Methods for producing a rubber base compound and its use
The method of creating a filler-plasticizer precursor addresses the challenge of incorporating large amounts of filler in rubber mixtures by ensuring even distribution and preventing alcohol release, maintaining vulcanizate properties and safety.
Patent Information
- Application Number
- DE102019202029
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-02-15
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2039-02-15
AI Technical Summary
Existing methods face challenges in incorporating large amounts of filler into rubber mixtures without negatively affecting the properties of the vulcanizates, particularly with silica, which can lead to ignitable mixtures due to the silanization reaction releasing alcohol.
A method involving the creation of a filler-plasticizer precursor by mixing plasticizer oil and/or liquefied plasticizer resin with filler separately, then adding it to the rubber mixture in an internal mixer, with a specific ratio of silica to plasticizer oil ranging from 1:0.4 to 1:3, allowing for even distribution of filler without increasing plasticizer amounts.
Enables the homogeneous mixing of large amounts of filler without altering the target hardness of the mixture, reducing air entrainment, and preventing alcohol release that could cause ignitable mixtures, while maintaining vulcanizate properties.
Abstract
Description
[0001] The invention relates to a process for producing a rubber base mixture containing at least diene polymers, plasticizer oil and / or plasticizer resin, and more than 80 phr of filler in an internal mixer. Furthermore, the invention relates to the use of such a rubber base mixture for the production of vehicle tires.
[0002] Rubber compounds are typically manufactured by first producing a base compound in one or more mixing stages, containing all components (associated chemicals) except the vulcanization system (sulfur and vulcanization-influencing substances). The final compound is created by adding the vulcanization system in a final mixing stage. The final compound is further processed, for example, through an extrusion process, and formed into the appropriate shape. Further processing then takes place through vulcanization. Internal mixers (kneaders) are typically used to produce the base rubber compounds.
[0003] An alternative process for producing a rubber mixture is disclosed in DE 10 2015 225 985 A1, in which a low-viscosity premix is produced from a low-viscosity rubber component and filler and this premix is then mixed with a higher-viscosity rubber premix.
[0004] Today, a wide variety of rubber compounds are manufactured with a high proportion of fillers. These fillers contribute to the cost reduction of the compounds, while also having a decisive influence on a wide range of material properties of the compound and the resulting vulcanizate. Examples of fillers used in rubber compounds include carbon black, silica, aluminosilicates, chalk, starch, magnesium oxide, titanium dioxide, and rubber gels, as well as carbon nanotubes, graphite, graphene, and so-called "carbon-silica dual-phase fillers."
[0005] In order to reduce the rolling resistance of pneumatic vehicle tires, it has long been known to use silica as a filler, even in larger quantities, for the rubber compound of the tread.
[0006] If the filler content is increased in rubber compounds, the associated hardening of the rubber must be counteracted by adding plasticizer oil or plasticizer resin to achieve a specified hardness. Examples of suitable plasticizer oils include aromatic, naphthenic, or paraffinic mineral oil plasticizers, such as MES (mild extraction solvate) or RAE (residual aromatic extract) or TDAE (treated distillate aromatic extract), or rubber-to-liquid oils (RTL) or biomass-to-liquid oils (BTL), as well as vegetable oils, such as rapeseed oil, and liquid polymers.
[0007] Large amounts of filler are difficult to incorporate in an internal mixer in a single mixing step. If the filler is silica, silane coupling agents are often added to these base mixtures to bond the silica to the surrounding polymers. This poses the additional problem that the reaction between silica and the silane coupling agent (silanization reaction) releases alcohol, which can lead to flammable mixtures in the mixer or mixer shaft.
[0008] The invention is based on the object of providing a process for producing a rubber base mixture which allows the simple introduction of large amounts of filler without negatively affecting the properties of the vulcanizates from the mixture.
