Rubber compound, process for its manufacture, vulcanizate thereof and use in the manufacture of vehicle tires
A sulfur-crosslinkable rubber mixture with zinc soap-based processing aids and zinc oxide/stearic acid improves abrasion, wet braking, and rolling resistance in vehicle tires, addressing the trade-offs in traditional formulations.
Patent Information
- Application Number
- DE102015216308
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2015-08-26
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2035-08-26
AI Technical Summary
Existing rubber mixtures for vehicle tires face a conflict between abrasion resistance, wet braking performance, and rolling resistance, with improvements in one property often leading to deterioration in another.
A sulfur-crosslinkable rubber mixture containing 5.5 to 15 phr of a processing aid A, which is a mixture of zinc soaps of fatty acids with up to 0.1% by weight of esters, along with 0.5 to 5 phr of zinc oxide and/or stearic acid, is used to enhance the balance between abrasion resistance, wet braking, and rolling resistance.
The rubber mixture achieves improved abrasion resistance, wet braking performance, and reduced rolling resistance, with the optimal amount of processing aid exceeding traditional levels to enhance solubility in the rubber mixture.
Abstract
Description
[0001] The invention relates to a sulphur-crosslinkable rubber mixture, in particular for treads of Vehicle tires, a vulcanizate thereof and a use for producing vehicle tires and a process for Production of the rubber mixture.
[0002] The rubber composition of the tread largely determines the driving characteristics of a tire, especially a vehicle tire. Likewise, the rubber compounds used in belts, hoses and straps Used especially in areas subject to high mechanical stress, for stability and longevity of these Rubber products are essentially responsible for these rubber compounds. Therefore, these rubber compounds are used for vehicle tires, belts, Belts and hoses are subject to very high demands.
[0003] To influence the mixture and vulcanizate properties, the mixtures are given a wide variety of Aggregates are added and / or special polymers are used. Examples of aggregates include at this point fillers (e.g. carbon black), plasticizers, anti-aging agents and cross-linking systems made of sulfur, Accelerators and activators are called additives. If a property is improved by varying the mixture, this is often with a deterioration of another property, so that certain conflicting objectives exist. In the case of mixtures for In the case of vehicle tyre treads, such conflicting objectives exist, for example, with regard to abrasion behaviour and increased heat build-up, which results in poorer rebound elasticity and consequently poorer rolling resistance.
[0004] Processing aids such as metal soaps of fatty acids are known as additives to increase the viscosity of the rubber mixture and to increase the dispersion of the fillers contained therein, especially silica, and thus improving their miscibility. Typical amounts of such processing aids are 1 to 3 phr. US 2003 / 0111770 A1 3 phr of a process aid. Also in DE 102011076490 A1 and DE 102004005132 A1 3 phr processing aids, such as a mixture of zinc soaps, are used to improve miscibility, disclosed, in particular the dispersion of silicon dioxide with a high surface area is to be improved.
[0005] EP 2033813 B1 discloses a tread of a vehicle tire, the rubber composition of which 1 to 10 phr of a product of zinc oxide and resin acid. Such a rubber mixture shows improved Wet grip properties, although this has a detrimental effect on the rebound elasticity at 100 °C as a possible Rolling resistance indicator.
[0006] The influence on the abrasion behavior is not investigated in EP 2033813 B1.
[0007] JP S60-31541 A discloses compositions containing fatty acid metal salts and esters of polyvalent Alcohols with unsaturated fatty acids.
[0008] DE 199 51 977 A1 relates to a process for producing a finely divided rubber powder and discloses In addition, rubber mixtures containing a fatty acid, zinc oxide and zinc soaps of unsaturated fatty acids.
[0009] The present invention is based on the object of providing a sulfur-crosslinkable rubber mixture, especially for treads of vehicle tires, whose vulcanizate is an improvement over the State of the art with regard to the conflict of objectives between abrasion resistance, wet braking indicators and the has rolling resistance indicators.
[0010] This object is achieved by a sulfur-crosslinkable rubber mixture containing: - at least one diene rubber and - 5.5 to 15 phr of one or more processing aids A, wherein the processing aid A is a mixture of zinc soaps of fatty acids and wherein the processing aid A contains 0 to 0.1 wt.% ester, - and wherein the sulfur-curable rubber mixture additionally contains 0.5 to 5 phr zinc oxide and / or 0.5 to 5 phr Contains stearic acid.
[0011] Surprisingly, it was found that with a comparatively high amount of the processing aid, the above the solubility in the rubber mixture, in a rubber mixture according to the invention produced vulcanizate according to the invention an improvement with regard to the conflict of objectives between abrasion resistance, wet braking indicators and rolling resistance indicators.
