COATED CUTTING TOOL
A coated cutting tool with a Ti compound layer, α-Al O intermediate layer, and controlled TiCN top layer addresses wear and breaking strength issues, enhancing tool life by preventing grain fallout and crater wear.
Patent Information
- Application Number
- DE102019008746
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-01-18
- Filing Date
- 2019-12-17
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2039-12-17
AI Technical Summary
Conventional coated cutting tools experience issues with wear resistance and breaking strength under high-speed cutting conditions, leading to reduced tool life due to crater wear and grain fracture, particularly when a TiCN layer is used as the top layer.
A coated cutting tool design featuring a lower Ti compound layer, an intermediate α-Al O layer, and a top TiCN layer with controlled grain aspect ratio and misalignment, enhancing wear resistance and breaking strength.
The design significantly improves wear resistance and breaking strength, extending the tool's life by preventing grain fallout and crater wear, especially under demanding cutting conditions.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Technical application area
[0001] The present invention relates to a coated cutting tool. State of the art
[0002] It is well known that a conventional coated cutting tool, which is used for cutting steel, Cast iron, etc., is used; it is a coated cutting tool that is created by deposition via chemical processes. Vapor deposition of a coating layer with a total thickness of 3 µm or more to 20 µm or less on a surface of a substrate consisting of a hard metal is obtained. A well-known example of the above A coating layer is a coating layer consisting of a single layer of a type that has been selected is from the group consisting of a Ti carbide, a Ti nitride, a Ti carbonitride, a Ti carboxide, a Ti- Oxycarbonitride and aluminium oxide or from several layers of two or more selected species consists.
[0003] For example, JP 2017-530 019 A discloses a coated cutting tool made from a substrate of hard metal, a cermet, a ceramic, steel or a cubic boron nitride and a multi-layered abrasion-resistant The coating consists of a total coating thickness of 5 µm or more up to 25 µm or less, and has at least two refractory coating layers applied by chemical vapor deposition (CVD) or a Chemical vapor deposition at moderate temperature (MT-CVD) is used for deposition, whereby at least two fire-resistant coating layers have a first coating layer and a second coating layer, which are deposited on top of each other, with the first coating layer being made of titanium aluminum nitride or titanium aluminum- Carbonitride TiAlCN, with 0.2 ≤ u ≤ 1.0, 0 ≤ v ≤ 0.25 and 0.7 ≤ w ≤ 1.15, consists of and is produced by CVD in a 1-uuvw The second coating layer is deposited at a reaction temperature in the range of 600°C to 900°C. titanium carbonitride Ti CN with 0.85 ≤ x ≤ 1.1 and 0.4 ≤ y ≤ 0.85 and on the first coating layer xy 1-y is deposited by MT-CVD at a reaction temperature in the range of 600°C to 900°C, with the second Ti CN xy 1- -The coating layer has a columnar grain morphology and the overall fiber texture of the Ti CN - yxy 1-y coating layer is characterized by a texture coefficient TC (111) > 2, where TC (111) is defined as follows is: ... (in the formula, (hkl) = measured intensity of the (hkl) reflection; I (hkl) = standard intensity of the 0 Standard powder diffraction data according to JCPDF card no. 42-1489; n = number of samples used in the calculation Reflections; for the (hkl) reflections, (111), (200), (220) and (311) are used. JP 2012 - 196 726 A discloses a Cutting tool with a TiCN layer, which has a lower layer and consists of columnar crystals with a produced with an average crystal width of 0.1 to 1 µm, an Al O₂ layer and a TiCN layer, which forms an upper 2 3 The layer is made of columnar crystals. JP H08 - 158 052 A discloses a cutting tool made of a coated hard alloy, which is formed by a hard coating layer on the surface of a base material consisting of a is obtained from sintered hard alloy or cermet. Summary Technical problem
[0004] An increase in speed, feed and depth of cut has recently been observed in cutting obvious, and it is necessary to further examine the wear resistance and fracture strength of a tool. to improve upon those in the state of the art. In particular, there has been an increase in recent years of Number of cutting operations in which a load is applied to a coated cutting tool, such as a High-speed cutting of steel, and under such difficult cutting conditions, conventional methods encounter problems. Tools suffer from crater wear and cracking due to precipitates of grains from the coating layer, which causes it This makes it impossible to extend the tool's lifespan.
[0005] Since the coated cutting tool disclosed in JP 2017-530 019 A does not have an α-Al₂O₃ layer, the 2 3 Insufficient resistance to crater wear. Furthermore, generally, if a TiCN layer is applied as the top layer on The structure of the α-Al O layer is formed in the coating layer of the coated cutting tool. 2 3 The TiCN layer is granular because CH₄ gas is used as a carbon source. For this reason, it is difficult to determine the 4 To control alignment in the TiCN layer, and Fracture occurs due to grains falling from the TiCN layer of the upper layer, making it difficult to determine a to form a thick TiCN layer.
[0006] The present invention was made in view of the above circumstances and addresses a problem of the present The invention is to provide a coated cutting tool that offers excellent wear resistance and exhibits fracture resistance and therefore enables an extended tool lifespan. Solution to the problem
[0007] The present inventor has conducted research on extending the tool life of a coated Cutting tool from the above perspective and found that with a design in which a Coating layer: a lower layer that has one or more Ti compound layers, an intermediate layer, which has an α-Al O₂ layer, and an upper layer which has a TiCN layer, in that order 2 3 exhibits and in which the upper layer contains specific TiCN grains with a controlled aspect ratio. and exhibits a misalignment of the (111) orientation in a specific ratio, a specific thickness on the The surface of the intermediate layer, which has an α-Al₂O₃ layer, makes it possible to prevent the shedding of grains. 2 3 to prevent the TiCN layer of the upper layer, thereby enabling the wear resistance and the To improve fracture resistance, thus extending the tool life of the cutting tool. The present invention was developed based on this discovery.
[0008] That is, the core of the present invention can be summarized as follows. [1] A coated cutting tool comprising: a substrate and a coating on a surface of the substrate formed coating layer, wherein: The coating layer consists of a lower layer, an intermediate layer, and an upper layer. The sequence starts from the substrate side; the lower layer has one or more Ti compound layers, which are a Ti compound of Ti and have an element of at least one kind that is selected from the group consisting of C, N, O and B; and the intermediate layer has a α-Al O layer which has α-Al O; and the 2 3 2 3 The upper layer has a TiCN layer containing TiCN; an average coating layer thickness of 5.0 µm or more and 30.0 µm or less is, and an average thickness of the top layer is 1.0 µm or more and 6.0 µm or less amounts; in a cross-section perpendicular to the surface of the substrate, a ratio of the grains with a side- or aspect ratio of 2 or more and 10 or less from the grains in the upper layer forming TiCN layer is 60 area percent or more and 95 area percent or less; and in the grains with an aspect ratio of 2 or more and 10 or less from the Grains in the TiCN layer forming the upper layer exhibit a misalignment A, fulfilling a condition that represented by the following formula (1): 40≤RSA1≤90 where in the formula RSA is a ratio (unit: area percent) of a cross-sectional area of grains, 1 which have a misalignment A of 0° or more and less than 10°, to a cross-sectional area of Grains that have a misalignment A of 0° or more and 45° or less, and which Misalignment A is an angle (unit: degrees) formed by a normal to the surface of the substrate and a normal to a (111) alignment of the grains of the TiCN layer in the upper layer is formed. [2] Coated cutting tool according to [1], wherein the RSA is 60% or more of the surface area and 90% of the surface area 1 or less. [3] Coated cutting tool according to [1] or [2], wherein a ratio of the cross-sectional area of the grains, which exhibit a misalignment A of 0° or more and less than 10°, a ratio of a cross-sectional area of the grains that exhibit a misalignment A of 10° or more and less than 20°, a ratio of Cross-sectional area of the grains exhibiting a misalignment A of 20° or more and less than 30°, and a ratio of the cross-sectional area of the grains, which a exhibit misalignment A of 30° or more and 45° or less, relative to the cross-sectional area of the grains, which Exhibit misalignment of 0 degrees or more and 45 degrees or less, respectively, by RSA, RSA, RSA and RSA 1 2 3 4 is specified where RSA is the largest value, and RSA is the second largest of RSA, RSA, RSA and RSA. 1 4 1 2 3 4 [4] Coated cutting tool according to any one of [1] to [3], wherein an average thickness of the The intermediate layer is 3.0 µm or more and 15.0 µm or less. [5] Coated cutting tool according to any one of [1] to [4], wherein an average thickness of the lower layer 3.0 µm or more and 15.0 µm or less. [6] Coated cutting tool according to any one of [1] to [5], wherein the lower layer is at least a layer that is selected from the group consisting of a TiN layer that has TiN, a TiC layer containing TiC, a TiCN layer containing TiCN, a TiCNO layer containing TiCNO, a TiON- A layer containing TiON, and a TiB layer containing TiB. 2 2 [7] Coated cutting tool according to [1] to [6], wherein the substrate is any material from a hard metal, a cermet, a ceramic or a sintered body made of cubic boron nitride. Advantageous effects of the invention
[0009] The present invention can provide a coated cutting tool which has an excellent It has wear resistance and fracture resistance, thus enabling an extended tool life. Brief description of the drawings Fig. 1 is a schematic view showing an example of a coated cutting tool according to the The present invention is shown. Description of the embodiments
[0010] One embodiment for carrying out the present invention (hereinafter simply referred to as “present invention”) The embodiment (referred to as "evolution") is described in detail below with reference to the drawings in the appendix, provided that appropriately described. However, the present invention is not limited to the embodiment described below. limited. Various modifications can be made to the present invention without altering the core of the to deviate from the invention. In the drawings, positional relationships, such as vertical and horizontal relationships, are based on the positional relationships shown in the drawings, unless otherwise specified. Furthermore, the The dimensional relationships of the drawings are not limited to those shown here.
