed angle with the axial direction of the core wire 10-2, preferably in the range of 45-135°, more preferably 80-100°.

[0081] In one embodiment, the fiber fluff 10-1 is fixedly arranged on a section from the axis of the core line 10-2 to form, but not limited to, a flat straight-line structure, a Y-shaped structure, a cross structure, or a snowflake structure. The "Y-shaped structure, cross structure, or snowflake structure" refers to a pattern formed by the radial projection of the fiber fluff 10-1 on a sufficiently long section of velvet material on the core line 10-2.

[0082] In one embodiment, the connection point between the fiber fluff 10-1 and the core wire 10-2 is spiral or ring-shaped along the axis of the core wire 10-2. In one embodiment, the ring-shaped means that, like a ring, a ring of fiber fluff 10-1 is placed on the core wire 10-2 at a certain distance, and the rings are not connected; the spiral structure has a pitch of 0.2-50mm, preferably 1.2-5mm.

[0083] In one embodiment, the central thickness of the thread-shaped structure corresponds to the diameter of the core material, the thread thickness is proportional to the diameter of the fiber fluff 10 - 1 , and the thread pitch corresponds to the inverse of the twist of the velvet structure material.

[0084] In one embodiment, the fiber fluff 10 - 1 is arranged in a periodic structure along the axial direction of the core wire 10 - 2 .

[0085] In one embodiment, the ends of the fiber fluff 10 - 1 are in contact with the inner wall of the nanofiber membrane layer shell 10 - 3 .

[0086] In one embodiment, the fiber fluff 10 - 1 has a fiber fineness of 0.5-133 dtex, preferably a fiber fineness of 2.0-22 dtex.

[0087] In one embodiment, the core wire 10 - 2 is made of a degradable or recyclable material.

[0088] In one embodiment, the core wire 10-2 has a fineness of at least 2 tex, preferably 5-80 tex; a strength of at least 2N, and in one embodiment, a strength of at least 10N.

[0089] Example 1

[0090] A method for preparing a filter rod comprises the following steps:

[0091] (1) Spinning solution preparation: Weigh 2 g of cellulose diacetate and add it to a mixed solvent prepared by 12 g of acetone and 6 g of dimethylacetamide, and stir at room temperature for 1.5 h until the spinning solution is uniform;

[0092] (2) Using 6 tex diacetate cellulose filament as the core yarn, 8.8 dtex monofilament diacetate cellulose fiber tow as the velvet yarn, a 4.2 gauge was selected, the rotating head speed was 15000 r / min, the twist direction could be Z twist, the spindle speed was set to 1200 r / min, the roller speed was set to 6 r / min, and a single material diacetate cellulose fiber chenille yarn was spun;

[0093] (3) The spinning solution prepared in step (1) is transferred to an electrospinning machine, and the velvet structure material obtained in step (2) is used as a receiving body. The filter rod of the utility model is spun by electrospinning technology, and the process parameters of the electrospinning process are set to a positive pressure range of 15 kV, a negative pressure range of -5 kV, and a receiving distance of 15 cm. The receiving body is driven by active constant-speed transmission motors at both ends, and the rotation speed is set to 400 rpm. The entire spinning process time is maintained for 100 minutes, thereby obtaining a filter rod with the velvet structure material as the filter element and the diacetate cellulose nanofiber membrane as the outer shell.

[0094] Conventional electrospinning receivers are rollers or plates, flexible receivers are fabrics or flowing liquids, and linear receivers are mostly hard material rods, which can be received by being driven by a motor on one side. This technology is not suitable for the utility model; the utility model uses flexible yarn with twist as the receiver, and is driven by equal-speed transmission motors on both sides, otherwise untwisting or over-twisting will occur, resulting in the inability to smoothly proceed with the spinning filter rod manufacturing process.

[0095] When a hard material is used as the receiver, one end is actively transmitted and the other end is clamped and passively rotated to achieve synchronization.