[0009] This task is solved by the fact that in the procedure of the type mentioned at the beginning - a rubber mixture reduced in or free of plasticiser oil and / or plasticiser resin and reduced in or free of filler is produced in the internal mixer, - at least plasticizer oil and / or liquefied plasticizer resin and the remaining filler are mixed separately in a mixing device for fluids to form a filler-plasticizer precursor - and then this filler-plasticizer precursor is added to the rubber mixture in the internal mixer and mixed in and - where the remaining filler is silica and the ratio of silica to plasticizer oil and / or liquefied plasticizer resin during premixing is 1:0.4 to 1:3.
[0010] By creating a filler-plasticizer precursor from plasticizer oil and / or liquefied plasticizer resin and filler, it is possible to even mix large amounts of filler evenly into a rubber compound. This is achieved without increasing the amount of plasticizer required to achieve the desired target hardness of a compound. The amount of plasticizer in the resulting (final) base compound can remain unchanged compared to a conventionally produced compound. The vulcanizate properties are not negatively affected. In addition, the process according to the invention offers the advantage that the amount of air entrapped in the filler and thus introduced into the rubber compound can be significantly reduced. The amount of free plasticizer not present on the filler or unwetted filler is reduced in the process according to the invention compared to a conventional process for producing a base compound.If the filler is used in granular form, its inner hollow structure is largely filled with plasticizer. If the plasticizer has already been mixed with other chemicals, such as a silane coupling agent, the inner surface of the filler also becomes accessible to other chemicals, such as silane coupling agents. This allows chemical reactions, such as the silanization reaction, to be carried out during pre-product production.
[0011] In the case of a rubber compound with reduced filler content in the internal mixer, the filler reduction can be reduced to 0 phr. However, it is advantageous if at least 20 phr of filler is mixed into the rubber compound in the internal mixer in the first step. The phr (parts per hundred parts of rubber by weight) used in this document is the standard quantity for compound formulations in the rubber industry. The dosage of the parts by weight of the individual substances is always based on 100 parts by weight of the total mass of all rubbers present in the compound. The mass of all rubbers present in the compound adds up to 100.
[0012] The mixing device for fluids can be a simple stirring device, but preferably a fluid mixer is used.
[0013] The rubber base mixture produced by the process according to the invention contains at least one diene polymer. Several diene polymers can also be used in blends. Diene rubbers include all rubbers with an unsaturated carbon chain that are derived at least partially from conjugated dienes.
[0014] The rubber base mixture can contain polyisoprene (IR, NR) as a diene rubber. This can be either cis-1,4-polyisoprene or 3,4-polyisoprene. However, the use of cis-1,4-polyisoprenes with a cis-1,4 content of > 90 wt.% is preferred. Such a polyisoprene can be obtained by stereospecific polymerization in solution with Ziegler-Natta catalysts or using finely divided lithium alkyls. Natural rubber (NR) is also such a cis-1,4-polyisoprene, and the cis-1,4 content in natural rubber is greater than 99 wt.%. Natural rubber (NR) is understood to be rubber that can be obtained by harvesting sources such as rubber trees (Hevea brasiliensis) or non-rubber tree sources (such as guayule or dandelion (e.g. Taraxagum koksaghyz)).
[0015] If the rubber base compound contains polybutadiene (BR) as the diene rubber, it can be cis-1,4-polybutadiene. The preferred material is cis-1,4-polybutadiene with a cis-1,4 content of greater than 90 wt.%, which can be produced, for example, by solution polymerization in the presence of rare earth catalysts.
[0016] Other diene rubbers that can be used include vinyl-polybutadienes and styrene-butadiene copolymers. Vinyl-polybutadienes and styrene-butadiene copolymers can be solution-polymerized (styrene)-butadiene copolymers (S-(S)BR) with a styrene content, based on the polymer, of approximately 0 to 45 wt.% and a vinyl content (content of 1,2-bonded butadiene, based on the total polymer) of 10 to 90 wt.%, which can be produced, for example, using lithium alkyls in an organic solvent. S-(S)BR can also be coupled and end-group modified. However, emulsion-polymerized styrene-butadiene copolymers (E-SBR) and blends of E-SBR and S-(S)BR can also be used. The styrene content of the E-SBR is approximately 15 to 50 wt.% and the types known from the prior art, which were obtained by copolymerization of styrene and 1,3-butadiene in aqueous emulsion, can be used.
