Ceramic multilayer capacitor
The ceramic multilayer capacitor addresses high ESR issues by employing optimized geometry and electrode arrangements with copper and Zr-rich PZT ceramic, achieving low ESR and ESL values, enhanced robustness, and cost-effective production.
Patent Information
- Application Number
- DE102012104033
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2012-05-08
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2032-05-08
AI Technical Summary
Existing ceramic multilayer capacitors exhibit high equivalent series resistance (ESR) values, which hinder their performance in high-performance applications such as AC/DC or DC/DC converters.
A ceramic multilayer capacitor design featuring specific aspect ratios (B/H ≥ 0.2, L/B ≥ 1, L/H ≥ 0.8) and internal electrode layer arrangements, including floating electrodes, along with a copper-based electrode material and a Zr-rich PZT ceramic composition, enhances the electrode cross-section and reduces ESR.
The design achieves a significantly lower ESR value (3-5 mΩ) and ESL, improves current-carrying capacity, and ensures mechanical and thermal robustness, while maintaining low manufacturing costs.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[0001] A ceramic multilayer capacitor is specified, particularly suitable for high-performance applications. The multilayer capacitor can be used, for example, as a filter element in an AC / DC or DC / DC converter.
[0002] The document WO 2011 / 085932 A1 describes a capacitor which comprises a heating element and a capacitor region with dielectric layers and internal electrodes arranged between the layers, wherein the heating element and the capacitor region are thermally conductively connected to one another.
[0003] Ceramic multilayer components are described in the publications US 7 808 770 B2, JP 2000-106 320 A and DE 103 45 500 A1.
[0004] It is an object to be achieved in at least some embodiments to provide a ceramic multilayer capacitor which, compared to known multilayer capacitors, has improved properties, such as a particularly low ESR value (equivalent series resistance).
[0005] This object is achieved by a subject matter according to the independent patent claim. Advantageous embodiments and further developments of the subject matter are further apparent from the dependent patent claims, the following description, and the drawings.
[0006] A ceramic multilayer capacitor according to at least one embodiment has a base body. The base body has a cuboid shape. The base body comprises dielectric layers arranged along a layer stacking direction to form a stack. The dielectric layers are preferably formed as ceramic layers. The base body further comprises first and second electrode layers arranged between the ceramic layers. For example, a first and a second electrode layer can each be arranged spaced apart from one another in the same layer plane. Furthermore, the first and second electrode layers can each be arranged in different layer planes of the stack.
[0007] According to a further embodiment, the base body comprises a first external contact. The external contact is preferably arranged on a first side surface of the base body and is electrically conductively connected to the first electrode layers. Preferably, the first electrode layers are directly electrically conductively connected to the first external contact, i.e., the first electrode layers directly border the first external contact and are directly connected to the first external contact. The first electrode layers preferably extend to the first side surface.
[0008] Furthermore, the base body has a second external contact, which is arranged on a second side surface of the base body opposite the first side surface and is electrically connected to the second electrode layers. Preferably, the second electrode layers are directly electrically connected to the second external contact, i.e., the second electrode layers directly border the second external contact and are directly connected to the second external contact. The second electrode layers preferably extend to the second side surface.
[0009] According to a further embodiment, the base body has a width B along the layer stacking direction. B here denotes the spatial extent of the base body of the multilayer capacitor along the layer stacking direction. Furthermore, the base body has a height H perpendicular to the first side surface. The height H can thus be understood as the spatial extent of the base body perpendicular to the first side surface of the base body. Preferably, the height H also runs perpendicular to the second side surface of the base body. Furthermore, the base body has a length L perpendicular to the height H and perpendicular to the layer stacking direction. The length L therefore denotes the spatial extent of the base body in a direction perpendicular to the width B and the height H.
[0010] According to a further embodiment, the relationship B / H ≥ 0.2 applies to the ratio of width B to height H. According to a preferred embodiment, B / H ≥ 0.3 applies. According to a further preferred embodiment, B / H ≥ 1.0 applies. According to a particularly preferred embodiment, B / H ≈ 0.35 applies.
[0011] According to a further embodiment, the ratio of the length L to the width BL / B ≥ 1. Furthermore, preferably L / B ≤ 5, and particularly preferably L / B ≤ 3.5.
