spark plug
The spark plug design with a Pt-Ni stress relief layer and Pt-Rh discharge layer addresses interface separation issues by managing thermal stress and shock, ensuring effective ignitability and wear resistance.
Patent Information
- Application Number
- DE102018200211
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-01-23
- Filing Date
- 2018-01-09
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2038-01-09
AI Technical Summary
Conventional spark plugs experience interface separation between the electrode base element and the relaxation layer, as well as between the relaxation layer and the discharge layer, due to thermal stress and thermal shock, leading to impaired ignitability.
A spark plug design featuring a stress relief layer made of a Pt-Ni alloy with a thickness of at least 0.05 mm and a discharge layer composed of a Pt-Rh alloy, with controlled crystal grain sizes and compositions to manage thermal stress and prevent interface separation.
The design effectively reduces thermal stress and suppresses interface separation, maintaining ignitability by controlling crystal grain sizes and compositions to manage thermal expansion and shock, thereby enhancing spark wear resistance.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Technical area
[0001] The present invention relates to a spark plug and, more particularly, to a spark plug in which a tip serving as a Main component contains Pt, is provided on an electrode. State of the art
[0002] In order to improve the spark wear resistance of an electrode, a spark plug is known in which a first Electrode and a second electrode, each formed by connecting a tip containing Pt as the main component to an electrode base element, are arranged opposite each other. Patent Document 1 discloses a Technique for using a tip formed by bonding a discharge layer made of a Pt-Ir alloy with a stress relief layer made of a Pt-Ni alloy to absorb thermal stress due to a difference in thermal expansion between a tip and an electrode base element reduce. Further prior art is disclosed in the following documents: US 4 670 684 A, DE 11 2016 006 310 T5, EP 3 139 457 A1 and JP H06 - 60 959 A. State-of-the-art documents patent document Patent Document 1
[0003] Laid-open publication (kokai) of Japanese Patent Application No. H06-60959 A Summary of the invention Technical task
[0004] However, the conventional technique described above has the problem that interface detachment between an electrode base element and a stress relief layer, and interface delamination between a relaxation layer and a discharge layer occurs due to thermal stress caused by thermal caused by shock or the like.
[0005] The present invention aims to solve the problem described above and an object of the present The invention is to provide a spark plug which suppresses the interface detachment between the relaxation layer and the discharge layer. Technical solution
[0006] To solve the problem described above, a spark plug having the features of claim 1 is provided. Further advantages of the embodiment are set out in the dependent claims. Effects of the invention
[0007] In a spark plug according to a first aspect of the present invention, the stress relief layer comprising Pt as the main component, made of an alloy containing Ni as the second component, and has a thickness of not less than 0.05 mm. Therefore, the stress relief layer reduces thermal stress caused by a difference in the thermal expansion between the electrode base element, which is made of Ni, or an alloy containing Ni as main component, and the discharge layer formed from an alloy containing Pt as main component and contains Rh as a second component. According to the invention, the discharge layer consists of an alloy containing rhodium as a second component and a third component selected from the group Cr, Ti, Si, Y and Sr.
[0008] Furthermore, the structure of the discharge layer and the relaxation layer after welding differ the tip to the electrode base element, the average crystal grain size of the discharge layer and the average crystal grain size of the stress relief layer. can cause cracking at the crystal grain boundary between the discharge layer and the relaxation layer which enables the reduction of thermal stress.This can provide an effect to suppress the Interface delamination between the electrode base element and the stress relief layer and interface delamination between the relaxation layer and the discharge layer.
[0009] In the spark plug according to a second aspect of the present invention, in the structure of the discharge layer and the relaxation layer after welding the tip to the electrode base element, the average Crystal grain size of the discharge layer larger than the average crystal grain size of the relaxation layer. This can cause cracking at the crystal grain boundary of the discharge layer due to thermal stress, so that the thermal stress can be reduced. In addition to the effect achieved by the first aspect, the effect of further suppressing interfacial detachment can be achieved.
[0010] In the spark plug according to a third aspect of the present invention, a value obtained by dividing a Thickness of the discharge layer after welding the tip to the electrode base element by a thickness of the Relaxation layer obtained after welding the tip to the electrode base element is less than 3. This allows In addition to the effect achieved by the second aspect, the discharge layer is heated by thermal stress be easily deformed and an effect of reducing thermal stress can be ensured.
[0011] In the spark plug according to a fourth aspect of the present invention, in the structure of the discharge layer and the relaxation layer after welding the tip to the electrode base element, the average Crystal grain size of the discharge layer is smaller than the average crystal grain size of the relaxation layer. Crack formation at the crystal grain boundary of the stress relief layer can easily be caused by thermal stress. This allows, in addition to the effect achieved by the first aspect, an effect to reduce the thermal stress due to cracking at the crystal grain boundary of the stress relief layer and furthermore the Suppression of interfacial detachment can be achieved.
[0012] In the spark plug according to a fifth aspect of the present invention, the stress relief layer contains more than 3 Ma% of Ni. Thus, the linear expansion coefficient of the stress relief layer near the midpoint between the linear expansion coefficient of the discharge layer and the linear expansion coefficient of the In addition to the effect achieved by the fourth aspect, the The effect can be to further suppress the interface detachment.
