Layer resistor with a carbon-containing resistance material, method for its production and sensor element
The sheet resistor with a carbon-containing material and chromium-nickel doping addresses the challenge of specifying temperature coefficients and creep behavior, enhancing sensor accuracy by minimizing intrinsic drift and extrinsic errors.
Patent Information
- Application Number
- DE102015006057
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2015-05-15
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2035-05-15
AI Technical Summary
Existing sheet resistors face challenges in simultaneously specifying the temperature coefficients of electrical resistance and intrinsic creep behavior, leading to significant creep errors and drift over time, which affect the accuracy of sensors using these resistors.
A sheet resistor with a carbon-containing resistance material embedded with electrically conductive clusters, primarily composed of a doping material mixture of chromium and another metal like nickel, is developed, allowing for precise control of intrinsic creep behavior and temperature coefficients through careful selection of the doping material ratio.
The solution achieves low intrinsic creep values, minimal drift, and compensation for extrinsic errors, ensuring high measurement accuracy and stability of sensors over time, even under varying temperatures.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[0001] The invention relates to a film resistor with a carbon-containing resistance material on a Carrier substrate, wherein electrically conductive clusters are embedded in the carbon-containing resistance material. Further Aspects of the invention relate to a method for producing such a sheet resistor and a sensor element comprising at least one such sheet resistor.
[0002] Film resistors are used, for example, as components of sensors for recording mechanical measured values such as pressure sensors or force sensors. Such sensors comprise an elastic element such as a Force sensor or a membrane, whereby the elastic element deforms under the influence of the quantity to be measured. A sensor layer is arranged on the elastic element, which is deformed together with it. Deformation of the sensor layer can be detected electrically. If the sensor layer is designed as a sheet resistor, A deformation of the sensor layer can be detected via a change in electrical resistance. For a high To ensure the accuracy of the sensors, the film resistors used must have a high linearity, high sensitivity, low hysteresis and low intrinsic errors. Furthermore, the temperature coefficient of the electrical resistance must be small. Intrinsic errors are understood in this description as errors which are due to the sheet resistance. These intrinsic errors include in particular an intrinsic Creep and intrinsic drift. Contributions to the sensor's measurement error that cannot be attributed to the sheet resistance are called extrinsic errors.
[0003] Intrinsic drift is a change in electrical resistance over time that occurs due to The intrinsic drift value of a resistor is strongly dependent on the pretreatment of the resistance and the ambient conditions. For example, the intrinsic drift value can be reduced by a temperature treatment that leads to leading to premature aging.
[0004] Creep is defined as a continuous change in the value determined by the sensor. Both the elastic elements and the sheet resistances are affected. In this case, intrinsic creep is the Creep due to sheet resistance. The creep of the elastic elements is This is called extrinsic creep. The intrinsic creep of the sheet resistance manifests itself as a continuous change of the electrical resistance with constant influence of the measured quantity such as pressure or force and constant ambient conditions, especially at constant temperature. The intrinsic Creep is generally temperature dependent, with intrinsic creep being particularly strong at higher temperatures. In the case of elastic elements, the extrinsic creep is due to an elastic aftereffect The elastic elements generally exhibit a positive creep behavior, i.e. the creep over the The electrical resistance measured by the sheet resistance arranged on the elastic element increases slowly over time To compensate for this effect at least partially, film resistors are preferably used that have a exhibit negative intrinsic creep behavior, i.e. their electrical resistance under constant influence of the Measured quantity decreases over time.
[0005] Another extrinsic source of error is, among other things, the thermal expansion of the elastic element. This acts as an apparent stretching of the elastic element and causes a measurable change in resistance a sheet resistance associated with the elastic element. Other extrinsic sources of error can For example, in the case of bonded film resistors, the adhesive used and the electrical contacts especially when using solder.
[0006] The magnitude of the change in the electrical resistance of the sheet resistor with the deformation is determined by the k- factor, where a large k-factor indicates strong change and thus high sensitivity. Conventional Film resistors such as thin-film resistors with a thin metal layer of NiCr or constantan have a k- Factor of 2.
[0007] WO 2009 / 129 930 A1 discloses a sheet resistor with a layer of carbon-containing material, into which conductive material is introduced. The conductive material, for example nickel, forms in the layer clusters separated by carbon. The temperature coefficient of electrical resistance is by the proportion of cluster material in the carbonaceous layer. The k-factor of such a Sheet resistance is typically more than 20.
[0008] The generic document DE 10 2009 044 980 A1 relates to a method for producing a Sensor component without passivation and a sensor component. This is a sensor element, In particular, it is a thin-film high-pressure sensor that deformation body and a piezoresistive sensor layer, which are applied to the deformation body. The piezoresistive sensor layer comprises at least one metal and carbon and / or hydrocarbon. The layer structure of the sensor component is terminated. Due to the materials used, a final Covering the sensor layer with a thin-film passivation layer can be omitted. Advantageously, Additional contact layers for contacting the sensor layer are not required. The contact can be made directly on the sensor layer using a bonding wire.