[0012] A further object of the present invention is a use of the rubber mixture according to the invention for Production of vehicle tyres, which preferably in one component, in particular at least in the tread, at least a vulcanizate of at least one sulfur-crosslinkable rubber mixture having the above-mentioned features. Vehicle tires containing the rubber mixture according to the invention at least in the tread have a Improvement in the conflict of objectives between abrasion, wet braking and rolling resistance, and in particular an increased Abrasion resistance.
[0013] In the context of the present invention, vehicle tires are understood to mean pneumatic vehicle tires and solid rubber tires, including tires for industrial and construction vehicles, truck, car and two-wheel tires.
[0014] The rubber mixture according to the invention is also suitable for other components of vehicle tires, such as especially sidewall, tread pattern and internal tire components.
[0015] The rubber mixture according to the invention is also suitable for other technical rubber articles, such as bellows, Conveyor belts, air springs, belts, straps or hoses, as well as shoe soles, whereby due to the requirement profile is particularly suitable for conveyor belts.
[0016] In the following, the components of the sulfur-crosslinkable rubber mixture according to the invention are described in more detail All statements also apply to the uses according to the invention for the production of Vehicle tires or the vulcanizate according to the invention.
[0017] The term phr (parts per hundred parts of rubber by weight) used in this document is the term used in the The dosage of the parts by weight of the individual In this document, substances are calculated as 100 parts by weight of the total mass of all substances present in the mixture. high molecular weight (weight average molecular weight Mw according to GPC from 250000 to 5000000 g / mol) and thus made of solid rubber.
[0018] The rubber mixture according to the invention contains at least one diene rubber. Rubbers produced by polymerization or copolymerization of dienes and / or cycloalkenes and thus have C=C double bonds either in the main chain or in the side groups. In the diene rubber may be natural polyisoprene and / or synthetic polyisoprene and / or epoxidized polyisoprene and / or Styrene-butadiene rubber (SBR) and / or butadiene rubber (BR, polybutadiene) and / or styrene-isoprene rubber and / or halobutyl rubber and / or polynorbornene and / or isoprene-isobutylene copolymer and / or ethylene-propylene-diene- Rubber and / or nitrile rubber and / or chloroprene rubber and / or acrylate rubber and / or fluororubber and / or silicone rubber and / or polysulfide rubber and / or epichlorohydrin rubber and / or styrene-isoprene Butadiene terpolymer and / or hydrogenated acrylonitrile butadiene rubber and / or hydrogenated styrene butadiene rubber and / or butadiene-isoprene rubber.
[0019] In particular, nitrile rubber, hydrogenated acrylonitrile butadiene rubber, chloroprene rubber, butyl rubber, Halobutyl rubber or ethylene-propylene-diene rubber are used in the production of technical rubber articles, such as belts, straps and hoses, and / or shoe soles.
[0020] Preferably, the diene rubber is selected from the group consisting of natural polyisoprene, synthetic Polyisoprene, styrene-butadiene rubber and butadiene rubber.
[0021] The natural and / or synthetic polyisoprene of all embodiments can be either cis- 1,4-polyisoprene as well as 3,4-polyisoprene. However, the use of cis-1,4-polyisoprene with a cis 1,4 content > 90 wt.%. On the one hand, such a polyisoprene can be prepared by stereospecific polymerization in solution with Ziegler-Natta catalysts or using finely divided lithium alkyls. Natural rubber (NR) is such a cis-1,4 polyisoprene, the cis-1,4 content in natural rubber is larger 99% by weight. Furthermore, a mixture of one or more natural polyisoprenes with one or more synthetic Polyisoprene(s) are conceivable.
[0022] The butadiene rubber (= BR, polybutadiene) can be any type known to the person skilled in the art. These include the so-called high-cis and low-cis types, whereby polybutadiene with a cis content greater than or equal to 90 wt.% as high-cis type and polybutadiene with a cis content of less than than 90 wt.% is referred to as low-cis type. A low-cis polybutadiene is, for example, Li-BR (lithium-catalyzed butadiene- rubber) with a cis content of 20 to 50 wt.%. With a high-cis BR, particularly good abrasion properties are achieved. and a low hysteresis of the rubber compound is achieved. The polybutadiene(s) used can be modified and functionalized end-group modified and / or functionalized along the polymer chains. The modification can be those with hydroxy groups and / or ethoxy groups and / or epoxy groups and / or siloxane groups and / or amino- Groups and / or aminosiloxane and / or carboxy groups and / or phthalocyanine groups and / or silane sulfide groups However, there are also other modifications known to the expert, also known as functionalizations Metal atoms can be a component of such functionalizations.