[0013] In the spark plug according to a sixth aspect of the present invention, the compositions of Discharge layer and relaxation layer in the structure of the discharge layer and relaxation layer according to heating the tip to 1200 °C for 33 hours so that the average crystal grain size of the discharge layer is larger than the average crystal grain size of the relaxation layer. In addition, Effect achieved by any of the first to fifth aspects, an effect can be achieved that in an environment in which the first electrode is heated to about 1000 °C in a combustion chamber, a tiny crack can easily form at the crystal grain boundary of the discharge layer can be generated and the thermal stress can be reduced.
[0014] In the spark plug according to a seventh aspect of the present invention, the compositions of Discharge layer and relaxation layer in the structure of the discharge layer and relaxation layer according to heating the tip to 1200 °C for 33 hours so that the average crystal grain size of the discharge layer is smaller than the average crystal grain size of the relaxation layer. In addition, Effect achieved by any of the first to fifth aspects, an effect can be achieved that in an environment in which the first electrode is heated to about 1000 °C in a combustion chamber, cracking at the crystal grain boundary of the A relaxation layer can be easily created and thermal stress can be reduced.
[0015] In the spark plug according to an eighth aspect of the present invention, the discharge layer does not contain less than 85 Ma% of Pt and Rh. Thus, in addition to the effect achieved by any of the first to seventh aspects an effect of improving spark wear resistance can be achieved. Short description of the drawings Fig. 1 View of a spark plug, half of it shown in cross-section, according to a Embodiment of the present invention. Fig. 2 Cross-sectional view of a center electrode and a ground electrode. Embodiments of the invention
[0016] In the following, preferred embodiments of the present invention are described with reference to the accompanying drawings. Fig. 1 is a representation of a spark plug 10, half of which is shown in cross-section is, according to an embodiment of the present invention, and Fig. 2 is a cross-sectional view of a Center electrode 13 and a ground electrode 18. In Fig. 1 and Fig. 2 the underside of the drawing sheet serves as Front side of the spark plug 10, and the top of the drawing sheet serves as the back side of the spark plug 10.
[0017] As shown in Fig. 1, the spark plug 10 includes an insulator 11, the center electrode 13 (second electrode), a metal sleeve 17 and a ground electrode 18 (first electrode). The insulator 11 is a nearly cylindrical element, which made of aluminum oxide or the like, which has excellent mechanical properties and insulating properties at high temperatures. The insulator 11 has an axial bore 12 which extends along an axial line 0 penetrates.
[0018] The center electrode is a rod-shaped electrode which is inserted into the axial bore 12 and is surrounded by the insulator 11 is held along the axial line 0. The center electrode 13 includes an electrode base element 14 and a Tip 15, which is connected to the end of the electrode base element 14. A core material with excellent Thermal conductivity is embedded in the electrode base element 14. The electrode base element 14 consists of a Metal made of Ni or an alloy containing Ni as the main component, and the core material is made of copper or an alloy containing copper as the main component. The tip 15 is made of a precious metal such as Platinum, iridium, ruthenium or rhodium with a higher spark wear resistance than the electrode base element 14, or an alloy containing such a precious metal as its main component.
[0019] A metal clamp 16 is a rod-shaped element to which a high-voltage cable (not shown) is connected, and the front portion of the metal clamp 16 is arranged in the insulator 11. The metal clamp 16 is electrically connected to the center electrode 13 in the axial bore. The metal sleeve 17 is a nearly cylindrical element made of metal, the element being mounted in a screw hole (not shown) of an internal combustion engine The metal sleeve 17 is fixed to the outer circumference of the insulator 11.
[0020] The ground electrode 18 includes an electrode base member 19 connected to the metal sleeve 17, and a Tip 20, which is connected to the electrode base element 19. A core material with excellent thermal conductivity is embedded in the electrode base member 19. The electrode base member 19 is made of an alloy containing Ni as main component, or a metal material made of Ni, and the core material consists of copper or a Alloy containing copper as the main component. Of course, the core material can also be omitted and the Electrode base member 19 may be formed entirely from an alloy containing Ni as the main component, or a metal material of Ni. The electrode base member 19 is inclined towards the center electrode 13, and the tip 20 is located opposite the center electrode 13, with a spark gap G between them (see Fig. 2).
[0021] The spark plug 10 is manufactured, for example, in a process described below. First, the Center electrode 13 is inserted into the axial bore 12 of the insulator 11. The center electrode 13 is in a state arranged in which the front end of the center electrode 13 is at the front end of the axial bore 12 at the outside is exposed. After the metal terminal 16 is inserted into the axial bore 12 and the electrical connection between the metal clamp 16 and the center electrode 13 is ensured, the metal sleeve 17 with which the Electrode base element 19 is pre-connected, mounted on the outer circumference of the insulator 11. The tip 20 is connected to the Electrode base element 19 and the electrode base element 19 is bent so that the tip 20 is in a Direction of the axial line 0 opposite the center electrode 13 to obtain the spark plug 10.
