Positive plate and electrochemical device

By constructing a gradient pore structure on the surface of the positive electrode, the problems of lithium deposition and wrinkling at the edges of silicon negative electrodes in electrochemical devices are solved, extending the cycle life of the battery and maintaining its capacity.

CN222029112UActive Publication Date: 2024-11-19REPT BATTERO ENERGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202323456142.2
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-12-18
Publication Date
2024-11-19
Estimated Expiration
2033-12-18

AI Technical Summary

Technical Problem

In existing electrochemical devices, when the silicon content in the negative electrode exceeds 10%, lithium plating and wrinkling are prone to occur at the edges, leading to battery capacity loss or short circuits, and the active material layer is prone to detachment after long-term cycling.

Method used

A gradient distribution of pores is constructed along the width direction of the positive electrode surface from the edge to the center region, with more pores at the edge region and fewer pores at the center region, to create a gradient NP ratio, reduce the degree of silicon lithium intercalation, and reduce the expansion and wrinkling of the negative electrode.

Benefits of technology

It effectively extends battery cycle life, reduces lithium plating and active material layer shedding, and improves battery capacity retention.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN222029112U_ABST
    Figure CN222029112U_ABST
Patent Text Reader

Abstract

The utility model provides a positive plate and an electrochemical device, the positive plate provided by the utility model comprises a positive current collector and a positive active material layer attached to at least one surface of the positive current collector, the surface of the positive active material layer is provided with a plurality of holes, and the distribution of the holes is reduced from the edge of the width direction of the positive plate to the central area. According to the positive plate provided by the invention, the gradient-distributed pore structure is constructed on the surface of the positive plate along the width direction of the positive plate, the number of pores in the edge region is large, the number of pores in the central region is small, the central region expands to the edge region, the NP ratio of the battery is gradually increased, and then the gradient NP ratio is constructed, and the larger the NP ratio of the battery is, the lower the lithium intercalation degree of silicon in the negative plate is; the lithium precipitation phenomenon is difficult to occur; meanwhile, the lower the lithium intercalation degree is, the smaller the expansion of the negative plate is, and the edge is less prone to wrinkling and material falling, so that the cycle life of the battery is effectively prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to the technical field of batteries, in particular to a positive electrode sheet and an electrochemical device. Background Art

[0002] With the widespread popularity of electric vehicles, their cruising range has become a core concern for users. By adding some silicon materials to the negative electrode side of the power battery, the energy density of the battery can be significantly improved, thereby increasing the cruising range of the car.

[0003] The silicon anode has a high theoretical specific capacity (3579mAh / g) and a high lithium insertion potential (about 0.4V vs Li / Li + ), is one of the mainstream trends in the development of negative electrode materials in the future. However, it will undergo a huge volume change (about 300%) during the process of lithium insertion and extraction, which will significantly damage the structure of the negative electrode sheet.

[0004] During the experiment, the researchers of this application found that in the composite negative electrode, when the mass proportion of silicon material is greater than 10%, the edge overhang area of ​​the negative electrode sheet will show wrinkles due to uneven stress after one or more charge and discharge processes. The appearance of such wrinkles will damage the electrode interface and easily cause lithium deposition at the edge of the electrode sheet. At the same time, after long-term cycling, the active material layer in the edge wrinkle area is very easy to fall off from the surface of the negative electrode current collector, causing loss of battery capacity or short circuit.

[0005] Therefore, it is particularly important to design the battery electrode structure accordingly to improve the edge wrinkling and shedding of the silicon-containing negative electrode, reduce the capacity loss of the battery, and improve the cycle performance.

[0006] In view of this, the present utility model is proposed. Utility Model Content

[0007] The main purpose of the utility model is to provide a positive electrode sheet and an electrochemical device to solve the problem that the silicon content in the negative electrode sheet used in the electrochemical device in the prior art is greater than 10wt%. During the charge and discharge process, lithium deposition is very likely to occur at the edge of the negative electrode sheet, and the active material layer in the edge wrinkle area is very likely to fall off after a long cycle, resulting in loss of battery capacity or short circuit.

[0008] In order to achieve the above-mentioned purpose, according to one aspect of the utility model, a positive electrode sheet is provided, which includes a positive electrode collector and a positive electrode active material layer attached to at least one surface of the positive electrode collector, and a plurality of holes are arranged on the surface of the positive electrode active material layer, and the distribution of the holes decreases from the edge in the width direction of the positive electrode sheet to the center area.