[0023] In the event that styrene-butadiene rubber (styrene-butadiene copolymer) is contained in the rubber mixture, It can be either solution-polymerized styrene-butadiene rubber (SSBR) or emulsion-polymerized Styrene-butadiene rubber (ESBR), although a mixture of at least one SSBR and at least one ESBR can be used. The terms ´´styrene-butadiene rubber´´ and ´´styrene-butadiene copolymer´´ are used in used synonymously in the context of the present invention. The styrene-butadiene copolymer used can be modified with the polybutadiene modifications mentioned above and Functionalizations can be end-group modified and / or functionalized along the polymer chains.
[0024] The rubber mixture according to the invention particularly preferably contains at least one styrene-butadiene rubber and / or polybutadiene, very particularly preferably at least one styrene-butadiene rubber, particularly preferably in amounts of 50 to 95 phr. Preferably, the styrene-butadiene rubber is a solution-polymerized styrene-butadiene Rubber (SSBR). Especially SSBR has a wide variety of commercially available types with different glass transition temperatures, which allow a targeted adjustment of the glass transition temperature of the rubber compound. Preferably, the SSBR is also functionalized or modified as described above. It particularly preferably has functional groups for interaction with silica as a filler. Such functional Groups are, for example and in particular, hydroxy groups and / or ethoxy groups and / or epoxy groups and / or siloxane groups and / or aminosiloxane and / or carboxy groups.
[0025] According to the invention, the rubber mixture contains 5.5 to 15 phr of one or more processing aids A, wherein the Processing aid A is a mixture of zinc soaps of fatty acids and wherein the processing aid A contains 0 to 0.1 wt.% ester contains.
[0026] The fatty acids are preferably stearic acid, palmitic acid and / or oleic acid. In addition may also include saponification products of capron, caprylic, capric, lauric, myristic, arachin, elaidin, vaccene, gadolein, It may contain icosenoic, cetoleic, erucic, linoleic and linolenic acid.
[0027] The (at least one) processing aid A contained according to the invention has such a long Hydrocarbon chains, preferably with at least 8 carbon atoms, particularly preferably with at least 10 carbon atoms, so that it is able to form micelles.
[0028] The processing aid A preferably has a zinc content of 5 to 10 wt.%, particularly preferably 7 to 10 wt.%. %. With a processing aid A with a zinc content of 5 to 10 wt.%, a significantly better abrasion resistance than with a processing aid with a zinc content of less than 0.1 wt.%.
[0029] A suitable processing aid A is available, for example, under the trade name Struktol EF44 from Schill & Available from Seilacher.
[0030] The processing aid A preferably has a melting point according to Differential Scanning Calorimetry (DSC) of 85 to 100 °C. This ensures that the process aid A is completely melted and distributed in the rubber mixture.
[0031] According to the invention, zinc oxide and stearic acid as such do not belong to the processing aid A. The The rubber mixture according to the invention additionally contains 0.5 to 5 phr of zinc oxide and / or 0.5 to 5 phr of stearic acid. The rubber mixture particularly preferably additionally contains 0.5 to 4 phr of zinc oxide and / or 0.5 to 3 phr of stearic acid.
[0032] The rubber mixture according to the invention contains 5.5 to 15 phr of the processing aid A, particularly preferably 5.5 to 12 phr, especially preferably 5.5 to 10 phr. Surprisingly, the improvement mentioned in the conflicting objectives from abrasion, rolling resistance and wet grip by using amounts of processing aid A where the solubility in the rubber mixture is exceeded.
[0033] By increasing the amount above the usual level of up to 3 phr, a rubber mixture can thus be surprising advantage can be achieved. The optimal amount of a particular process aid A is then determined by the respective solubility limit and can then be determined by successively increasing and, for example, observing the dynamic modulus G' (1% elongation, 70 °C) of the unvulcanized rubber compound can be determined as a measure of the viscosity. Above the Solubility limit, no further influence of increasing amounts of processing aid on the viscosity can be observed.
[0034] An excessive amount of processing aid of more than 15 phr is not advantageous, since the rubber mixture the rotors of the mixing unit and can no longer be mixed properly. This reduces the quality of the Mixture and is undesirable.
[0035] The processing aid A is used in the production of the sulfur-crosslinkable rubber mixture according to the invention added in a basic mixing stage. Thus, a further subject of the present invention is a process for Production of a rubber mixture containing the above-mentioned components including all embodiments and additional components.
[0036] Preferably, there is only one process aid A, which means that for the process according to the invention a simple dosing. Processing aid A is present as a mixture, as described above.
[0037] The invention further relates to a use of the rubber mixture according to the invention for Production of vehicle tires which in at least one component contains at least one vulcanizate of at least one sulfur-crosslinkable rubber mixture which was produced by the process according to the invention. Preferably, the component is at least the tread. For treads with a cap / base construction Preferably it is at least the cap.