[0017] The diene rubbers used in the mixture, especially the styrene-butadiene copolymers, can also be used in partially or fully functionalized form. The functionalization can be carried out with groups that can interact with the fillers used, especially with fillers containing OH groups. This can, for example, involve functionalization with hydroxyl groups and / or epoxy groups and / or siloxane groups and / or amino groups and / or phthalocyanine groups and / or carboxyl groups and / or silane sulfide groups. The diene rubbers can also be coupled additionally or alternatively.
[0018] In addition to the diene rubbers mentioned, the mixture may also contain other types of rubber, such as styrene-isoprene-butadiene terpolymer, butyl rubber, halobutyl rubber or ethylene-propylene-diene rubber (EPDM).
[0019] The rubber base mixture produced by the process according to the invention contains plasticizer oil and / or plasticizer resin. These can be different types in different quantities. Several types of plasticizer oils and plasticizer resins can also be present simultaneously. Examples of plasticizer oils that can be used include aromatic, naphthenic, or paraffinic mineral oil plasticizers, such as MES (mild extraction solvate) or RAE (residual aromatic extract) or TDAE (treated distillate aromatic extract), or rubber-to-liquid oils (RTL) or biomass-to-liquid oils (BTL), as well as vegetable oils, such as rapeseed oil, and liquid polymers. Plasticizer resins that melt up to a temperature of 140°C and can be absorbed by the filler in liquefied form can be used.
[0020] According to an advantageous development of the invention, plasticizer oil and / or liquefied plasticizer resin are preheated before being introduced into the fluid mixing device. This allows these substances to be mixed more quickly with the filler and penetrate into the pores of the filler.
[0021] The rubber base mixture contains more than 80 phr of filler. Preferably, the rubber base mixture contains 95 to 250 phr of filler. The process according to the invention has proven particularly advantageous for such highly filled rubber mixtures.
[0022] The filler can be a wide variety of materials, either individually or as mixtures. Examples of fillers used in rubber compounds include carbon black, silica, aluminosilicates, chalk, starch, magnesium oxide, titanium dioxide, or rubber gels, as well as carbon nanotubes, graphite, graphene, and so-called "carbon-silica dual-phase fillers." For example, the base mixture produced using this process can contain carbon black and silica in varying amounts. Different types of fillers can be used, for example, with different active surfaces. The fillers can be used in the form of granules or powder.
[0023] The ratio of filler to plasticizer oil and / or liquefied plasticizer resin during premixing is preferably adjusted such that the addition of the precursor changes the hardness (Shore A at room temperature) of the rubber base mixture, if the latter were produced without the inventive process with the addition of the filler-plasticizer precursor, by less than 5 hardness points. A ratio of filler to plasticizer oil and / or liquefied plasticizer resin that changes the hardness (Shore A at room temperature) of the rubber base mixture by less than 2 hardness points is particularly preferred.
[0024] When using pearlized fillers, it is also advantageous to adjust the ratio of filler to plasticizer oil and / or liquefied plasticizer resin during premixing to maintain the filler's pearling properties. Such a filler-plasticizer precursor can be easily metered and added using standard dosing systems for fillers.
[0025] The remaining filler, which is mixed into the filler-plasticizer precursor in a fluid mixing device, is silica. Silica is particularly difficult to incorporate into rubber compounds in large quantities without causing mixing problems.
[0026] To ensure good mixing of silica and plasticizer oil or liquefied plasticizer resin and problem-free mixing of the filler-plasticizer precursor into the remaining rubber mixture, the ratio of silica to plasticizer oil and / or liquefied plasticizer resin during premixing is 1:0.4 to 1:3.