[0009] Furthermore, the depth of the pore is L, and the thickness of the positive electrode active material layer is H, wherein 0<L≤0.3H.

[0010] Further, the longitudinal section of the hole is an inverted triangle, an inverted trapezoid, a U-shape, a square or a semicircle. Further, the cross section of the hole in the plane where the upper surface of the positive electrode active material layer is located is a circle, and its radius is R1, and R1 satisfies: 6μm≤R1<30μm; or, the cross section of the hole in the plane where the upper surface of the positive electrode active material layer is located is a square, and its side length is R2, and R2 satisfies: 6μm≤R2<30μm.

[0011] Furthermore, along the width direction of the positive electrode sheet, at least two rows of holes are spaced apart on the surface of the positive electrode active material layer, each row of holes includes at least two holes, and a center line is formed by connecting the center points of all the holes in each row of holes; wherein the spacing d between the two center lines of any two adjacent rows of holes is 5 to 100 μm.

[0012] Furthermore, the positive electrode active material layer includes a positive electrode active material, a conductive agent and a binder, wherein the positive electrode active material is selected from at least one of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium cobalt oxide, lithium iron phosphate, lithium manganese iron phosphate or lithium-rich manganese.

[0013] According to another aspect of the present invention, an electrochemical device is provided, which includes a positive electrode sheet, a separator and a negative electrode sheet; wherein the positive electrode sheet is the positive electrode sheet provided in the first aspect.

[0014] Furthermore, the negative electrode sheet includes a negative electrode active material, the negative electrode active material includes a silicon material, and the mass proportion of the silicon material in the negative electrode active material is greater than 10%.

[0015] Furthermore, the mass proportion of the silicon material in the negative electrode active material is greater than 15wt%.

[0016] Furthermore, the silicon material is at least one of a silicon-carbon composite material and a silicon-oxygen composite material.

[0017] By applying the technical solution of the utility model, the positive electrode sheet provided by the present application constructs a gradient-distributed pore structure on the surface of the positive electrode sheet along the width direction of the positive electrode sheet from the edge to the center area. The number of pores in the edge area is large, and the number of pores in the center area is small. The center area expands toward the edge area, and the NP ratio of the battery gradually increases, thereby constructing a gradient NP ratio. The larger the battery NP ratio, the lower the degree of lithium insertion in the silicon of the negative electrode sheet, and the less likely it is for lithium precipitation to occur. At the same time, the lower the degree of lithium insertion, the smaller the expansion of the negative electrode sheet, and the less likely it is for wrinkles and material falling off to occur at the edge, thereby effectively extending the cycle life of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The drawings constituting part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation on the present invention. In the drawings:

[0019] Figure 1 A schematic top view of a positive electrode sheet provided according to Embodiment 1 of the utility model is shown.

[0020] Among them, the above-mentioned Figure 1 The following reference numerals are included:

[0021] 100. Positive electrode active material layer; 101. Hole. DETAILED DESCRIPTION

[0022] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present utility model will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0023] As analyzed in the background technology of this application, the electrochemical device in the prior art uses a negative electrode sheet containing silicon material, which is more conducive to improving the energy density of the battery and increasing the cruising range of the car. However, when the mass proportion of silicon material in the negative electrode active material in the negative electrode sheet is greater than 10%, the edge area of ​​the negative electrode sheet will appear wrinkled due to uneven stress during one or more charge and discharge processes. The appearance of such wrinkles will destroy the electrode interface and lithium deposition will easily occur at the edge of the electrode sheet. At the same time, after long-term circulation, the active material layer in the edge wrinkle area will easily fall off from the surface of the current collector, causing battery capacity loss or short circuit. In order to solve this problem, the present application provides a positive electrode sheet and an electrochemical device.

[0024] In a first typical embodiment of the present application, a positive electrode sheet is provided, which includes a positive electrode collector and a positive electrode active material layer 100 attached to at least one surface of the positive electrode collector, and a plurality of holes 101 are arranged on the surface of the positive electrode active material layer, and the distribution of the holes 101 decreases from the edge of the positive electrode sheet in the width direction to the center area.