[0011] The coated cutting tool of the present embodiment has a substrate and a surface on a A coating layer forms on the surface of the substrate. The coating layer has a lower layer, a The intermediate layer and an upper layer, in that order from the substrate side, consist of a middle layer and an upper layer. The lower layer has a or multiple Ti compound layers that have a Ti compound, wherein the Ti compound has Ti, and a An element of at least one type, selected from the group consisting of C, N, O, and B. The intermediate layer has an α-Al₂O₃ layer containing α-Al₂O₃; and the upper layer has a TiCN layer containing TiCN 2 3 2 3 contains. An average coating layer thickness is 5.0 µm or more and 30.0 µm or less, and The average thickness of the top layer is 1.0 µm or more and 6.0 µm or less. In a cross-section Perpendicular to the surface of the substrate, the ratio of grains has an aspect ratio of 2. or more and 10 or less from the grains in the TiCN layer forming the upper layer 60 area percent or more and 95 percent of the surface area or less; in the grains with an aspect ratio of 2 or more and 10 or less A misalignment A of the grains in the TiCN layer forming the upper layer fulfills a condition that is determined by The following formula (1) is represented: 40≤RSA1≤90 (in the formula, RSA is a ratio (unit: area percent) 1 a cross-sectional area of grains having a misalignment A of 0° or more and less than 10°, to a Cross-sectional area of grains that have a misalignment A of 0° or more and 45° or less, and which Misalignment A an angle (unit: degree) that passes through a normal to the surface of the substrate and a normal to an (111) orientation the grains of the TiCN layer are formed in the upper layer.)
[0012] The coated cutting tool of the present embodiment has the designs described above. This allows the wear resistance and fracture resistance of the coated cutting tool to be increased. improve; consequently, the tool lifespan can be extended. The factors for the improvements in the wear resistance and fracture resistance of the coated cutting tool of the present embodiment can be explained as follows. However, the present invention is in no way limited by the following. limited by the factors outlined. In other words, the coated cutting tool of the present invention exhibits First, as the lower layer of the coating layer, at least one Ti compound layer, which is a Ti compound consisting of Ti and an element of at least one kind selected from the group consisting of C, N, O and B. If the coated cutting tool of the present embodiment has such a lower layer between the substrate and the intermediate layer containing an α-Al O₂ layer containing α-aluminum oxide (α-Al O₂), 2 3 2 3 This results in improved wear resistance and adhesion. Furthermore, since the coated The cutting tool of the present embodiment has an upper layer comprising a TiCN layer as a The outer layer, with respect to the intermediate layer which has an α-Al₂O₃ layer, is the TiCN layer of the 2 3 The upper layer is in contact with the workpiece material in front of the α-Al₂O₃ layer. As a result, the coated surface enables... 2 3 The cutting tool of the present embodiment prevents crater wear in the α-Al O layer, 2 3 would be caused by something else, especially until the cutting temperature has risen. While the mechanism As has not been made clear here, the reason for the above restriction can be deduced to be that, with regard to hardness, At low temperatures, the hardness of the TiCN layer is higher than that of the α-Al₂O₃ layer. In the coated 2 3 The cutting tool of the present embodiment has a higher hardness in the upper layer because it contains the TiCN layer. This results in improved wear resistance. Furthermore, the coated cutting tool exhibits... In the present embodiment, the upper layer consists of TiCN grains having an aspect ratio of 2 or more and 10 or exhibit fewer. If the aspect ratio of the in the upper layer of the coated cutting tool of the In the present embodiment, the presence of 2 or more TiCN grains results in an effect of preventing the falling of Grains of the TiCN layer are obtained from the upper layer. Meanwhile, while the aspect ratio of the grains in the upper layer If the layer contains 10 or fewer TiCN grains, the cutting tool can be easily manufactured. Furthermore, if in the coated cutting tool of the present embodiment the ratio of the grains which a Aspect ratio of 2 or more and 10 or less of the grains of the TiCN layer forming the upper layer If 60 percent or more of the surface area is perpendicular to the substrate's surface in cross-section, an effect of the Preventing grains from the TiCN layer from falling off the upper layer is achieved. As a result, the The fracture resistance of the coated cutting tool of the present embodiment is further improved. However, if In the coated cutting tool of the present embodiment, the ratio of the grains, which have an aspect ratio of 2 or more and 10 or fewer from the grains of the TiCN layer forming the upper layer, 95 If the area is a percentage or less of the surface perpendicular to the substrate's surface, the cutting tool can simply are manufactured. Furthermore, the coated cutting tool of the present embodiment fulfills the requirements in which Grains with an aspect ratio of 2 or more and 10 or less from the grains in the upper layer TiCN layer misalignment A a condition represented by the following formula (1): 40≤RSA1≤90 (in In the formula, RSA is a ratio (unit: area percent) of a cross-sectional area of grains that exhibit misalignment. 1 A of 0° or more and less than 10° to a cross-sectional area of grains exhibiting a misalignment A of 0° or more than 45° or less, and the misalignment A is an angle (unit: degrees) formed by a normal to the Surface of the substrate and a normal to a (111) orientation of the grains of the TiCN layer in the upper layer is formed.)
[0013] If the RSA is 40 area percent or more, the wear resistance of the coated cutting tool will be 1 the present embodiment is further improved. Although the mechanism of this is not clear, it is assumed that assumed that in the case of the (111) orientation of a cubic crystal, since the structure is densely packed, the RSA 1 When the TiCN layer covers 40% or more of the surface area, it becomes dense and the hardness is improved, thereby increasing the The wear resistance of the coated cutting tool is improved. However, if the RSA is 90 percent of the surface area or 1 Since the amount of material required is less, the coated cutting tool of the present embodiment can be easily manufactured. Furthermore, if the average thickness of the top layer is 1.0 µm or more, the effect shown can be described as a result of the cutting tool of the present invention, which has the upper layer. However, if the If the average thickness of the top layer is 6.0 µm or less, the fracture strength is mainly due to The prevention of peeling of the coating layer is improved. Furthermore, in the coated Cutting tool of the present embodiment, in which the average thickness of the coating layer is 5.0 µm or more, improving wear resistance, and if the average thickness of the coating layer is 30.0 If the thickness is µm or less, the fracture strength is primarily due to the prevention of peeling. The coating layer is improved. The combination of the above designs enables the coated Cutting tool of the present embodiment, in that it has improved wear resistance and fracture resistance exhibits [something] and therefore it can be assumed that the tool life can be extended.