[0009] DE 199 54 164 A1 relates to a sensor for determining the condition of parameters on mechanical Components using amorphous carbon layers with piezoresistive properties. The sensor serves the measurement of current loads acting on a surface of a mechanical component, where the sensor an amorphous layer preferably doped with at least one metallic and / or non-metallic element Carbon layer with piezoresistive properties is used, which is connected to a measuring device via contacts Furthermore, DE 199 54 164 A1 refers to the use of preferably metallic and / or non-metallic elements doped carbon layers with piezoresistive properties as a sensor for Load measurements and a method for measuring current loads on stressed surfaces mechanical components, whereby the measuring sensor is preferably a metallic and / or non-metallic elements doped amorphous carbon layer is used.
[0010] Extrinsic errors affect the sheet resistance and are detected by it as apparent strain. The extrinsic errors are more noticeable in resistance materials with a high k-factor.
[0011] The creep value for the intrinsic creep of known sheet resistors with k-factors of more than 2 is after exposure typically at least -100 ppm (parts per million) in 30 minutes at a temperature of 85°C. The value of the intrinsic creep value is significantly higher than the value of the extrinsic creep value of the elastic elements, so that the negative creep of the sheet resistances exceeds the positive creep of conventional elastic elements overcompensated. Thus, a sensor element comprising an elastic element and a sheet resistor would exhibit a creep error, in which the quantity measured by the sensor element appears to change over time.
[0012] From the publication Grange et al., Sens. Actuators, A, 46-47, (1995) 213-217, a strain gauge known, in which a film resistor with two layers of different resistance materials is placed on a substrate made of temperature-resistant polyimide. The two resistance materials have a different pronounced creep. By carefully selecting the layer thickness ratio of the layers, the creep behavior of the Sheet resistance can be adjusted.
[0013] The disadvantage of the known film resistors is that a simultaneous targeted setting of the Temperature coefficients of electrical resistance and intrinsic creep behavior of the resistance are not is possible.
[0014] An object of the present invention can be seen in providing a sheet resistor with a To provide resistance material whose intrinsic creep behavior can be specifically specified, whereby in particular an improved compensation of the creep behavior of a sensor comprising such a A further object of the invention is to provide a To provide a film resistor with a resistance material that is subject to low aging effects and has a small drift value of the electrical resistance. Furthermore, an object of the invention can be seen in to provide a sensor with an elastic element and a sheet resistor in which extrinsic Errors of the elastic element are compensated by the sheet resistance. Disclosure of the invention
[0015] A film resistor with a carbon-containing resistance material on a carrier substrate proposed, in which electrically conductive clusters are embedded in the carbon-containing resistance material. the carbon-containing resistance material comprises a doping material, wherein the doping material is a mixture of chromium and a metal selected from cobalt, nickel, vanadium, tungsten, palladium, iron, platinum, copper, silver and gold Preferably, the doping material consists of a mixture of chromium and a metal selected from cobalt, Nickel, vanadium, tungsten, palladium, iron, platinum, copper, silver and gold.
[0016] Preferably, the proposed sheet resistor has exactly one resistance material layer on the The thickness of the carbon-containing resistance material is preferably from 10 to 500 nm, particularly preferably from 30 to 250 nm.
[0017] The carbon in the carbonaceous layer is preferably in the form of amorphous carbon (aC), hydrogen-containing amorphous carbon (aC:H) or graphite-like carbon. Amorphous carbon is also known as DLC (diamond-like carbon). The carbon in the carbonaceous layer serves as a carbon matrix in which the clusters are embedded. In the following, carbon materials with embedded clusters of the cluster material X, briefly as X:aC in the case of amorphous carbon and as X:aC:H in the case of of hydrogen-containing amorphous carbon. Furthermore, the term Carbon matrix is understood to mean both layers of aC and aC:H in which clusters are embedded.
[0018] The carbon-containing resistance material may be in the form of a carbon-containing layer with the embedded clusters can be produced, for example, using a reactive sputtering process, where carbon and the Dopant material is deposited onto the carrier substrate.
[0019] The electrically conductive clusters represent islands of cluster material in the carbon matrix, whereby the clusters comprise at least parts or components of the doping material as cluster material.
[0020] In one embodiment, the doping material is completely or almost completely absorbed into the clusters, so that no or only a small residue of the dopant material is present in the carbon matrix itself. In this In this embodiment, the cluster material and the doping material are identical.
[0021] In a further embodiment, part of the doping material is contained in the carbon matrix and a Another part of the doping material has been absorbed into the clusters. In a sub-variant, it is planned that the Clusters are essentially formed by the selected metal, so that the chromium of the dopant material is completely or partially distributed in the carbon matrix and the clusters have a correspondingly reduced proportion of chromium In another sub-variant, the ratio of chromium to the selected metal in the cluster material identical or substantially identical to the ratio in the dopant material, wherein a portion of the dopant material in the carbon matrix and the remaining part of the dopant material is in the form of embedded clusters.