[0012] According to a further embodiment, the ratio of length L to height HL / H ≥ 0.8 applies. According to a preferred embodiment, L / H ≥ 1 applies. According to a further preferred embodiment, L / H ≥ 1.2 applies.
[0013] By specifying the ratios between the width B and height H of the base body, the ratio of the supply cross-section of the electrode layers to the effective cross-section, i.e., the area that determines the capacitance, can be significantly increased in a ceramic multilayer capacitor described here. This allows the ceramic multilayer capacitor described here to have a particularly low ESR (equivalent series resistance). For example, a ceramic multilayer capacitor described here, e.g., with a capacitance between 4µF and 10µF, can have an ESR between 3 mΩ and 5 mΩ when operated at a frequency between 100 kHz and 1 MHz.
[0014] According to a further embodiment, the base body has third electrode layers that are not electrically connected to either the first or the second external contact. Preferably, the third electrode layers are not electrically connected to any external contact. The third electrode layers may also be referred to here and below as floating electrodes.
[0015] According to a further embodiment, the third electrode layers overlap with the first electrode layers. In other words, the third electrode layers each have at least one partial region that, when projected in the layer stacking direction of the stack, could be made to coincide with at least one partial region of the first electrode layers. Furthermore, the third electrode layers can overlap with the second electrode layers. For example, a first and a second electrode layer can each be arranged spaced apart from one another in a same layer plane of the base body and each overlap with at least one third electrode arranged in a further layer plane.
[0016] The use of first, second, and free third electrode layers—that is, the use of serial internal electrodes—advantageously increases the breakdown field strength, which is beneficial for the robustness and reliability of the multilayer capacitor. Furthermore, this enables a reduction in the dielectric layer thickness, that is, the layer thickness of the ceramic layers. This results in an increase in the cross-section of an electrode layer per volume of ceramic, thus improving the ESR (equivalent series resistance) value and the current-carrying capacity of the component for application currents.
[0017] According to a further embodiment, the ceramic layers have a layer thickness between 3 µm and 200 µm. According to a further preferred embodiment, the ceramic layers have a layer thickness between 10 µm and 100 µm. Particularly preferably, the ceramic layers have a layer thickness of approximately 25 µm.
[0018] According to a further embodiment, the electrode layers have a layer thickness between 0.1 µm and 10 µm. According to a preferred embodiment, the electrode layers have a layer thickness between 1 µm and 4 µm. Particularly preferably, the electrode layers have a layer thickness of approximately 3.5 µm.
[0019] According to a further embodiment, the base body has at least ten ceramic layers. According to a further embodiment, the base body has at least ten first electrode layers. According to a further embodiment, the base body has at least ten second electrode layers.
[0020] According to a further embodiment, the following relationship applies to the number of first electrode layers provided in the base body and the width B of the base body: the ratio of the number of first electrode layers to the width B ≥ 10 / mm. In other words, the base body has at least ten first electrode layers per mm of width. Furthermore, the base body preferably has at least ten second electrode layers per mm of width.
[0021] According to a further embodiment, the electrode layers comprise a base metal. Preferably, the electrode layers comprise copper. According to a preferred embodiment, the electrode layers are made of copper. Particularly after sintering of the multilayer capacitor, the electrode layers can be made of pure copper. Due to the high thermal and electrical conductivity of copper, a particularly low ESR (equivalent series resistance) value can be achieved in the multilayer capacitor described here. Furthermore, the use of base metals can advantageously reduce the cost of manufacturing the multilayer capacitor.
[0022] According to a further embodiment, the first and second side surfaces are surface-treated. For example, the first and second side surfaces can be lapped. Furthermore, it is possible for the first and second side surfaces to be ground, scrubbed, or plasma-etched. By means of the surface-treated side surfaces, particularly good contact between the external contacts and the first or second electrode layers can advantageously be achieved. In particular, by means of the surface treatment of the first and second side surfaces, ceramic material present between individual first electrode layers or between individual second electrode layers can be removed, so that the first and second electrode layers can be reliably applied to the surface of the base body using the process.For example, the external contacts can then be applied without the penetration of a gas flow, for example using a standard sputtering process.