[0022] As shown in Fig. 2, the tip 20 consists of a composite material comprising a relaxation layer 21 and a discharge layer 22 stacked on the relaxation layer 21, and has the shape of a disc. The discharge layer 22 is metallurgically bonded to the stress relief layer 21 by a Processes such as a rolling process, an explosion welding process, a diffusion process or an explosion welding rolling process. The stress relief layer 21 of the tip 20 is formed by resistance welding with the Electrode base element 19.
[0023] The discharge layer 22 is an alloy containing Pt as the main component and Rh as the second component. the discharge layer 22 contains Pt and Rh, the oxidation resistance and the spark wear resistance ´´Contains Pt as the main component´´ means that the Pt content in the discharge layer 22 is not less than 50 Ma%. The discharge layer 22 may contain a third component such as Ni, Cr, Ti, Si, Y or Sr in addition to Pt and Rh. Desirably, the discharge layer 22 contains not less than 85 Ma% of Pt and Rh to improve the spark wear resistance. According to the invention, the discharge layer has third component a component selected from the group Cr, Ti, Si, Y and Sr in addition to platinum and rhodium. The previously described alternative that the third component can be nickel is not claimed.
[0024] The stress relief layer 21 is an alloy containing Pt as the main component and Ni as the second component, wherein the alloy has a thickness of not less than 0.05 mm. The stress relief layer 21 is between the Electrode base element 19 and the discharge layer 22 and reduces thermal stress due to a Difference in thermal expansion between the electrode base element 19 and the discharge layer 22. ´´Contains Pt as the main component´´ means that the content of Pt in the stress relief layer 21 is not less than 50 Desirably, the stress relief layer 21 contains more than 3 Ma% Ni, so that an effect for Reduction of thermal stress is ensured by the relaxation layer 21.
[0025] Since the stress relief layer 21 has a thickness of not less than 0.05 mm, the weldability between the electrode base element 19 and the relaxation layer 21. However, if the thickness of the stress relief layer 21 is not less than 0.05 mm, interface detachment easily occurs between the Electrode base element 19 and the relaxation layer 21 as well as an interface detachment between the relaxation layer 21 and the discharge layer 22 due to the thermal stress caused by a Difference in thermal expansion between the electrode base element 19 and the discharge layer 22 Since the discharge layer 22 or the tip 20 floats due to the occurrence of interface detachment, the spark gap G is reduced and the ignitability of the spark plug 10 is impaired. If the discharge layer 22 or the tip 20 drops due to the progression of the interface detachment, the spark gap G is increased and the Ignition capability of the spark plug 10 is impaired. These interface detachments can be caused by thermal shock during a Maximum temperature of about 600 °C to about 1000 °C.
[0026] In order to suppress the interface detachment, the crystal grain sizes of the relaxation layer 21 and the discharge layer 22. If the crystal grain size is large, the region (length) in which dislocations occur more frequently, large and the amount of accumulated dislocations increases. This can easily lead to Stress concentration can be caused and crack formation can easily occur at the crystal grain boundary. means that the average crystal grain size of the relaxation layer 21 and the average crystal grain size the discharge layer 22 are formed differently, crack formation at a crystal grain boundary of the relaxation layer 21 or the discharge layer 22, whichever has the larger average crystal grain size, so that thermal stress can be reduced and interfacial delamination can be suppressed. Crystal grain sizes of the relaxation layer 21 and the discharge layer 22 can be controlled by controlling the Processing conditions and compositions of the relaxation layer 21 and the discharge layer 22 be adjusted.
[0027] Since the structures of the relaxation layer 21, which consists of a PtNi alloy, and the discharge layer 22, which consists of a PtRh alloy, rarely change at a temperature of about 600 °C, the structures of the relaxation layer 21 and the discharge layer 22 after they have been welded to the electrode base element 19, a great influence on the reduction of thermal stress caused by thermal shock at a Maximum temperature of about 600 °C. The structures of the relaxation layer 21 and the discharge layer 22, after they have been welded to the electrode base element 19, the processing conditions of the relaxation layer 21 and the discharge layer 22.
[0028] At the same time, the structures of the relaxation layer 21 and the discharge layer 22 temporarily change as a result of the Heating to about 1000 °C, and the average crystal sizes of the stress relief layer 21 and the Discharge layer 22 are changed. The structures of the relaxation layer 21 and the Discharge layer 22 controlled by the compositions of the relaxation layer 21 and the discharge layer 22 The structures of the relaxation layer 21 and the discharge layer 22, which are determined by the compositions of the relaxation layer 21 and the discharge layer 22 have a great influence on the reduction of thermal stress caused by thermal shock at a maximum temperature of about 1000 °C becomes.
[0029] The average crystal grain sizes of the relaxation layer 21 and the discharge layer 22 can be determined according to Annex C ´´Evaluation by intercept method´´ of JIS G0551 (2013), which is based on ISO643 (edition 2003). An average crystal grain size refers to an average length per Crystal grain of a test line through the interior of the crystal grain appearing on a flat cross-section of a test piece, which has been polished for microscopic examination. In the present embodiment, at least one from one test line, which is a straight line parallel to the axial line 0, one test line, which is a straight line perpendicular to the axial line 0, and a test line which is a straight Line which crosses the axial line 0 at an angle of 45°, drawn at the intersection which crosses the axial line 0 so that the average crystal grain size is obtained. An average length per Crystal grain of a test line across the interior of the crystal grain can be determined from an average number of recorded Crystal grains per 1 mm of a test line or an average number of intersection points per 1 mm of a test line The number of crystal grains detected is the number of crystals through which a test line passes or recorded on a test line, and the number of intersection points is the number of intersection points between the Crystal grain boundary and a test line.