[0022] The proportion of doping material in the resistance material is chosen so that it is below the percolation threshold. This means that the clusters, which are formed from at least parts of the dopant material, are each surrounded by carbon and there are no continuous paths from the dopant material or parts of the doping material in the sheet resistor or in the resistance material. The individual clusters surrounded by a shell of carbon atoms, with the carbon in the vicinity of the clusters preferably in the form of graphite-like carbon. Approximately 1 to 10 layers of graphite-like carbon form around the The clusters are also in a thermodynamically stable form, meaning that the clusters dissolve do not appear in the carbon matrix or significantly change their size or structure. The shape and size of the clusters are depending on the conditions during the deposition of the resistive material. The clusters preferably have a Size in the range of 10 to 500 nm, particularly preferably 30 to 250 nm. The size of a cluster is defined as the The largest length between two points on the smallest projection area of a cluster. The shape of the clusters can be approximately spherical, elliptical or elongated, although irregular shapes are also possible For example, the clusters can be in the form of rods, with the rods pointing in the growth direction of the resistance layer, the height of the rods is in the range of the layer thickness of the resistance layer and the largest dimension in the layer plane is in the range from 5 to 100 nm, preferably from 10 to 50 nm.
[0023] The clusters embedded in the carbon-containing resistance material preferably comprise or consist of the Doping material or parts of the doping material. The doping material preferably comprises a mixture of chromium and another selected metal or consists of a mixture of chromium and another selected metal. The metal is selected from cobalt, nickel, vanadium, tungsten, palladium, iron, platinum, copper, silver and gold. Preferably, the doping material comprises ≥ 95% by weight, particularly preferably ≥ 98% by weight and particularly preferably ≥99% by weight a mixture of chromium and the selected metal. Accordingly are preferably less than 5%, particularly preferably less than 2% and most particularly preferably less than 1% of contain impurities. 6
[0024] The doping material shows a good electrical conductivity of more than 10 A / (V · m). Resistance of the mixture of chromium and the selected metal has a temperature coefficient that depends on the temperature coefficient of the carbon matrix. The carbon matrix has, compared to the dopant material has a comparatively poor electrical conductivity, which depends strongly on the form of the carbon and in the case of aC:H also depends on the hydrogen content. If the resistance layer is deformed by force, the distance between the clusters embedded in the layer changes, which changes the electrical resistance of the material changes significantly. The strength of the change in electrical resistance with deformation is determined by the k-factor where a large k-factor indicates strong change and thus high sensitivity. The carbonaceous Resistor material with the embedded clusters has k-factors of up to about 30, while metallic Thin film resistors, for example a CrNi layer, only have a k-factor of about 2.
[0025] The intrinsic creepage value of the proposed sheet resistance can be determined by the choice of the doping material If a mixture comprising or consisting of chromium and the selected metal as doping material used, the mixing ratio of chromium to the selected metal is between 0.1:99.9 and 50:50 according to A mixing ratio of 2:98 and 20:80 by weight is preferred and particularly The mixing ratio of chromium to the selected metal is preferably in the range of 5:95 to 20:80 according to Weight selected.
[0026] The use of a chromium-containing doping material results in stabilization of the carbon-containing The stabilization is expressed, among other things, by the fact that the The layer formed from the resistive material has only a small intrinsic drift value, which is typically below 10 ppm / h at an ambient temperature of 85°C. Comparable coatings with nickel without the addition of chromium as dopant material exhibit intrinsic drift values of more than 10 ppm / h at an ambient temperature of 85°C. By means of a temperature treatment, the intrinsic drift value of the film resistors according to the invention can be further improved so that drift values of below 1 ppm / h are achieved.
[0027] Preferably, the sheet resistance at a temperature of 85°C has an intrinsic drift value in the range of 0 to 2 ppm / h and particularly preferably in the range of 0.01 to 1 ppm / h.
[0028] Preferably, the chromium of the carbon-containing resistance material is at least partially coated with the carbonaceous layer to form a carbide. It is assumed that a bond between chromium and the carbon of the carbon matrix to form a carbide, which stabilizes the clusters in the carbon matrix. The clusters have It has a chromium content that is reduced in accordance with the chromium content contained in the carbon matrix. Preferably, the doping material comprises a mixture of chromium and nickel or consists of a mixture of chromium and Nickel, whereby the mixing ratio of chromium to nickel determines the intrinsic creep behavior of the resistance layer Advantageously, even with a chromium content of about 50% by weight in the mixture, the required Nickel, the high sensitivity of the resistive layer is maintained. For a resistive layer with a carbon-containing layer embedded clusters of nickel without admixture of chromium is known from WO 2009 / 129 930 A1 a high k-factor in the range of about 20 is known. By the proposed addition of chromium, so that Doping material is a mixture of chromium and nickel, a chromium to nickel mixing ratio of about 0.01:99.99 by weight to about 50:50 by weight the high k-factor and thus the high sensitivity is maintained. If the proportion of chromium in the mixture is further increased, the k-factor approaches that of pure chromium, whereby the k-factor of a sheet resistor with only chromium as dopant is approximately 3.