[0025] It should be noted that, for the sake of convenience, the “width direction of the positive electrode sheet” in this application is as follows: Figure 1 Arrow direction in the diagram.

[0026] The positive electrode sheet provided in the present application constructs a gradient-distributed hole 101 structure from the edge to the center area along the width direction of the positive electrode sheet on the surface of the positive electrode sheet, with more holes in the edge area and fewer holes in the center area. The center area expands toward the edge area, and the NP ratio of the battery gradually increases (specifically, it can be understood that at the position containing holes, the NP ratio increases from the center area to the edge area, and the NP ratio of the part outside the holes remains unchanged; but when magnified to the entire battery level, the number of holes in the edge area is large, and the number of holes in the center area is small. In total, the center area expands toward the edge area, and the NP ratio of the battery gradually increases), thereby constructing a gradient NP ratio. The larger the NP ratio of the battery, the lower the degree of lithium insertion in the silicon of the negative electrode sheet, and the less likely it is to have lithium precipitation; at the same time, the lower the degree of lithium insertion, the smaller the expansion of the negative electrode sheet, and the less likely it is to have wrinkles and falling off at the edge of the negative electrode sheet, thereby effectively extending the cycle life of the battery.

[0027] In the present application, the specific distribution form of the holes 101 decreasing from the edge of the positive electrode sheet in the width direction to the central area is not limited, including but not limited to sequential reduction and irregular reduction, preferably sequential reduction.

[0028] In order to further improve the battery capacity, the depth of the hole 101 is preferably L, and the thickness of the positive electrode active material layer 100 is H, wherein 0<L≤0.3H, and the thickness of L is 0.05H, 0.08H, 0.1H, 0.15H, 0.2H, 0.25H, 0.3H or a range of any two values.

[0029] In the present application, if the positive electrode active material layer 100 is provided on only one surface of the positive electrode current collector, the thickness of the positive electrode active material layer 100 refers to the thickness of the positive electrode active material layer 100; if the positive electrode active material layer 100 is provided on both surfaces of the positive electrode current collector, the thickness of the positive electrode active material layer 100 refers to the thickness of the single-layer positive electrode active material layer 100.

[0030] The specific longitudinal section of the hole 101 is not specifically limited, and the longitudinal section of the hole 101 includes but is not limited to any one of an inverted triangle, an inverted trapezoid, a U-shape, a square or a semicircle; wherein the square includes both a square and a rectangle. The shape of the hole 101 includes but is not limited to any one of a cone, a truncated cone, a cylinder, a prism or a sphere.

[0031] In the present application, the longitudinal section of the pore 101 refers to a section along the thickness direction of the positive electrode active material layer (100).

[0032] In order to further reduce the lithium deposition phenomenon in the negative electrode sheet, in some embodiments, the cross-section of the hole 101 on the positive electrode sheet in the plane where the upper surface of the positive electrode active material layer 100 is located is circular, and its radius is R1, and its radius is R1, and R1 satisfies: 6μm≤R1<30μm. In other embodiments, the cross-section of the hole 101 is a square, and its side length is R2, and R2 satisfies: 6μm≤R2<30μm. Typically but not restrictively, R1 and R2 are each independently 6μm, 8μm, 10μm, 15μm, 20μm, 25μm, 30μm, or a range of any two values.

[0033] It should be noted that the cross section refers to the cross section of the plane where the surface of the positive electrode active material layer 100 away from the positive electrode current collector is located. It can also be understood that the hole 101 and the surface of the positive electrode active material layer 100 away from the positive electrode current collector intersect to form a cross section.

[0034] In order to further improve the edge wrinkling and falling-off phenomenon of the silicon-containing negative electrode sheet, preferably, along the width direction of the positive electrode sheet, at least two rows of holes are arranged on the surface of the positive electrode active material layer 100 at intervals, each row of holes includes at least two holes 101, and a center line is formed by connecting the center points of all the holes 101 in each row of holes; wherein the spacing d between the two center lines of any two adjacent rows of holes is 5 to 100 μm, such as 5 μm, 8 μm, 10 μm, 20 μm, 50 μm, 80 μm, 100 μm or a range value consisting of any two numerical values.