[0030] If in the structure of the discharge layer 22 and the relaxation layer 21 after welding to the Electrode base element 19, the average crystal grain size of the relaxation layer 21 and the average Crystal grain size of the discharge layer 22 are the same, there is the problem that interface detachment between the electrode base element 19 and the relaxation layer 21 as well as interface detachment between the Relaxation layer 21 and discharge layer 22 by a thermal shock at a maximum temperature of about 600 °C.
[0031] If, on the other hand, in the structure of the discharge layer 22 and the relaxation layer 21 after welding on the electrode base member 19, the average crystal grain size of the discharge layer 22 is larger than the average crystal grain size of the relaxation layer 21 is at the crystal grain boundary of the discharge layer 22 cracking is easily caused by thermal shock at a maximum temperature of about 600 °C, so that the Discharge layer 22 (the tip 20) can be easily deformed. Thus, thermal stress can be caused by cracking at the crystal grain boundary of the discharge layer 22 and deformation of the discharge layer 22 (the tip 20) can be reduced and interface detachment can be suppressed.
[0032] When crystal grains due to the progression of crack formation at the crystal grain boundary of the discharge layer 22 the ignition capability of the spark plug 10 may be impaired. However, since the size of the cracks on the Crystal grain boundary can be reduced by the deformation of the discharge layer 22 (the tip 20), can be prevented that the crack formation at the crystal grain boundary of the discharge layer 22 has a negative influence on the Ignition capability of the spark plug 10.
[0033] If in the structure of the discharge layer 22 and the relaxation layer 21 after welding to the Electrode base element 19, the average crystal grain size of the discharge layer 22 is smaller than the average Crystal grain size of the stress relief layer 21, cracking can occur at the crystal grain boundary of the stress relief layer 21 caused by a thermal shock at a maximum temperature of about 600 °C. Thus, thermal Stress can be reduced by crack formation at the crystal grain boundary of the stress relief layer 21 and can Since the stress relief layer 21 is not a part that performs a function such as For example, discharge can, even if cracking occurs at the crystal grain boundary of the stress relief layer 21 occurs, the crack formation can be prevented from having a negative influence on the ignitability of the spark plug 10.
[0034] Furthermore, if in the structure of the discharge layer 22 and the relaxation layer 21 after heating the Tip 20 at 1200 °C for 33 hours the compositions of the discharge layer 22 and the relaxation layer 21 so that the average crystal grain size of the discharge layer 22 larger than the average crystal grain size of the stress relief layer 21, at the crystal grain boundary of the Discharge layer 22 easy cracking due to thermal shock at a maximum temperature of about 1000°C This reduces thermal stress and suppresses the formation of interfaces.
[0035] If in the structure of the discharge layer 22 and the relaxation layer 21 after heating the tip 20 at 1200 °C for 33 hours, the compositions of the discharge layer 22 and the relaxation layer 21 are be determined that the average crystal grain size of the discharge layer 22 is smaller than the average Crystal grain size of the relaxation layer is 21, can be easily Crack formation can be caused by a thermal shock at a maximum temperature of about 1000°C. This allows thermal stress is reduced and interface formation is suppressed.
[0036] Regarding the thickness of each of the discharge layer 22 and the relaxation layer 21, a value which by dividing a thickness of the discharge layer 22 after welding the tip 20 to the electrode base member 19 by a thickness of the relaxation layer 21 after welding the tip 20 to the electrode base element 19 is obtained, preferably less than 3. The reason for this is that if the thickness of the discharge layer 22 with respect to the thickness of the relaxation layer 21 is less than 3, the discharge layer 22 by thermal stress is easily deformed and the effect of reducing thermal stress is ensured. The thickness of each the discharge layer 22 and the relaxation layer 21 is a thickness at the intersection, which the axial line 0 with the center of each of the discharge layer 22 and the relaxation layer 21. Examples
[0037] The present invention will be described in more detail with reference to examples. However, the present Invention is not limited to these examples. <Produktion von Mustern>
[0038] An examiner presented various types of tip 20, which differ in shape and composition, average crystal grain size and the thickness of each of the discharge layer 22 and the relaxation layer 21 distinguish, by solid phase diffusion connection between the discharge layer 22 and the relaxation layer 21 Samples of the spark plug 10 were produced, each by joining, by means of resistance welding, the Discharge layer 22 with the electrode base element 19, which consists of NFC600, and by providing different types of tip 20 on the ground electrode 18. A list of the manufactured samples is shown in Table 1 Since a large number of evaluations were carried out for each pattern, a large number of the pattern were every type manufactured.