[0038] The rubber mixture according to the invention further preferably contains at least one filler such as in particular Silica and / or carbon black.
[0039] The terms ´´silicic acid´´ and ´´silica´´ are used in the context of the present invention, as well as in the professional world common, used synonymously.
[0040] According to a particularly preferred embodiment of the invention, the rubber mixture contains 50 to 250 phr, preferably 95 to 250 phr, particularly preferably 105 to 250 phr, very particularly preferably 105 to 180 phr, at least a silica.
[0041] With the combination of components according to the invention, comparatively high amounts of silica, particularly preferably 105 to 250 phr, most preferably 105 to 180 phr, which has a beneficial effect on the conflicting objectives of wet grip vs. rolling resistance of the rubber compound.
[0042] The silicas can be those known to the person skilled in the art and used as fillers for Tire rubber compounds are suitable. However, it is particularly preferred if a finely divided, precipitated Silica is used which has a nitrogen surface area (BET surface area) (according to DIN ISO 9277 and DIN 66132) of 35 2 2 2 to 400 m / g, preferably from 60 to 350 m / g, particularly preferably from 120 to 320 m / g, and a CTAB surface 2 2 2 (according to ASTM D 3765) from 30 to 380 m / g, preferably from 50 to 330 m / g, particularly preferably from 110 to 300 m / g, has.
[0043] According to a preferred development of the invention, the rubber mixture contains 1 to 20 phr, preferably 1 to 10 phr, particularly preferably 1 to 7 phr of at least one carbon black. In the context of the present invention, all Carbon black types known to those skilled in the art are conceivable. However, preference is given to using a carbon black which has an iodine adsorption number according to ASTM D 1510 from 20 to 180 g / kg, particularly preferably 30 to 140 kg / g, and a DBP number according to ASTM D 2414 from 30 to 200 ml / 100 g, preferably 90 to 180 ml / 100 g, particularly preferably 90 to 150 ml / 100 g. A particularly suitable Carbon black in the context of the present invention is, for example, a carbon black of ASTM type N339 with an iodine adsorption number of 90 g / kg and a DBP value of 120 ml / 100g. This is for use in vehicle tires, especially in the tread. particularly good properties were achieved with regard to the technical task.
[0044] The rubber mixture according to the invention can contain, preferably as small amounts as possible, ie preferably 0 to 2 phr, contain other fillers. Other (non-reinforcing) fillers in the context of this Invention alumosilicates, kaolin, chalk, starch, magnesium oxide, titanium dioxide or rubber gels as well as fibers (such as Example: aramid fibers, glass fibers, carbon fibers, cellulose fibers).
[0045] Other reinforcing fillers are, for example, carbon nanotubes (CNT) including discrete CNTs, so-called hollow carbon fibers (HCF) and modified CNTs containing one or more functional groups, such as Hydroxy, carboxy and carbonyl groups), graphite and graphene and so-called ´´carbon-silica dual-phase filler´´.
[0046] Zinc oxide is not one of the fillers in the context of the present invention.
[0047] To improve the processability and to bind the silica and other polar Silane coupling agents can be used in rubber compounds by adding fillers to the diene rubber. One or more different silane coupling agents can be used in combination. Rubber compounds can therefore contain a mixture of different silanes. The silane coupling agents react with the surface silanol groups of the silica or other polar groups during mixing of the rubber or the rubber mixture (in situ) or even before the addition of the filler to the rubber in the sense of a Pretreatment (premodification). Silane coupling agents can be any known to the person skilled in the art for use in Silane coupling agents known from rubber compounds can be used. Such prior art known coupling agents are bifunctional organosilanes, which have at least one alkoxy, cycloalkoxy group on the silicon atom. or phenoxy group as a leaving group and which have as other functionality a group which may, after cleavage, enter into a chemical reaction with the double bonds of the polymer. The latter group can include, for example, the following chemical groups: -SCN, -SH, -NH or -S - (with x = 2 to 8). 2 x
[0048] Thus, as silane coupling agents, for example, 3-mercaptopropyltriethoxysilane, 3-thiocyanatopropyltrimethoxysilane or 3,3'-bis(triethoxysilylpropyl)polysulfides with 2 to 8 sulfur atoms, such as 3,3'-bis(triethoxysilylpropyl)tetrasulfide (TESPT), the corresponding disulfide (TESPD) or mixtures of the sulfides with 1 to 8 sulfur atoms with different contents of the various sulphides. TESPT can also be used as Mixture with industrial carbon black (trade name X50S® from Evonik) can be added. Preferably, a silane mixture is used which contains 40 to 100 wt.% disulfides, particularly preferably 55 to 85 wt.% % disulfides and most preferably 60 to 80 wt.% disulfides. Such a mixture is known, for example, from Trade name Si 261® from Evonik, which is described in DE 102006004062 A1. Blocked mercaptosilanes, such as those known from WO 99 / 09036, can be used as silane coupling agents Silanes, such as those described in WO 2008 / 083241 A1, WO 2008 / 083242 A1, WO 2008 / 083243 A1 and WO 2008 / 083244 A1 can be used. For example, silanes sold under the name NXT (e.g. 3-(Octanoylthio)-1-Propyl-Triethoxysilane) in various variants from Momentive, USA, or those under marketed under the name VP Si 363® by Evonik Industries.