[0023] According to a further embodiment, the first and second external contacts each have at least one first sputter layer, wherein the first sputter layers are in direct contact with the first or second electrode layers. Preferably, a first sputter layer is applied to the first side surface of the base body, which is in direct contact with exit surfaces of the first electrode layers from the base body. Likewise, a first sputter layer can be applied to the second side surface of the base body, which is in direct contact with exit surfaces of the second electrode layers from the base body. The sputter layers can, for example, have a layer thickness between 0.1 µm and 1.5 µm. Preferably, the first sputter layers comprise chromium or consist of chromium.
[0024] According to a further embodiment, the first and second external contacts each have a second sputter layer, wherein the second sputter layers are preferably applied directly to the first sputter layers. The second sputter layers preferably comprise copper or consist of copper.
[0025] According to a further embodiment, the first and second external contacts each have a third sputter layer, wherein the third sputter layers are preferably applied directly to the second sputter layers. The third sputter layers preferably comprise gold or consist of gold. Alternatively, the third sputter layers can also comprise silver or consist of silver.
[0026] According to the invention, the ceramic layers comprise a ceramic material for which the following formula applies: Pb(1-1.5a-0.5b+1.5d+e+0.5f)AaBb(Zr1- x Ti x )1-cdef Li d c eFe f Si c O3 + y PbO (I) where A is selected from the group consisting of La, Nd, Y, Eu, Gd, Tb, Dy, Ho, Er, and Yb; where B is selected from the group consisting of Na, K, and Ag; and where C is selected from the group consisting of Ni, Cu, Co, and Mn; with 0 < a < 0.12; 0.05 ≤ x ≤ 0.3; 0 ≤ b < 0.12; 0 ≤ c < 0.12; 0 ≤ d < 0.12; 0 ≤ e < 0.12; 0 ≤ f < 0.12; 0 ≤ y < 1, where b + d + e + f > 0.
[0027] Preferably, a particularly Zr-rich PZT solid solution phase is selected from the phase diagram. Furthermore, the condition b + d + e + f > 0 stipulates that, in addition to a dopant from the defined group A (rare earth element), the ceramic material must contain at least one element from the group consisting of Li, Na, K, Ag, Fe, Ni, Cu, Co, and Mn (lithium, iron, and groups B and C). This makes it possible to provide a ceramic material that is sinterable at temperatures from 1000 °C to 1120 °C, which enables combination with other materials that are not resistant to higher temperatures during the ceramic material manufacturing process. For example, sintering the ceramic material (“co-firing” process) with electrode layers made of base metals, such as silver or copper, is possible.In addition, the ceramic material has a higher switching field strength and / or higher relative permittivity (dielectric constant) compared to the PZT material doped only with group A.
[0028] In addition, low sintering temperatures favor the formation of small grain sizes in the ceramic material, which has a positive effect on the dielectric properties. More precisely, the dielectric properties of PZT ceramics are generally also determined by the domain size. Domains are defined as regions in the ceramic with the same polarization. The domain size depends on the grain size. The number of domains per grain increases with increasing grain size. The changing domain size has consequences for the material properties of the ceramic. Therefore, it is desirable to be able to control the grain size or grain growth.
[0029] Preferably, the doped lead zirconate titanate ceramic has a perovskite lattice which can be described by the general formula ABO3, where A stands for the A sites and B for the B sites of the perovskite lattice.
[0030] The perovskite lattice is characterized by a high tolerance to doping and vacancies.
[0031] The perovskite structure of lead zirconate titanate (PZT) can be described by the general formula ABO3. A unit cell of the PZT crystal lattice can be described by a cube. The A sites are occupied by Pb. 2+ -ions, which sit on the corners of the cube. In the center of each cube face sits an O 2- Ion. In the center of the cube is a Ti 4+ -ion and a Zr 4+-ion (B sites). This structure exhibits a high tolerance to substitution of the metal ions by other metal ions and defects, which makes it easy to dope.
[0032] Depending on the size difference between the ion introduced by doping and the ion replaced, the highly symmetric coordination polyhedron can be distorted. This distortion can change the crystal's center of symmetry and thus influence its polarizability.