[0027] If the rubber compound contains silica, silane coupling agents can be added to the compound to improve processability and bond the polar filler to the rubber. The silane coupling agents react with the surface silanol groups of the silica or other polar groups during mixing of the rubber or rubber compound (in situ) or even before the addition of the filler to the rubber as a pretreatment (premodification). All silane coupling agents known to those skilled in the art for use in rubber compounds can be used as silane coupling agents.Such coupling agents known from the prior art are bifunctional organosilanes that possess at least one alkoxy, cycloalkoxy, or phenoxy group as a leaving group on the silicon atom and that have, as another functionality, a group that, optionally after cleavage, can enter into a chemical reaction with the double bonds of the polymer. The latter group can be, for example, the following chemical groups: -SCN, -SH, -NH2, or -S. x- (where x = 2-8). Silane coupling agents that can be used include, for example, 3-mercaptopropyltriethoxysilane, 3-thiocyanatopropyltrimethoxysilane, or 3,3'-bis(triethoxysilylpropyl)polysulfides with 2 to 8 sulfur atoms, such as 3,3'-bis(triethoxysilylpropyl)tetrasulfide (TESPT), the corresponding disulfide, or mixtures of sulfides with 1 to 8 sulfur atoms with varying contents of the various sulfides. The silane coupling agents can also be added as a mixture with industrial carbon black, such as TESPT on carbon black (trade name X50S® from Evonik). Blocked mercaptosilanes, such as those known from WO 99 / 09036, can also be used as silane coupling agents. Silanes, such as those described in WO 2008 / 083241 A1, WO 2008 / 083242 A1, WO 2008 / 083243 A1, and WO 2008 / 083244 A1, can also be used. Examples of suitable compounds include:Silanes marketed in various versions under the name NXT® by Momentive, USA, or those marketed under the name VP Si 363® by Evonik Industries. Also suitable are so-called "silated core polysulfides" (SCPs), which are described, for example, in US 20080161477 A1 and EP 2 114 961 B1.
[0028] According to an advantageous development of the invention, a silane coupling agent is added to the process during the production of the filler-plasticizer precursor from plasticizer oil and / or liquefied plasticizer resin and silica. This allows at least partial bonding (hydrophobization) of the silane coupling agent to the silica to occur in a preliminary step.
[0029] The alcohol produced during this reaction can escape and be collected before it is mixed into the remaining rubber mixture and no longer causes problems in the internal mixer or mixer shaft due to the possible formation of flammable mixtures.
[0030] In order to carry out the hydrophobization reaction between silica and silane coupling agent as far as possible and to remove the resulting alcohol as completely as possible before mixing the filler-plasticizer precursor into the remaining rubber mixture, it is preferred if the production of the filler-plasticizer precursor takes place at a temperature of more than 80 °C, preferably more than 120 °C.
[0031] In addition to the substances already mentioned, the rubber base mixture can contain other additives commonly used in the rubber industry in the usual parts by weight. These additives include, for example, ageing inhibitors such as N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (6PPD), N-isopropyl-N'-phenyl-p-phenylenediamine (IPPD), 2,2,4-trimethyl-1,2-dihydroquinoline (TMQ) and other substances such as those known from J. Schnetger, Lexikon der Kautschuktechnik, 2nd edition, Hüthig Buch Verlag, Heidelberg, 1991, pp. 42-48, activators such as zinc oxide and fatty acids (e.g. stearic acid), waxes, tackifier resins such as hydrocarbon resins and rosin, and mastication aids such as ethylenediamine dimethyl ether. B. 2,2'-dibenzamidodiphenyl disulfide (DBD).
[0032] The rubber base compound produced by the process according to the invention is typically further processed into a finished compound. For this purpose, vulcanization chemicals such as sulfur, sulfur donors, or peroxides, and vulcanization-influencing substances such as vulcanization accelerators, vulcanization retarders, and vulcanization activators are added.
[0033] The rubber base compound produced by the process according to the invention can be used in a wide variety of products. These products include rubber bellows, conveyor belts, air springs, belts, hoses, printing blankets, vibration dampers, and shoe soles. However, the rubber base compound produced by the process according to the invention is preferably used for the production of vehicle tires, since large amounts of filler are often incorporated into rubber base compounds for vehicle tires.