[0014] Fig. 1 is a schematic cross-sectional view showing an example of a coated cutting tool according to the This embodiment represents a coated cutting tool 6 with a substrate 1 and a A coating layer 5 is provided, which is arranged on a surface of the substrate 1, and a lower layer 2, a Intermediate layer 3 and an upper layer 4 are in this order from the substrate side in the Coating layer 5 laminated in one direction upwards.
[0015] A coated cutting tool according to the present embodiment has a substrate and a surface on a A coating layer forms on the surface of the substrate. Specific examples of types include... Coated cutting tools include a reversible cutting insert for milling or turning, a drill bit, and a Face milling cutter.
[0016] The substrate in the present embodiment is not particularly limited as long as it serves as a substrate for a Coated cutting tools can be used. Examples of such substrates include carbide, Cermet, ceramic, a sintered body made of cubic boron nitride, a diamond sintered body, and high-speed steel. Made of In the examples above, the substrate preferably comprises a hard metal, cermet, ceramic or a sintered body made of a cubic boron nitride, as this provides further excellent wear resistance and fracture strength and is suitable for use under the From the same perspective, the substrate preferably comprises a hard metal.
[0017] It should be emphasized that the surface of the substrate can be modified. For example, if the substrate is a If the hard metal is present, a β-free layer can form on its surface, and if the substrate is a If cerium is present, a hardened layer may form on its surface. The operation and effects the present invention will also be provided even if the substrate surface is modified in this way became.
[0018] The average thickness of the coating layer used in the present embodiment is 5.0 µm or more and 30.0 µm or less. Furthermore, the coated cutting tool of the present Embodiment in which the average thickness of the coating layer is 5.0 µm or more, which Improved wear resistance, and when the average thickness of the coating layer is 30.0 µm or less The fracture resistance is improved primarily due to the prevention of peeling of the coating layer. From the same perspective, the average thickness of the coating layer is preferably 8.0 µm or more and 25.0 µm or less, preferably 10.0 µm or more, 23.0 µm or less and even more preferably 11.5 µm or more and 22.5 µm or less. It should be emphasized that for the average thickness of a each layer and the average thickness of the entire coating layer in the coated cutting tool In the present embodiment, each such average thickness can be obtained by: measuring the thickness of each layer or the thickness of the entire coating layer of each of the cross-sectional areas at three or more positions in each layer or in the entire coating layer; and calculating the arithmetic Using the resulting measurements. lower layer
[0019] The lower layer used in the present embodiment has at least one or more Ti- Compound layers consisting of a Ti compound of Ti and an element of at least one type selected from of the group consisting of C, N, O and B. If the coated cutting tool of the present An embodiment has such a lower layer between a substrate and an intermediate layer which has an Σ- The presence of an aluminium oxide (α-Al O -) layer leads to improved wear resistance and adhesion. 2 3
[0020] Examples of Ti compound layers include a TiC layer containing TiC, a TiN layer containing TiN, a TiCN layer containing TiCN, a TiCO layer containing TiCO, a TiCNO layer containing TiCNO, a TiON- A layer containing TiON, and a TiB layer containing TiB. 2 2
[0021] The lower layer can consist of a single layer or multiple layers (for example, two or three layers) The lower layer is preferably formed by several layers, preferably by two. or three layers are formed and is further preferably formed by three layers. From the point of view of a To further improve wear resistance and adhesion, the lower layer preferably has a layer of at least one type selected from the group consisting of a TiN layer made of TiN is composed of, a TiC layer composed of TiC, a TiCN layer composed of TiCN is a TiCNO layer composed of TiCNO, a TiON layer composed of TiON, and a TiB layer composed of TiB. In the coated cutting tool of the present case 2 2 In an embodiment where at least one layer of the lower layer is a TiCN layer, this indicates the tendency to that the wear resistance is further improved. In the coated cutting tool of the present embodiment in which at least one layer of the lower layer is a TiN layer, and in which such a TiN- The formation of a layer on the surface of a substrate indicates a tendency for adhesion to be further improved. will be. In the coated cutting tool of the present embodiment, if at least one layer of the The lower layer is a TiCNO layer, and when such a TiCNO layer forms to bond with the intermediate layer, The fact that an Σ-Al O layer comes into contact indicates a tendency for adhesion to be further improved. 2 3 If the bottom layer is formed by three layers: can it be a TiC layer or a TiN layer, which serves as a first layer? The layer functions as a surface of the substrate; a TiCN layer that acts as a second layer, can be formed on a surface of the first layer; and a TiCNO layer or a TiCO layer, which is considered a The third layer can be located on a surface of the second layer. This is particularly relevant to the lower layer. Layer: a TiN layer, acting as a first layer, can be formed on a surface of the substrate; a A TiCN layer, acting as a second layer, can be formed on a surface of the first layer; and a TiCNO- A layer that functions as a third layer can be formed on a surface of the second layer.
[0022] The average thickness of the coating layer used in the present embodiment is preferably 3.0 µm or more and 15.0 µm or less. If the average thickness of the lower layer is 3.0 µm or more, the wear resistance of the coated cutting tool of the present type tends to be The embodiment can be further improved. However, if the average thickness of the lower layer is 15.0 µm or less, the fracture strength of the coated cutting tool of the present embodiment tends to to be improved, mainly due to the prevention of peeling of the coating layer. Under the From the same perspective, the average thickness of the TiCN layer is preferably 4.0 µm or more and 13.0 µm or less, and even more preferably 4.5 µm or more and 10.5 µm or less.
[0023] From the perspective of further improving wear resistance and fracture strength, the Average thickness of the TiC layer or the TiN layer preferably 0.05 µm or more and 1.0 µm or less. From the same perspective, the average thickness of the TiC or TiN layer is preferably 0.10 µm. or more and 0.50 µm or less, and more preferably 0.15 µm or more and 0.30 µm or less.
[0024] From the perspective of further improving wear resistance and fracture strength, the Average thickness of the TiCN layer preferably 3.0 µm or more and 12.0 µm or less. Under the same From this perspective, the average thickness of the TiCN layer is preferably 3.5 µm or more and 11.0 µm. or less, and even more preferably 4.0 µm or more and 10.0 µm or less.
[0025] From the perspective of further improving wear resistance and fracture strength, the Average thickness of the TiCNO layer or the TiCO layer preferably 0.1 µm or more and 1.0 µm or less. From the same perspective, the average thickness of the TiCNO layer or the TiCO layer is preferably 0.15 µm or more and 0.70 µm or less, and even more preferably 0.20 µm or more and 0.50 µm or fewer.
[0026] The Ti compound layer consists of a Ti compound of Ti and an element of at least one type, which It is selected from the group consisting of C, N, O, and B. However, such a Ti compound layer can be very small. The quantity of components differs from the elements above, as long as they affect functionality. and provides for the effects of the lower layer. Intermediate shift
[0027] The intermediate layer used in the present embodiment has an α-Al O₂ layer. 2 3
[0028] The average thickness of the intermediate layer used in the present embodiment is preferably 3.0 µm or more and 15.0 µm or less. If the average thickness of the α-Al₂O₃ layer 2 3 If the intermediate layer has a thickness of 3.0 µm or more, the crater resistance at the rake face of the coated surface tends to be higher. The cutting tool of the present embodiment is to be further improved. If the average thickness The intermediate layer containing the α-Al₂O₃ layer is 15.0 µm or less, and peeling of the 2 3 The coating layer is further suppressed, and the fracture resistance of the coated cutting tool tends to decrease further. to be improved. From the same perspective, the average thickness of the Intermediate layer preferably 4.0 µm or more and 13.0 µm or less, and even more preferably 5.0 µm or more and 10.0 µm or less.