[0033] The various doping options can be classified based on the valence of the doping ion. Isovalent doping, i.e., the replacement of one ion with another of the same valence, does not affect possible vacancies in the ceramic material. When lower-valence cations (acceptors) replace cations with a higher valence, vacancies are created in the anion lattice. Higher-valence cations (donors), when they replace lower-valence cations, create vacancies in the cation lattice. Doping with acceptors and donors each leads to characteristic changes in the material properties. Acceptor-doped ceramics are also referred to as "hard" ceramics, while donor-doped ceramics are referred to as "soft" ceramics.
[0034] Doping, for example with Nd 3+(or another rare earth element from group A), on the A-sites represents a donor doping. Due to the ionic radius of neodymium, this is deposited on the Pb 2+ -sites. Charge equalization occurs through the corresponding formation of Pb vacancies. The effect of doping is metric changes in the lattice and the influence of longer-acting interactions between the unit cells.
[0035] Doping, for example with K + or Fe 3+ , on the A and B sites represents an acceptor doping. Due to the ionic radius of potassium, this is deposited on the Pb 2+ -places, while Fe 3+ on the Zr 4+ or Ti 4+ -places. The charge balancing is achieved by reducing Pb 2+-Vacancies (A vacancies) and / or the corresponding formation of oxygen vacancies. The effect of doping is the formation of oxygen vacancies, which promotes grain growth and sinter densification and is induced by K acceptors at the sintering temperature. During the cooling process, recombination with the Nd donors can occur, forming quasi-neutral {Nd / K} defect pairs, so that there is no or only a very low concentration of lead or oxygen vacancies in the finished ceramic.
[0036] This doping affects the grain growth of the material, which depends on the concentration of the added dopant. Small amounts of dopant ions contribute to grain growth, whereas excessive amounts of dopant ions can inhibit grain growth.
[0037] The properties of donor-doped PZT materials, such as those found in the case where Nd occupies Pb sites, are essentially based on increased domain mobility caused by the Pb vacancies. These vacancies make the domains susceptible to influence even by small electric fields. Compared to undoped PZT ceramics, this leads to easier displacement of the domain boundaries and thus to higher dielectric constants.
[0038] Acceptor and donor dopants are present simultaneously in the ceramic material. This compensates for the negative properties that occur when the ceramic is doped with only one of the two doping types. For example, if only acceptor dopants were present, this often leads to decreasing dielectric constants, meaning the constants are lower than those of the undoped ceramic. If only donor dopants are present, grain growth is inhibited, and the ceramic bodies do not reach the desired size. However, the existing combination of dopants stands out positively from the undoped ceramic in these respects. It exhibits higher dielectric constants, which is also the case at lower sintering temperatures.
[0039] According to a preferred embodiment, 0.1 ≤ x ≤ 0.2 applies, since the polarization curves can be better adjusted in this range.
[0040] According to a further embodiment, 0≤y≤0.05.
[0041] According to a further embodiment, 0.001 < b < 0.12, more preferably d = e = f = 0.
[0042] According to a further embodiment, 0.001 < e < 0.12 applies, wherein more preferably b = d = f = 0 applies.
[0043] According to a further preferred embodiment, B is sodium (Na). This has a particularly advantageous effect on the material properties, in particular by lowering the sintering temperature compared to PZT material containing only a rare earth element, while simultaneously increasing the switching field strength.
[0044] According to a further preferred embodiment, the relative permittivity at an electric field strength of 1 kV / mm, preferably 2 kV / mm, is at least 60% of the relative permittivity at an electric field strength of 0 kV / mm. Further preferably, the relative permittivity (dielectric constant) of the ceramic material at a field strength of 2 to 5 kV / mm, preferably 1 kV / mm to 10 kV / mm, is at least 60% of the relative permittivity at an electric field strength of 0 kV / mm. The measurements are preferably carried out at a temperature of the ceramic material of 125°C.
[0045] According to a further preferred embodiment, the ceramic material has a relative permittivity of at least 500, preferably at least 1500, at an electric field strength of 1 kV / mm, preferably 2 kV / mm. More preferably, the ceramic material has a relative permittivity of at least 500, preferably at least 1500, at an electric field strength of 2 to 5 kV / mm, preferably 1 kV / mm to 10 kV / mm. The measurements are preferably carried out at a temperature of the ceramic material of 125°C.