[0034] The invention will now be explained in more detail using exemplary embodiments in conjunction with the following tables. The comparison mixtures are marked with Ref. or V, while the mixtures produced according to the invention are marked with E. In the tables, the Shore A hardness at room temperature was measured using a durometer according to DIN ISO 7619-1, and the rebound resilience at room temperature was measured according to DIN 53 512. Table 1: Silica mixture with TESPD Components Unit Ref. 1 Ref. 2 E1 E2 Diene polymer phr 100 100 100 100 Silica a phr 120 70 70 70 plasticizer oil b phr 50 0 0 0 Silane coupling agent c Filler-plasticizer precursor with silane phr 9 5 5 5 Coupling agent phr 0 0 52 104 Anti-aging agents phr 2 2 2 2 zinc oxide phr 2 2 2 2 Stearic acid phr 1 1 1 1 Process aids phr 2 2 2 2 Sulfur crosslinking system phr 5 4 4,5 5 Material properties Hardness at RT Shore A 70 70 70 70 Rebound resilience at RT % 23 40 30 23 a) Ultrasil ® VN3, Evonik Company b) MES-Öl c) TESPD, Bis(3-Triethoxysilylpropyl-)disulfide
[0035] Four rubber base compounds were produced in an internal mixer according to Table 1. Reference compound 1 contained 120 phr of silica. This required a long mixing time with multiple additions of silica to achieve the most homogeneous distribution of silica in the mixture.
[0036] For the mixtures in Table 1, which were mixed according to the process according to the invention, a filler-plasticizer precursor with silane coupling agent was first produced in a fluid mixer from 48 parts by weight of processing oil, 48 parts by weight of silica, and 4 parts by weight of silane coupling agent. This filler-plasticizer precursor was then added to the other mixture components in the internal mixer during the production of the rubber base mixture. The amounts of pure silica, silane coupling agent, and pure processing oil were reduced accordingly in the precursor stage so that the resulting rubber base mixtures contained 95 and 120 phr of silica, respectively. These rubber base mixtures were significantly easier to produce and process than the reference mixtures. The silica could be mixed homogeneously in a short time.
[0037] Subsequently, the rubber base compounds were further processed into finished compounds and used in the production of pneumatic vehicle tires. No differences in the vulcanizate properties were observed. For compounds E1 and E2, the vulcanizates had the same hardness despite different amounts of precursor. Table 2: Silica mixture with blocked mercaptosilane Components Unit Ref. 3 Ref. 4 E3 E4 Diene polymer phr 100 100 100 100 Silica a phr 120 70 70 70 plasticizer oil b phr 50 0 0 0 Silane coupling agent c Filler-plasticizer precursor with silane phr 10 6 6 6 Coupling agent phr 0 0 52 104 Anti-aging agents phr 2 2 2 2 zinc oxide phr 2 2 2 2 Stearic acid phr 1 1 1 1 Process aids phr 2 2 2 2 Sulfur crosslinking system phr 5 3 4 5 Material properties Hardness at RT Shore A 65 65 65 65 Rebound resilience at RT % 28 42 34 28 a) Ultrasil ® VN3, Evonik Company b) MES-Öl c) blocked mercaptosilane, NXT® silane from Momentive
[0038] Four rubber base compounds were produced in an internal mixer according to Table 2. Reference compound 3 contained 120 phr of silica. This required a long mixing time with multiple additions of silica to achieve the most homogeneous distribution of silica in the mixture.
[0039] For the mixtures in Table 2, which were mixed according to the process according to the invention, a filler-plasticizer precursor with silane coupling agent was first produced in a fluid mixer from 48 parts by weight of processing oil, 48 parts by weight of silica, and 4 parts by weight of silane coupling agent. This filler-plasticizer precursor was then added to the other mixture components in the internal mixer during the production of the rubber base mixture. The amounts of pure silica, silane coupling agent, and pure processing oil were reduced accordingly in the precursor stage, so that the resulting rubber base mixtures contained 95 and 120 phr of silica, respectively. These rubber base mixtures were significantly easier to produce and process than the reference mixtures. The silica could be mixed homogeneously in a short time.