[0029] The intrinsic creep value of a resistance layer with only chromium as doping material is so small that This is not detectable. For the proposed resistance layers with a mixture of chromium and nickel, The intrinsic creep value depends on the mixing ratio, whereby already at a chromium content of about 10% Weight the amount of intrinsic creepage value compared to a comparable sheet resistance without addition of Chromium is significantly reduced, while the high k-factor is advantageously retained.
[0030] The sheet resistor is designed so that the mixing ratio of chromium to the selected metal, in particular nickel, is chosen so that an intrinsic creep of the electrical resistance of the resistance layer under a mechanical load is set to a predetermined negative value. The amount of the predetermined negative value is equal to the amount of positive extrinsic creep of an elastic element, which is combined with the sheet resistor to form a sensor element.
[0031] The mixture of chromium and another selected metal is electrically conductive, the electrical resistance of the dopant material has a temperature coefficient that differs from that of the carbon matrix. Temperature coefficient of the electrical resistance of the resistance material is determined by specifying the The ratio of carbon to dopant in the resistance material can be adjusted. Resistance of the sheet resistor for temperatures in the range of about 100 K to about 700 K an approximate linear temperature dependence.
[0032] Preferably, the ratio of carbon to dopant material in the carbon-containing resistance material is Range from 20:80 to 80:20 atom %.
[0033] Preferably, the proportion of the doping material in the resistance layer or in the carbon-containing Resistance material is selected so that the temperature coefficient of the electrical resistance of the resistance material takes on a given value.
[0034] In one embodiment, the temperature coefficient of the electrical resistance of the sheet resistor or the resistance material is set to a value of 0.
[0035] In a further embodiment, the temperature coefficient of the electrical resistance of the The sheet resistance is adjusted to compensate for temperature-dependent extrinsic errors. In particular, the temperature coefficient is set so that a change in resistance due to a strain caused by a thermal expansion of an elastic element to which the sheet resistor is to be connected, compensated becomes.
[0036] Preferably, the sheet resistance is designed so that both the intrinsic creep behavior and the Temperature coefficient of electrical resistance corresponds to specified values.
[0037] Another aspect of the invention is to provide a method for producing a film resistor, wherein carbon-containing resistance material is applied to a carrier substrate and wherein the application is carried out in a reactive sputtering process with a sputtering material under a reactive atmosphere of a carbon-containing gas is carried out so that the carbon-containing gas is dissociated and a carbon-containing layer comprising Sputter material is deposited as dopant material on the carrier substrate, wherein the carrier substrate is Carrying out the reactive sputtering process is heated to a predetermined temperature at which electrically form conductive clusters comprising at least parts of the dopant material, wherein the sputtering material is a mixture of chromium and a metal selected from cobalt, nickel, vanadium, tungsten, palladium, iron, platinum, copper, silver and Gold is.
[0038] Since the method is designed to produce the described sheet resistor, the conditions of use within the scope of The characteristics described for the sheet resistance apply to the process and vice versa within the framework of The characteristics described in the process apply accordingly to the sheet resistance.
[0039] To produce the carbon-containing layer, a PVD process (physical vapor deposition, Physical vapor deposition), particularly preferably a sputtering process, in combination with a CVD (chemical vapor deposition (chemical vapor deposition). The doping material is deposited via the PVD process and the carbon is deposited via CVD. The application of the carbon-containing resistance material takes place in a vacuum chamber into which the carrier substrate is introduced. The carrier substrate is sputtered from a target, whereby atoms from the target are deposited onto the carrier substrate. Reactive RF sputtering is preferred, in which the target is connected to a high-frequency source. Depending on the design, the substrate can be grounded or subjected to a bias voltage. Furthermore, reactive DC Sputtering can be used as a sputtering process in which a direct voltage is applied between the target and the substrate. DC sputtering can also be performed in pulsed mode.
[0040] In the reactive sputtering process, a plasma forms between the carrier substrate and the target, through which Atoms of the target material are moved towards the carrier substrate. The reactive sputtering process takes place in a Protective gas atmosphere with an inert gas, e.g. with argon, with a carbon-containing reactive gas, such as Ethane, ethene or ethyne is introduced in a given concentration, so that when the plasma is formed by Dissociation carbon or hydrocarbon is formed, which is deposited on the carrier substrate together with the In this way, the sputtering material is distributed as a dopant in the carbonaceous layer is present.
[0041] The purity of the sputtering targets used is typically > 99.5%.
[0042] The substrate is kept at an elevated temperature during the reactive sputtering process so that the The formation of thermodynamically stable clusters is enabled. The elevated temperature of the carrier substrate represents a Energy input that allows the doping material to sta clusters. In this way, the sheet resistor can be manufactured in a single step. Preferably, the temperature of the carrier substrate during the reactive sputtering process is between 100°C and 600°C, especially between 150°C and 400°C.