[0046] Measuring polarization hysteresis is a standard method for determining relative permittivity (dielectric constant). Quasi-static methods are available for frequency-independent measurements, in which the hysteresis loop is measured point by point. For example, polarization measurements can be performed using the TF Analyzer 2000 from aixACCT Systems GmbH.
[0047] According to a further preferred embodiment, the ceramic material is an antiferroelectric dielectric. For this purpose, the base material PZT is preferably used from the antiferroelectric-orthorhombic phase region (O phase). The antiferroelectric order is characterized by a superposition of several polar sub-lattices whose electric dipole moments cancel each other out. An antiferroelectric crystal therefore does not possess spontaneous polarization, but rather special dielectric properties. If an electric field is applied to the antiferroelectric, it initially behaves like a linear dielectric. Above a certain critical field strength, a sudden transition to the ferroelectric phase is induced, and the formerly antiparallel dipoles flip into the energetically more favorable, parallel orientation. The reverse transition, however, occurs at a lower field strength.This results in a so-called double hysteresis loop.
[0048] Compared to ferroelectric ceramic materials, antiferroelectric ceramic materials exhibit less pronounced polarization-field strength hysteresis. This leads to lower energy losses when used in capacitors. For this reason, the use of antiferroelectric ceramic materials is preferred.
[0049] To produce pure and variously doped lead zirconate titanate (PZT) powders, the classic mixed oxide process or solvent-based processes, also known as "sol-gel" processes, can be used. The starting point is, for example, solutions of the acetates or alcoholates of the constituent metals, which are converted into granulated xerogels, the ceramic precursors, using various drying processes. Drying methods include spray drying and spray freeze granulation followed by freeze-drying. The precursors are then pyrolyzed to form the oxides. Powders produced in this way can be easily deagglomerated and conditioned for further processing.
[0050] A ceramic multilayer capacitor described here is characterized in particular by a particularly low ESR value (equivalent series resistance) and a particularly low ESL value (equivalent series inductance).
[0051] At the same time, the arrangement of the electrode layers described here is favorable for process control during the production of a multilayer capacitor described here. Both debinding and sintering require a gas exchange / equilibrium of debinding products and process gases, which is favored in the multilayer capacitor described here. The structure promotes improved process control options via the relatively short electrode layers in the lateral direction, which consequently also enables ceramic parts that are relatively large in volume compared to conventional multilayer capacitors. Furthermore, the multilayer capacitor described here results in synergy effects from the described arrangement of the electrode layers and the selected ceramic material of the ceramic layers, which have a positive impact on the ESR value, the ESL value, and the mechanical and thermal robustness.In particular, the combination of the ceramic material with the above-mentioned aspect ratios between W, H, and L, as well as the geometry of the electrode layers, can improve the electrical and thermal properties of the component. For example, the short paths that the current can take through the electrodes (geometry effect) combined with the thermal stability of the insulation resistance (ceramic property) have a highly positive effect on the current-carrying capacity of the component.
[0052] Further advantages and advantageous embodiments of the ceramic multilayer capacitor result from the following in connection with the Fig. 1 and Fig. 2 described embodiments.
[0053] They show: Fig. 1 a perspective schematic view of a ceramic multilayer capacitor according to an embodiment, Fig. 2 a cross-section of the ceramic multilayer capacitor Fig. 1.
[0054] In the exemplary embodiments and figures, identical or similarly functioning components may be provided with the same reference numerals. The illustrated elements and their relative sizes are generally not to scale. Rather, individual elements, such as layers, components, and regions, may be depicted as exaggeratedly thick or oversized for clarity and / or clarity.
[0055] The Fig. 1 and Fig. 2 show various schematic views of a ceramic multilayer capacitor 1 according to an exemplary embodiment. The multilayer capacitor 1 comprises a base body 2 having a cuboid shape with six side surfaces. The base body 2 has ceramic layers 3 and first and second electrode layers 41, 42 arranged between the ceramic layers 3, wherein the ceramic layers 3 and the electrode layers 41, 42 are arranged to form a stack along a layer stacking direction S. In particular, the base body 2 has at least 10 first and at least 10 second electrode layers 41, 42. In the exemplary embodiment shown, the ceramic layers 3 have a layer thickness of approximately 25 µm. The electrode layers 41, 42 have a layer thickness of approximately 3.5 µm. Alternatively, the ceramic layers 3 and the electrode layers 41, 42 can also have other layer thicknesses.