[0096] The tubular filter rod prepared by the utility model has a structure in which the nanofiber membrane spun in an electrostatic field fits tightly to the "test tube brush-like" clustered fiber villi, and the internal structure of the velvet thread supported by the "test tube brush-like" clustered villi can be observed, that is, the "traces" of the original velvet thread can be observed, and the fit is very tight.

[0097] Example 2

[0098] A method for preparing a filter rod comprises the following steps:

[0099] (1) Spinning solution preparation: Weigh 2 g of cellulose diacetate polymer and add it to a mixed solvent prepared by 12 g of acetone and 6 g of dimethylformamide, and stir at room temperature for 2 h until the spinning solution becomes uniform;

[0100] (2) Using 6 tex diacetate cellulose filament as the core yarn, 8.8 dtex monofilament diacetate cellulose fiber tow as the velvet yarn, using a 4.5 gauge, a rotating head speed of 12000 r / min, a Z twist, a spindle speed of 1000 r / min, and a roller speed of 8 r / min, to spin a single material diacetate cellulose fiber chenille structure material;

[0101] (3) The spinning solution prepared in step (1) is transferred to an electrospinning machine, and the velvet yarn obtained in step (2) is used as a receiving body. The electrospinning technology is adopted to spin the Lechebang material of the utility model, and the process parameters of the electrospinning process are set as follows: the positive pressure is set to 10 kV, the negative pressure is set to -5 kV, the receiving distance is 10 cm, the receiving body is driven by active constant-speed transmission motors at both ends, the speed is set to 500 rpm, and the entire spinning process time is maintained for 100 minutes, so as to obtain a filter rod with the velvet yarn as the filter element and the diacetate cellulose nanofiber membrane as the outer shell.

[0102] Example 3

[0103] A method for preparing a filter rod comprises the following steps:

[0104] (1) Spinning solution preparation: Weigh 12 g of cellulose diacetate polymer and add it to a mixed solvent prepared by 60 g of acetone and 30 g of dimethylacetamide, and stir at room temperature for 1 h until the spinning solution is uniform;

[0105] (2) The core yarn is cellulose diacetate filament with a bundle fineness of 8.3 tex, the monofilament fineness of cellulose diacetate fiber bundle is 8.8 dtex as the pile yarn, the model is 4.2 gauge, and the rotating head speed is 12000 r·min -1, the twist direction can be Z twist, the spindle speed is set to 1000r / min, the roller speed is set to 8r / min, and the single material diacetate cellulose fiber chenille structure material is spun;

[0106] (3) The spinning solution prepared in step (1) is transferred to an electrospinning machine, and the velvet yarn obtained in step (2) is used as a receiving body. The filter rod is spun by electrospinning technology, and the process parameters of the electrospinning process are set as follows: the positive pressure is set to 15 kV, the negative pressure is set to 0 kV, the receiving distance is 10 cm, the receiving body is driven by active constant-speed transmission motors at both ends, the speed is set to 600 rpm, and the entire spinning process time is maintained for 120 minutes, thereby obtaining a filter rod with a velvet structural material as a filter element and a cellulose diacetate nanofiber membrane as an outer shell.

[0107] Example 4

[0108] A method for preparing a filter rod comprises the following steps:

[0109] (1) Spinning solution preparation: Weigh 12 g of cellulose diacetate polymer and add it to a mixed solvent prepared by 60 g of acetone and 30 g of dimethylacetamide, and stir at room temperature for 1 h until the spinning solution is uniform;

[0110] (2) Using cellulose diacetate filaments with a bundle fineness of 8.3 tex as the core yarn, cellulose diacetate fiber tow with a monofilament fineness of 8.8 dtex as the velvet yarn, a 4.2 gauge was selected, the rotating head speed was 12000 r / min, the twist direction could be Z twist, the spindle speed was set to 1000 r / min, and the roller speed was set to 8 r / min, to spin a single material cellulose diacetate fiber chenille yarn;

[0111] (3) The spinning solution prepared in step (1) is transferred to an electrospinning machine, and the velvet yarn obtained in step (2) is used as a receiving body. The filter rod of the utility model is spun by electrospinning technology, and the process parameters of the electrospinning process are set as follows: the positive pressure is set to 15 kV, the negative pressure is set to 0 kV, the receiving distance is 10 cm, the receiving body is driven by active constant-speed transmission motors at both ends, the speed is set to 600 rpm, and the entire spinning process time is maintained for 120 minutes, thereby obtaining a filter rod with a velvet structural material as a filter element and a cellulose diacetate nanofiber membrane as an outer shell.