[0043] Preferably, the application of the resistance material is followed by a tempering of the film resistor. This For example, at a temperature of about 180°C in a convection oven in air for a period of about 3 hours.
[0044] In the event that the sputtering material comprises a mixture of chromium and a metal or consists of the mixture exists, it is preferred if i) the sputtering material in the form of a target made of an alloy of the selected metal and chromium is present, or ii) the sputtering material is in the form of two targets, one for chromium and one for the selected metal and in the reactive sputtering process from both targets sputter material is deposited at the same time, or iii) the sputtering material is in the form of two targets, one for chromium and one for the selected metal and in the reactive sputtering process alternately from the first and the second target sputter material is deposited, whereby in a subsequent Temperature treatment in vacuum clusters of at least parts of the dopant material form cluster material.
[0045] In variant i), the reactive sputtering process is carried out as described above, whereby the target already has the Contains doping material as a mixture in the desired ratio.
[0046] In variant ii), two targets are placed in the vacuum chamber, one target each for chromium and one for the selected metal. The mixing ratio of chromium to the selected metal is preferably by separately setting the parameters used for sputtering for each target. For example, in the case of RF sputtering, each target is connected to its own radio frequency source, so that the The amount of material deposited from each target can be easily adjusted.
[0047] In variant iii), two targets are also introduced into the vacuum chamber, with only one Target at the same time material is deposited. This can be done both by the time period with which the respective Target material is sputtered, as well as the parameters used for sputtering for each target. The amount of deposited material can be adjusted to ensure that both doping materials combine to form a common A subsequent heat treatment is planned to enable the clusters to connect. The increased temperature the mobility of the atoms of the dopant material is increased, so that these clusters can be combined with a cluster material from a Form a mixture of chromium and the selected metal.
[0048] To form the carbon-containing layer, carbon must be introduced into the reactive sputtering process This is preferably done by adding a carbon-containing gas, which is preferably ethane, ethene or ethyne.
[0049] In the process, the ratio of carbon to dopant material is preferably determined via the concentration of the carbon-containing gas, whereby the concentration of the carbon-containing gas is preferably adjusted so that that the clusters, which comprise at least parts or components of the doping material as cluster material, in the Resistance material is separated from each other by a carbon layer.
[0050] Particularly preferably, the proportion of doping material in the resistance layer is selected such that a specified temperature coefficient of electrical resistance for the sheet resistance.
[0051] In one embodiment, the temperature coefficient of the electrical resistance is preferably set to 0 set.
[0052] In a further embodiment, the temperature coefficient of the electrical resistance is determined as a function on the properties of the carrier substrate used and / or the elastic element to which the sheet resistance is applied, adjusted so that, taking into account the influence of the carrier substrate and / or the elastic Element on the sheet resistance the electrical resistance of the sheet resistance no temperature dependence In particular, the temperature coefficient is adjusted so that this temperature-dependent extrinsic error compensated.
[0053] For example, the temperature coefficient is set so that it reduces the resistance change due to a strain caused by the thermal expansion of the carrier substrate and / or the elastic element compensated.
[0054] Preferably, the carrier substrate is selected from stainless steel, an aluminum alloy, a titanium alloy, glass, ceramic, especially Al O and ZrO , and polyimide. 2 3 2
[0055] If an electrically conductive carrier substrate is used, it is preferred if, before applying the resistance material, the carrier substrate is provided with an insulating coating. For example, Insulating layers made of SiO , Si N or Al O . The insulating coating can be applied, for example, with a 2 3 4 2 3 applied to the carrier substrate using a vapor deposition process.
[0056] Another aspect of the invention is a sensor element for measuring a force or a pressure to provide, wherein the sensor element comprises an elastic element and at least one with the elastic element associated sheet resistance as described herein.
[0057] The elastic element is preferably a force transducer, a pressure measuring cell or a strain transducer. The elastic element is designed in such a way that it deforms when a force is applied. The deformation is transferred on the connected sheet resistor, whose electrical resistance changes depending on the applied force.
[0058] The sheet resistor is designed in such a way that the carbon-containing resistance layer Doping material, wherein the doping material comprises a mixture of chromium and a metal selected from cobalt, nickel, vanadium, tungsten, palladium, iron, platinum, copper, silver and gold, or preferably from this mixture where the mixing ratio of the selected metal to chromium is chosen so that the intrinsic creep of the at least one sheet resistor at a given load, preferably within a given load range, which corresponds in magnitude to the extrinsic creep of the elastic element and the extrinsic creep of the elastic element. This balances the influences of intrinsic and extrinsic creep.
[0059] Furthermore, the sheet resistance is preferably designed such that by adjusting the ratio of Dopant to carbon the temperature coefficient of the electrical resistance of the resistance material temperature-dependent extrinsic errors are compensated. In particular, the temperature coefficient is adjusted so that a change in resistance due to a strain caused by a thermal expansion of the elastic Elements is compensated.