[0029] The intermediate layer can contain α-aluminum oxide (α-Al₂O₃), or can contain other components besides α- 2 3 Whether or not they contain aluminium oxide (α-Al₂O₃), as long as they maintain the operational capability and effects of the present 2 3 The invention provides for. upper layer
[0030] The upper layer used in the present embodiment has a TiCN layer. In the coated The cutting tool of the present embodiment leads the upper layer, which has the TiCN layer, to a high Hardness, which leads to improved wear resistance. Furthermore, the coated cutting tool functions as a... In the present embodiment, the upper layer comprising the TiCN layer is a layer located outside the An intermediate layer exists which has an α-Al₂O₃ layer. Since the coated cutting tool of the present type... 2 3 In this embodiment, the upper layer having the TiCN layer is considered an outer layer with respect to which the Σ-Al O - 2 3 The TiCN layer of the upper layer, which functions as an intermediate layer, is present in the workpiece material. the α-Al₂O₃ layer is in contact. Thus, the coated cutting tool of the present embodiment enables 2 3 the prevention of crater wear of the α-Al₂O₃ layer, which would otherwise be caused, until the 2 3 The cutting temperature was increased.
[0031] Furthermore, the upper layer used in the present embodiment has TiCN grains which exhibit an aspect ratio of 2 or more and 10 or less. If the coated cutting tool... In the present embodiment, if the aspect ratio of the TiCN grains is 2 or more, an effect of suppression may occur. the falling of grains of the TiCN layer of the upper layer are obtained. Meanwhile, while the aspect ratio If the number of TiCN grains contained in the upper layer is 10 or less, the coated cutting tool can The present embodiment can be easily manufactured. Furthermore, the coated cutting tool features the In the present embodiment, in a cross-section perpendicular to the surface of the substrate, a ratio of the grains with an aspect ratio of 2 or more and 10 or less from the grains in the TiCN- forming the upper layer Layer thickness of 60% or more and 95% or less. If the coated cutting tool... In the present embodiment, the ratio of the grains having an aspect ratio of 2 or more and 10 or less in the TiCN layer forming the upper layer has 60 percent or more of the surface area in the cross-section perpendicular to the surface of the substrate, an effect of preventing the detachment of grains from the TiCN layer of the upper layer can be obtained. The fracture toughness of the coated cutting tool of the present embodiment will be determined. further improved. However, if the ratio of grains having an aspect ratio of 2 or more and 10 or less in the TiCN layer forming the upper layer, exhibiting 95 percent or less of the surface area in the cross-section perpendicular to the Since the surface of the substrate is [unclear], the cutting tool of the present embodiment can be easily manufactured. From the same perspective, in a cross-section perpendicular to the surface of the substrate, the ratio of Grains with an aspect ratio of 2 or more and 10 or less in the upper layer forming TiCN layer of preferred 60 area percent or more and 93 area percent or less; and furthermore preferred 60 percent or more of the area and 92 percent or less.
[0032] In the coated cutting tool of the present embodiment, the grains are filled with a Aspect ratio of 2 or more and 10 or less of the grains in the TiCN layer forming the upper layer a misalignment A a condition represented by the following formula (1): 40≤RSA1≤90 (in the formula is RSA is a ratio (unit: area percent) of a cross-sectional area of grains exhibiting a misalignment A of 0° or 1 exhibiting more and less than 10°, to a cross-sectional area of grains exhibiting a misalignment A of 0° or more and exhibit 45° or less, and the misalignment A is an angle (unit: degrees) formed by a normal to Surface of the substrate and a normal to a (111) orientation of the grains of the TiCN layer in the upper layer is trained.)
[0033] If the RSA is 40 area percent or more, the wear resistance of the coated cutting tool will be 1 the present embodiment is further improved. Although the mechanism of this is not clear, it is assumed that assumed that in the case of the (111) orientation of a cubic crystal, since the orientation is densely packed, wherein the When the RSA is 40% or more, the TiCN layer becomes dense and the hardness is improved, thereby increasing the 1 The wear resistance of the coated cutting tool is improved. However, if the RSA is 90 percent of the surface area or 1 If the value is less, the coated cutting tool of the present embodiment can be easily manufactured. From the same perspective, the RSA is preferably 50 percent or more of the area and 90 percent or 1 less, and even more preferred are 60 percent or more of the area and 90 percent or less.
[0034] Furthermore, in the coated cutting tool of the present embodiment, it is preferred if the Ratio of the cross-sectional area of the grains that have a misalignment A of 0° or more and less than 10°, a Ratio of the cross-sectional area of the grains that have a misalignment A of 10° or more and less than 20°, a ratio of the cross-sectional area of the grains that have a misalignment A of 20° or more and less than 30°, and a ratio of a cross-sectional area of the grains exhibiting a misalignment A of 30° or more and 45° or less have, to a cross-sectional area to grains that have a misalignment A of 0° or more and 45° or less, each is specified by RSA, RSA, RSA and RSA, and preferably RSA is the largest value, and RSA is the 1 2 3 4 1 4 The second largest is RSA, RSA, RSA, and RSA. If RSA is the largest and RSA is the second largest, the 1 2 3 4 1 4 The wear resistance of the coated cutting tool of the present embodiment is to be further improved. will. The mechanism behind this is unclear, but it is assumed that if the RSA is the second largest, 4 The ratio of TiCN grains with a misalignment A tends to be higher, with those of TiCN grains having a 0-degree orientation. have grown to an angle of misalignment A of 0° or more and less than 10°, so that the The wear resistance of the coated cutting tool tends to be further improved. However, if the RSA, being the second largest, tends to have a ratio of TiCN grains with a misalignment A, which is more towards the 10-degree side. 2 from the TiCN grains with a misalignment A of 0° or more and less than 10°, in addition to increase. Furthermore, if the RSA is the second largest, the ratio of TiCN grains tends to increase with a 3 Misalignment A, which is more towards the 10-degree side of the TiCN grains with a misalignment A of 0° or more and have grown by less than 10°, to increase. It is assumed that this difference the The wear resistance of the coated cutting tool is affected.
[0035] Furthermore, in the coated cutting tool of the present embodiment, the average Top layer thickness 1.0 µm or more and 6.0 µm or less. If the average top layer thickness 1.0 µm or more, the effect shown can be attributed to the cutting tool of the present invention, which the upper layer is obtained. However, if the average thickness of the upper layer is 6.0 µm or If the value is less, the breaking strength is mainly due to the prevention of peeling. The coating layer has improved. From the same perspective, the average thickness of the Intermediate layer preferably 1.5 µm or more and 5.9 µm or less, and even more preferably 2.0 µm or more and 5.8 µm or less.
[0036] In the present embodiment, the ratio of the grains, which have an aspect ratio of 2 or more and 10 or fewer grains of the TiCN layer forming the upper layer have, by observing the cross-sectional structure the upper layer containing the TiCN layer is determined using an electron backscatter diffraction device (EBSD). are, which are in a commercially available field emission scanning electron microscope (FE-SEM) or a The transmission electron microscope (TEM) is integrated. In particular, the cross-section of the upper layer, which contains the TiCN- layer consisting of cross-sections perpendicular to the surface of the substrate in the coated cutting tool, mirror-polished, and the resulting mirror-polished surface is used as the cross-sectional structure. The process of Mirror polishing of the cross-section of the upper layer containing the TiCN layer is not particularly limited and Examples include a polishing process using a diamond paste and / or colloidal silicon dioxide and Ion milling. A sample exhibiting the cross-sectional structure of the coated cutting tool is analyzed in FE-SEM. The cross-sectional structure of the sample is determined and the cross-sectional structure is determined using an electron beam with an accelerating voltage of irradiated with 15 kV and an irradiation current of 1.0 nA at an angle of incidence of 70°. It is preferred that the Cross-sectional structure in the upper layer, which has the TiCN layer of the coated cutting tool, by means of EBSD in the range of the average thickness of the upper layer, which has the TiCN layer × 50 µm, and the To measure a step size of 0.1 µm. At this point, a limit is reached that has a misalignment of 5° or more. a crystal grain boundary is considered, and an area surrounded by the crystal grain boundary is used as a grain. Here, the crystal grain size refers to a crystal grain size in a direction perpendicular to the film thickness direction. Coating layer. The aspect ratio is a value obtained by determining the crystal grain size of the grain in the Foil thickness direction of the coating layer due to the crystal grain size of the grain in the direction perpendicular to the The film thickness direction is divided. At this point, image analysis software can be used if the The crystal grain size is obtained from the cross-sectional structure of the upper layer containing the TiCN layer. Crystal grain size of the upper layer, which is the TiCN layer in the range of the average thickness of the upper layer The area of the TiCN layer, which has a thickness of 50 µm, is measured, and the aspect ratio of all grains can be determined from the Crystal grain size can be obtained in every direction. Here, assuming the range of average Thickness of the upper layer, which has the TiCN layer × 50 µm, is 100 area percent, the ratio of the The area covered is calculated for TiCN grains that have an aspect ratio of 2 or more and 10 or less.