[0035] Specifically, Figure 1 For example, illustratively, along the width direction of the positive electrode sheet (i.e. Figure 1 The direction of the arrow in Figure 1 ), 5 rows of holes are arranged on the surface of the positive electrode active material layer 100 at intervals. For ease of understanding, the 5 rows of holes from top to bottom are referred to as the first row of holes, the second row of holes, the third row of holes, the fourth row of holes, and the fifth row of holes in sequence. Among them, the first row of holes includes 13 holes, and the center points of the 13 holes are connected to form a center line; the second row of holes includes 10 holes, and the center points of the 10 holes are connected to form a center line; the third row of holes includes 6 holes, and the center points of the 6 holes are connected to form a center line; the fourth row of holes includes 10 holes, and the center points of the 10 holes are connected to form a center line; the fifth row of holes includes 13 holes, and the center points of the 13 holes are connected to form a center line. It can be seen that along the width direction of the positive electrode sheet, the number of the first row of holes and the fifth row of holes located in the edge area is the largest, while the number of the third row of holes located in the center area is the smallest. It can be seen that the distribution of the holes 101 is reduced from the edge of the width direction of the positive electrode sheet to the central area.

[0036] In the present application, the hole 101 on the positive electrode sheet is prepared according to conventional methods in the art, including but not limited to mechanical roller pore making or laser pore making.

[0037] In the present application, the positive electrode active material layer 100 includes a positive electrode active material, a conductive agent and a binder, wherein the active material is a commonly used positive electrode active material in the art, including but not limited to a mixture of any one or more of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium cobalt oxide, lithium iron phosphate, lithium manganese iron phosphate or lithium-rich manganese.

[0038] In the application, the conductive agent is a commonly used conductive agent for positive electrode sheets in the art, which will not be described in detail here. The adhesive is a commonly used adhesive for positive electrode sheets in the art, which will not be described in detail here.

[0039] In order to further reduce the preparation cost of the positive electrode sheet, the positive electrode current collector is preferably one of commonly used aluminum foil, carbon-coated aluminum foil and composite current collector aluminum foil.

[0040] In some specific embodiments, the positive electrode sheet is prepared according to the following steps:

[0041] Step S1, according to the conventional electrode sheet manufacturing method in the art, after the processes of batching, coating, baking, etc., a rolled positive electrode sheet is obtained;

[0042] Step S2, mechanical rolling scheme or laser pore making scheme:

[0043] Mechanical rolling scheme: Use a roller with a specific convex point distribution on the surface to roll and form holes on the rolled positive electrode sheet obtained in S1, so as to obtain a positive electrode sheet with a special hole 101 distribution on the surface; Laser hole making scheme: First use a conventional roller with a smooth surface to roll the positive electrode sheet, and then control the intensity, distribution density, processing time and other parameters of the laser to melt the positive electrode material in a specific area on the surface of the electrode sheet after rolling and form holes 101.

[0044] In a second aspect of the present application, an electrochemical device is also provided. The electrochemical device includes a positive electrode sheet, a separator and a negative electrode sheet, wherein the positive electrode sheet is the positive electrode sheet provided in the first aspect above.

[0045] The electrochemical device provided in the present application constructs a gradient-distributed pore structure on the surface of the positive electrode sheet from the edge to the center area along the width direction of the positive electrode sheet, with more pores in the edge area and fewer pores in the center area. The center area expands toward the edge area, and the NP ratio of the battery gradually increases, thereby constructing a gradient NP ratio. The larger the battery NP ratio, the lower the degree of lithium insertion in the silicon of the negative electrode sheet, and the less likely it is for lithium precipitation to occur. At the same time, the lower the degree of lithium insertion, the smaller the expansion of the negative electrode sheet, and the less likely it is for wrinkles and material falling off to occur at the edge, thereby effectively extending the cycle life of the battery.

[0046] In order to further improve the energy density of the battery, the negative electrode sheet preferably includes a negative electrode active material, the negative electrode active material includes a silicon material, and the mass proportion of the silicon material in the negative electrode active material is greater than 10%. In particular, when the mass proportion of the silicon material in the negative electrode active material is greater than 15%, it is more conducive to reducing the edge expansion phenomenon of the negative electrode sheet, thereby more effectively extending the cycle life of the battery.

[0047] The specific composition of the above silicon material is not limited, and any silicon material commonly used in the battery field can be used, including but not limited to any one or more mixtures of silicon-carbon composite materials and silicon-oxygen composite materials.