[0056] In the illustrated embodiment, the electrode layers comprise copper. This allows the multilayer capacitor 1 to have the lowest possible ESR value, while also reducing the cost of manufacturing the multilayer capacitor 1.
[0057] The multilayer capacitor 1 further comprises a first external contact 51 arranged on a first side surface 61 of the base body 2, and a second external contact 52 arranged on a second side surface 62 of the base body 2. The first electrode layers 41 are electrically conductively connected to the first external contact 51, and the second electrode layers 42 are electrically conductively connected to the second external contact 52. The first and second side surfaces 61, 62 are surface-treated, with the surface treatment preferably being performed before the application of the external contacts 51, 52. In particular, the first and second side surfaces 61, 62 can be lapped, scrubbed, ground, or plasma-etched.By means of the surface-treated side surfaces 61, 62, a particularly good contact between the external contacts 51, 52 and the first and second electrode layers 41, 42 can advantageously be achieved.
[0058] In the exemplary embodiment shown, a first and a second electrode layer 41, 42 are each arranged at a distance from one another in the same plane. This plane is formed by a layer plane that is perpendicular to the layer stacking direction S of the stack. A so-called gap, i.e., a space, is present between the first electrode layers 41 and the second electrode layers 42. This gap represents a region between a first electrode layer 41 and a second electrode layer 42 in the layer plane in which no electrode layers are arranged. According to an alternative exemplary embodiment, it is also possible for the first and second electrode layers 41, 42 to be arranged in different layer planes.
[0059] The base body 2 further comprises third electrode layers 43, which are not electrically connected to either the first or the second external contact 51, 52. The third electrode layers 43 overlap with both the first and the second electrode layers 41, 42, i.e., the third electrode layers 43 each have at least one partial region which, in a conceptual projection in the layer stacking direction S of the stack, could be made to coincide with at least one partial region of both the first and the second electrode layers 41, 42. According to the alternative exemplary embodiment, in which the first and second electrode layers 41, 42 are each arranged in different layer planes, it is possible for the first and second electrode layers 41, 42 to overlap with one another.
[0060] The first and second external contacts 51, 52 each have a first sputter layer, wherein the first sputter layers are each applied directly to the base body 2. The first sputter layers are in direct contact with the first and second electrode layers 41, 42, respectively. The first sputter layers preferably comprise chromium. Second sputter layers are each applied to the first sputter layers, wherein the second sputter layers preferably comprise copper. Furthermore, third sputter layers, which preferably comprise gold, are each applied to the second sputter layers. Alternatively, the third sputter layers can also comprise silver.
[0061] The base body 2 has a width B along the layer stacking direction S. In other words, B denotes the extension of the base body 2 in the direction parallel to the layer stacking direction S. Preferably, at least 10 first electrode layers and at least 10 second electrode layers are provided in the base body 2 per mm of width B of the base body. Furthermore, the base body 2 has a height H perpendicular to the first side surface 51. The base body 2 therefore has an extension perpendicular to the first side surface 51 that corresponds to the height H. Furthermore, the base body 2 has a length L perpendicular to the height H and perpendicular to the layer stacking direction S, which length corresponds to the extension of the base body 2 perpendicular to the layer stacking direction and perpendicular to the height H. The ratio of the width B to the height H of the base body 2 is B / H ≥ 0.2.Furthermore, the ratio of the length L to the width B of the base body is L / B ≥ 1 and the ratio of the length L to the height H of the base body is L / H ≥ 1.
[0062] In the illustrated embodiment, the base body 2 has a width B of approximately 2.5 mm, a height H of approximately 7.0 mm, and a length L of approximately 7.0 mm. Thus, the ratio B / H in the illustrated embodiment is approximately 0.36. The ratio L / B is approximately 2.8, and the ratio L / H is approximately 1.0.