[0037] In the present embodiment, RSA, RSA, RSA and RSA can be obtained by the following method 1 2 3 4 will be. In the grains that have an aspect ratio of 2 or more and 10 or less from the grains of the upper The sum (RSA) of the cross-sectional areas of the grains, which form a layer-forming TiCN layer, is determined by the layer-forming TiCN layer. Total Misalignment A of the angle formed between the normal to the surface of the substrate, and the Normals to the (111) alignment of the grains of the TiCN layer in the upper layer of 0° or more and 45° or less, taken as 100 area percent, a ratio (area percent) of the sum of the cross-sectional areas of the grains, which A misalignment A of 0° or more and 10° or less to the RSA can be determined, and this Total The ratio can be used as the RSA. Once the RSA (area percent) is obtained, the cross-sectional area can be calculated. 1 of each grain by means of, for example, an electron backscatter diffraction device (EBSD) located in a scanning electron microscope (SEM) or field emission scanning electron microscope (FE-SEM) or similar It is integrated and can be measured. In EBSD, the crystal orientation of each crystal within the grains is determined. The cross-sectional area of the grain with the specified crystal orientation is divided into one of the subdivisions, for example, The grains are classified at 5° intervals, and the cross-sectional areas of the grains in each subdivision are preserved. The following, for example, will yield a sum of the cross-sectional areas of the grains for the following subdivisions: a subdivision of 0° or more and less than 10°, a subdivision of 10° or more and less than 20°, a Subdivision of 20° or more and less than 30°, and a subdivision of 30° or more to 45° or less, a Ratio of the cross-sectional areas of the grains for each of the subdivisions to the RSA (100 area percent) is Total obtained, and the resulting ratios are used as RSA , RSA , RSA and RSA in the order above. 1 2 3 4
[0038] The upper layer may contain TiCN and may or may not contain components that differ from TiCN They may differ, as long as they provide for the operational capability and the effects of the present invention. Method for forming the coating layer
[0039] In the coated cutting tool of the present embodiment, each of the layers that the Forming a coating layer, created by chemical vapor deposition or physical vapor deposition Specific examples of a method for forming the layers of the coating layer are shown in the The following procedures are described. However, the process of layer formation is not limited to this. Chemical vapor separation
[0040] For example, a Ti compound layer comprising a Ti nitride layer (hereinafter also referred to as “TiN- layer (referred to as "layer"), are formed by chemical vapor deposition with a raw material composition of TiCl₂: from 5.0 mol% or more to 10.0 mol% or less, N₂: from 20 mol% or more to 60 mol% or less, and H₂ 4 2 2 : the equilibrium, a temperature of 850 °C or higher to 950 °C or lower and a pressure of 300 hPa or higher up to 400 hPa or lower.
[0041] A Ti compound layer comprising a Ti carbide layer (hereinafter also referred to as the ‘TiC layer’) (designated), can be formed by chemical vapor deposition with a raw material composition of TiCl; 4 from 1.5 mol% or more to 3.5 mol% or less, CH₄: from 3.5 mol% or more to 5.5 mol% or less, and H₂: 4 2 the equilibrium of a temperature of 950°C or higher to 1050°C or lower and a pressure of 70 hPa or higher to 80 hPa or lower.
[0042] A Ti compound layer comprising a Ti carbonitride layer (hereinafter also referred to as the ‘TiCN layer’) (designated), can be formed by chemical vapor deposition with a raw material composition of TiCl: 4 from 5.0 mol% or more to 7.0 mol% or less, CH₄CN: from 0.5 mol% or more to 1.5 mol% or less, and H₂: 3 2 the equilibrium of a temperature of 800°C or higher to 900°C or lower and a pressure of 60 hPa or higher to 80 hPa or lower.
[0043] A Ti compound layer comprising a Ti oxycarbonitride layer (hereinafter also referred to as the ‘TiCNO layer’) (designated), can be formed by chemical vapor deposition with a raw material composition of TiCl; 4 from 3.0 mol% or more to 4.0 mol% or less, CO: from 0.5 mol% or more to 1.0 mol% or less, N: from 30 2 mol% or more to 40 mol% or less, and H: the equilibrium of a temperature of 950°C or higher to 1050°C 2 °C or lower and a pressure of 50 hPa or higher to 150 hPa or lower.
[0044] A Ti compound layer comprising a Ti carbide layer (hereinafter also referred to as the ‘TiCO layer’) (designated), can be formed by chemical vapor deposition with a raw material composition of TiCl: 4 from 1.0 mol% or more to 2.0 mol% or less, CO: from 2.0 mol% or more to 3.0 mol% or less, and H: the 2 Equilibrium of a temperature of 950°C or higher to 1050°C or lower and a pressure of 50 hPa or higher down to 150 hPa or lower.
[0045] An intermediate layer comprising an α-Al O layer (hereinafter referred to simply as an ‘Al O’ layer) 2 3 2 3 (designated), can be obtained, for example, by the procedure outlined below.
[0046] First, a lower layer comprising one or more Ti compound layers is deposited on a surface of a Substrates are formed. Next, a surface layer is formed from such layers, which is attached to the substrate. The furthest away is oxidized. Afterwards, an intermediate layer, which has an α-Al₂O₃ layer, forms on the surface. 2 3 the layer that is furthest from the substrate.
[0047] In particular, the oxidation of the surface of the layer furthest from the substrate, carried out under conditions of a gas composition of CO; from 0.3 mol% or more up to 1.0 mol% or 2 less and H: the equilibrium of a temperature of 950°C or higher to 1050°C or lower and a pressure 2 from 50 hPa or higher to 70 hPa or lower. Here, the oxidation processing time is preferably 1 minute or more to 3 minutes or less (oxidation step).
[0048] The α-Al₂O₃ layer is then formed by chemical vapor deposition using a 2 3 Raw material gas composition of AlCl₃: from 2.0 mol% or more to 5.0 mol% or less, CO: from 2.5 mol% or 3 2 more than 4.0 mol% or less, HCI: from 2.0 mol% or more to 3.0 mol% or less, HS: from 0.3 mol% or more 2 up to 0.40 mol% or less, and H: the equilibrium at a temperature of 950°C 2 or higher to 1,050°C or lower and a pressure of 60 hPa or higher to 80 hPa or lower (a (Separation step).
[0049] Furthermore, an upper layer comprising a Ti carbonitride layer (hereinafter referred to as a ‘TiCN layer’) (designated), formed on a surface of the α-Al O layer. 2 3
[0050] A TiCN layer can be formed by chemical vapor deposition at a temperature of 900°C to 980°C and a pressure of 60 hPa to 80 hPa using a raw material composition comprising TiCl₂ : 6.0 mol% 4 up to 10.0 mol%, CH₄CN: 0.5 mol% to 1.5 mol%, N₂: 10.0 mol% to 30.0 mol% and H₂: the equilibrium (formation step) 3 2 2 an upper layer).