[0049] Furthermore, it is conceivable that one of the above-mentioned mercaptosilanes, in particular 3-mercaptopropyltriethoxysilane, in combination with processing aids (listed below), especially PEG carboxylic acid esters become.
[0050] According to a preferred embodiment of the invention, the rubber mixture contains a combination of 3- Mercaptopropyltriethoxysilane and PEG carboxylic acid esters, which result in particularly good properties, namely particularly with regard to the technical task to be solved and overall a good level of properties with regard to the other properties.
[0051] Furthermore, the rubber mixture may contain further activators and / or agents for the binding of fillers, especially carbon black. This can be, for example, the compound S- disclosed in EP 2589619 A1. (3-Aminopropyl)thiosulfuric acid and / or its metal salts which, especially when combined with at least one carbon black as a filler, results in very good physical Properties of the rubber compound.
[0052] The silanes and activators mentioned are preferably used in the production of the rubber mixture in at least added to a basic mixing stage.
[0053] According to a preferred embodiment, the rubber mixture according to the invention contains at least one Plasticizer, wherein the total amount of plasticizer is preferably 1 to 50 phr, particularly preferably 10 to 50 phr, This results in a particularly good Processability of the rubber compound, especially of the extrudates before crosslinking, with good Rolling resistance indicators and good (and therefore low) heat build-up.
[0054] The plasticizers used in the present invention include all those known to the person skilled in the art Plasticizers such as aromatic, naphthenic or paraffinic mineral oil plasticizers, such as MES (mild extraction solvate) or RAE (Residual Aromatic Extract) or TDAE (treated distillate aromatic extract), or rubberto-liquid oils (RTL) or biomass-to-liquid oils (BTL), preferably with a polycyclic aromatics content of less than 3 wt.% according to method IP 346 or rapeseed oil or factisse or plasticising resins or liquid polymers, the average Molecular weight (determination by GPC = gel permeation chromatography, based on BS ISO 11344:2004) between 500 and 20000 g / mol. If additional liquid polymers are used in the rubber mixture according to the invention as If plasticizers are used, they are not considered as rubber in the calculation of the composition of the polymer matrix a.
[0055] The plasticizer resins may in particular and preferably be unmodified phenolic resins.
[0056] The plasticizer is preferably selected from the group consisting of the above-mentioned plasticizers.
[0057] Mineral oils are particularly preferred as plasticizers.
[0058] When using mineral oil, this is preferably selected from the group consisting of DAE (Distilled Aromatic Extracts) and / or RAE (Residual Aromatic Extract) and / or TDAE (Treated Distilled Aromatic Extracts) and / or MES (Mild Extracted Solvents) and / or naphthenic oils.
[0059] According to a preferred embodiment of the invention, the rubber mixture contains at least one Mineral oil plasticizers, preferably at least TDAE and / or RAE as plasticizers. This results in particularly good Processability, especially good miscibility of the rubber compound.
[0060] The plasticizer(s) are preferably used in the production of the rubber mixture according to the invention in added to at least one basic mixing stage.
[0061] Furthermore, the rubber mixture may contain conventional additives in conventional parts by weight, which Production preferably in at least one basic mixing stage. These additives include a) Anti-aging agents such as N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (6PPD), N,N'-diphenyl- p-phenylenediamine (DPPD), N,N'-ditolyl-p-phenylenediamine (DTPD), N-isopropyl-N'-phenyl-p-phenylenediamine (IPPD), 2,2,4-trimethyl-1,2-dihydroquinoline (TMQ), b) other activators, such as zinc complexes such as zinc ethylhexanoate, which contain short carbon chains of up to to 7 carbon atoms and are therefore not or only slightly able to form micelles, c) waxes, d) Mastication aids, such as 2,2'-dibenzamidodiphenyl disulfide (DBD).
[0062] The proportion of the total amount of further additives is 3 to 150 phr, preferably 3 to 100 phr and particularly preferably 5 to 80 phr.
[0063] In the total amount of other additives, zinc oxide (ZnO) can be added as described above in the above mentioned quantities.