[0060] Particularly preferably, in the sheet resistor according to the invention, both the temperature coefficient of the electrical resistance and the intrinsic creep are adjusted so that the elastic element and the The sensor formed by the sheet resistance must compensate for extrinsic and intrinsic errors as accurately as possible, so that the Sensor does not exhibit any errors caused by creep and also shows no temperature dependence. Examples Comparison example 1:
[0061] A film resistor with Ni:aC:H as resistance material without addition of chromium was produced by a reactive sputtering process. A nickel target was used as the sputtering target and a carrier substrate was Glass. Ethylene (CH ) was used as a reactive gas and carbon source. In the reactive sputtering process 2 4 Under the reactive atmosphere of the carbon-containing gas, the carbon-containing gas is dissociated and a carbon-containing layer comprising sputter material (nickel) as doping material deposited on the carrier substrate. Nickel clusters are formed from the doping material. The manufacturing process and suitable parameters for the reactive sputtering process are described, for example, in the publication S. Ulig et al. Sensors and Actuators A 193 (2013) 129- 135 and a corresponding sheet resistance is known from WO 2009 / 129930 A1. After applying the The resistance material was annealed at a temperature of 180°C for 3 hours. Comparison example 2:
[0062] A Cr:aC:H sample was prepared by a reactive sputtering process in which the dopant material was chromium from a chromium target onto a carrier substrate. The preparation was carried out as in Comparative Example 1 described. After applying the resistor material, the film resistor was annealed. Example 1
[0063] Film resistors were tested using NiCr:aC:H as resistance material with different ratios of chromium to Nickel. The production was carried out using a reactive co-sputtering process in which a nickel target and a chromium target were used as dopant sources. The reactive gas and carbon source were Ethene (CH ) was used. The parameters used in the sputtering process are the same as those of Comparative Example 1 2 4 comparable, Depending on the desired ratio of chromium to nickel, the sputtering power of the respective targets was adjusted. In the process, a carbon-containing layer comprising sputtering material as dopant was deposited on the substrate deposited, whereby clusters are formed in the carbon-containing layer, which contain at least parts of the doping material The nickel introduced into the carbon-containing layer via the doping material is essentially used as component into the clusters, while at least part of the chromium combines with the carbon of the carbonaceous layer a carbide is formed. After applying the resistor material, the film resistor was annealed.
[0064] Glass was used as the carrier substrate. The properties of the resistance layer are not dependent on the carrier substrate. dependent, so that other carrier substrates such as stainless steel, aluminum alloys, titanium alloys, Ceramic and polyimide can be used. Example 2:
[0065] NiCr:aC:H samples were investigated which were produced by a reactive sputtering process in which the Dopant material was deposited from an alloy target containing nickel and chromium. The parameters for the used reactive sputtering process are comparable to those of Comparative Example 1. After applying the The film resistor was annealed to produce the resistance material. Short description of the characters
[0066] Shown are: Fig. 1 Measuring setup for determining the intrinsic creep value, Fig. 2 relative resistance change at constant load, Fig. 3 Creep value at constant load, Fig. 4 relative resistance change with time without load, and Fig. 5 Drift value at constant temperature without load.
[0067] In Fig. 1, a measuring arrangement for determining the intrinsic creepage value of a sheet resistor 10 The film resistor 10 comprises a carrier substrate 12 on which resistor material 14 has been deposited. To carry out measurements, the resistance material 14 of the film resistor 10 is removed by partially removing the resistance material 14 from the carrier substrate 12. The resistance material 14 is structured so that the Film resistor 10 has an active region 20 and a contact region 22. The contact region 22 comprises four electrical contacts 16, via which a four-wire measurement of the electrical resistance is carried out.
[0068] The film resistor 10 is arranged on a base 24 which has an edge 26. The edge 26 is adjoined by an area of the base 24 is formed which is curved with the radius of curvature r. The sheet resistor 10 is thus a flat area of the base 24, that a clamped area 22 rests on the base 24 and the active area 20 extends beyond the edge 26.
[0069] To measure the intrinsic creepage value of the sheet resistance 10, the clamped area 22 opposite end of the sheet resistor 10 a constant force F is applied to the sheet resistor 10, so that the sheet resistor 10 and in particular the active region 20 is deformed. Due to the deformation, a immediate change in the electrical resistance of the sheet resistor 10, which is determined via a four-wire measurement The applied force F is then kept constant and the further temporal change of the electrical resistance measured.
[0070] For the measurements of the intrinsic creep value shown below, a base 24 with a A radius of curvature r of 1000 mm was used. The measurements were taken at an ambient temperature of 85 °C. The force F used for the measurements was chosen so that the previously protruding part of the sheet resistance 10 on the curved section of the base 24. The creepage value (KW) in ppm can be determined from the temporal resistance changes after the curvature of the sheet resistance 10 via the relationship KW(t)= ΔR(t)Ri⋅106 can be obtained. Here, R is the resistance value directly after the bending by the i Action of the force F and ΔR(t) is the deviation of the resistance value from R at time t. i
[0071] Fig. 2 shows the time course of the intrinsic creep value KW(t) as a relative resistance change ΔR(t) / R i at constant load in ppm for selected sheet resistors. The intrinsic creep value was determined using the method shown in Fig. 1 described arrangement. Only the intrinsic creep of the sheet resistance was taken into account consisting of a carrier substrate and a resistance layer was measured, the sheet resistance was not connected to an elastic element.