[0063] The multilayer capacitor 1 according to the embodiment shown is characterized in particular by a low ESR value, a low ESL value and high mechanical and thermal robustness. For example, the multilayer capacitor 1 shown in the embodiment according to the Fig. 1 and Fig.The ceramic multilayer capacitor (380V / 10µF) shown in Figure 2 exhibits the following frequency-dependent values: ESR(min)=3 mΩ, ESR(100kHz)=5 mΩ, and ESL<4 nH. Furthermore, the multilayer capacitor 1 can be produced cost-effectively. List of reference symbols 1 multilayer capacitor 2 basic bodies 3 ceramic layers 41 first electrode layers 42 second electrode layers 43 third electrode layers 51 first external contact 52 second external contact 61 first side surface 62 second side surface H Height of the base body B Width of the base body L Length of the base body S Layer stacking direction
Claims
[1] Ceramic multilayer capacitor (1) with - a base body (2) comprising ceramic layers (3) arranged along a layer stacking direction (S) to form a stack, and first and second electrode layers (41, 42) arranged between the ceramic layers (3), wherein the base body (2) has a cuboid shape, - a first external contact (51) which is arranged on a first side surface (61) of the base body (2) and is electrically conductively connected to the first electrode layers (41), and - a second external contact (52) which is arranged on a second side surface (62) of the base body (2) opposite the first side surface (61) and is electrically conductively connected to the second electrode layers (42), wherein - the base body (2) has a width B along the layer stacking direction (S), - the base body (2) has a height H perpendicular to the first side surface (61), - the base body (2) has a length L perpendicular to the height H and perpendicular to the layer stacking direction (S), - where B / H ≥ 0.2, wherein the ceramic layers (3) comprise a ceramic material for which the following formula applies: Pb (1-1,5a-0,5b+1,5d+e+0,5f) A a B b (Zr1- x Ti x ) 1-c-d-e-f Li d c e Fe f Si c O3 + y.PbO (I) wherein A is selected from the group consisting of La, Nd, Y, Eu, Gd, Tb, Dy, Ho, Er, and Yb; B is selected from the group consisting of Na, K, and Ag; C is selected from the group consisting of Ni, Cu, Co, and Mn; and 0 <a<0,12 0.05≤x≤0.3 0≤b≤0.12 0≤c≤0.12 0≤d≤0.12 0≤e≤0.12, 0≤f≤0.12 0≤y≤1, where b + d + e + f > 0. [2] Multilayer capacitor according to claim 1, wherein L / B ≥ 1. [3] Multilayer capacitor according to one of claims 1 or 2, wherein L / H ≥ 1. [4] Multilayer capacitor according to one of the preceding claims, wherein the base body (2) has third electrode layers (43) which are not electrically conductively connected to either the first or the second external contact (51, 52). [5] A multilayer capacitor according to claim 4, wherein the third electrode layers (43) overlap with the first and second electrode layers (41, 42). [6] Multilayer capacitor according to one of the preceding claims, wherein the ceramic layers (3) have a layer thickness between 3 µm and 200 µm. [7] Multilayer capacitor according to one of the preceding claims, wherein the electrode layers (3) have a layer thickness between 0.1 µm and 10 µm. [8] Multilayer capacitor according to one of the preceding claims, wherein the base body (2) has at least 10 first electrode layers (41) and at least 10 second electrode layers (42). [9] Multilayer capacitor according to one of the preceding claims, wherein the following relationship applies: Number of first electrode layers / width B ≥ 10 / mm. [10] Multilayer capacitor according to one of the preceding claims, wherein the electrode layers (41, 42, 43) comprise copper. [11] Multilayer capacitor according to one of the preceding claims, wherein the first and second side surfaces (61, 62) are surface-treated. [12] Multilayer capacitor according to claim 11, wherein the first and second side surfaces (61, 62) are lapped, ground or plasma etched. [13] Multilayer capacitor according to one of the preceding claims, wherein the first and the second external contact (51, 52) each have at least one sputter layer which is in direct contact with the first or second electrode layers (41, 42).
Citation Information
Patent Citations
ceramic multilayer component
DE10345500A1
Laminated ceramic capacitor
JP2000106320A
Monolithic ceramic capacitor
US7808770B2
Temperature-independent capacitor and capacitor module
WO2011085932A1
JP002000106320A