[0064] This can be any type of zinc oxide known to the person skilled in the art, such as ZnO granules or - 2 Powder. The zinc oxide commonly used typically has a BET surface area of less than 10 m / g. 2 However, it can also be a zinc oxide with a BET surface area of 10 to 100 m / g, such as so-called ´´nano-zinc oxides´´, be used.
[0065] The vulcanization of the sulfur-crosslinkable rubber mixture according to the invention is carried out in the presence of Sulphur and / or sulphur donors with the help of vulcanization accelerators, whereby some Vulcanization accelerators can also act as sulfur donors. The accelerator is selected from the Group consisting of thiazole accelerators and / or mercapto accelerators and / or sulfenamide accelerators and / or thiocarbamate accelerators and / or thiuram accelerators and / or thiophosphate accelerators and / or Thiourea accelerators and / or xanthate accelerators and / or guanidine accelerators. Preference is given to using a sulfenamide accelerator selected from the group consisting of N- Cyclohexyl-2-benzothiazolesufenamide (CBS) and / or N,N-Dicyclohexylbenzothiazole-2-sulfenamide (DCBS) and / or Benzothiazyl-2-sulfenemorpholide (MBS) and / or N-tert-butyl-2-benzothiazylsulfenamide (TBBS).
[0066] As sulphur-donating substance, all sulphur-donating substances known to the person skilled in the art If the rubber mixture contains a sulfur-donating substance, this is preferably selected from the group containing e.g. thiuram disulfides, such as tetrabenzylthiuram disulfide (TBzTD) and / or Tetramethylthiuram disulfide (TMTD) and / or tetraethylthiuram disulfide (TETD), and / or thiuram tetrasulfides, such as Dipentamethylenethiuram tetrasulfide (DPTT), and / or dithiophosphates, such as DipDis (bis-(diisopropyl)thiophosphoryl disulfide) and / or bis(O,O-2-ethylhexyl-thiophosphoryl)polysulfide (e.g. Rhenocure SDT 50®, Rheinchemie GmbH) and / or zinc dichloryldithiophosphate (e.g. Rhenocure ZDT / S®, Rheinchemie GmbH) and / or zinc alkyl dithiophosphate, and / or 1,6-bis(N,N-dibenzylthiocarbamoyldithio)hexane and / or diaryl polysulfides and / or Dialkyl polysulfides.
[0067] Other network-forming systems, such as those sold under the trade names Vulkuren®, Duralink® or Perkalink®, or network-forming systems as described in WO 2010 / 049216 A2, can be used in the rubber compound. This system contains a vulcanizing agent which is Functionality greater than four and at least one vulcanization accelerator. The vulcanizing agent, which is a functionality of greater than four has, for example, the general formula A): G[CH -CH -SY] A) where G is a a 2a 2 bc polyvalent cyclic hydrocarbon group and / or a polyvalent heterohydrocarbon group and / or a polyvalent siloxane group containing 1 to 100 atoms; wherein each Y is independently selected from a rubber-active group, sulfur-containing functionalities; and where a, b and c are integers for which Independently: a equals 0 to 6; b equals 0 to 8; and c equals 3 to 5.
[0068] The rubber-active group is preferably selected from a thiosulfonate group, a dithiocarbamate group, a thiocarbonyl group, a mercapto group, a hydrocarbon group and a sodium thiosulfonate group (Bunte salt group). This results in very good abrasion and tear properties of the rubber mixture according to the invention achieved.
[0069] In the context of the present invention, sulfur and sulfur donors, including sulfur-donating silanes such as TESPT, and vulcanization accelerators as described above and vulcanizing agents with a functionality greater than four, as described in WO 2010 / 049216 A2, such as a vulcanizing agent of formula A), and The above-mentioned systems Vulkuren®, Duralink® and Perkalink® are conceptually summarized as vulcanizing agents.
[0070] The rubber mixture according to the invention is preferably prepared by adding at least one Vulcanizing agent selected from the group containing, particularly preferably consisting of, sulfur and / or Sulphur donors and / or vulcanization accelerators and / or vulcanizing agents with a functionality greater four crosslinking agents are added in the final mixing stage. This allows the mixed ready-mixed mixture by vulcanization a sulfur-crosslinked rubber mixture, especially for Application in vehicle tires.
[0071] The use of the accelerators TBBS and / or CBS and / or diphenylguanidine (DPG) is particularly preferred.
[0072] In addition, vulcanization retarders may be present in the rubber mixture.
[0073] The terms ´´vulcanized´´ and ´´crosslinked´´ are used synonymously in the context of the present invention.
[0074] According to a preferred embodiment of the invention, in the production of the sulfur-crosslinkable Several accelerators are added to the rubber mixture in the final mixing stage. The sulfur-crosslinkable rubber mixture according to the invention is produced according to the The process used in the rubber industry involves first mixing a base mixture with all the components other than the vulcanization system (sulfur and vulcanization-influencing substances). The final mix is created by adding the vulcanization system in a final mixing stage. is further processed, for example, by an extrusion process or calendering and brought into the appropriate shape. The subsequent processing is carried out by vulcanisation, whereby due to the scope of the present Invention added vulcanization system, sulfur crosslinking takes place.