[0072] In the diagram of Fig. 2, Comparative Examples 1 and 2 are shown as dotted lines, where for the Comparative Example 1 with nickel as doping material, the largest intrinsic creep value is achieved. Intrinsic creep for the second comparison example with chromium as dopant material is, however, so low that it is not is measurable.
[0073] The measurement results for sheet resistances according to the first example are shown as solid lines and the Measurement results for sheet resistances according to the second example are shown as dashed lines. The proportion of chromium in the mixture of chromium and nickel is indicated next to the curves.
[0074] As can be seen from the diagram in Fig. 2, the intrinsic creep slows down caused resistance change over time.
[0075] Fig. 3 shows a diagram in which the intrinsic creepage value KW(t) for different sheet resistances with varying proportion of chromium and nickel in the carbon-containing resistance material. The intrinsic Creep value KW(t) is plotted on the Y-axis and is for a period of time t of 30 minutes after application of the load. The intrinsic creep value (KW) is given in ppm after 30 min. On the X-axis, the Chromium content in the doping material applied.
[0076] The film resistors according to the invention are indicated as squares and diamonds, that Comparative Example 1 with exclusively nickel as cluster material is entered as a filled circle and the comparison example 2 with exclusively Chromium as a doping material is shown as an open circle. Figure 3 shows that comparative example 1 It can also be seen that a sheet resistor with only chromium as doping material according to Comparative Example 2 has an intrinsic creep value which does not deviate from the value 0 Film resistors according to the invention with a doping material which is a mixture of chromium and Nickel, have an intrinsic creep value that is lower than that of Comparative Example 1 and approaches the value 0 with increasing chromium content. By deliberately varying the ratio of chromium to Nickel, the intrinsic creep value of the sheet resistance can be adjusted between the values achieved by pure chromium or pure nickel as Doping material can be freely adjusted within the limits specified.
[0077] In the diagram of Fig. 3, for NiCr:ac:H, two measuring points are not shown as squares, but as diamonds These examples indicate film resistors with a chromium content of 10% and 50% by weight, The film resistors were manufactured according to Example 2. The film resistors shown as squares were obtained according to Example 1.
[0078] Fig. 4 shows the time course of the intrinsic drift value as a relative resistance change ΔR / R without O Load in ppm for selected film resistors. The drift value behaves approximately linearly with time and its The change did not diminish significantly even after a period of about 100 hours.
[0079] The intrinsic drift value DW indicates the change in electrical resistance over time at unchanged ambient conditions and is given by the relationship DW=ΔRR0⋅1h106 in ppm / h, where R 0 the electrical resistance at time t=0, ΔR is the change in electrical resistance and h is the elapsed time in hours. The measurements were conducted at a temperature of 85°C.
[0080] Fig. 5 shows a diagram in which, for selected sheet resistors, the intrinsic drift value of the electrical resistance without load.
[0081] In the diagram of Fig. 5, the Y-axis shows the intrinsic drift value in ppm / h and the X-axis the proportion of chromium in weight%. It is clearly visible that the comparison example shown as a filled circle 1, which does not contain chromium in the doping material, has the largest drift value at about 10 ppm / h. Sheet resistance therefore has only low stability and is subject to significant changes during aging. Comparative Example 2 with chromium as well as the film resistors according to the invention with a mixture of chromium and Nickel as dopant material has significantly lower intrinsic drift values, whereas chromium as dopant material has a A drift value of less than 0.1 ppm / h was determined, and for the mixture of chromium and nickel a drift value of around 1 ppm / h was determined. A small addition of chromium leads to a significant reduction of the intrinsic drift value of the inventive Sheet resistances compared to the sheet resistance without chromium according to comparative example 1.
[0082] The invention is not limited to the embodiments described here and the features presented therein. Rather, within the scope of the claims, a multitude of Modifications are possible that are within the scope of professional action.
Claims
1. A film resistor (10) comprising a carbon-containing resistance material (14) on a carrier substrate (12), wherein electrically conductive clusters are embedded in the carbon-containing resistance material (14), wherein the carbon-containing resistance material (14) comprises a doping material, wherein the doping material is a mixture of chromium and a metal selected from cobalt, nickel, vanadium, tungsten, palladium, iron, platinum, copper, silver and gold and wherein the electrically conductive clusters are formed at least from parts of the doping material, characterized characterized in that the mixing ratio of chromium to the selected metal is in the range of 0.1:99.9 to 50:50 by weight is selected such that creep of the electrical resistance of the sheet resistor (10) under a mechanical load is set to a negative value, which corresponds to an extrinsic creep value of an elastic element to which the sheet resistor (10) is connected, is equal in magnitude to and opposite to this.