[0051] To determine the ratio of grains having an aspect ratio of 2 or more and 10 or less from the upper The ability to define the temperature in the layer-forming TiCN layer grains within a specific area can be achieved by controlling the temperature in the The formation step of the upper layer can be controlled, or CH₄CN can be used instead of conventional CH₄ as a raw material. 3 4 can be used, and the ratio of CH₄CN and / or TiCl in the raw material composition can be controlled. 3 4 The aspect ratio of the TiCN grains is increased, in particular, by increasing the temperature during the formation step of the The upper layer is reduced, or the ratio of TiCl in the raw material composition is increased. 4 Consequently, it is possible to adjust the ratio of TiCN grains to an aspect ratio of 2 or more or 10 or less. to increase. Furthermore, the aspect ratio of the TiCN grains is also increased by increasing the ratio of TiCl to CH₄CN. 4 3 (TiCl₂ / CH₄CN) in the raw material composition is increased during the formation step of the upper layer. Consequently, it 4 3 It is possible to increase the ratio of TiCN grains with an aspect ratio of 2 or more or 10 or less. However, increasing the temperature during the formation step of the upper layer or increasing the ratio of The presence of CH₄CN in the raw material composition reduces the aspect ratio of the TiCN grains. Consequently, it is possible to 3 to reduce the ratio of TiCN globules with an aspect ratio of 2 or more or 10 or less.
[0052] Furthermore, to define RSA in a specific area during the upper layer formation step, the 1 Temperature and / or pressure can be controlled, or CH₄CN can be used instead of conventional CH₄ as a raw material. 3 4 can be used, and the ratio of CH₄, CN, and / or N in the raw material composition can be controlled. 3 2 RSA can be reduced, in particular, by lowering the temperature during the formation step of the upper layer. 1 or the pressure is increased. However, RSA can be increased by changing the ratio of CH₄, CN₂ and / or N₂ in the 1 3 2 The raw material composition is increased during the training step of the upper layer.
[0053] The thickness of each layer in the coating layer of the coated cutting tool of the present The embodiment can be measured by creating a cross-sectional structure of the coated cutting tool using an optical microscope, a scanning electron microscope (SEM), a field emission scanning electron microscope (FE- REM) or similar. It should be emphasized that for the average thickness of each layer in the The coated cutting tool of the present embodiment can achieve such an average thickness. can be done by: measuring the thickness of each layer at three or more positions close to 50 µm from the edge, in Direction of the center point of the rake face of the coated cutting tool; and calculation of the arithmetic Average of the resulting measurements. Furthermore, the composition of each layer in the coating layer can be determined. of the coated cutting tool of the present embodiment from a cross-sectional structure of the coated Cutting tool using an energy-dispersive X-ray spectroscope (EDS), a wavelength-dispersive X-ray spectroscopy (WDS) or similar instruments can be used.
[0054] The coated cutting tool of the present embodiment can, due to its excellent Fracture strength and wear resistance are considered capable of controlling the effect of the extension of the to achieve a longer tool lifespan than is possible with the prior art. This is particularly relevant in coated applications. The cutting tool of the present embodiment prevents the falling of grains from the TiCN layer of the upper layer below. such conditions that a load is applied which leads to a high feed rate and a low cutting load, prevented, which is obviously the reason why the wear resistance and also the fracture resistance are improved. This can result in the effect of extending the tool life compared to conventional methods. can be. However, the factor contributing to such an extension of tool life is not limited to this. Examples
[0055] Although the present invention is described in detail below with reference to examples, the The present invention is not limited to such examples.
[0056] The substrate used was a hard metal comprising a composition of 88.7WC-8.1Co-1.5TiN-1.4NbC-0.3Cr C 3 2 (the above figures are mass percentages) and machined to a form of CNMG120412, and a hard metal, exhibiting a composition of 89.9WC-7.1Co-1.5TiN-1.4NbC-0.1Cr C (the above numbers are 3 2 Mass percentages) and processed into an application form of CNMG120412. The edges of these substrates The substrates were subjected to round honing using a SiC brush, and the surfaces were then washed. Examples of the invention 1 to 12 and comparative examples 1 to 8
[0057] After the substrate surface was washed, a coating layer was applied by chemical means Vapor separation was formed. First, the substrate was placed in an externally heatable chemical bath. A vapor separation device was used and a lower layer, the composition of which is shown in Table 2, was applied to the substrate surface in the order of a first layer, a second layer, and a third layer. trained to achieve the average thickness shown in Table 2 among those shown in Table 1 to have raw material composition, temperature, and pressure conditions. Then the surface of the lower Layer oxidized for 1 minute under the following conditions: a gas composition of CO : 0.5 mol% and H : 99.5 mol%, 2 2 at a temperature of 1,000°C and a pressure of 60 hPa. Then, next, an Σ-aluminum oxide was added. an intermediate layer is formed on the oxidized surface of the lower layer in order to achieve the properties shown in Table 2 The average thickness shown under the raw material composition, temperature and to have pressure conditions. Finally, an upper layer, the composition of which is shown in Table 2, was applied to the surface of the intermediate layer is formed in order to achieve the average thickness shown in Table 2 under the in Table 3 shows the raw material composition, temperature, and pressure conditions. In the following... The coated cutting tools of samples 1 to 12 of the invention and of comparison samples 1 to 8 were obtained. [Table 1] Composition of temperature, pressure, raw material composition each layer (°C) (hPa) (mol-%) TiCl: 7.5%, N: 40.0%, H: 52.5% Lower layer TiN 900 350 4 2 2 TiCl₂: 2.4%, CH₄: 4.6%, H₂: 4 4 2 TiC 1000 75 93.0% TiCl₂: 6.0%, CH₄CN: 1.0%, H₂: 4 3 2 TiCN 850 70 93.0% TiCl₂: 3.5%, CO: 0.7%, N: 4 2 TiCNO 1000 100 35.5%, H: 60.3% 2 AlCl: 2.5%, CO: 3.0%, HCl: 2.3%, H 3 2 2 -Al O Intermediate shift 1000 70 2 3 S: 0.35%, H: 91.85% 2 [Table 2] Sample number coating layer Average thickness of the entire Bottom layer Intermediate layer Top layer coating layer (µm) thickness of the entire First shift Second shift Third shift lower layer Average Average Average Composition Thickness (µm) Thickness (µm) Thickness (µm) Sample 1 of the TiN 0.2 TiCN 6.0 TiCNO 0.3 invention Sample 2 of the TiN 0.2 TiCN 6.0 TiCNO 0.3 invention Sample 3 of the TiN 0.2 TiCN 6.0 TiCNO 0.3 invention Sample 4 of the TiN 0.2 TiCN 6.0 TiCNO 0.3 invention Sample 5 of the TiC 0.2 TiCN 6.0 TiCNO 0.3 invention Sample 6 of the TiN 0.2 TiCN 6.0 TiCNO 0.3 invention Sample 7 of the TiN 0.2 TiCN 6.0 TiCNO 0.3 invention Sample 8 of the TiN 0.2 TiCN 8.0 TiCNO 0.3 invention Sample 9 of the TiN 0.2 TiCN 6.0 TiCNO 0.3 invention Sample 10 of the invention Sample 11 of the TiN 0.2 TiCN 4.0 TiCNO 0.3 invention Sample 12 of the TiN 0.2 TiCN 10.0 TiCNO 0.3 invention Comparison sample 1 TiN 0.2 TiCN 6.0 TiCNO 0.3 Comparison sample 2 TiN 0.2 TiCN 6.0 TiCNO 0.3 Comparison sample 3 TiN 0.2 TiCN 15.0 TiCNO 0.3 Comparison sample 4 TiN 0.2 TiCN 6.0 TiCNO 0.3 Comparison sample 5 TiN 0.2 TiCN 6.0 TiCNO 0.3 Comparison sample 6 TiN 0.2 TiCN 6.0 TiCNO 0.3 Comparison sample 8 TiN 0.2 TiCN 6.0 TiCNO 0.3 [Table 3] upper layer TiCl / CH CN Temperature (°C) Pressure (hPa) Raw material composition (mol-%) 4 3 TiCl CH CN CH NH 4 3 4 2 2 Sample 1 of the invention 950 70 8.0 1.0 0.0 15.0 76.0 8.0 Sample 2 of the invention 950 70 8.0 1.0 0.0 10.0 81.0 8.0 Sample 3 of the invention 900 70 10.0 0.8 0.0 15.0 74.2 12.5 Sample 4 of the invention 980 70 8.0 1.0 0.0 15.0 76.0 8.0 Sample 5 of the invention 950 70 8.0 1.0 0.0 30.0 61.0 8.0 Sample 6 of the invention 900 70 9.0 1.0 0.0 15.0 75.0 9.0 Sample 7 of the invention 900 70 9.0 1.0 0.0 15.0 75.0 9.0 Sample 8 of the invention 950 70 9.0 1.0 0.0 30.0 60.0 9.0 Sample 9 of the invention 950 70 8.0 1.0 0.0 10.0 81.0 8.0 Sample 10 of the invention 950 70 6.0 0.5 0.0 10.0 83.5 12.0 Sample 11 of the invention 950 70 9.0 1.5 0.0 15.0 74.5 6.0 Sample 12 of the invention 950 70 8.0 1.0 0.0 30.0 61.0 8.0 Comparison sample 1 1050 70 8.0 0.0 1.5 5.0 85.5 - Comparison sample 2 950 150 8.0 1.0 0.0 0.0 91.0 8.0 Comparison sample 3 950 70 9.0 1.0 0.0 30.0 60.0 9.0 Comparison sample 4 950 70 6.0 0.0 0.0 30.0 64.0 - Comparison sample 5 900 70 9.0 1.0 0.0 15.0 75.0 9.0 Comparison sample 6 950 200 8.0 0.0 1.5 5.0 85.5 - Comparison sample 7 1000 70 8.0 1.0 1.5 5.0 84.5 8.0 Comparison sample 8 1000 70 8.0 1.0 1.5 5.0 84.5 8.0 Average thickness of each layer