[0112] (4) Using the filter rod obtained in step (3) to replace the velvet yarn obtained in step (2) as the receiving body, repeating the spinning operation process of step (3) with the same process, a filter rod with velvet structural material as the filter core and diacetate cellulose nanofiber membrane as the outer shell is obtained.

[0113] The above-mentioned related explanations and descriptions of the embodiments are for the convenience of ordinary technicians in the technical field to understand and apply the utility model. It is obvious that those familiar with the technology in the field can easily make various modifications to these contents and apply the general principles described here to other embodiments without creative work. Therefore, the utility model is not limited to the above-mentioned related explanations and descriptions of the embodiments. Improvements and modifications made by technicians in the field based on the disclosure of the utility model without departing from the scope of the utility model should be within the scope of protection of the utility model.

Claims

1. A filter rod, comprising a filter element, Features: The filter element comprises at least one or more velvet structural materials, the outer peripheral surface of the velvet structural material is covered with a nanofiber membrane layer shell to form the filter rod; the velvet structural material comprises a core wire and fiber fluff extending outward along the axis of the core wire.

2. The filter rod according to claim 1, Features: The nanofiber membrane layer is composed of several single layers.

3. The filter rod according to claim 1, Features: The core wire coincides with or is parallel to the axis of the filter rod.

4. The filter rod according to claim 1, Features: The fiber fluff is freely scattered outward from the axis of the core wire or forms a fixed angle with the axial direction of the core wire.

5. The filter rod according to claim 4, Features: The angle range is 45-135°.

6. The filter rod according to claim 4, Features: The angle range is 80-100°.

7. The filter rod according to claim 1, Features: The fiber fluff is fixedly arranged on the axial section of the core wire to form but not limited to a straight-line structure, a Y-shaped structure, a cross structure, and a snowflake structure.

8. The filter rod according to claim 1, Features: The connection point between the fiber fluff and the core wire is spiral or ring-shaped along the axis of the core wire.

9. The filter rod according to claim 8, Features: The central thickness of the spiral corresponds to the diameter of the core material, the spiral thickness is proportional to the diameter of the fiber fluff, and the spiral pitch corresponds to the inverse of the twist of the velvet structure material.

10. The filter rod according to claim 8, Features: The pitch of the spiral is 0.2-50 mm.

11. The filter rod according to claim 8, Features: The pitch of the spiral is 1.2-5 mm.

12. The filter rod according to claim 1, Features: The fiber fluff is arranged periodically along the axial direction of the core wire, and includes one or more combinations of cones, cylinders, and truncated cones.

13. The filter rod according to claim 12, Features: The circumferential spacing of the periodically arranged structure is 0.5-80 mm.

14. The filter rod according to claim 12, Features: The circumferential spacing of the periodically arranged structure is 5-30 mm.

15. The filter rod according to claim 1, Features: The thickness of the nanofiber membrane layer is 0.01-4.5 mm.

16. The filter rod according to claim 1, Features: The thickness of the nanofiber membrane layer is 0.1-1 mm.

17. The filter rod according to claim 1, Features: The filter rod has a diameter of 4-9 mm.

18. The filter rod according to claim 1, Features: The porosity of the filter rod is 20%-99.9%.

19. The filter rod according to claim 1, Features: The porosity of the filter rod is 50%-99.5%.

20. The filter rod according to claim 1, Features: The porosity of the filter rod is 90%-99%.

Citation Information

Cited By

  • Filter stick material and preparation method thereof

    CN117859955A