[0040] Subsequently, the rubber base compounds were further processed into finished compounds and used in the production of pneumatic vehicle tires. No differences in the vulcanizate properties were observed. For compounds E3 and E4, the vulcanizates had the same hardness despite different amounts of precursor. Table 3: Carbon black mixture Components Unit Ref. 5 Ref. 6 V1 V2 Diene polymer phr 100 100 100 100 soot a phr 120 70 70 70 plasticizer oil b phr 50 0 0 0 Filler-plasticizer precursor phr 0 0 50 100 Anti-aging agents phr 2 2 2 2 zinc oxide phr 2 2 2 2 Stearic acid phr 1 1 1 1 Process aids phr 2 2 2 2 Sulfur crosslinking system phr 3 3 3 3 Material properties Hardness at RT Shore A 73 73 73 73 Rebound resilience at RT % 19 38 27 19 a) Soot N339 b) MES-Öl
[0041] Four rubber base compounds were produced in an internal mixer according to Table 3. Reference compound 5 contained 120 phr of carbon black. This required a long mixing time with multiple additions of the carbon black to achieve the most homogeneous distribution of the carbon black in the compound.
[0042] For the compounds shown in Table 3, which were mixed using a different process, a filler-plasticizer precursor consisting of 45 parts by weight of plasticizer oil and 55 parts by weight of carbon black was first produced in a fluid mixer. This filler-plasticizer precursor was then added to the other compound components in the internal mixer during the production of the rubber base compound. The amounts of carbon black and pure plasticizer oil were reduced accordingly in the precursor stage, so that the resulting rubber base compounds contained 97.5 and 125 phr of carbon black, respectively. These rubber base compounds were significantly easier to produce and process than the reference compounds. The carbon black could be mixed homogeneously in a short time.
[0043] Subsequently, the rubber base compounds were further processed into finished compounds and used in the production of pneumatic vehicle tires. No differences in the vulcanizate properties were observed. For compounds V1 and V2, the vulcanizates had the same hardness despite different amounts of precursor.
Claims
[1] Process for producing a rubber base mixture containing at least one diene polymer, at least plasticizer oil and / or plasticizer resin and more than 80 phr of filler in an internal mixer, wherein - a rubber mixture reduced in or free of plasticiser oil and / or plasticiser resin and reduced in or free of filler is produced in the internal mixer, - at least plasticizer oil and / or liquefied plasticizer resin and the remaining filler are mixed separately in a mixing device for fluids to form a filler-plasticizer precursor - and then this filler-plasticizer precursor is added to the rubber mixture in the internal mixer and mixed in, the remaining filler being silica and the ratio of silica to plasticizer oil and / or liquefied plasticizer resin during premixing being 1:0.4 to 1:
3. [2] A process for producing a rubber base mixture according to claim 1, characterized by that plasticizer oil and / or liquefied plasticizer resin are preheated before being introduced into the fluid mixing device. [3] Process for producing a rubber base mixture according to at least one of claims 1 or 2, characterized by that a silane coupling agent is added during the production of the filler-plasticizer precursor from plasticizer oil and / or liquefied plasticizer resin and silica. [4] A process for producing a rubber base mixture according to claim 3, characterized by that the production of the filler-plasticizer precursor takes place at a temperature of more than 80 °C, preferably more than 120 °C. [5] Use of the rubber base mixtures produced by the processes according to claims 1 to 4 for the production of vehicle tires.
Citation Information
Patent Citations
Method for producing a rubber compound
DE102015225985A1
Silated core polysulfides, their preparation and use in filled elastomer compositions
EP2114961B1
Silated core polysulfides, their preparation and use in filled elastomer compositions
US20080161477A1
Blocked mercaptosilane coupling agents for filled rubbers
WO1999009036A1
Tire compositions and components containing free-flowing filler compositions
WO2008083241A2