[0048] In some embodiments, the negative electrode active material includes silicon material and graphite.

[0049] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material attached to at least one surface of the negative electrode current collector. In order to further reduce the cost, the negative electrode current collector is preferably copper foil.

[0050] In some embodiments, the negative electrode sheet is prepared according to the following steps: graphite, silicon-oxygen composite material, binder PAA (polyacrylic acid) and conductive agent SP are mixed evenly, dissolved in deionized water, and prepared into a slurry with solid content and viscosity that meet the requirements according to the common dispersion process in the art, copper foil is used as the current collector, and after the slurry coating, rolling and slitting processes, a graphite-doped silicon electrode sheet is obtained.

[0051] The electrochemical device provided in the present application is a power battery commonly used in the art, including but not limited to a lithium battery.

[0052] In some embodiments, a lithium battery is prepared according to the following steps: a positive electrode sheet, a negative electrode sheet and a separator are stacked to form a soft-pack battery, and after injecting an electrolyte, the battery is made into a lithium-ion battery through aging, formation, secondary sealing, and capacity division. The battery liquid is a mixed solution of 1 mol / L LiPF6 (lithium hexafluorophosphate) dissolved in EC (ethylene carbonate) and EMC (ethyl methyl carbonate) (volume ratio of 1:2). The electrolyte also contains additives, including 10% FEC (fluoroethylene carbonate), 2% VC (vinyl carbonate), 2% LiFSI (bis(fluorosulfonyl)imide lithium salt) and 0.5% DTD (vinyl sulfate). The beneficial effects of the present application will be further illustrated in conjunction with the embodiments below.

[0053] The above description is only the preferred embodiment of the utility model, and is not intended to limit the utility model. For those skilled in the art, the utility model can have various modifications and changes. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the utility model shall be included in the protection scope of the utility model.

Claims

1. A positive electrode sheet, characterized in that: The positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer (100) attached to at least one surface of the positive electrode current collector, a plurality of holes (101) are arranged on the surface of the positive electrode active material layer (100), and the distribution of the holes (101) decreases from the edge to the central area in the width direction of the positive electrode sheet.

2. The positive electrode sheet according to claim 1, characterized in that: The depth of the hole (101) is L, and the thickness of the positive electrode active material layer (100) is H, wherein 0<L≤0.3H.

3. The positive electrode sheet according to claim 1, characterized in that: The longitudinal section of the hole (101) is in the shape of an inverted triangle, an inverted trapezoid, a U-shape, a square or a semicircle.

4. The positive electrode sheet according to claim 1, wherein the cross section of the hole (101) in the plane where the upper surface of the positive electrode active material layer (100) is located is circular, and its radius is R1, and R1 satisfies: 6μm≤R1<30μm; Alternatively, the cross section of the pore (101) on the plane of the upper surface of the positive electrode active material layer (100) is a square, and its side length is R2, and R2 satisfies: 6μm≤R2<30μm.

5. The positive electrode sheet according to claim 1, characterized in that: At least two rows of holes are arranged at intervals on the surface of the positive electrode active material layer (100) along the width direction of the positive electrode sheet, each row of holes includes at least two holes (101), and a center line is formed by connecting the center points of all the holes (101) in each row of holes; wherein the spacing d between the two center lines of any two adjacent rows of holes is 5 to 100 μm.

6. The positive electrode sheet according to any one of claims 1 to 5, characterized in that: The positive electrode active material layer (100) comprises a positive electrode active material, a conductive agent and a binder, wherein the active material is selected from at least one of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium cobalt oxide, lithium iron phosphate, lithium manganese iron phosphate and lithium-rich manganese.

7. An electrochemical device, characterized in that: The electrochemical device comprises a positive electrode sheet, a separator and a negative electrode sheet, wherein the positive electrode sheet is the positive electrode sheet according to any one of claims 1 to 6.

8. The electrochemical device according to claim 7, characterized in that The negative electrode sheet includes a negative electrode active material, the negative electrode active material includes a silicon material, and the mass proportion of the silicon material in the negative electrode active material is greater than 10%.

9. The electrochemical device according to claim 8, characterized in that The silicon material accounts for more than 15% by mass of the negative electrode active material.

10. The electrochemical device according to claim 8 or 9, characterized in that: The silicon material is at least one of a silicon-carbon composite material and a silicon-oxygen composite material.