[0039] In the samples 1 to 56, the tip 20 in which the discharge layer 22 and the relaxation layer 21 made of a composite material, are provided on the ground electrode 18. In the patterns 57 to 62, a Tip in which the discharge layer 22 and the relaxation layer 21 do not exist independently of each other, at the Ground electrode 18. The values in the sections ´´Discharge layer´´ and ´´Relaxation layer´´ of the Peaks in Table 1 represent mass percent of an element. Of samples 1 to 56, only samples 23, 24, 36, 45, 50 embodiments of the invention. The further examples are helpful for understanding the present Invention.
[0040] For each sample, the examiner conducted two types of tests to determine the spark wear resistance (a test 1 and one test 2) and two types of thermal cycling repetition test (one thermal test 1 and a thermal test 2), in which the ground electrode 18 is heated by a burner and cooled again became.
[0041] In addition to these tests, the examiner embedded the tip 20 in synthetic resin and then polished the tip 20 before the test, which was welded to the electrode base element 19, by an average length (average crystal grain size) per crystal grain by microscopic examination of the test lines across the interior of the crystal grains that appeared at the intersection containing the axial line 0 (at least one of each the straight line parallel to the axial line 0, the straight line perpendicular to the axial line 0 and the straight line crossing the axial line 0 at an angle of 45°). Values obtained by dividing the average crystal grain size of the discharge layer 22 by the average crystal grain size of the relaxation layer 21 were shown in the section ´´front´´ of ´´Crystal grain size´´ in Table 1. At the same time, values were obtained which were calculated by dividing the thickness of the discharge layer 22 located at the intersection including the axial line 0, through the thickness of the relaxation layer 21. These values were shown in the ´´Thickness´´ section in Table 1.
[0042] In addition, the tester cut the electrode base member 19 to which the tip 20 was welded before the test. The cut electrode base element 19 and the cut tip 20 were heated to 1200 °C for 33 hours and then the electrode base member 19 and the tip 20, both embedded in synthetic resin, polished to obtain an average length (average crystal grain size) per crystal grain of the test lines over to preserve the interior of the crystal grain, which is intersection containing the axial line 0 (at least one of each of the straight lines parallel to the axial line 0, the straight line perpendicular to the axial line 0 and the straight line connecting the axial line 0 at an angle of 45°). Values obtained by dividing the average crystal grain size of the Discharge layer 22 by the average crystal grain size of the relaxation layer 21 were obtained in section ´´rear´´ of ´´crystal grain size´´ shown in Table 1. <Funkenverschleißbeständigkeit: Testverfahren und Evaluierungsverfahren in Test 1>
[0043] The examiner mounted each sample of the spark plug 10 in a four-cylinder direct injection engine with a displacement of 2.0 l, which was equipped with a turbocharger device of the exhaust turbine type, and then actuated the motor. A spark gap (a gap between the discharge layer 22 and the center electrode 13 of the individual The sample was 0.75 mm. The engine operating condition included a rotation of 4000 rpm, the air / fuel Ratio was 12.0, the load was an indicated mean effective pressure (IMEP) of 190 kPa and one engine operating phase was 200 hours continuously.
[0044] The examiner measured the spark gap of each sample after the test using a test pin and The test determined the growth rate (wear rate) of the spark gaps. The rating was ´´A´´ if the Increment size was less than 0.15 mm, the rating was ´´B´´ if the increment size was in the range of not less than 0.15 mm and less than 0.20 mm, and the rating was ´´C´´ if the increment size was not less than than 0.20 mm. <Funkenverschleißbeständigkeit: Testverfahren und Evaluierungsverfahren in Test 2>
[0045] Similar to Test 1, except that the spark gaps of the samples were 1.05 mm, a motor in which the samples of the spark plug 10 were mounted.
[0046] The examiner measured the spark gap of each sample after the test using a test pin and The test then determined the gap growth rate (wear rate). The rating was ´´S´´ if the Increment size was less than 0.15 mm, the rating was ´´A´´ if the increment size was in a range of was not less than 0.15 mm and less than 0.20 mm, the rating was ´´B´´ if the increase size was in the range of not less than 0.20 mm and less than 0.30 mm, and the rating was ´´C´´ if the increment was not less than 0.30 mm. <Testverfahren im thermischen Test 1>
[0047] The tester performed 1000 cycles on the electrode base element 19, where one cycle is defined as a period in which the front end of the electrode base member 19 (a portion furthest from the metal sleeve 17 away) was heated for two minutes using a burner so that the temperature of the front end reached 600 °C and was then allowed to cool for one minute. <Testverfahren im thermischen Test 2>
[0048] The tester performed 1000 cycles on the electrode base element 19, where one cycle is defined as a period in which the front end of the electrode base element 19 was heated for two minutes by means of a burner, so that the temperature of the front end was 1000°C, and then allowed to cool for one minute. <Evaluierungsverfahren für Grenzflächenablösung>