[0058] The average thickness of each of the layers of each of the samples obtained was determined as follows The average thickness was obtained using an FE-SEM by measuring the... Thickness of each layer at each of the three positions on the cross-sectional area near the position 50 µm from the edge of the coated cutting tool in the direction of the center of its rake face; and calculating the arithmetic Using the resulting measurements. The measurement results are shown in Table 2. Composition of each layer
[0059] Using an EDS, the composition of each layer of the obtained samples was determined from the cross-sectional area near the position of approximately 50 µm from the edge of the coated cutting tool towards the center of the The rake area was measured. The measurement results are shown in Table 2. ratio of area X
[0060] In the sample obtained, the ratio of grains with an aspect ratio of 2 or more and 10 or less from the grains of the TiCN layer forming the upper layer using an EBSD integrated in the FE-SEM measured. In particular, the cross-section of the upper layer, which is the TiCN layer, is measured from the cross-sections perpendicular to each other. to the surface of the substrate in the sample, mirror-polished with a diamond paste and then with collodial Silicon dioxide was end-polished, and the resulting mirror-polished surface was defined as the cross-sectional structure of the coated Cutting tool used. The sample, which exhibits the cross-sectional structure of the coated cutting tool, was in FE-SEM and the cross-sectional structure of the sample was determined with an electron beam with a The device was irradiated with an accelerating voltage of 15 kV and an irradiation current of 1.0 nA at an angle of incidence of 70°. The cross-sectional structure in the upper layer, which features the TiCN layer of the coated cutting tool, was by EBSD in the measurement range of the average thickness of the upper layer, which has the TiCN layer × 50 µm, and The step size was measured at 0.1 µm. At this point, a limit was reached that allowed for a misalignment of 5° or more. has, is considered a crystal grain boundary, and an area surrounded by the crystal grain boundary is called a grain used. Here, the crystal grain size refers to a crystal grain size in a direction perpendicular to the film thickness direction. the coating layer. The aspect ratio was obtained by determining the crystal grain size of the grain in the Foil thickness direction of the coating layer due to the crystal grain size of the grain in the direction perpendicular to the The film thickness direction is divided. At this point, image analysis software was being used when the The crystal grain size is obtained from the cross-sectional structure of the upper layer containing the TiCN layer. Crystal grain size of the upper layer, which is the TiCN layer in the range of the average thickness of the upper layer The area of the TiCN layer, measuring 50 µm, was measured, and the aspect ratio of all grains was determined from the... Crystal grain size obtained in every direction. Here, it was assumed that the range of average thickness of the upper layer, which has the TiCN layer × 50 µ, was 100 area percent, the ratio of the TiCN- The area covered is calculated based on grains that have an aspect ratio of 2 or more and 10 or less. The results are shown in Fig. 4. RSA, RSA, RSA and RSA 1 2 3 4
[0061] RSA, RSA, RSA and RSA in the obtained samples are calculated by the following procedure. In particular 1 2 3 4 was in the grains that have an aspect ratio of 2 or more and 10 or less from the grains of the upper layer exhibiting a TiCN-forming layer, the sum (RSA) of the areas of the cross-sections of the grains that show a misalignment Total A of the angle that is between the normal to the surface of the substrate and the normal to the (111) orientation the grains of the TiCN layer in the upper layer are formed at angles of 0° or more and 45° or less, the cross-sections, The areas perpendicular to the surface of the substrate in the sample, taken as 100 area percent, represent a ratio (Area percent) of the sum of the areas of the cross-sectional areas of the grains that have a misalignment A of 0° or more and 10° or less than the RSA, was determined and this ratio was used as the RSA. To obtain the Total 1 RSA (area percent) was calculated by measuring the cross-sectional area of each grain using an EBSD integrated into FE-SEM. In the EBSD, the crystal orientation of each grain crystal was specified, as well as the cross-sectional area of the grain. The specified crystal orientation is classified into one of the subdivisions at, for example, 5° intervals, and The cross-sectional areas of the grains in each subdivision were obtained. Then the sum of the Cross-sectional areas of the grains for each Subdivision consisting of a subdivision of 0° or more and less than 10°, a subdivision of 10° or more and less than 20°, a subdivision of 20° or more and less than 30°, and a subdivision of 30° or more up to 45° or less obtained, a ratio of the cross-sectional areas of the grains for each of the subdivisions to RSA (100 Total (area percent) was obtained, and the resulting ratios were given as RSA, RSA, RSA and RSA in the above. 1 2 3 4 The sequence used is shown in Table 4. The above measurement results are presented in Table 4. In addition, the Cross-sectional area of the grains of the top layer in the measurement range of EBSD as the total sum of the pixels in The area is used as the equivalent. That is, the sum of the cross-sectional areas of the grains in each subdivision for each A 10° or 15° inclination based on a misalignment of the grains in each layer was achieved by summing the pixels that were occupied by the cross-section according to each subdivision and the The total was converted into an area. [Table 4] Sample number, top layer ratio of the grains with a RSA (100 Total Aspect ratio of 2 or more and 10 or (percent of area) less (percentage of area) RSA RSA RSA RSA 2 3 4 10 degrees or more, 20 degrees or more, 30 degrees or more 0 degrees or more and less than 10 degrees and less than 20 and less than 30 and 45 degrees or Degrees less Sample 1 of the invention 79 70 3 3 24 Sample 2 of the invention 72 41 8 24 27 Sample 3 of the invention 89 52 20 10 18 Sample 4 of the invention 60 73 8 6 13 Sample 5 of the invention 68 85 3 1 11 Sample 6 of the invention 88 63 13 9 15 Sample 7 of the invention 92 77 6 3 14 Sample 8 of the invention 85 82 6 2 10 Sample 9 of the invention 80 42 26 15 17 Sample 10 of the invention 85 40 23 16 21 Sample 11 of the invention 64 47 19 15 19 Sample 12 of the invention 71 88 2 1 9 Comparison sample 1 51 68 12 10 10 Comparison sample 2 70 28 30 25 17 Comparison sample 3 86 80 5 3 12 Comparison sample 4 28 45 14 15 26 Comparison sample 5 90 75 6 4 15 Comparison sample 7 75 32 26 15 27 Comparison sample 8 72 25 15 18 42
[0062] Cutting tests 1 and 2 were carried out under the following conditions with the samples obtained, i.e. samples 1 to 12 of the invention and comparative examples 1 to 8, carried out. The cutting test 1 is a wear test to determine the To assess wear resistance, and cutting test 2 is a fracture test to assess fracture strength. The results of the respective cutting tests are shown in Table 5. Cutting test 1
[0063] Material of the workpiece: S45C round bar, Cutting speed: 200 m / min, Feed rate: 0.30 mm / rev Cutting depth: 2.0 mm Coolant: used Evaluation elements: A time at which a sample broke or a maximum flank wear width of 0.3 mm was defined as the end of the tool life, and the machining time to reach the end of the The tool lifespan was measured. Cutting test 2
[0064] Material of the workpiece: S45C round bar with four grooves Cutting speed: 120 m / min Feed rate: 0.30 mm / rev Cutting depth: 1.5 mm Coolant: Used, Evaluation elements: A time at which a sample broke or a maximum flank wear width of 0.3 mm was defined as the end of the tool life, and the machining time to reach the end of the To achieve tool lifespan, measurements were taken, and the number of vibrations that occurred until the end of the The tool lifespan was measured. Furthermore, the degree of damage was assessed when the number of [unclear - possibly "useful" or "expected"] [unclear - possibly "expected ... The vibrations reached 5,000 and were tested with a SEM. The number of vibrations was then measured. Increased by 15,000.