[0075] The above-described rubber mixture according to the invention or the vulcanizate thereof is particularly suitable for Suitable for use in the manufacture of vehicle tires, especially pneumatic vehicle tires. all tire components are conceivable in principle, especially in a tread, especially in the cap of a tread with cap / base construction.
[0076] The cap is the part of the tread of the vehicle tire that comes into contact with the road surface, while the base is the radially underlying inner part of the tread that is not in contact with the road surface comes.
[0077] For use in vehicle tires, the mixture is preferably prepared as a ready-mix before vulcanization in the form a tread and applied as known during the production of the green vehicle tire.
[0078] The preparation of the rubber mixture according to the invention for use as a body mixture in vehicle tires is carried out as already described. The difference lies in the shaping after the extrusion process or the Calendering the mixture. The resulting shapes of the unvulcanized rubber mixture for one or more Different body mixtures are then used to construct a tire blank. The body compound refers to the rubber mixtures for the other outer and inner components of a tire referred to as essentially squeegee, sidewall, inner core (inner layer), core profile, belt, shoulder, belt profile, Carcass, bead reinforcement, bead profile, horn profile and bandage.
[0079] For use of the rubber mixture according to the invention in belts and straps, in particular in conveyor belts, The extruded, still unvulcanized mixture is brought into the appropriate shape and during or after this, often with Reinforcements such as synthetic fibers or steel cords are used. This usually results in a multi-layer structure, consisting of one and / or more layers of rubber mixture, one and / or more layers of the same and / or various reinforcements and one and / or more further layers of the same and / or another Rubber compound.
[0080] The invention will now be explained by means of comparative and exemplary embodiments, which are summarized in Table 1 are explained in more detail.
[0081] The comparison mixtures are marked with V, the mixtures according to the invention are marked with E.
[0082] The mixture was prepared according to the usual procedure in the rubber industry under usual Conditions in three stages in a laboratory mixer in which initially in the first mixing stage (basic mixing stage) all Components other than the vulcanization system (sulfur and vulcanization-influencing substances). In the second mixing stage, the basic mixture was mixed again. By adding of the vulcanization system in the third stage (finished mix stage), the finished mix was produced, at 90 to 120 ° C was mixed.
[0083] Test specimens were prepared from all mixtures by vulcanization after 20 minutes under pressure at 160°C manufactured and with these test specimens, material properties typical for the rubber industry were determined with the following specified test procedures. • Shore A hardness at room temperature (RT) according to DIN ISO 7619-1 • Rebound resilience at room temperature and 70°C according to ISO 4662 or ASTM D 1054 • Mooney viscosity ML 1+4 at 100 °C (Mooney units ME) ASTM D1646 • Dynamic modulus G' of the unvulcanized compound as viscosity at 70 °C and 1% elongation according to ASTM D5289, D6204, D6601, D7605 with an RPA2000 • Dynamic modulus G' of the vulcanized compound as a dispersion indicator at 70 °C and 1% elongation according to ASTM D5289, D6204, D6601, D7605 with an RPA2000
[0084] Furthermore, tire tests were carried out in the comparative examples V1 to V5 and in the Inventive Example E1 with the mixture as a tread cap. The following test methods were used: • Wet braking: ABS braking, braking distance from 80 km / h, wet asphalt, low µ (low µ) • Dry braking: ABS braking, braking distance from 100 km / h, dry asphalt, high µ (high µ) • Rolling resistance: according to ISO 28580 • Wear: Weight loss of the respective tires after 15000 km of road driving at an average temperature of + 15 °C.