[0049] The examiner embedded the ground electrode 18 in synthetic resin after the test, polished the embedded electrode and exposed the cross section that included the center of tip 20. Assuming that ´´A´´ is the length of tip 20 represents (measure along the interface between the tip 20 and the electrode base element 19), ´´a´´ the length of a section in which no interface detachment occurs and the relaxation layer 21 and the Electrode base element 19 are connected to each other, and ´´b´´ represents the length of a section in which no Interfacial detachment occurs and the discharge layer 22 and the relaxation layer 21 are connected to each other, the interfacial detachment ratio, i.e. X=(Aa) / A(%), Y=(Ab) / A(%), was determined by microscopic observation The rating was ´´S´´ if the greater of X and Y was less than 10%, the rating The result was 'A' if the larger value of X and Y was within a range of not less than 10% and less than 40% the rating was ´´B´´ if the larger value of X and Y was within a range of not less than 40% and was less than 50%, and the rating was 'C' if the greater of X and Y was not less than 50%. <Evaluierungsverfahren für interkristalline Rissbildung>
[0050] The examiner determined a proportion (%) of an area of a section affected by intergranular cracking at the Cross-sectional area of each of the discharge layer 22 and the relaxation layer 21 was lost, in the cross section, on which the above-described evaluation of the interface detachment was carried out (the cross-section that shows the center the tip 20, which was obtained by embedding the ground electrode 18 in synthetic resin after the test and by exposing the Tip 20 was obtained by polishing). The rating was 'A' if the proportion was less than 1%, the The rating was ´´B´´ if the share was in the range of not less than 1% and less than 10%, and the The rating was 'C' if the share was not less than 10%. <Evaluierungsverfahren für Verformung>
[0051] A deformation amount (µm) of the tip 20 was defined as a value obtained by subtracting a projection amount the tip 20 from the electrode base member 19, measured using a micrometer before the thermal Test, from a projection size of the tip 20 from the electrode base member 19, measured using a micrometer after the thermal test. <Verfahren für die Gesamtevaluierung>
[0052] By digitizing the evaluations, giving the rating ´´S´´ 3 points, the rating ´´A´´ 2 points were awarded, the rating ´´B´´ was awarded one point and the rating ´´C´´ was given 0 points The total score was calculated. The overall evaluation was 'S' if the total score was not was less than 18 points, the overall evaluation was ´´A´´ if the total score was in the range of 15 points to 17 points, the overall evaluation was ´´B´´ if the total score was in a range of 11 points to 14 points, and the overall evaluation was ´´C´´ if the total score was in a range of 0 points to 10 points. If even one rating of ´´C´´ occurred in any of the evaluations, the Overall evaluation ´´C´´, regardless of the total score. <ergebnisse>
[0053] As seen in the section ´´Composition´´ of ´´Lace´´ in Table 1, the samples 1 to 52 were samples in in which the discharge layer consisted of the PtRh alloy and the relaxation layer of the PtNi alloy Samples 53 and 54 were samples in which the stress relief layer consisted of the PtNi alloy and the discharge layer was made of a metal other than the PtRh alloy. Samples 55 and 56 were samples in which the discharge layer consisted of the PtRh alloy and the relaxation layer of a different metal other than the PtNi alloy. Samples 57 to 62 were samples in which a tip was used that was not made of a composite material.
[0054] In the evaluation of the interface detachment in the thermal test 1, samples 53 to 56, 57, 59, 60 and 62 was evaluated as C, whereas samples 1 to 14, 17 to 52, 58 and 61 were evaluated as S to B. Among samples 1 to 14, 17 to 52, 58 and 61, samples 1 to 14 and 17 to 52, except samples 58 and 61, were classified as A or B in Test 1 evaluated for spark wear resistance.
[0055] As can be seen from the section ´´front´´ of ´´crystal grain size´´ in Table 1, among the samples 1 to 52 the patterns 15 and 16 in the average crystal grain size of the discharge layer 22 and the average Crystal grain size of the stress relief layer 21 after welding to the electrode base element 19 is the same. The samples 1 to 14 and 17 to 52 differed in the average crystal grain size of the discharge layer 22 and the average crystal grain size of the stress relief layer 21 after welding to the electrode base element 19 from each other. It was confirmed that when, as in samples 1 to 14 and 17 to 52, in each of which the Discharge layer consists of the PtRh alloy and the relaxation layer consists of the PtNi alloy, which average crystal grain size of the discharge layer 22 and the average crystal grain size of the Relaxation layer 21 are formed differently from each other after welding to the electrode base element 19, Interfacial delamination can be suppressed in thermal test 1, where the highest temperature is 600 °C.
[0056] Among the samples 1 to 14 and 17 to 52, the samples 1 to 14 were samples in which the average Crystal grain size of the discharge layer 22 after welding to the electrode base element 19 is smaller than the average crystal grain size of the stress relief layer was 21. Samples 17 to 52 were samples in which the average crystal grain size of the discharge layer 22 after welding to the electrode base element 19 larger than the average crystal grain size of the stress relief layer 21. In the thermal test 1, found that in samples 1 to 14 the area of intergranular cracking in the stress relief layer 21 is larger than the area of intergranular cracking in the discharge layer 22. In contrast, in the thermal test 1 found that in samples 17 to 52 the area of intergranular cracking in the discharge layer 22 is larger than is the area of intergranular cracking in the stress relief layer 21.
[0057] Based on these results, it is assumed that thermal stresses caused by a thermal Shock in the thermal test 1 could be reduced and interface detachment by intergranular cracking could be suppressed, which occurred in the discharge layer 22 or the relaxation layer 21 occurred, depending on which had the larger average crystal grain size.