2. Film resistor (10) according to claim 1, characterized in that the mixing ratio of chromium to the selected metal is between 2:98 and 20:80 by weight.
3. Film resistor (10) according to claim 1 or 2, characterized in that the chromium of the doping material is at least is partially bonded with carbon from the carbon-containing resistance material (14) to form a carbide.
4. Sheet resistor (10) according to one of claims 1 to 3, characterized in that the ratio of carbon to the doping material in the carbon-containing resistance material (14) is selected such that the temperature coefficient of the electrical resistance of the sheet resistor (10) assumes a predetermined value.
5. Sheet resistor (10) according to one of claims 1 to 4, characterized in that the ratio of carbon to the dopant material in the carbon-containing resistance material (14) is in the range of 20:80 to 80:20 atom %.
6. A method for producing a film resistor (10) according to one of claims 1 to 5, wherein carbon-containing Resistance material (14) is applied to a carrier substrate (12), wherein the application is carried out in a reactive sputtering process is carried out with a sputtering material under a reactive atmosphere of a carbon-containing gas, so that the carbon-containing gas is dissociated and a carbon-containing layer comprising the sputtering material as Doping material is deposited on the carrier substrate (12) and wherein the carrier substrate (12) during the Carrying out the reactive sputtering process is heated to a predetermined temperature at which electrically form conductive clusters comprising at least parts of the dopant material, wherein the sputtering material is a mixture of chromium and a metal selected from cobalt, nickel, vanadium, tungsten, palladium, iron, platinum, copper, silver and Gold, characterized in that the ratio of chromium to the selected metal in the doping material is is adjusted so that the ratio of chromium to the selected metal in the resistance material (14) in the Range from 0.1:99.9 to 50:50 by weight is selected in such a way that creep of the electrical resistance of the sheet resistance (10) under a mechanical load is set to a negative value, which corresponds to extrinsic creep value of an elastic element to which the sheet resistance (10) is connected, in terms of corresponds to and is opposite to it.
7. A method according to claim 6, characterized in that the ratio of chromium to the selected metal in Doping material is adjusted so that the ratio of chromium to the selected metal in the resistance material (14) is between 2:98 and 20:80 by weight.
8. Method according to claim 6 or 7, characterized in that i) the sputtering material is in the form of a target made of an alloy of the selected metal and chromium, or ii) the sputtering material is in the form of two targets, one for chromium and one for the selected metal used and in the reactive sputtering process sputter material is deposited from both targets simultaneously will, or iii) the sputtering material is in the form of two targets, one for chromium and one for the selected metal used and in the reactive sputtering process alternately from the first and the second target Sputtering material is deposited, whereby the temperature treatment during sputtering and a subsequent temperature treatment in vacuum, the electrically conductive clusters of at least parts of the Dopant material introduced sputter material.
9. Method according to one of claims 6 to 8, characterized in that the temperature of the carrier substrate (12) during the reactive sputtering process is between 100°C and 600°C, in particular between 150°C and 400°C.
10. A process according to any one of claims 6 to 9, characterized in that the carbon-containing gas is ethane, ethene or ethyne.
11. A method according to any one of claims 6 to 10, characterized in that the concentration of the carbon-containing gas determines the proportion of the dopant material in the resistance material (14), wherein the concentration of the carbon-containing gas is adjusted so that the clusters in the resistance material (14) are separated from each other by a carbon layer.
12. Method according to claim 12, characterized in that the proportion of the doping material in the resistance material (14) is chosen so that a given temperature coefficient of the electrical resistance for the resistance material (14).
13. Method according to one of claims 6 to 12, characterized in that the carrier substrate (12) is selected made of stainless steel, an aluminum alloy, a titanium alloy, glass, ceramics, in particular AlO and ZrO and polyimide. 2 3 2 14. Method according to one of claims 6 to 13, characterized in that when using an electrically conductive carrier substrate (12) before applying the resistance material (14) an insulation layer on the carrier substrate is applied.
15. Sensor element comprising an elastic element and a sensor connected to the elastic element Film resistor (10) according to one of claims 1 to 5, characterized in that the mixing ratio of the selected metal to chromium is selected such that the creep of the at least one sheet resistor (10) at a given load corresponds in magnitude to the creep of the elastic element and the creep of the elastic element is opposite.
16. Sensor element according to claim 15, characterized in that the ratio of doping material to carbon is such is selected such that the temperature coefficient of the electrical resistance of the resistance material (14) temperature-dependent extrinsic errors of the elastic element are compensated.
Citation Information
Patent Citations
Method for manufacturing a sensor component without passivation and sensor component
DE102009044980A1
Sensor for measuring actual condition parameters on surfaces of mechanical components involves using an amorphous carbon layer with piezo-resistive properties
DE19954164A1
Film resistor with a constant temperature coefficient and production of a film resistor of this type
WO2009129930A1