[0085] The determined values were converted into performance, whereby the comparison mixture V1 was used for each tested property was standardized to 100% performance. All other compound performances refer to this Comparison mixture V1. Values < 100% mean a deterioration in the properties, while values > 100% represents an improvement. Table 1 Components Unit V1 V2 V3 V4 V5 E1 NR TSR phr 20 20 20 20 20 20 a) phr 80 80 80 80 80 80 SBR Carbon black N339 phr 5 5 5 5 5 5 b) phr 115 115 115 115 115 115 Silica c) phr 39 39 39 39 39 39 oil ZnO phr 3 3 3 3 3 3 Stearic acid phr 2 2 2 2 2 2 d) phr - 3 3 - - 6 Process aids e) phr - - 3 - - - Process aids f) phr - - - 6 - - Process aids G) phr - - - - 6 - Process aids h) phr 12 12 12 12 12 12 Silane i) phr 8 8 8 8 8 8 Ageing protection j) phr 5.3 5.3 5.3 5.3 5.3 5.3 accelerator Sulfur phr 1 1 1 1 1 1 Physical properties Mooney ME 80 68 67 69 67 65 G' unvulk. kPa 649 501 478 466 470 474 G' vulk. MPa 2.53 2.23 1.78 1.66 1.55 1.64 Shore hardness A Shore A 68 65 65 64 63 64 Rebound RT % 18 19 19 21 20 20 Rebound 70°C % 45 48 52 51 53 53 Tire results Wet braking % 100 100 101 100 101 Dry braking % 100 100 100 100 100 Rolling resistance % 96 100 101 100 101 Abrasion % - 100 95 96 105
[0086] Substances used: a) SBR: SSBR, SLR 4602, Trinseo b) Silica VN3, Evonik c) TDAE d) Processing aid: Struktol EF44, Schill & Seilacher; melting point 95 °C, zinc content 8.3 wt.%, mixture from zinc soaps of fatty acids e) Processing aid: Ultraflow 700 S, Performance Additives; melting point 103°C, zinc content 8.5 wt.%, Mixture of zinc soaps of unsaturated fatty acids and their esters f) Processing aid: HT254, Schill & Seilacher; melting point 75 °C, zinc content < 0.1 wt.%, mixture of N- (2-hydroxyethyl)-hexadecanamide and N-(2-hydroxyethyl)-octanamide G) Processing aid: Ultralube 160, Performance Additives; melting point 102°C, zinc content <0.1 wt.%, Mixture of calcium soaps of fatty acids and their amides h) Silan NXT, Momentive i) Anti-aging agents: 6PPD, DTPD, ozone protection wax j) Vulcanization accelerators: CBS, TBBS, TBzTD, MBT (2-mercaptobenzothiazole) and DPG
[0087] As can be seen from Table 1, the rubber mixture E1 according to the invention containing 6 phr of a Mixture of zinc soaps of fatty acids as processing aids surprisingly compared to rubber mixtures from the state of the art V2 to V5 in the tire test an improvement in the conflict of objectives between rolling resistance, wet braking and abrasion, with the abrasion behavior in particular being significantly improved. Compared to a mixture with a Amount of 3 phr from the state of the art of process aid A is mixed with E1 with a quantity of 6 phr of a A mixture of zinc soaps and fatty acids as a processing aid, in particular, improved rolling resistance is achieved. Compared to 6 phr calcium soaps as processing aid (V5) or 6 phr of a processing aid which has only low amounts or no zinc (< 0.1 wt.% zinc) (V4), E1 is particularly suitable for improved abrasion behaviour (less abrasion) is achieved.
Claims
1. Sulphur-curable rubber mixture containing - at least one diene rubber and - 5.5 to 15 phr of one or more processing aids A, wherein the processing aid A is a mixture of zinc soaps of fatty acids and wherein the processing aid A contains 0 to 0.1 wt.% ester, - and wherein the sulfur-curable rubber mixture additionally contains 0.5 to 5 phr zinc oxide and / or 0.5 to 5 phr Contains stearic acid.
2. Rubber mixture according to claim 1, characterized in that the fatty acids are stearic acid, Palmitic acid and / or oleic acid.
3. Rubber mixture according to claim 2, characterized in that the processing aid A has a zinc content of 5 to 10 wt.%.
4. Rubber mixture according to one of the preceding claims, characterized in that it contains 50 to 250 phr of at least contains a silica.
5. Rubber mixture according to claim 4, characterized in that it contains 105 to 250 phr of silica.
6. Rubber mixture according to one of the preceding claims, characterized in that it contains 50 to 95 phr of at least a styrene-butadiene rubber and / or polybutadiene.
7. A process for producing a rubber mixture according to one of claims 1 to 6, characterized in that one or more process aids A are added in a basic mixing stage.
8. Method according to claim 7, characterized in that there is only one process aid A.
9. Vulcanizate obtained by sulfur vulcanization of the rubber mixture according to one of claims 1 to 6.
10. Use of the sulfur-crosslinkable rubber mixture according to at least one of claims 1 to 6 for Manufacture of vehicle tires.
11. Use of the vulcanizate according to claim 9 for the production of vehicle tires.
Citation Information
Patent Citations
Polymer mixture, useful for tire production, comprises precipitated silica and amino compound which reduces viscosity and improves processing properties
DE102004005132A1
rubber compounds
DE102006004062A1
Rubber composition, vulcanized product and use of these compositions for a tire tread and pneumatic tires
DE102011076490A1
Process for the production of rubber powders based on NR / carbon black and rubber powders produced in this way
DE19951977A1
Tire with tread having enhanced wet traction
EP2033813B1