[0058] In the evaluation of the interface detachment in the thermal test 1, when comparing samples 8, 9, 17 to 20, 34 and 35, the samples 17 to 20, 34 and 35, in each of which a Ni content in the stress relief layer 21 is not was more than 3 Ma%, was evaluated as B. In contrast, samples 8 and 9, in which the stress relief layer 21 contained more than 3 Ma% Ni (5 Ma%) than S. Based on these results, it is assumed that the Interfacial delamination could be suppressed because in the stress relief layer 21, which contained more than 3 Ma% Ni, the linear expansion coefficient of the relaxation layer 21 near the midpoint between the linear Expansion coefficient of the discharge layer 22 and the linear expansion coefficient of the Electrode base element 19.
[0059] When in the evaluation of the interface separation in the thermal test 1, the samples 31 to 33 are were compared, samples 32 and 33, each of which had a value calculated by dividing the thickness of the Discharge layer 22 was obtained by the thickness of the relaxation layer 21, after welding to the Electrode base element 19 was not less than 3, was evaluated as B. On the other hand, samples 29 to 31, in which each a value obtained by dividing the thickness of the discharge layer 22 by the thickness of the relaxation layer 21 was less than 3, was evaluated as S. Based on these results, it is assumed that if the thickness of the discharge layer 22 has been reduced, the discharge layer 22 may be slightly deformed by thermal stresses and an effect to reduce thermal stress could be improved.
[0060] In the evaluation of Test 2 for spark wear resistance, when comparing samples 6, 7, 13 and 14, sample 14, in which the discharge layer 22 contained 80 wt% Pt and Rh, was evaluated as C. In contrast, Samples 6, 7 and 13, in each of which the discharge layer 22 contained not less than 85 Ma% Pt and Rh, as A or B. Accordingly, in the evaluation of Test 1 for spark wear resistance at Comparison of samples 6, 7, 13 and 14, sample 14, in which the discharge layer 22 contained 80 Ma% Pt and Rh, as B In contrast, samples 6, 7 and 13, in each of which the discharge layer 22 contains not less than 85 Ma% Pt and Rh was evaluated as A. Based on these results, it was determined that if the discharge layer 22 is not contains less than 85 mass% Pt and Rh, the spark wear resistance can be improved.
[0061] In the evaluation of the interface detachment and the intergranular crack formation in thermal test 2, Samples 8 to 12 were compared with samples 13 and 14, samples 17 to 24 were compared with samples 25 to 33 and samples 34 to 36 were compared with samples 37 to 44. Samples 8 to 12, 17 to 24 and 34 to 36 were samples in which the average crystal grain size of the stress relief layer 21 after heating the Electrode base element 19 and tip 20 at 1200 °C for 33 hours larger than the average crystal grain size of the discharge layer 22. Samples 13, 14, 25 to 33 and 37 to 44 were samples in which the average Crystal grain size of the discharge layer 22 after heating the electrode base member 19 and the tip 20 to 1200 °C for 33 hours was larger than the average crystal grain size of the stress relief layer 21.
[0062] By comparing the results, it was confirmed that patterns 8 to 12, 17 to 24 and 34 to 36 were larger than the patterns 13, 14, 25 to 33 and 37 to 44 were in the area of a part of the relaxation layer 21, which was intergranular cracking is lost. It was found that when, as in samples 8 to 12, 17 to 24 and 34 to 36, the compositions of the relaxation layer 21 and the discharge layer 22 are adjusted so that the average crystal grain size of the stress relief layer 21 after heating to 1200 °C for 33 hours is greater than is the average crystal grain size of the discharge layer 22, intergranular cracking in the thermal test 2, where the highest temperature is 1000 °C. Thus, the thermal stress reduced and the interface detachment of tip 20 can be suppressed.
[0063] It was confirmed that the samples 13, 14, 25 to 33 and 37 to 44 were smaller than the samples 8 to 12, 17 to 24 and 34 to 36 in the area of the part of the stress relief layer 21 that is lost due to intergranular cracking. It was found that when, as in samples 13, 14, 25 to 33 and 37 to 44, the compositions of the Relaxation layer 21 and discharge layer 22 are adjusted so that the average crystal grain size the discharge layer 22 after heating to 1200 °C for 33 hours is larger than the average crystal grain size the relaxation layer 21, suppresses intergranular cracking in the relaxation layer 21 and a tiny intergranular cracking in the discharge layer 22 in the thermal test 2, in which the highest temperature was 1000 ° C. This can easily cause thermal stress to be reduced and the interface detachment the top 20 are suppressed.
[0064] Regarding the deformation size of the thermal test 2, when comparing the samples 17 to 24 and 34 to 36 with each other confirmed that the samples 23, 24 and 36, in each of which the discharge layer 22 has a third component may be smaller in deformation size than the other samples 17 to 22, 34 and 35.
[0065] In the examples, various evaluations were carried out on samples 1 to 62, in each of which the Tip 20 with a disc or prism shape is provided on the ground electrode 18. In samples 1 to 62, confirms that the evaluation results are not influenced by the shape of the peak 20.