[0065] For the processing time to determine the end of the tool's service life in cutting test 1 (wear test) Evaluations with a rating of "A" for 41 minutes or more, and a rating of "B" for 30 minutes were used to determine the maximum time. or more and less than 41 minutes, and a rating of "C" was given for less than 30 minutes. Furthermore, regarding the number of vibrations until the end of the tool's service life in cutting test 2 (breakage test) Evaluations with a rating of "A" for 13,000 or more, rating "B" for 11,000 or more and 12,999 or less, and a rating of "C" was given for 10,999 or less. In such evaluations, "A" stands for excellent. 'B' stands for good and 'C' for poor, meaning that a sample with a higher number of 'As' or 'Bs' It has excellent cutting performance. The evaluation results are shown in Table 5. [Table 5] Cutting test Cutting test 2 1 Processing time Damage status after 5,000 number of shocks Quality (Min.) Vibrations (Vibrations) Sample 1 of the 41 A Normal wear and tear 14000 A invention Sample 2 of the 33 B Normal wear and tear 14800 A invention Sample 3 of the 37 B Normal wear and tear 13800 A invention Sample 4 of the 36 B Normal wear and tear 13600 A invention Sample 5 of the 42 A Normal wear 14200 A invention Sample 6 of the 36 B Normal wear and tear 12800 B invention Sample 7 of the 38 B Normal wear and tear 12200 B invention Sample 8 of the 42 A Normal wear 14400 A invention Sample 9 of the 34 B Normal wear and tear 14800 A invention Sample 10 of the 33 B Normal wear and tear 14600 A invention Sample 11 of the 30 B Normal wear and tear 15000 A invention Sample 12 of the 44 A Normal wear and tear 11400 B invention Comparison sample 1 22 C chipping 12400 B Comparison sample 2 18 C Normal wear 14200 A Comparative sample 3 42 A - 4000 C Comparison sample 4 27 C chipping 10000 C Comparison sample 5 43 A chipping 6000 C Comparative sample 6 22 C Normal wear 13400 A Comparative sample 7 14 C Normal wear 13800 A Comparison sample 8 20 C Normal wear 12000 B * In cutting test 2, the comparison example 3 chipped off after 4,000 vibrations.
[0066] The results in Table 5 show that each sample of the invention received a rating of "A" in both the wear test and the breakage test. or had "B". However, with regard to the evaluations carried out in the comparative examples, each Comparative example either in the wear test or in the breakage test or in both the rating ‘CC’.
[0067] It is evident from the above results that each sample of the invention has an excellent exhibits wear resistance and fracture resistance, resulting in a longer tool life. Industrial applicability
[0068] The coated cutting tool according to the present invention exhibits excellent wear resistance, This does not result in a reduction in fracture toughness, so the tool life is longer than when stationary. the technology can be extended, and from this point of view, the coated cutting tool possesses industrial applicability. List of reference symbols
[0069] 1: Substrate, 2: Lower layer, 3: Intermediate layer, 4: Upper layer, 5: Coating layer, 6: Coated Cutting tool
Claims
1. A coated cutting tool comprising: a substrate; and a coating formed on a surface of the substrate Coating layer, where: the coating layer comprises a lower layer, an intermediate layer and an upper layer in this order from the substrate side; the lower layer comprises one or more Ti compound layers comprising a Ti compound of Ti and an element of at least one type selected from the group consisting of C, N, O and B; and the intermediate layer an α-Al O layer comprising α-Al O; and the upper layer comprises a TiCN layer comprising TiCN 2 3 2 3 contains; an average thickness of the coating layer is 5.0 µm or more and 30.0 µm or less, and average thickness of the upper layer is 1.0 µm or more and 6.0 µm or less; in a cross-section perpendicular to the surface of the substrate, a ratio of grains with an aspect ratio of 2 or more and 10 or less of the grains in the TiCN layer forming the upper layer 60 area percent or more than 95 percent of the area or less; and in the grains with an aspect ratio of 2 or more and 10 or less from the grains in which the upper layer forming TiCN layer, a misalignment A satisfies a condition represented by the following formula (1): 40≤ RSA1≤90 where in the formula RSA is a ratio expressed in area percentage of a cross-sectional area of grains 1 which have a misalignment A of 0° or more and less than 10°, to a cross-sectional area of grains which have a misalignment A of 0° or more and 45° or less, and the misalignment A is an angle expressed in degree, which is defined by a normal to the surface of the substrate and a normal to a (111) orientation of the grains of the TiCN layer is formed in the upper layer.
2. Coated cutting tool according to claim 1, wherein the RSA is 60 area percent or more and 90 area percent 1 or less.
3. Coated cutting tool according to claim 1 or 2, wherein a ratio of the cross-sectional area of the grains having a misalignment A of 0° or more and less than 10°, a ratio of a cross-sectional area of the grains that have a misalignment of 10° or more and less than 20°, a ratio of a cross-sectional area of the Grains having a misalignment A of 20° or more and less than 30° and a ratio of Cross-sectional area of grains that have a misalignment of 30° or more and 45° or less to a Cross-sectional area of grains exhibiting a misalignment of 0° or more or 45° or less, each divided by RSA , RSA , 1 2 RSA and RSA, where RSA is the largest value, and RSA is the second largest of RSA , RSA , RSA and RSA 3 4 1 4 1 2 3 4 is.
4. Coated cutting tool according to one of claims 1 to 3, wherein an average thickness of the intermediate layer is 3.0 µm or more and 15.0 µm or less.
5. Coated cutting tool according to one of claims 1 to 4, wherein an average thickness of the lower layer is 3.0 µm or more and 15.0 µm or less.
6. Coated cutting tool according to one of claims 1 to 5, wherein the lower layer comprises at least one layer which is selected from the group consisting of a TiN layer containing TiN, a TiC layer containing TiC contains, a TiCN layer containing TiCN, a TiCNO layer containing TiCNO, a TiON layer containing TiON, and a TiB layer containing TiB. 2 2 7. Coated cutting tool according to one of claims 1 to 6, wherein the substrate is any of hard metal, Cermet, ceramic or a sintered body made of cubic boron nitride.
Citation Information
Patent Citations
Coated hard alloy
JP1996158052A
Cutting tool
JP2012196726A
Coated cutting tool insert with mt-cvd TiCN on tial(c,n)
JP2017530019A
JP000H08158052A
JP002012196726A