[0066] Although the invention has been described above on the basis of the embodiments, the invention by no means limited to the above embodiments. It is understood that various modifications can be made without departing from the essence of the present invention.
[0067] Although the embodiments described the case in which the tips 20 each have a disc or prism shape, but the present invention is not necessarily limited to this. Other shapes can also be used. Other shapes of tip 20 include, for example, the shape a truncated cone, an elliptical cylinder and the like.
[0068] Although the above embodiments described the case in which the tip 20 is in each case by means of resistance welding to the electrode base element 19, but the present invention is not necessarily limited to this. Of course, the top 20 can also be connected to the Electrode base element 19. Other methods include, for example, laser welding.
[0069] Although the above embodiments described the case in which the tip 20 (the relaxation layer 21 and the discharge layer 22) is provided on the ground electrode 18, but the present The invention is not necessarily limited to this. Of course, the tip 20 can also be used with the Electrode base element 14 of the center electrode 13, instead of the tip 15 which is connected to the center electrode 13 In this case, the same action and effect as in the above described in the embodiments.
[0070] Although the above embodiments described the case in which the metal sleeve 17 connected electrode base element 19 is bent, but the present invention is not necessarily Of course, a straight electrode base element can also be used instead of the curved electrode base element 19. In this case, the front side of the metal sleeve 17 extends in the Direction of the axial line 0 and the straight electrode base element is connected to the metal sleeve 17, so that the Electrode base element opposite the center electrode 13.
[0071] Although the above embodiments described the case in which the axial line 0 of the Center electrode 13 coincides with the tip 20 and the ground electrode 18 is arranged so that the tip 20 of the Center electrode 13 in the direction of the axial line 0, but the present invention is not necessarily limited to this. A spatial relationship between the ground electrode 18 and the center electrode 13 can be adjusted as required. A further spatial relationship between the ground electrode 18 and the Center electrode 13 includes the arrangement of the ground electrode 18 such that a side surface of the center electrode 13 and the ground electrode 18 are opposite each other. Description of reference symbols 10 Spark plug 13 Center electrode (second electrode) 18 Ground electrode (first electrode) 19 Electrode base element 20 lace 21 relaxation layer 22 discharge layer< / ergebnisse>
Claims
1. Spark plug (10), comprising: a first electrode (18) including: a tip (20) in which a discharge layer (22) containing Pt as a main component, and a relaxation layer (21) containing Pt as a main component, and an electrode base member (19) made of Ni or an alloy containing Ni as a main component, wherein the relaxation layer (21) is welded to the electrode base element (19); and a second electrode (13) opposite the discharge layer (22), with a spark gap therebetween, wherein the discharge layer (22) consists of an alloy containing Rh as a second component and a third component selected from the group containing Cr, Ti, Si, Y and Sr, the stress relief layer (21) consists of an alloy containing Ni as a second component and has a thickness of not less than 0.05 mm, and in a structure of the discharge layer (22) and the relaxation layer (21) after welding the tip (20) to the electrode base member (19) has an average crystal grain size of the discharge layer (22) and a average crystal grain size of the relaxation layer (21) differ from each other.
2. Spark plug (10) according to claim 1, wherein in the structure of the discharge layer (22) and the relaxation layer (21) after welding the tip (20) to the electrode base element (19), the average crystal grain size of the Discharge layer (22) is larger than the average crystal grain size of the relaxation layer (21).
3. Spark plug (10) according to claim 2, wherein a value obtained by dividing a thickness of the discharge layer (22) after Welding the tip (20) to the electrode base element (19) through a thickness of the stress relief layer (21) after obtained by welding the tip (20) to the electrode base element (19) is less than 3.
4. Spark plug (10) according to claim 1, wherein in the structure of the discharge layer (22) and the relaxation layer (21) after welding the tip (20) to the electrode base element (19), the average crystal grain size of the Discharge layer (22) is smaller than the average crystal grain size of the relaxation layer (21).
5. Spark plug (10) according to claim 4, wherein the stress relief layer (21) contains more than 3 Ma% Ni.
6. Spark plug according to one of claims 1 to 5, wherein the compositions of the discharge layer (22) and the Relaxation layer (21) in the structure of the discharge layer (22) and the relaxation layer (21) after heating the tip (20) to 1200 °C for 33 hours so that the average crystal grain size of the discharge layer (22) is larger than the average crystal grain size of the relaxation layer (21).
7. Spark plug (10) according to one of claims 1 to 5, wherein the compositions of the discharge layer (22) and the Relaxation layer (21) in the structure of the discharge layer (22) and the relaxation layer (21) according to the Heating the tip (20) to 1200 °C for 33 hours so that the average crystal grain size of the Discharge layer (22) is smaller than the average crystal grain size of the relaxation layer (21).
8. Spark plug (10) according to one of claims 1 to 7, wherein the discharge layer (22) contains not less than 85 Ma% Pt and Rh contains.
Citation Information
Patent Citations
Spark plug
DE112016006310T5
Spark plug and method for producing the same
EP3139457A1
Spark plug for internal combustion engine
JP1994060959A
Spark plug
US4670684A
JP0000H0660959A